Adhesive tape, method for manufacturing hard disk drive, and hard disk drive sealing structure
The use of an adhesive tape with a multi-layer structure addresses the sealing challenges in hard disk drive manufacturing by providing effective moisture barrier and bending adhesion, enabling increased HDD capacity and improved sealing performance.
Patent Information
- Application Number
- PCT/JP2024/019705
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-29
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional hard disk drive manufacturing faces challenges in sealing helium gas within the housing as the number of platters increases, making it difficult to accommodate gaskets for effective sealing, and moisture ingress affects the performance of HAMR technology used in magnetic disk devices.
An adhesive tape with excellent barrier properties and L-shaped bending adhesion is used for sealing the hard disk drive casing from the outside, featuring a multi-layer structure with a foam-based first base layer, acrylic adhesive layers, and an inorganic layer, which provides high bending rigidity and water vapor barrier performance.
The adhesive tape ensures effective sealing of the hard disk drive casing, preventing moisture ingress and allowing for the expansion of HDD capacity without the need for internal gaskets, while maintaining high sealing performance and ease of manufacturing.
Smart Images

Figure JP2024019705_05122024_PF_FP_ABST
Abstract
Description
Adhesive tape, hard disk drive manufacturing method, and hard disk drive sealing structure
[0001] The present invention relates to an adhesive tape, a method for manufacturing a hard disk drive using the adhesive tape, and a hard disk drive sealing structure.
[0002] Adhesive tapes have a configuration in which an adhesive layer (pressure-sensitive adhesive layer) is provided on a substrate, and are widely used in a variety of applications for purposes such as joining, fixing, protecting, sealing, etc. Adhesive tapes are also used in electronic device applications, for example, to airtightly seal the internal space of a magnetic disk drive. Prior art that discloses adhesive tapes that can be used in such electronic device applications includes Patent Documents 1 to 4.
[0003] Japanese Patent Application Laid-Open No. 2019-163368 International Publication No. 2021 / 106997 International Publication No. 2020 / 218430 Japanese Patent Application Laid-Open No. 04-053841
[0004] Conventionally, during the manufacturing process of hard disk drives (hereinafter also referred to as "HDDs"), gaskets (sealants) have been installed inside the housing to seal helium gas. However, in order to achieve high capacity, the number of platters (disks coated with magnetic material) installed has tended to increase, making it difficult to provide space within the housing for gasket sealing. In response to this, consideration has been given to switching from gasket sealing from the inside of the housing to sealing with adhesive tape from the outside of the housing. In other words, if helium gas can be sealed by applying adhesive tape from the outside of the housing, space can be secured within the housing, making it possible to promote the expansion of HDD capacity. In this application, the adhesive tape is typically removed after the helium gas filling process.
[0005] When sealing from the outside of a housing with adhesive tape, from the viewpoint of improving sealing performance, it is necessary to fold the adhesive tape into an L-shape and attach it to the housing (L-shaped bend attachability). Furthermore, to achieve high productivity, it is desirable to seal the housing in one go by attaching the adhesive tape to one side of the housing, pressing a mold against it, and then folding and attaching the adhesive tape.
[0006] In recent years, magnetic disk devices employing HAMR (Heat Assist Magnetic Recording) have been studied to further increase capacity. HAMR is, in short, a technology that uses a laser beam to increase areal recording density. With this technology, the presence of moisture in the system causes laser attenuation, adversely affecting the write life. Therefore, with HAMR, it is desirable to prevent moisture from entering from the outside as much as possible.
[0007] The present invention aims to provide an adhesive tape that has excellent barrier properties and L-shaped bend application properties. It is also an object of the present invention to provide a method for manufacturing a hard disk drive that has excellent sealing properties even when the housing is sealed from the outside by using the adhesive tape. It is also an object of the present invention to provide a hard disk drive sealing structure that is sufficiently sealed even when the housing is sealed from the outside.
[0008] Disclosure 1 has a water vapor permeability of 7.5 g / (m 2 · day) or less, and the bending stiffness at 25 ° C. at a bending width of 2.0 mm in at least one of the MD direction and the TD direction is 1.0 N · mm 2 The present disclosure 2 is a pressure-sensitive adhesive tape having a flexural rigidity of 0.45 N mm at a bending width of 2.0 mm at 25°C in at least one of the MD and TD directions. 2 The pressure-sensitive adhesive tape of Disclosure 1, wherein the 10% heat shrinkage temperature is 95°C or less in at least one of the MD and TD directions. Disclosure 3 is the pressure-sensitive adhesive tape of Disclosure 1 or 2, wherein the pressure-sensitive adhesive tape has two or more layers, the two or more layers including at least a first base layer and a first pressure-sensitive adhesive layer, and all of the two or more layers of the pressure-sensitive adhesive tape satisfy a product of a tensile storage modulus and a thickness at 25°C of 200 MPa mm or less. Disclosure 5 is the pressure-sensitive adhesive tape of Disclosure 6, wherein the first base layer has a water vapor permeability of 40 g / (m 2The pressure-sensitive adhesive tape of Disclosure 4, wherein the first base layer has a 10% heat shrinkage temperature of 95°C or less in at least one of the MD and TD directions. Disclosure 6 is the pressure-sensitive adhesive tape of Disclosure 4 or 5, wherein the first base layer contains a foam. Disclosure 7 is the pressure-sensitive adhesive tape of Disclosure 6, wherein the foam contains a polyolefin foam. Disclosure 8 is the pressure-sensitive adhesive tape of Disclosure 4, 5, 6, or 7, wherein the first base layer has a 10% heat shrinkage temperature of 95°C or less in at least one of the MD and TD directions. Disclosure 9 is the pressure-sensitive adhesive tape of Disclosure 8, wherein the first base layer has a 10% heat shrinkage temperature of 95°C or less in the MD and TD directions. The present disclosure 10 provides a pressure-sensitive adhesive tape comprising the first base material layer, the first pressure-sensitive adhesive layer, the second base material layer, and the second pressure-sensitive adhesive layer in this order, the first base material layer containing a foam, and the first base material layer having a water vapor transmission rate of 40 g / (m 2The pressure-sensitive adhesive tape of Disclosure 4, 5, 6, 7, 8, or 9, wherein the product of the average values of the tensile storage moduli at 25°C in the MD and TD directions and the thickness of the first base material layer is 50 MPa mm or less, and the second base material layer has a 10% heat shrinkage temperature of 95°C or less in at least one of the MD and TD directions. Disclosure 11 is the pressure-sensitive adhesive tape of Disclosure 4, 5, 6, 7, 8, 9, or 10, further having an inorganic layer. Disclosure 12 is the pressure-sensitive adhesive tape of Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, or 11, wherein the thickness is 0.20 mm or more. Disclosure 13 is a method for manufacturing a hard disk drive having a main body portion equipped with a hard disk and a lid portion, the method comprising the step of sealing the hard disk drive by applying the adhesive tape of Disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12 to the main body portion and the lid portion. Disclosure 14 is a method for manufacturing a hard disk drive according to Disclosure 13, wherein the step of sealing the hard disk drive comprises folding the adhesive tape from the lid portion to the main body portion and applying it, and then thermally shrinking the adhesive tape. Disclosure 15 is a method for manufacturing a hard disk drive according to Disclosure 14, wherein the main body portion includes a main body bottom portion and a main body sidewall portion protruding upward from an outer periphery of the main body bottom portion, and the lid portion is configured to be attached to the main body sidewall portion of the main body portion, and the step of sealing the hard disk drive comprises step (I) of folding the adhesive tape from the lid portion to the main body sidewall portion and applying it, and step (II) of thermally shrinking the adhesive tape after step (I). Disclosure 16 is a method for manufacturing a hard disk drive according to Disclosure 15, wherein the main body has a main body corner on a surface of the main body side wall to which the lid is attached, and the lid has a lid corner that contacts the main body corner, and in step (I), the adhesive tape is folded and attached from at least the lid corner to the main body corner, and in step (II), the portion of the adhesive tape that is attached from the lid corner to the main body corner is thermally shrunk.Disclosure 17 is the method for manufacturing a hard disk drive according to Disclosure 15 or 16, wherein in step (I), the lid is attached to the main body sidewall, the adhesive tape is attached to the outer peripheral edge of the upper surface of the lid so that a portion of the adhesive tape is located outside the outer peripheral edge of the upper surface of the lid, a mold including a mold bottom and a mold sidewall protruding downward from the outer peripheral edge of the mold bottom is pressed against the main body sidewall so that the upper surface of the lid faces the lower surface of the mold bottom, the adhesive tape is folded so that the portion of the adhesive tape that is not in contact with the upper surface of the lid is located between the mold sidewall and the main body sidewall, and the adhesive tape is attached to the main body sidewall, thereby bonding the main body and the lid. Disclosure 18 is the method for manufacturing a hard disk drive according to Disclosure 17, wherein the mold is heated to 35°C or higher and 60°C or lower when the upper surface of the lid is pressed against the lower surface of the mold bottom so that the upper surface of the lid faces the lower surface of the mold bottom. Disclosure 19 is the method for manufacturing a hard disk drive according to Disclosures 15, 16, 17, or 18, wherein in step (I), the adhesive tape is frame-shaped and has a shape corresponding to the outer peripheral edge of the upper surface of the lid, and the frame-shaped adhesive tape is attached so that the outer frame is positioned outside the outer peripheral edge of the upper surface of the lid. Disclosure 20 is the method for manufacturing a hard disk drive according to Disclosures 15, 16, 17, 18, or 19, wherein in step (II), the adhesive tape is heat-shrunk by 10% or more in at least one of the MD and TD directions, and the temperature of the adhesive tape is 95°C or less. Disclosure 21 is a hard disk drive sealing structure including a main body and a lid, the main body and the lid being fixed together via heat-shrunk adhesive tape. The present invention will be described in detail below.
[0009] The present inventors have investigated adjusting the water vapor permeability, bending rigidity in at least one of the MD and TD directions, 180° peel strength from SUS, and thickness of a pressure-sensitive adhesive tape to each fall within an appropriate range. As a result, they have found that a pressure-sensitive adhesive tape with excellent barrier properties and L-shaped bend adhesion can be obtained, leading to the completion of the present invention. In this specification, the term "L-shaped" refers to a bent state, and does not only mean a state bent at a right angle, but also includes a state bent two or more times.
[0010] The pressure-sensitive adhesive tape of the present invention has an upper limit of water vapor permeability of 7.5 g / m at 40°C and 90% RH. 2 The water vapor permeability of the pressure-sensitive adhesive tape of the present invention at 40°C and 90% RH is 7.5 g / (m 2 ·day) or less, the resulting pressure-sensitive adhesive tape will have excellent barrier properties. The preferred upper limit of the water vapor permeability of the pressure-sensitive adhesive tape of the present invention at 40°C and 90% RH is 5.0 g / (m 2 ·day), and a more preferable upper limit is 3.0 g / (m 2 ·day), and a more preferable upper limit is 2.0 g / (m 2 ·day), and a particularly preferred upper limit is 1.0 g / (m 2 ·day), and the most preferred upper limit is 0.5 g / (m 2 The pressure-sensitive adhesive tape of the present invention has no particular lower limit for the water vapor transmission rate at 40°C and 90% RH, but it is substantially 0.1 g / (m 2 In this specification, the water vapor permeability at 40°C and 90% RH can be measured, for example, in accordance with JIS K 7129 Method B, by measuring the water vapor permeability in the thickness direction of the pressure-sensitive adhesive tape under conditions of 40°C and 90% RH using a water vapor permeability measuring device (such as "PERMATRAN-W" manufactured by MOCON Corporation).
[0011] Methods for adjusting the water vapor permeability of the pressure-sensitive adhesive tape of the present invention at 40°C and 90% RH to within the above-mentioned range include, for example, a method for adjusting the water vapor permeability of the substrate layer or adhesive layer of the pressure-sensitive adhesive tape described below, and a method for adding another substrate layer or adhesive layer.
[0012] The pressure-sensitive adhesive tape of the present invention has a bending stiffness (hereinafter sometimes simply referred to as "bending stiffness") at 25°C at a bending width of 2.0 mm in at least one of the MD and TD directions of 1.0 N mm 2 The pressure-sensitive adhesive tape of the present invention has a bending rigidity of 1.0 N mm in at least one of the MD and TD directions. 2 When the bending rigidity of the pressure-sensitive adhesive tape of the present invention is 1.0 N mm or less, the pressure-sensitive adhesive tape is likely to be maintained in a folded state, and peeling from the adherend can be suppressed even when the pressure-sensitive adhesive tape is folded and applied, and the pressure-sensitive adhesive tape obtained has excellent L-shaped bending adhesion properties. 2 When the pressure-sensitive adhesive tape of the present invention has a bending rigidity of 0.45 N mm or less, the pressure-sensitive adhesive tape is less likely to be inhibited from heat shrinking, as will be described later, and is more likely to shrink at a lower temperature. 2 , and a more preferable upper limit is 0.30 N mm 2 The preferred lower limit of the bending rigidity of the pressure-sensitive adhesive tape of the present invention in at least one of the MD and TD directions is 0.003 N mm 2 The pressure-sensitive adhesive tape of the present invention has a bending rigidity of 0.003 N mm in at least one of the MD and TD directions. 2 A more preferable lower limit of the bending rigidity of the pressure-sensitive adhesive tape of the present invention in at least one of the MD and TD directions is 0.006 N mm 2 , and a more preferable lower limit is 0.01 N mm 2In this specification, the "MD direction" means the machine direction, i.e., the flow direction during production, and the "TD direction" means the transverse direction, i.e., the direction perpendicular to the MD direction. When the flow direction during production is unknown, the longitudinal direction of the pressure-sensitive adhesive tape is taken as the MD direction, and when the pressure-sensitive adhesive tape is square or the like and has no longitudinal direction, the direction of any one side is taken as the MD direction. The bending rigidity of the pressure-sensitive adhesive tape of the present invention is calculated by the following formula (1) as the bending rigidity when the pressure-sensitive adhesive tape is folded with the outermost pressure-sensitive adhesive layer on the inside as shown in the right diagram of Figure 1.
[0013]
[0014] In the above formula (1), E i is the tensile storage fault modulus (MPa) at 25°C of the ith layer from the innermost surface, I i is the second moment of area of the ith layer from the outermost surface (mm 4 ), b is the bending width (mm), h i represents the total thickness (mm) from the innermost layer to the i-th layer, and λ represents the distance (mm) from the neutral axis of the pressure-sensitive adhesive tape to the outermost surface, calculated by the following formula (2).
[0015]
[0016] In the above formula (2), E i is the tensile storage fault modulus (MPa) at 25°C of the ith layer from the innermost surface, and h i is the total thickness from the innermost layer to the i-th layer (mm), t i represents the thickness (mm) of the ith layer from the innermost surface.
[0017] Methods for adjusting the bending rigidity of the adhesive tape of the present invention to fall within the above-mentioned range include, for example, using an adhesive tape having a substrate, adjusting the thickness of the adhesive tape, adjusting the tensile storage modulus of each layer constituting the adhesive tape, such as the substrate layer and adhesive layer, changing the thickness of each layer constituting the adhesive tape, and changing the stacking order of each layer constituting the adhesive tape.
[0018] The pressure-sensitive adhesive tape of the present invention has a 180° peel strength against SUS (hereinafter sometimes simply referred to as "180° peel strength") at 23°C of 5.0 N / 25 mm as a lower limit. When the pressure-sensitive adhesive tape of the present invention has a 180° peel strength of 5.0 N / 25 mm or more, the resulting pressure-sensitive adhesive tape has high adhesive strength and improved L-shaped bend application properties. The pressure-sensitive adhesive tape of the present invention preferably has a lower limit of 7.0 N / 25 mm, more preferably 9.0 N / 25 mm as a lower limit. Furthermore, the pressure-sensitive adhesive tape of the present invention preferably has an upper limit of 30 N / 25 mm as a upper limit. When the pressure-sensitive adhesive tape of the present invention has a 180° peel strength of 30 N / 25 mm or less, the resulting pressure-sensitive adhesive tape has excellent removability and can be more suitably used in the HDD manufacturing method described below. The pressure-sensitive adhesive tape of the present invention more preferably has an upper limit of 20 N / 25 mm, even more preferably 10 N / 25 mm as an upper limit. The 180° peel strength of the pressure-sensitive adhesive tape of the present invention against SUS at 23°C can be measured, for example, by the following method. First, the pressure-sensitive adhesive tape is cut into a flat rectangular shape measuring 25 mm wide and 150 mm long, and the tape is pressed against a SUS304 plate (washed with ethanol and then wiped dry) with a surface finish of 2B as specified in JIS G 4305 by rolling the tape back and forth twice at a speed of 10 mm / sec using a 2 kg rubber roller at 23°C and 50% RH. The tape is then allowed to stand for 20 minutes at 23°C and 50% RH. Then, a 180° peel test is performed in accordance with JIS Z 0237 using a tensile tester (Shimadzu Corporation, "AGS-X," etc.) at 23°C, 50% RH, and a peel speed of 300 mm / min, thereby peeling the pressure-sensitive adhesive tape from the SUS plate.
[0019] Methods for adjusting the 180° peel strength of the pressure-sensitive adhesive tape of the present invention from SUS at 23°C within the above-mentioned range include, for example, changing the adhesive in the pressure-sensitive adhesive layer, adjusting the thickness of the pressure-sensitive adhesive tape, and changing the material of the base material layer.
[0020] The pressure-sensitive adhesive tape of the present invention has a lower limit of thickness of 0.20 mm. Having a thickness of 0.20 mm or more improves adhesion to an adherend, provides sufficient adhesion when a mold is pressed against the tape and the tape is folded for application, and is also advantageous in ensuring the barrier properties of the resulting pressure-sensitive adhesive tape. The pressure-sensitive adhesive tape of the present invention preferably has a lower limit of thickness of 0.30 mm, more preferably 0.40 mm. The pressure-sensitive adhesive tape of the present invention preferably has an upper limit of thickness of 2.4 mm. Having a thickness of 2.4 mm or less makes it easy to reduce bending rigidity. The pressure-sensitive adhesive tape of the present invention more preferably has an upper limit of thickness of 1.5 mm, even more preferably 1.0 mm. In this specification, examples of methods for measuring thickness include a method using a dial thickness meter (such as the "ABS Digimatic Indicator" manufactured by Mitutoyo Corporation) and a method using a digital microscope (such as the "VHX-900" manufactured by Keyence Corporation) to photograph the cross section of the adhesive tape and measure the thickness of each layer of the adhesive tape from the photographed image.
[0021] The pressure-sensitive adhesive tape of the present invention preferably has two or more layers. By having two or more layers, the pressure-sensitive adhesive tape of the present invention has an appropriate thickness, which improves adhesion to an adherend and provides more excellent barrier properties.
[0022] The two or more layers preferably include at least a first base material layer and a first pressure-sensitive adhesive layer. By having the pressure-sensitive adhesive tape of the present invention have the first base material layer and the first pressure-sensitive adhesive layer, the obtained pressure-sensitive adhesive tape has appropriate stiffness and is therefore more excellent in L-shaped bending application property.
[0023] The upper limit of the product of the tensile storage modulus and thickness at 25°C (hereinafter sometimes simply referred to as the "product of tensile storage modulus and thickness") of all of the two or more layers of the pressure-sensitive adhesive tape of the present invention is preferably 200 MPa mm. When the product of the tensile storage modulus and thickness of all of the two or more layers of the pressure-sensitive adhesive tape of the present invention satisfies a value of 200 MPa mm or less, the flexibility of the resulting pressure-sensitive adhesive tape is further improved, and the L-shaped bend application property is further improved. A more preferred upper limit of the product of the tensile storage modulus and thickness is 50 MPa mm, and an even more preferred upper limit is 25 MPa mm. There is no particular preferred lower limit for the product of the tensile storage modulus and thickness, but the lower limit is substantially about 0.01 MPa mm. When the layer for which the product of the tensile storage modulus and thickness is calculated is a substrate layer, the average value of the tensile storage modulus at 25°C in the MD and TD directions is used as the tensile storage modulus at 25°C.
[0024] The first substrate layer preferably contains a foam. By containing a foam, the first substrate layer has appropriate flexibility, which makes it easier to adjust the bending rigidity of the pressure-sensitive adhesive tape of the present invention within the above-mentioned range, thereby further improving L-shaped bend application properties. In addition, it makes it easier to adjust the tensile storage modulus of the first substrate, which will be described later, within an appropriate range.
[0025] Examples of the foam include polyurethane foam, polyolefin foam, rubber foam, acrylic foam, etc. Among these, polyolefin foam is preferred from the viewpoint that the water vapor permeability of the first base layer described below at 40°C and 90% RH can be easily adjusted to an appropriate range, thereby further improving the barrier properties of the resulting pressure-sensitive adhesive tape, and that the first base layer has appropriate flexibility, making it easy to adjust the bending rigidity of the resulting pressure-sensitive adhesive tape to the above-mentioned range, thereby further improving L-shaped bend application properties. That is, the foam preferably contains polyolefin foam.
[0026] Examples of the polyolefin foam include foams containing polyethylene resin, polypropylene resin, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, etc. Among these, foams containing polyethylene resin are preferred from the viewpoint of providing the first base layer with appropriate flexibility. Specific examples of the polyethylene resin include polyethylene resins polymerized with a polymerization catalyst such as a Ziegler-Natta compound, a metallocene catalyst, or a chromium oxide compound, and among these, polyethylene resins polymerized with a metallocene catalyst are preferred from the viewpoint of improving the removability due to the improved strength of the polyethylene resin.
[0027] Examples of the metallocene catalyst include bis(cyclopentadienyl) metal complexes having a structure in which a transition metal is sandwiched between π-electron unsaturated compounds. More specifically, examples include compounds in which one or more cyclopentadienyl rings or analogs thereof are present as ligands on a tetravalent transition metal such as titanium, zirconium, nickel, palladium, hafnium, or platinum. Such metallocene catalysts have uniform active site properties, with each active site having the same activity. Polymers synthesized using metallocene catalysts have high uniformity in molecular weight, molecular weight distribution, composition, composition distribution, etc., so when a sheet containing a polymer synthesized using a metallocene catalyst is crosslinked, crosslinking proceeds uniformly.
[0028] Examples of the ligand include cyclic compounds such as a cyclopentadienyl ring and an indenyl ring. These cyclic compounds may be substituted with a hydrocarbon group, a substituted hydrocarbon group, a hydrocarbon-substituted metalloid group, or the like. Examples of the hydrocarbon group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an n-hexyl group, a 2-ethylhexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and a phenyl group. Alternatively, an oligomer of the cyclic compound may be used as the ligand. In addition to π-electron unsaturated compounds, monovalent anionic ligands such as chlorine and bromine, or divalent anionic chelating ligands, hydrocarbons, alkoxides, arylamides, aryloxides, amides, arylamides, phosphides, arylphosphides, and the like may also be used.
[0029] Examples of metallocene catalysts containing a tetravalent transition metal or a ligand include cyclopentadienyltitanium tris(dimethylamide), methylcyclopentadienyltitanium tris(dimethylamide), bis(cyclopentadienyl)titanium dichloride, and dimethylsilyltetramethylcyclopentadienyl-t-butylamide zirconium dichloride.
[0030] The metallocene catalyst, when combined with a specific cocatalyst (promoter), acts as a catalyst during the polymerization of various olefins. Examples of the cocatalyst include methylaluminoxane (MAO) and boron-based compounds. The ratio of the cocatalyst to the metallocene catalyst is preferably 100,000 to 1,000,000 moles, and more preferably 50 to 5,000 moles.
[0031] Examples of the polymerized polyethylene resin include low-density polyethylene (density: 0.930 g / cm 3 less than 0.930 g / cm 3 Above, 0.942g / cm 3 less than 0.942 g / cm 3or more). As the low-density polyethylene resin, linear low-density polyethylene is preferred. The linear low-density polyethylene is more preferably a linear low-density polyethylene obtained by copolymerizing ethylene (for example, 75% by mass or more, preferably 90% by mass or more, based on the total amount of monomers) with a small amount of an α-olefin as needed. Specific examples of the α-olefin include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene. Among these, α-olefins having 4 to 10 carbon atoms are preferred from the viewpoint of low tensile storage modulus and productivity. The density of the polyethylene resin, for example, the linear low-density polyethylene described above, is 0.870 to 0.925 g / cm from the viewpoint of flexibility. 3 is preferably 0.890 to 0.925 g / cm 3 More preferably, 0.910 to 0.925 g / cm 3 As the polyethylene resin, a plurality of polyethylene resins may be used, and a polyethylene resin having a density outside the above-mentioned range may be added. Furthermore, from the viewpoint of barrier properties, it is preferable to use high-density polyethylene or a combination of high-density polyethylene and low-density polyethylene.
[0032] Examples of the polypropylene resin include homopolypropylene and propylene-α-olefin copolymers containing 50% by mass or more of propylene. Specific examples of the α-olefins constituting the propylene-α-olefin copolymers include ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene. Among these, α-olefins having 6 to 12 carbon atoms are preferred from the viewpoints of barrier properties and productivity. These polypropylene resins may be used alone or in combination of two or more.
[0033] The lower limit of the foam content in the first substrate layer is preferably 70% by mass, more preferably 80% by mass, and even more preferably 90% by mass.
[0034] The first substrate layer may further contain additives such as a heat stabilizer, a colorant, a flame retardant, an antistatic agent, a bulking agent, a filler having a function of enhancing barrier properties, a layered clay mineral, etc. The first substrate layer may also be crosslinked by ionizing radiation or the like.
[0035] The first base layer can be produced, for example, by feeding a foaming composition containing a polyethylene resin and a foaming agent into an extruder, melt-kneading the composition, and then extruding the composition from the extruder.
[0036] From the viewpoint of productivity, thermally decomposable foaming agents are preferred as the foaming agent. Organic and inorganic foaming agents can be used as the thermally decomposable foaming agent. Examples of the organic foaming agent include azo compounds such as azodicarbonamide, azodicarboxylic acid metal salts (e.g., barium azodicarboxylate), and azobisisobutyronitrile; nitroso compounds such as N,N'-dinitrosopentamethylenetetramine; hydrazine derivatives such as hydrazodicarbonamide, 4,4'-oxybis(benzenesulfonylhydrazide), and toluenesulfonylhydrazide; and semicarbazide compounds such as toluenesulfonylsemicarbazide. Examples of the inorganic foaming agent include ammonium carbonate, sodium carbonate, ammonium bicarbonate, sodium bicarbonate, ammonium nitrite, sodium borohydride, and anhydrous monosodium citrate. Among these, azo compounds are preferred, and azodicarbonamide is more preferred, from the viewpoints of obtaining fine bubbles and of economy and safety. Such thermal decomposition type foaming agents may be used alone or in combination of two or more.
[0037] The foamable resin composition may contain a decomposition temperature regulator such as zinc oxide, zinc stearate, or urea, in order to lower the decomposition temperature or increase the decomposition rate of the thermally decomposable foaming agent.
[0038] The foamable resin composition may contain an antioxidant, such as a phenol-based antioxidant such as 2,6-di-t-butyl-p-cresol, a sulfur-based antioxidant, a phosphorus-based antioxidant, or an amine-based antioxidant.
[0039] The density of the first substrate layer has a preferred lower limit of 0.01 kg / m 3 and the preferred upper limit is 0.8 kg / m 3 When the density of the first base material layer is within the above range, the resulting pressure-sensitive adhesive tape has better barrier properties and better L-shaped bending application properties. A more preferable lower limit of the density of the first base material layer is 0.05 kg / m 3 , and a more preferable upper limit is 0.6 kg / m 3 , and a more preferable lower limit is 0.1 kg / m 3 , and a more preferable upper limit is 0.3 kg / m 3 The density of the first base layer means an apparent density, and can be measured, for example, in accordance with JIS K 7222 using an underwater displacement electronic pycnometer (for example, the "EDM series" manufactured by AS ONE Corporation).
[0040] Examples of methods for adjusting the density of the first base material layer include a method of adjusting the type or content of the foaming agent contained in the foaming composition, and a method of adjusting the foaming temperature.
[0041] The water vapor permeability of the first substrate layer at 40°C and 90% RH is preferably 40 g / (m 2 The water vapor permeability of the first substrate layer at 40°C and 90% RH is 40 g / (m 2 A more preferable upper limit of the water vapor permeability of the first base layer at 40°C and 90% RH is 21 g / (m 2 ·day), and a more preferable upper limit is 1.0 g / (m 2 Furthermore, there is no particular lower limit to the water vapor transmission rate of the first substrate layer at 40°C and 90% RH, but it is substantially 0.1 g / (m 2 ・day) is the lower limit.
[0042] Examples of methods for adjusting the water vapor permeability of the first substrate layer at 40°C and 90% RH include changing the thickness of the substrate layer, changing the material of the substrate layer, changing the expansion ratio when the substrate layer is a foam, incorporating an inorganic mineral into the substrate layer, and laminating an inorganic layer on the substrate layer. The expansion ratio is determined by measuring the apparent density and calculating the reciprocal thereof. The apparent density can be measured in accordance with JIS K 7222.
[0043] The first base layer has a 10% heat shrinkage temperature of preferably 95°C or lower in at least one of the MD and TD directions. When the first base layer has a 10% heat shrinkage temperature of 95°C or lower in at least one of the MD and TD directions, the resulting pressure-sensitive adhesive tape can be more suitably used in the HDD manufacturing method described below. The first base layer has a more preferred upper limit of 80°C, an even more preferred upper limit of 70°C, and a particularly preferred upper limit of 60°C in at least one of the MD and TD directions. It is more preferred that the first base layer has a 10% heat shrinkage temperature of 95°C or lower in the MD and TD directions. Furthermore, the first base layer has a preferred lower limit of 40°C in at least one of the MD and TD directions. When the 10% heat shrinkage temperature in at least one of the MD and TD directions of the first base layer is 40°C or higher, the pressure-sensitive adhesive tape can be stored at room temperature. A more preferable lower limit of the 10% heat shrinkage temperature in at least one of the MD and TD directions of the first base layer is 50°C, and an even more preferable lower limit is 60°C. In this specification, the 10% heat shrinkage temperature can be measured by the following method. That is, first, a test piece is prepared by cutting the base layer or pressure-sensitive adhesive tape to be measured into a planar square shape having a width of 50 mm and a length of 50 mm. The obtained test piece is immersed in approximately 1 L of water preheated to 50°C for 10 seconds, and then air-cooled to room temperature, and the width and length of the test piece are measured. The measured width and length are used to calculate the heat shrinkage rate at 50°C in the MD and TD directions, respectively, according to the following formula (3): Similarly, the sample was immersed in water at 60°C, 70°C, 80°C, 90°C, and 100°C, and then cooled to room temperature. The width and length were measured, and the heat shrinkage rates in the MD and TD directions at 60°C, 70°C, 80°C, 90°C, and 100°C were calculated using the following formula (3).Regarding the obtained heat shrinkage rate, if the heat shrinkage rate at 50°C exceeds 10%, the 10% heat shrinkage temperature is set to less than 50°C, and if the heat shrinkage rate at 100°C is less than 10%, the 10% heat shrinkage temperature is set to more than 100°C. In other cases, it is assumed that the temperature and heat shrinkage rate are proportional between the maximum temperature at which the heat shrinkage rate is less than 10% and the minimum temperature at which the heat shrinkage rate exceeds 10%, and the 10% heat shrinkage temperature is calculated. Heat shrinkage rate (%) = [(L. 0 -L 1 ) / L 0 ]×100 (3) (L 0 : Dimension of adhesive tape before immersion in heated water, L 1 : Dimensions of adhesive tape immersed in heated water and then cooled to room temperature)
[0044] Examples of methods for adjusting the 10% heat shrinkage temperature of the first base material layer include a method of changing the stretching ratio and a method of changing the material of the base material layer.
[0045] The first base layer has a tensile storage modulus at 25°C in at least one of the MD and TD directions of 0.1 MPa as a lower limit and 200 MPa as a preferred upper limit. The tensile storage modulus at 25°C in at least one of the MD and TD directions of the first base layer is within the above range, making it easier to adjust the product of the average tensile storage modulus in the MD and TD directions of the first base layer and the thickness within the above range, thereby further improving the L-shaped bend application property of the resulting pressure-sensitive adhesive tape. The tensile storage modulus at 25°C in at least one of the MD and TD directions of the first base layer is more preferably 1 MPa as a lower limit and 80 MPa as an upper limit, and even more preferably 5 MPa as a lower limit and 40 MPa as an upper limit. The tensile storage modulus of the first base layer at 25°C can be obtained by measurement using a dynamic viscoelasticity measuring device (manufactured by IT Measurement & Control Co., Ltd., "DVA-200") under the following conditions: measurement mode: tension, 25°C, frequency: 1 Hz, heating rate: 5°C / min, temperature range: 0 to 100°C, and set strain: 0.1%.
[0046] Examples of methods for adjusting the tensile storage modulus at 25° C. of the first base material layer include a method of changing the expansion ratio and a method of changing the material of the base material layer.
[0047] The thickness of the first base layer is preferably 100 μm at its lower limit and 2000 μm at its upper limit. When the thickness of the first base layer is within the above range, the resulting pressure-sensitive adhesive tape has better barrier properties and better L-shaped bend application properties. The thickness of the first base layer is more preferably 150 μm at its lower limit and 1000 μm at its upper limit, even more preferably 200 μm at its lower limit and 500 μm at its upper limit.
[0048] Examples of the first pressure-sensitive adhesive layer include pressure-sensitive adhesive layers containing pressure-sensitive adhesives such as acrylic pressure-sensitive adhesives, rubber-based pressure-sensitive adhesives, urethane pressure-sensitive adhesives, and silicone pressure-sensitive adhesives. Among these, acrylic pressure-sensitive adhesives are preferred from the viewpoint of further improving the L-shaped bending adhesion of the resulting pressure-sensitive adhesive tape. Furthermore, rubber-based pressure-sensitive adhesives are preferred from the viewpoint of easily reducing the water vapor permeability.
[0049] The acrylic pressure-sensitive adhesive contains a (meth)acrylic copolymer. The (meth)acrylic copolymer preferably contains a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 18 carbon atoms at the ester terminal. Examples of the (meth)acrylic acid alkyl ester having an alkyl group having 1 to 18 carbon atoms at the ester terminal include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, tridecyl methacrylate, and stearyl (meth)acrylate. Of these, n-butyl acrylate and 2-ethylhexyl acrylate are preferred from the viewpoint of ease of controlling adhesive strength. These (meth)acrylic acid alkyl esters may be used alone or in combination of two or more. In this specification, "(meth)acrylic" refers to acrylic or methacrylic.
[0050] The (meth)acrylic copolymer may, if necessary, contain a structural unit derived from another copolymerizable polymerizable monomer. Examples of the other copolymerizable polymerizable monomer include hydroxyalkyl (meth)acrylate, glycerin dimethacrylate, glycidyl (meth)acrylate, 2-methacryloyloxyethyl isocyanate, (meth)acrylic acid, itaconic acid, maleic anhydride, crotonic acid, maleic acid, and fumaric acid. Among these, functional monomers having a polar functional group such as a hydroxyl group or a carboxy group are preferred, as they form a crosslinked structure with a crosslinking agent, making it easier to adjust the gel fraction of the first pressure-sensitive adhesive layer. These other copolymerizable polymerizable monomers may be used alone, or two or more of them may be used in combination.
[0051] The weight-average molecular weight (Mw) of the (meth)acrylic copolymer has a preferred lower limit of 300,000 and a preferred upper limit of 2,000,000. When the weight-average molecular weight of the (meth)acrylic copolymer is within the above range, the first pressure-sensitive adhesive layer has an appropriate hardness and sufficient cohesive force, and the resulting pressure-sensitive adhesive tape has higher adhesive strength, thereby further improving L-shaped bending adhesion. The weight-average molecular weight of the (meth)acrylic copolymer is more preferably 500,000 in lower limit, 1,400,000 in upper limit, 600,000 in even more preferred limit, and 1,300,000 in even more preferred limit.
[0052] The ratio of the weight-average molecular weight (Mw) to the number-average molecular weight (Mn) of the (meth)acrylic copolymer (molecular weight distribution, Mw / Mn) preferably has a lower limit of 1.05 and an upper limit of 10.0. When the molecular weight distribution (Mw / Mn) of the (meth)acrylic copolymer is within the above range, the content of low-molecular-weight components and the like is reduced, thereby further improving the cohesive strength of the first pressure-sensitive adhesive layer and resulting pressure-sensitive adhesive tape having high adhesive strength. The molecular weight distribution (Mw / Mn) of the (meth)acrylic copolymer more preferably has a lower limit of 1.1, a more preferred upper limit of 8.0, an even more preferred lower limit of 1.2, and an even more preferred upper limit of 5.0.
[0053] In this specification, the number average molecular weight (Mn) and weight average molecular weight (Mw) are molecular weights calculated in terms of standard polystyrene by gel permeation chromatography (GPC). For GPC, for example, a 2690 Separations Model (manufactured by Waters) can be used. Alternatively, a GPC device (manufactured by Tosoh Corporation, such as "HLC-8220," column: TSKgelSuper HZM-N (4 columns)) can also be used, and tetrahydrofuran can be used as the solvent. Measurement conditions can be, for example, 40°C and a flow rate of 0.5 mL / min.
[0054] The weight average molecular weight and molecular weight distribution (Mw / Mn) of the (meth)acrylic copolymer can be adjusted to fall within the above ranges by adjusting polymerization conditions such as the polymerization initiator and polymerization temperature.
[0055] To obtain the (meth)acrylic copolymer, the monomer mixture may be subjected to a radical reaction in the presence of a polymerization initiator. The method for radically reacting the monomer mixture, i.e., the polymerization method, may be a conventionally known method, such as solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, or bulk polymerization. The reaction method for radically reacting the monomer mixture may be, for example, living radical polymerization or free radical polymerization.
[0056] Examples of the polymerization initiator include organic peroxides and azo compounds. Examples of the organic peroxides include 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-butylperoxy-3,5,5-trimethylhexanoate, and t-butylperoxylaurate. The azo compound is not particularly limited as long as it is one that is commonly used in radical polymerization.Examples of the azo compound include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 1,1-azobis(cyclohexane-1-carbonitrile), 1-[(1-cyano-1-methylethyl)azo]formamide, 4,4'-azobis(4-cyanovaleric acid), dimethyl-2,2'-azobis(2-methylpropionate), dimethyl-1,1'-azobis(1-cyclohexanecarboxylate), 2,2'-azobis{2-methyl-N-[1,1'-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2 '-Azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 2,2'-azobis(1-imino-1-pyrrolidino-2-methylpropane) dihydrochloride, 2,2'-azobis(2,4,4-trimethylpentane), and the like. Furthermore, as the polymerization initiator, the polymerization initiator that initiates living radical polymerization is not particularly limited, but an organic tellurium polymerization initiator is preferred. These polymerization initiators may be used alone or in combination of two or more.
[0057] When the monomer mixture is subjected to a radical reaction, a dispersion stabilizer may be used, such as polyvinylpyrrolidone, polyvinyl alcohol, methyl cellulose, ethyl cellulose, poly(meth)acrylic acid, poly(meth)acrylic acid ester, or polyethylene glycol.
[0058] When a polymerization solvent is used in the radical reaction of the monomer mixture, the polymerization solvent is not particularly limited. Examples of the polymerization solvent that can be used include nonpolar solvents such as hexane, cyclohexane, octane, toluene, and xylene. Examples of the polymerization solvent that can be used include highly polar solvents such as water, methanol, ethanol, propanol, butanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, tetrahydrofuran, dioxane, and N,N-dimethylformamide. These polymerization solvents may be used alone or in combination of two or more.
[0059] The rubber-based pressure-sensitive adhesive contains a rubber-based polymer. Examples of the rubber-based polymer include natural rubber and A-B-A block copolymer rubber. Specific examples of the natural rubber include styrene-butadiene rubber, polyisoprene, polybutene (1-butene and cis- or trans-2-butene), polyisobutylene, A-B-A block copolymer rubber, and hydrogenated versions thereof. Specific examples of the A-B-A block copolymer rubber include styrene-butadiene-styrene block (SBS) copolymer, styrene-isoprene-styrene block (SIS) copolymer, styrene-isobutylene-styrene block copolymer rubber, styrene-vinyl-isoprene-styrene block copolymer rubber, styrene-ethylene-butylene-styrene block (SEBS) copolymer rubber, which is a hydrogenated version of SBS, and styrene-ethylene-propylene-styrene block (SEPS) copolymer rubber and styrene-isoprene-propylene-styrene block copolymer, which are hydrogenated versions of SIS. These rubber-based polymers may be used alone or in combination of two or more.
[0060] The rubber-based polymer preferably contains less than 20% by mass of styrene-derived structural units. By containing less than 20% by mass of styrene-derived structural units in the rubber-based polymer, outgassing from the resulting pressure-sensitive adhesive tape can be further reduced (particularly, the suppression of gas generation that can reduce the durability, reliability, or operating accuracy of electronic devices such as magnetic disk drives). The styrene-derived structural units are more preferably less than 10% by mass, and it is particularly preferred that the rubber-based polymer does not contain any styrene-derived structural units.
[0061] The first pressure-sensitive adhesive layer preferably further contains an inorganic mineral. When the first pressure-sensitive adhesive layer contains an inorganic mineral, the barrier properties of the resulting pressure-sensitive adhesive tape are further improved.
[0062] Examples of the inorganic minerals include inorganic fillers and layered clay minerals. Specific examples of the inorganic fillers include silica fillers. Specific examples of the layered clay minerals include smectite (e.g., lipophilic sucmetite such as Lucentite SAN316, SAN, STN, and SPN (manufactured by Co-op Chemical Co., Ltd.)), micromica (e.g., MK-300 (manufactured by Katakura Co-op Agri Co., Ltd.)), and the like. These inorganic minerals may be used alone or in combination of two or more.
[0063] The preferred lower limit of the content of the inorganic mineral relative to 100 parts by mass of the pressure-sensitive adhesive is 10 parts by mass, and the preferred upper limit is 200 parts by mass. When the content of the inorganic mineral is 10 parts by mass or more, the barrier properties of the resulting pressure-sensitive adhesive tape are further improved. When the content of the inorganic mineral is 200 parts by mass or less, the resulting pressure-sensitive adhesive tape has higher adhesive strength and further improves L-shaped bending application properties. The more preferred lower limit of the content of the inorganic mineral is 30 parts by mass, and the more preferred upper limit is 100 parts by mass, and even more preferred lower limit is 40 parts by mass, and even more preferred upper limit is 75 parts by mass.
[0064] The first pressure-sensitive adhesive layer preferably further contains a crosslinking agent, which forms a crosslinked structure between the main chains of the resins constituting the first pressure-sensitive adhesive layer (e.g., the (meth)acrylic copolymer, the tackifier described below, etc.), thereby improving the cohesive strength of the first pressure-sensitive adhesive layer, resulting in a pressure-sensitive adhesive tape having higher adhesive strength and further improving L-shaped bend application properties.
[0065] Examples of the crosslinking agent include isocyanate-based crosslinking agents, aziridine-based crosslinking agents, epoxy-based crosslinking agents, metal chelate-based crosslinking agents, etc. Among these, isocyanate-based crosslinking agents are preferred from the viewpoint of ease of forming a crosslinked structure.
[0066] The content of the crosslinking agent relative to 100 parts by mass of the pressure-sensitive adhesive is preferably 0.01 parts by mass at the lower limit and 10 parts by mass at the upper limit. By having the content of the crosslinking agent within the above range, the L-shaped bend application property of the obtained pressure-sensitive adhesive tape is further improved. The content of the crosslinking agent is more preferably 0.1 parts by mass at the lower limit and 3 parts by mass at the upper limit.
[0067] The first pressure-sensitive adhesive layer may further contain a tackifier. When the first pressure-sensitive adhesive layer contains a tackifier, the resulting pressure-sensitive adhesive tape has higher adhesive strength and further improves L-shaped bend application properties.
[0068] Examples of the tackifier include rosin resins, rosin ester resins, hydrogenated rosin resins, terpene resins, terpene phenol resins, coumarone-indene resins, alicyclic saturated hydrocarbon resins, C5 petroleum resins, C9 petroleum resins, C5-C9 copolymer petroleum resins, hydrogenated C5 petroleum resins, hydrogenated C9 petroleum resins, and hydrogenated C5-C9 copolymer petroleum resins. Among these, hydrogenated rosin resins, alicyclic saturated hydrocarbon resins, hydrogenated C5 petroleum resins, hydrogenated C9 petroleum resins, and hydrogenated C5-C9 copolymer petroleum resins are preferred from the viewpoint of further reducing the polarity of the pressure-sensitive adhesive layer, further reducing the water vapor permeability at 40°C and 90% RH, and further improving the barrier properties of the resulting pressure-sensitive adhesive tape. Furthermore, from the viewpoint of adhesive strength control, rosin resins or terpene resins are preferred, and hydroxyl-containing rosin resins or hydroxyl-containing terpene resins are more preferred. These tackifiers may be used alone or in combination of two or more kinds.
[0069] The softening temperature of the tackifier preferably has a lower limit of 70°C and an upper limit of 170°C. When the softening temperature of the tackifier is 70°C or higher, the first pressure-sensitive adhesive layer can be prevented from becoming too soft. When the softening temperature of the tackifier is 170°C or lower, the wettability of the first pressure-sensitive adhesive layer to the adherend is increased. A more preferred lower limit of the softening temperature of the tackifier is 120°C, and a more preferred upper limit is 160°C. The softening temperature is measured according to JIS K 2207 (ring and ball method).
[0070] The first pressure-sensitive adhesive layer may further contain a silane coupling agent for the purpose of improving the pressure-sensitive adhesive tape. Examples of the silane coupling agent include epoxy silanes, acrylic silanes, methacrylic silanes, amino silanes, isocyanate silanes, vinyl silanes, and butadiene polymer-modified silanes.
[0071] The first pressure-sensitive adhesive layer has a water vapor permeability at 40°C and 90% RH of preferably 300 g / (m 2 The water vapor permeability of the first pressure-sensitive adhesive layer at 40°C and 90% RH is 300 g / (m2 A more preferable upper limit of the water vapor permeability of the first pressure-sensitive adhesive layer at 40°C and 90% RH is 200 g / (m 2 ·day), and a more preferable upper limit is 100 g / (m 2 Furthermore, there is no particular preferred lower limit for the water vapor transmission rate of the first pressure-sensitive adhesive layer at 40°C and 90% RH, but it is substantially 10 g / (m 2 The water vapor permeability of the first pressure-sensitive adhesive layer at 40°C and 90% RH can be measured by laminating the pressure-sensitive adhesive layer with a 200-mesh metal netting to prepare a sample of the pressure-sensitive adhesive layer in the same manner as the above-mentioned method for measuring water vapor permeability at 40°C and 90% RH.
[0072] The water vapor permeability of the first pressure-sensitive adhesive layer at 40°C and 90% RH can be adjusted by the type of pressure-sensitive adhesive used in the pressure-sensitive adhesive layer and the density of the pressure-sensitive adhesive layer. For example, selecting a material with a large polarity difference from water vapor, i.e., water molecules, results in low moisture permeability. That is, since water molecules are highly polar, selecting a material composed of low-polarity atomic groups results in low moisture permeability. Furthermore, when the pressure-sensitive adhesive is composed of a high-molecular polymer, the smaller the free volume of the high-molecular polymer, the lower the moisture permeability. That is, polymers with symmetrical side chains are more likely to pack, resulting in a smaller free volume and lower moisture permeability. Furthermore, polymers with a crystalline structure have even lower moisture permeability. The free volume can also be adjusted by changing the molecular weight, hydrogen bonding properties, molecular rigidity, and crosslinking density of the polymer to adjust the moisture permeability. In addition, adding and dispersing a layered viscosity compound or the like that inhibits the permeation of water molecules into the pressure-sensitive adhesive reduces the moisture permeability by blocking the water molecules.
[0073] The tensile storage modulus of the first pressure-sensitive adhesive layer at 25°C is preferably 0.01 MPa at its lower limit and 5 MPa at its upper limit. When the tensile storage modulus of the first pressure-sensitive adhesive layer at 25°C is within the above range, the product of the tensile storage modulus and thickness of the first pressure-sensitive adhesive layer can be easily adjusted to fall within the above range, further improving the L-shaped bend application property of the resulting pressure-sensitive adhesive tape. The tensile storage modulus of the first pressure-sensitive adhesive layer at 25°C is more preferably 0.05 MPa at its lower limit and more preferably 1 MPa at its upper limit, even more preferably 0.1 MPa at its lower limit and even more preferably 0.5 MPa at its upper limit. The tensile storage modulus of the first pressure-sensitive adhesive layer at 25°C can be obtained by the following method. That is, a plurality of pressure-sensitive adhesive layers are laminated to prepare a pressure-sensitive adhesive layer having a thickness of 1 mm for measurement, and then the shear storage modulus at 25°C is measured using a dynamic viscoelasticity measuring device (manufactured by IT Measurement Control Co., Ltd., "DVA-200") under the following conditions: measurement mode shear, 25°C, frequency 1 Hz, heating rate 5°C / min, temperature range 0 to 100°C, set strain 0.1%. The shear storage modulus at 25°C thus obtained is multiplied by 3 to obtain the tensile storage modulus at 25°C.
[0074] Examples of a method for adjusting the tensile storage modulus at 25° C. of the first pressure-sensitive adhesive layer include a method of changing the composition of the pressure-sensitive adhesive contained in the pressure-sensitive adhesive layer.
[0075] The thickness of the first pressure-sensitive adhesive layer preferably has a lower limit of 10 μm and an upper limit of 200 μm. When the thickness of the first pressure-sensitive adhesive layer is within the above range, the resulting pressure-sensitive adhesive tape has better barrier properties and better L-shaped bend application properties. The thickness of the first pressure-sensitive adhesive layer is more preferably 15 μm lower limit, more preferably 180 μm upper limit, even more preferably 18 μm lower limit, and even more preferably 150 μm upper limit.
[0076] The gel fraction of the first pressure-sensitive adhesive layer preferably has a lower limit of 1% by mass and an upper limit of 90% by mass. A gel fraction of the first pressure-sensitive adhesive layer of 1% by mass or more further improves the cohesive strength of the first pressure-sensitive adhesive layer. A gel fraction of the first pressure-sensitive adhesive layer of 90% by mass or less prevents the wettability of the first pressure-sensitive adhesive layer with respect to the adherend from decreasing too much. A more preferred lower limit of the gel fraction of the first pressure-sensitive adhesive layer is 20% by mass, a more preferred upper limit is 80% by mass, an even more preferred lower limit is 30% by mass, and an even more preferred upper limit is 70% by mass. The gel fraction of the first pressure-sensitive adhesive layer can be measured, for example, by the following method. A pressure-sensitive adhesive tape is cut into a 50 mm x 100 mm flat rectangular shape to prepare a test specimen. The test specimen is immersed in ethyl acetate at 23°C for 24 hours, then removed from the ethyl acetate, and dried at 110°C for 1 hour. The gel fraction can be measured by measuring the mass of the test piece after drying and calculating the gel fraction using the following formula (4). Note that no release film for protecting the pressure-sensitive adhesive layer is laminated on the test piece. Gel fraction (mass%) = 100 × (W 2 -W 0 ) / (W 1 -W 0 ) (4) (W 0 : Mass of the substrate, W 1 : mass of test piece before immersion, W 2 : Mass of test piece after immersion and drying)
[0077] The pressure-sensitive adhesive tape of the present invention may have other layers as long as the effects of the present invention are not impaired.
[0078] The pressure-sensitive adhesive tape of the present invention preferably has a structure in which a second substrate layer and a second pressure-sensitive adhesive layer are further laminated on the first pressure-sensitive adhesive layer side of a laminate having the first substrate layer and the first pressure-sensitive adhesive layer. That is, the pressure-sensitive adhesive tape of the present invention preferably has the first substrate layer, the first pressure-sensitive adhesive layer, the second substrate layer, and the second pressure-sensitive adhesive layer in this order. When the pressure-sensitive adhesive tape of the present invention has such a structure, the barrier property and the L-shaped bend application ability are further improved.
[0079] The second base layer may or may not contain a foam, but preferably does not contain a foam from the viewpoint of further improving the barrier properties of the resulting pressure-sensitive adhesive tape.
[0080] Examples of resins constituting the second base layer include olefin-based thermoplastic resins, thermoplastic elastomers, acrylic resins, and polyurethane-based resins. These may be used alone or in combination of two or more. In addition to these, silicone-based resins, vinyl chloride-based resins, styrene-based resins, polyester-based resins, polyamide-based resins, ionomer-based resins, and the like may also be used. Among these, from the viewpoint of easily adjusting the 10% heat shrinkage temperature (described later) within an appropriate range, it is preferable to contain at least one resin selected from the group consisting of olefin-based thermoplastic resins and thermoplastic elastomers. Furthermore, from the viewpoint of further improving the barrier properties of the resulting pressure-sensitive adhesive tape, it is more preferable to contain an olefin-based thermoplastic resin. The resin used in the second resin sheet layer may be used alone or in combination of two or more.
[0081] The second substrate layer has a water vapor permeability at 40°C and 90% RH of preferably 100 g / (m 2 The second substrate layer has a water vapor permeability of 100 g / (m at 40° C. and 90% RH. 2 The barrier properties of the obtained pressure-sensitive adhesive tape are further improved by setting the water vapor transmission rate of the second base layer at 40°C and 90% RH to 50 g / (m 2 ·day), and a more preferable upper limit is 30 g / (m 2 Furthermore, there is no particular lower limit to the water vapor permeability of the second substrate layer at 40°C and 90% RH, but it is substantially 0.1 g / (m 2 ・day) is the lower limit.
[0082] The 10% heat shrinkage temperature of the second base layer is preferably 95°C or lower in at least one of the MD and TD directions. When the 10% heat shrinkage temperature of the second base layer is 95°C or lower in at least one of the MD and TD directions, the resulting pressure-sensitive adhesive tape can be more suitably used in the HDD manufacturing method described below. The 10% heat shrinkage temperature of the second base layer in at least one of the MD and TD directions is more preferably 75°C, even more preferably 65°C, and particularly preferably 55°C. It is more preferable that the 10% heat shrinkage temperature of the second base layer is 95°C or lower in the MD and TD directions. Furthermore, the 10% heat shrinkage temperature of the second base layer is preferably 40°C or lower in at least one of the MD and TD directions. When the 10% heat shrinkage temperature of the second base material layer in at least one of the MD and TD directions is 40°C or higher, the pressure-sensitive adhesive tape can be stored at room temperature. A more preferred lower limit of the 10% heat shrinkage temperature of the second base material layer in at least one of the MD and TD directions is 50°C, and an even more preferred lower limit is 60°C.
[0083] The second base layer has a tensile storage modulus at 25 ° C. in at least one of the MD and TD directions of 0.1 MPa as a lower limit and 10,000 MPa as a preferred upper limit. Since the tensile storage modulus at 25 ° C. in at least one of the MD and TD directions of the second base layer is within the above range, the product of the average tensile storage modulus in the MD and TD directions of the second base layer and the thickness can be easily adjusted within the above range, thereby improving the L-shaped bend adhesion of the resulting adhesive tape. The tensile storage modulus at 25 ° C. in at least one of the MD and TD directions of the second base layer is more preferably 1 MPa as a lower limit and 5,000 MPa as an upper limit, and even more preferably 5 MPa as a lower limit and 3,000 MPa as an upper limit. The tensile storage modulus at 25 ° C. of the second base layer can be measured by the same method as that of the first base layer described above.
[0084] The thickness of the second substrate layer is preferably 10 μm at its lower limit and 2000 μm at its upper limit. By setting the thickness of the second substrate layer within the above range, the resulting pressure-sensitive adhesive tape has better barrier properties and better L-shaped bend application properties. The thickness of the second substrate layer is more preferably 20 μm at its lower limit and 1000 μm at its upper limit, even more preferably 25 μm at its lower limit and 500 μm at its upper limit.
[0085] The second pressure-sensitive adhesive layer may be the same as the first pressure-sensitive adhesive layer described above.
[0086] The pressure-sensitive adhesive tape of the present invention preferably further comprises an inorganic layer, which further improves the barrier properties of the pressure-sensitive adhesive tape of the present invention.
[0087] Examples of the inorganic layer include aluminum, silver, copper, alumina, etc. Among these, aluminum is preferred from the viewpoints of productivity and cost.
[0088] The inorganic layer is preferably laminated on the surface of the second base layer facing the second pressure-sensitive adhesive layer. Examples of methods for laminating the inorganic layer include vapor deposition and sputtering. Among these, vapor deposition is preferred from the viewpoint of productivity. Examples of methods for laminating the inorganic layer by vapor deposition include vacuum deposition.
[0089] The pressure-sensitive adhesive tape of the present invention comprises the first substrate layer, the first pressure-sensitive adhesive layer, the second substrate layer, and the second pressure-sensitive adhesive layer in this order, the first substrate layer containing a foam, and the first substrate layer having a water vapor permeability of 40 g / (m 2 Preferably, the first base material layer has a 10% heat shrinkage temperature of 95°C or less in at least one of the MD and TD directions, and the first base material layer has a 10% heat shrinkage temperature of 95°C or less in at least one of the MD and TD directions. When the pressure-sensitive adhesive tape of the present invention is in this state, the barrier properties and L-shaped bend application properties are further improved, and the pressure-sensitive adhesive tape can be more suitably used in the manufacturing method of an HDD described later.
[0090] The method for producing the pressure-sensitive adhesive tape of the present invention is not particularly limited, and it can be produced, for example, by the following method. Specifically, a pressure-sensitive adhesive solution is prepared by adding a pressure-sensitive adhesive such as a (meth)acrylic copolymer or a rubber-based polymer, and, if necessary, an inorganic mineral, a crosslinking agent, a tackifier, etc., and a solvent, and stirring thoroughly. The prepared pressure-sensitive adhesive solution is applied to the release-treated surface of a release film having a release-treated surface using an applicator, and dried at 110°C for 5 minutes to produce a laminate film (a) having a first pressure-sensitive adhesive layer. The resulting laminate film (a) is then overlaid on a prepared first base layer so that the first pressure-sensitive adhesive layer faces the prepared first base layer, thereby producing a laminate having a first base layer and a first pressure-sensitive adhesive layer. The release film of the obtained laminate is peeled off, and the laminate is bonded to a prepared second base layer. Then, in the same manner as for the laminate film (a), a laminate film (b) having a second pressure-sensitive adhesive layer is overlaid on the laminate film (b) so that the second pressure-sensitive adhesive layer faces the second base layer, thereby forming an integrated laminate. The adhesive tape can then be produced by curing the adhesive tape at 40° C. for 2 days.
[0091] The pressure-sensitive adhesive tape of the present invention has a 10% heat shrinkage temperature of preferably 95°C or lower in at least one of the MD and TD directions. Since the pressure-sensitive adhesive tape of the present invention has a 10% heat shrinkage temperature of 95°C or lower in at least one of the MD and TD directions, it can be more suitably used in the HDD manufacturing method described below. The pressure-sensitive adhesive tape of the present invention has a 10% heat shrinkage temperature of more preferably 80°C, even more preferably 70°C, and particularly preferably 60°C in at least one of the MD and TD directions. The pressure-sensitive adhesive tape of the present invention more preferably has a 10% heat shrinkage temperature of 95°C or lower in the MD and TD directions. Furthermore, the pressure-sensitive adhesive tape of the present invention has a 10% heat shrinkage temperature of preferably 40°C or lower in at least one of the MD and TD directions. Since the pressure-sensitive adhesive tape of the present invention has a 10% heat shrinkage temperature of 40°C or higher, it can be stored at room temperature. The lower limit of the 10% heat shrinkage temperature of the pressure-sensitive adhesive tape of the present invention is more preferably 50°C, and even more preferably 60°C.
[0092] The pressure-sensitive adhesive tape of the present invention is used, for example, in electronic devices. It is particularly preferably used for hard disks installed in electronic devices, specifically as a sealing material for the outer periphery of HDD housings in a gas-purged environment. The electronic devices are not particularly limited, and examples include mobile phones, cameras, displays, game consoles, electronic organizers, and personal computers. As described above, the pressure-sensitive adhesive tape of the present invention has excellent barrier properties and L-shaped bend adhesion, and is therefore preferably used for temporary fixing of components installed in electronic devices, particularly for temporary fixing to maintain a gas-purged environment. It is more preferably used for temporary fixing of the outer periphery of a housing containing a purged gas, and more specifically, it is even more preferably used for temporary fixing of the outer periphery of a hard disk housing in a gas-purged environment. Here, "temporary fixing" in this specification refers to fixing the outer periphery of a housing during transportation, etc., to prevent the release of purged gas and maintain a gas-purged environment, and then peeling it off when installing it in an electronic device, etc. By using the pressure-sensitive adhesive tape of the present invention on the outer periphery of a hard disk housing, a gas-purged environment can be maintained even if the housing has steps.
[0093] The present invention also provides a method for manufacturing an HDD having a body portion equipped with a hard disk and a lid portion, the method comprising the step of applying the adhesive tape of the present invention to the body portion and the lid portion to seal the HDD. The method for manufacturing an HDD of the present invention uses the adhesive tape of the present invention to seal gas from outside the housing, thereby enabling the manufacture of HDDs without compromising sealing performance, even when manufacturing high-capacity HDDs containing a large number of platters. In the method for manufacturing an HDD of the present invention, a step of attaching the lid portion to the body portion is usually carried out before the step of applying the adhesive tape of the present invention to the body portion and the lid portion to seal the HDD.
[0094] Specific examples of the process for sealing an HDD using the adhesive tape include the following processes. That is, using an HDD having a main body and a lid, attaching the lid of the HDD to the main body of the HDD, folding and attaching the adhesive tape from the outer edge of the lid to the main body of the HDD, thereby bonding the main body and the lid together, and sealing the outer edge of the HDD with the adhesive tape. In particular, the process for sealing an HDD using the adhesive tape preferably involves folding and attaching the adhesive tape from the lid to the main body, and then thermally shrinking the adhesive tape. By using the adhesive tape of the present invention, bonding the lid to the main body by folding and attaching the adhesive tape, and then thermally shrinking the attached adhesive tape, excellent sealing performance can be achieved even when sealing the housing from the outside.
[0095] The HDD preferably has a structure in which the main body includes a main body bottom and a main body sidewall protruding upward from the outer periphery of the main body bottom, and the lid is attached to the sidewall. This structure of the HDD further improves the sealing performance of the HDD manufacturing method of the present invention. Furthermore, the main body preferably has a main body corner on the surface of the main body sidewall where the lid is attached, and the lid has a lid corner that contacts the main body corner. When the HDD has this structure, the heat shrinking of the adhesive tape described below is performed at the portion where the main body corner and the lid corner of the adhesive tape are bonded, thereby further improving the sealing performance of the HDD manufacturing method of the present invention and further improving the manufacturing quality of the HDDs manufactured.
[0096] A schematic diagram of a preferred embodiment of the cover is shown in Figure 2, and a schematic diagram of a preferred embodiment of the main body is shown in Figure 3. Note that in Figure 3, the hard disk is omitted from illustration.
[0097] The step of sealing the HDD in the HDD manufacturing method of the present invention preferably includes a step (I) of folding and attaching the adhesive tape from the lid portion to the side wall portion of the main body, and a step (II) of thermally shrinking the adhesive tape after the step (I). By including the steps (I) and (II) in the HDD manufacturing method of the present invention, the sealability of the HDD manufacturing method of the present invention is improved.
[0098] In the method for manufacturing an HDD of the present invention, it is preferable that the main body has the main body corners and the lid has the lid corners, and in step (I), the adhesive tape is folded and attached at least to the main body corners and the lid corners, and in step (II), the adhesive tape is thermally shrunk at the attached portion from the lid corner to the main body corner. By carrying out the method for manufacturing an HDD of the present invention in this manner, the sealing performance is further improved, and the manufacturing quality of the manufactured HDD is further improved.
[0099] In the step (I), examples of the method for folding and adhering the adhesive tape from the lid portion to the side wall portion of the main body include a method in which the lid portion is attached to the side wall portion of the main body, and then the adhesive tape is attached so that a portion of the adhesive tape protrudes from the outer peripheral edge of the upper surface of the lid portion, and the protruding portion is folded and adhered from the lid portion to the side wall portion of the main body.
[0100] In the method for manufacturing an HDD of the present invention, in step (I), the lid is preferably attached to the main body sidewall, a portion of the adhesive tape is attached to the outer periphery of the upper surface of the lid so that the outer periphery of the upper surface of the lid is located outside the outer periphery of the upper surface of the lid, a mold including a mold bottom and a mold sidewall protruding downward from the outer periphery of the mold bottom is pressed against the upper surface of the lid so that the upper surface of the lid faces the lower surface of the mold bottom, the adhesive tape is bent so that the portion of the adhesive tape that is not in contact with the upper surface of the lid is located between the mold sidewall and the main body sidewall, and the adhesive tape is attached to the main body sidewall, thereby bonding the main body and the lid together. By performing the method for manufacturing an HDD of the present invention in this manner, it is easy to simultaneously and instantaneously bend the entire portion of the adhesive tape located outside the outer periphery of the upper surface of the lid using the mold, thereby improving the simplicity of the method for manufacturing an HDD of the present invention.
[0101] A schematic diagram of a preferred embodiment of the mold is shown in Figure 4. By pressing mold 4 against the upper surface of the lid of the HDD to which the adhesive tape has been attached, so that the lower surface 42 of the mold bottom of mold 4 faces the upper surface, the entire portion of the adhesive tape attached to the lid, which is located outside the outer periphery of the upper surface of the lid, can be easily folded. Furthermore, mold sidewall 43 of mold 4 makes it easier to maintain the folded adhesive tape in an L-shape, making it easier to seal the HDD and further improving the sealing performance of the HDD manufacturing method of the present invention. The bottom of the mold may be hollow.
[0102] FIG. 5 is a cross-sectional view showing a schematic state in which the adhesive tape is bent into an L-shape using the mold and attached to the lid portion and the side wall portion of the main body.
[0103] When the upper surface of the lid and the lower surface of the mold bottom are pressed against each other so that they face each other, it is preferable to heat the mold to a temperature of 35°C or higher and 60°C or lower. When the mold is heated to 35°C or higher, the adhesive tape can be easily folded and attached, improving the wettability of the adhesive layer, and the sealing performance of the HDD manufacturing method of the present invention is further improved. Furthermore, when the mold is heated to 60°C or lower, it is possible to further prevent the manufacturing quality of the HDD to be manufactured from being impaired. It is more preferable to heat the mold to 50°C or higher and 60°C or lower.
[0104] As a method for heating the metal, for example, a method in which the mold is placed on a heated hot plate can be mentioned.
[0105] In the step (I), the adhesive tape is preferably in a frame shape corresponding to the outer periphery of the upper surface of the lid, and the outer frame of the frame-shaped adhesive tape is preferably attached so as to be positioned outside the outer periphery of the upper surface of the lid. By using such a frame-shaped adhesive tape, interference with other functional components present on the surface of the HDD can be avoided.
[0106] As a method for forming the above-mentioned adhesive tape into a frame shape, there can be mentioned a method in which the adhesive tape is pressed with a punching blade to form a punching process.
[0107] In the step (II), it is preferable to heat shrink the pressure-sensitive adhesive tape by 10% or more in at least one of the MD and TD directions. By heat shrinking the pressure-sensitive adhesive tape by 10% or more in at least one of the MD and TD directions, the sealing property of the HDD manufacturing method of the present invention is further improved. It is more preferable to heat shrink the pressure-sensitive adhesive tape by 20% or more in at least one of the MD and TD directions, and it is even more preferable to heat shrink the pressure-sensitive adhesive tape by 30% or more. It is also more preferable to heat shrink the pressure-sensitive adhesive tape by 10% or more in both the MD and TD directions.
[0108] In the step (II), the upper limit of the temperature of the pressure-sensitive adhesive tape during heat shrinkage is preferably 95°C, i.e., the pressure-sensitive adhesive tape is preferably heat-shrunk at a temperature of 95°C or less. When the temperature of the pressure-sensitive adhesive tape during heat shrinkage is 95°C or less, the quality of the manufactured HDD is further improved. The upper limit of the temperature of the pressure-sensitive adhesive tape during heat shrinkage is more preferably 80°C, even more preferably 70°C, and particularly preferably 60°C.
[0109] The present invention also provides an HDD sealing structure that includes a main body and a lid, the main body and the lid being secured together via heat-shrunk adhesive tape. Because the HDD sealing structure of the present invention secures the HDD externally using heat-shrunk adhesive tape, it provides sufficient sealing even when sealing from the outside without using a gasket on the main body of the HDD. This ensures superior manufacturing quality, even for high-capacity HDDs with an increasing number of platters.
[0110] An example of the HDD sealing structure of the present invention is a sealing structure obtained by folding and attaching an adhesive tape from the lid portion of the HDD to the side wall portion of the main body using the HDD manufacturing method of the present invention, and then thermally shrinking the adhesive tape.
[0111] According to the present invention, it is possible to provide an adhesive tape having excellent barrier properties and L-shaped bend application properties. Also, according to the present invention, it is possible to provide a method for manufacturing a hard disk drive that has excellent sealing properties even when the housing is sealed from the outside by using the adhesive tape. Furthermore, according to the present invention, it is possible to provide a hard disk drive sealing structure that is sufficiently sealed even when the housing is sealed from the outside.
[0112] FIG. 1 is a schematic diagram of a model used for calculating bending rigidity. FIG. 2 is a schematic diagram showing a preferred embodiment of a lid of an HDD device used in the manufacturing method of the present invention. FIG. 3 is a schematic diagram showing a preferred embodiment of a main body of an HDD device used in the manufacturing method of the present invention. FIG. 4 is a schematic diagram showing a preferred embodiment of a mold used in the manufacturing method of the present invention. FIG. 5 is a cross-sectional view schematically illustrating a state in which an adhesive tape is bent into an L-shape using a mold and attached from the lid of an HDD to a side wall of the main body. FIG. 6 is a schematic diagram showing the shape of an adhesive tape used in evaluating peel resistance. FIG. 7 is a schematic diagram showing a state in which an HDD lid is attached to a side wall of the main body in evaluating peel resistance. FIG. 8 is a schematic diagram showing a state in which an adhesive tape is attached to the upper surface of a lid attached to a side wall of the main body in evaluating peel resistance. FIG. 9 is a schematic diagram showing a state in which an adhesive tape is bent into an L-shape using a mold in evaluating peel resistance and attached from the lid of an HDD to a side wall of the main body. FIG. 10 is a schematic diagram showing the shape of an adhesive tape used in evaluating housing sealability (without corner heating).
[0113] The following examples will explain the present invention in more detail, but the present invention is not limited to these examples.
[0114] (Preparation of Acrylic Copolymer-Containing Solution) Ethyl acetate was added to a reaction vessel as a polymerization solvent, and after bubbling with nitrogen, the reaction vessel was heated while flowing in nitrogen to initiate reflux. A polymerization initiator solution prepared by diluting 0.1 parts by mass of azobisisobutyronitrile 10 times with ethyl acetate was added to the reaction vessel. 96.9 parts by mass of n-butyl acrylate, 3 parts by mass of acrylic acid, and 0.1 parts by mass of 2-hydroxyethyl acrylate were added dropwise over 2 hours. After completion of the dropwise addition, a polymerization initiator solution prepared by diluting 0.1 parts by mass of azobisisobutyronitrile 10 times with ethyl acetate was again added to the reaction vessel, and a polymerization reaction was carried out for 4 hours to obtain an acrylic copolymer-containing solution.
[0115] (Preparation of Pressure-Sensitive Adhesive Solution A) To the obtained acrylic copolymer-containing solution, 30 parts by mass of Super Ester A-125 (manufactured by Arakawa Chemical Industries, Ltd.) as a tackifier was added relative to 100 parts by mass of the acrylic copolymer, and the mixture was stirred. Further, 2 parts by mass of Takenate D-101E (manufactured by Mitsui Chemicals, Inc.) as a crosslinking agent and ethyl acetate were added and the mixture was stirred thoroughly, thereby obtaining a pressure-sensitive adhesive solution A having a solid content of 30% by mass.
[0116] (Adhesive Solution B) SK Dyne 2563PS (a rubber-based adhesive solution, manufactured by Soken Chemical & Engineering Co., Ltd.) was used as adhesive solution B as it was.
[0117] (Preparation of adhesive solution C) To the obtained adhesive solution A, 50 parts by mass of MK-300 (micromica, manufactured by Katakura Co-op Agri Co., Ltd.) as an inorganic mineral was added per 100 parts by mass of the acrylic copolymer, and the mixture was stirred to obtain adhesive solution C.
[0118] (Preparation of adhesive solution D) 5 parts by mass of Coronate HX (manufactured by Tosoh Corporation) as a crosslinking agent was added to SK Dyne 2030U (acrylic adhesive solution, manufactured by Soken Chemical & Engineering Co., Ltd.) per 100 parts by mass of solid content, and the mixture was thoroughly stirred to obtain adhesive solution D.
[0119] (Preparation of Pressure-Sensitive Adhesive Solution E) A pressure-sensitive adhesive solution E was obtained in the same manner as in "(Preparation of Pressure-Sensitive Adhesive Solution A)" above, except that Super Ester A-125 was not added as a tackifier to the obtained acrylic copolymer solution.
[0120] (Preparation of adhesive solution F) To the obtained adhesive solution A, 50 parts by mass of MAE (Somasif, manufactured by Katakura Co-op Agri Co., Ltd.) as an inorganic mineral was added per 100 parts by mass of the acrylic copolymer, and the mixture was stirred to obtain adhesive solution F.
[0121] (Preparation of Pressure-Sensitive Adhesive Solution G) 50 parts by mass of FB-5D (spherical silica, manufactured by Denka Company Ltd.) as an inorganic mineral was added to 100 parts by mass of the acrylic copolymer in the pressure-sensitive adhesive solution A obtained, and the mixture was stirred to obtain a pressure-sensitive adhesive solution G.
[0122] (Preparation of Pressure-Sensitive Adhesive Solution H) 50 parts by mass of iM30K (hollow silica, glass bubbles, manufactured by 3M Corporation) as an inorganic mineral was added to 100 parts by mass of the acrylic copolymer in the obtained Pressure-Sensitive Adhesive Solution A, and the mixture was stirred to obtain Pressure-Sensitive Adhesive Solution H.
[0123] (Example 1) (Preparation of adhesive tape) The obtained adhesive solution A was applied using an applicator to the release-treated surface of a 50 μm thick release film ("SP3000" manufactured by Toyo Cross Co., Ltd.), and then heated and dried (110°C) to prepare a laminate film (a) having an adhesive layer A of 75 μm (0.075 mm) thickness as a first adhesive layer. The obtained laminate film (a) was laminated on a polyethylene foam ("Volara XL-H#0180015" manufactured by Sekisui Chemical Co., Ltd.) prepared as a first base layer, to obtain a laminate. The release film of the obtained laminate was peeled off, and a polyester shrink film ("Hishipet PX-40S" manufactured by Mitsubishi Chemical Corporation) prepared as a second base layer was laminated on the exposed surface of the adhesive layer A of the laminate. Then, a laminate film (b) having adhesive layer A formed thereon as a second adhesive layer in the same manner as for the laminate film (a) was overlaid with the adhesive layer facing the second base layer. The laminate was then left to stand at 40°C for 2 days to age, thereby obtaining an adhesive tape. The lamination was performed with all layers aligned in the MD direction. The measurements and calculations described below were performed with the release film peeled off.
[0124] (Measurement of tensile storage modulus of base material layer at 25°C) For each of the first base material layer and the second base material layer, the tensile storage modulus in the MD direction and the TD direction at 25°C was measured using a dynamic viscoelasticity measuring device (manufactured by IT Measurement Control Co., Ltd., "DVA-200") under the following conditions: measurement mode: tension, 25°C, frequency: 1 Hz, heating rate: 5°C / min, temperature range: 0 to 100°C, and set strain: 0.1%. The results are shown in Table 1.
[0125] (Calculation of tensile storage modulus of pressure-sensitive adhesive layer at 25°C) The obtained pressure-sensitive adhesive layers were laminated to prepare a pressure-sensitive adhesive layer having a thickness of 1 mm for measurement, and then the shear storage modulus at a temperature of 25°C was measured using a dynamic viscoelasticity measuring device (manufactured by IT Measurement Control Co., Ltd., "DVA-200") under the conditions of measurement mode shear, 25°C, frequency 1 Hz, heating rate 5°C / min, temperature range 0 to 100°C, and set strain 0.1%. The value obtained by multiplying the obtained shear storage modulus at a temperature of 25°C by 3 was regarded as the tensile storage modulus at 25°C. The tensile storage modulus at 25°C in the MD direction and the TD direction was calculated, and the results are shown in Table 1.
[0126] (Measurement of water vapor permeability at 40°C and 90% RH) The water vapor permeability in the thickness direction of the first base material layer, first pressure-sensitive adhesive layer, second base material layer, second pressure-sensitive adhesive layer, and the obtained pressure-sensitive adhesive tape was measured using a water vapor permeability measuring device (manufactured by MOCON, "PERMATRAN-W 1 / 50"). Note that for the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer, measurement samples were prepared by laminating the pressure-sensitive adhesive layer with a 200-mesh metal net. The results are shown in Table 1.
[0127] (Measurement of 10% heat shrinkage temperature) The first base material layer, the second base material layer, and the obtained pressure-sensitive adhesive tape were cut into a planar square shape with a width of 50 mm and a length of 50 mm to prepare test pieces. The obtained test piece was immersed in approximately 1 L of water preheated to 50 ° C for 10 seconds, and the width and length of the test piece after air-cooling to room temperature were measured. Using the measured width and length of the test piece, the heat shrinkage rates at 50 ° C in the MD direction and the TD direction were obtained according to the following formula (3). Similarly, the test piece was immersed in water at 60 ° C, 70 ° C, 80 ° C, 90 ° C, and 100 ° C for 10 seconds, and the width and length of the test piece after air-cooling to room temperature were measured. Using the measured width and length, the heat shrinkage rates at 60 ° C, 70 ° C, 80 ° C, 90 ° C, and 100 ° C in the MD direction and the TD direction were obtained according to the following formula (3). Regarding the obtained heat shrinkage rate, if the heat shrinkage rate at 50°C exceeded 10%, the 10% heat shrinkage temperature was set to less than 50°C, and if the heat shrinkage rate at 100°C was less than 10%, the 10% heat shrinkage temperature was set to more than 100°C. In other cases, the 10% heat shrinkage temperature was calculated on the assumption that the temperature and heat shrinkage rate were proportional between the maximum temperature at which the heat shrinkage rate was less than 10% and the minimum temperature at which the heat shrinkage rate exceeded 10%. The 10% heat shrinkage temperature was measured in both the MD and TD directions, and the results are shown in Table 1. Heat shrinkage rate (%) = [(L 0 -L 1 ) / L 0 ]×100 (3) (L 0 : Dimension of adhesive tape before immersion in heated water, L 1 : Dimensions of adhesive tape immersed in heated water and then cooled to room temperature)
[0128] (Calculation of bending rigidity of pressure-sensitive adhesive tape) For the pressure-sensitive adhesive tape obtained, the bending rigidity was calculated in each of the MD direction and the TD direction when the pressure-sensitive adhesive tape was bent to a bending width of 2.0 mm with the outermost pressure-sensitive adhesive layer facing inward, using the above-mentioned formula (1) and formula (2). The results are shown in Table 1.
[0129] (Measurement of 180° Peel Strength of Pressure-Sensitive Adhesive Tape from SUS at 23°C) The obtained pressure-sensitive adhesive tape was cut into a flat rectangular shape measuring 25 mm wide x 150 mm long, and was pressure-bonded to a SUS304 plate (prepared after cleaning with ethanol and wiping dry) with a surface finish of 2B as specified in JIS G 4305 using a 2 kg rubber roller, moving back and forth twice at a speed of 10 mm / sec under an environment of 23°C and 50% RH. After allowing the tape to stand for 20 minutes under an environment of 23°C and 50% RH, a 180° peel test was performed in accordance with JIS Z 0237 using a tensile tester (Shimadzu Corporation, "AGS-X") under conditions of 23°C, 50% RH, and a peel speed of 300 mm / min. The pressure-sensitive adhesive tape was peeled from the SUS plate, and the 180° peel strength of the pressure-sensitive adhesive tape from SUS at 23°C was measured. The results are shown in Table 1.
[0130] (Examples 2 to 9, 12 to 14, 16 to 29, 37 to 39, Comparative Examples 1 to 5) Pressure-sensitive adhesive tapes were prepared, and measurements and calculations were carried out, in the same manner as in Example 1, except that the type of base layer, the type of pressure-sensitive adhesive solution, and the thickness of the pressure-sensitive adhesive layer were changed as shown in Tables 1 to 6. The results are shown in Tables 1 to 6. In Examples 37 to 39, the pressure-sensitive adhesive layer (second pressure-sensitive adhesive layer) having a thickness of more than 0.15 mm was prepared by stacking multiple pressure-sensitive adhesive layers each having a thickness of 0.15 mm after heat drying, so as to achieve the thickness shown in Table 5.
[0131] (Example 10) An inorganic layer of 45 nm thick aluminum was laminated by vapor deposition under vacuum conditions on the second adhesive layer side of the prepared Hishipet PX-40S, and this was used as the second substrate layer. An adhesive tape was produced in the same manner as in Example 1, and measurements and calculations were carried out, except that the type of substrate layer, the type of adhesive solution, and the thickness of the adhesive layer were as shown in Table 2. The results are shown in Table 2.
[0132] (Example 11, Comparative Examples 6 and 7) Pressure-sensitive adhesive tapes were produced, and measurements and calculations were carried out in the same manner as in Example 1, except that pressure-sensitive adhesive layer A was laminated as a pressure-sensitive adhesive layer on a first base material layer shown in Tables 2 and 6. The results are shown in Tables 2 and 6.
[0133] (Example 15) In the above-mentioned "(Preparation of adhesive tape)", for a laminate before curing which had the first base material layer, first pressure-sensitive adhesive layer, second base material layer and second pressure-sensitive adhesive layer shown in Table 2 and was prepared in the same manner as in Example 1, the release film protecting the second pressure-sensitive adhesive layer was peeled off, and a polyester shrink film (manufactured by Mitsubishi Chemical Corporation, "HISHIPET LX-21S") prepared as a third base material layer was laminated on the second pressure-sensitive adhesive layer so that the TD direction overlapped the MD direction of the first and second base material layers, and the MD direction overlapped the TD direction of the first and second base material layers, respectively. Then, a laminate film (c) in which pressure-sensitive adhesive layer A was formed as the third pressure-sensitive adhesive layer in the same manner as for the laminate film (a) was overlaid with the pressure-sensitive adhesive layer A facing the third base layer, and the laminate film (c) was left to stand at 40°C for 2 days for aging, thereby obtaining a pressure-sensitive adhesive tape having, in this order, a first base layer, a first pressure-sensitive adhesive layer, a second base layer, a second pressure-sensitive adhesive layer, a third base layer, and a third pressure-sensitive adhesive layer. In the above-mentioned "(Preparation of Pressure-Sensitive Adhesive Tape)", measurements and calculations were carried out in the same manner as in Example 1, except that the pressure-sensitive adhesive tape was prepared in this manner. The results are shown in Table 2.
[0134] (Examples 30 to 35) An inorganic layer as shown in Tables 4 and 5 was laminated on the second adhesive layer side of the prepared Hishipet PX-40S (Examples 30, 33 to 35) or Space Clean S2600 (Examples 31 and 32), and this was used as a second substrate layer. Pressure-sensitive adhesive tapes were prepared in the same manner as in Example 1, with the type of substrate layer, type of adhesive solution, and thickness of the adhesive layer shown in Tables 4 and 5, and measurements and calculations were carried out. The results are shown in Tables 4 and 5. The inorganic layers in the pressure-sensitive adhesive tapes of Examples 30 to 34 (Al layer (Examples 30 to 32), Ag layer (Example 33), Cu layer (Example 34)) were formed by vapor deposition under vacuum conditions, and the inorganic layer (Al layer) in the pressure-sensitive adhesive tape of Example 35 was formed by sputtering under vacuum conditions.
[0135] (Example 36) On the second adhesive layer side of the prepared Space Clean S2600, a 70 nm thick aluminum layer was deposited under vacuum conditions as an inorganic layer, and this was used as the second base layer. In the above-mentioned "(Preparation of adhesive tape)", for the first base layer, the first adhesive layer, the second base layer, and the second adhesive layer shown in Table 5, the laminate before curing was prepared in the same manner as in Example 1, the release film protecting the second adhesive layer was peeled off, and the Space Clean S2600 prepared as the third base layer was laminated on the second adhesive layer so that the TD direction overlaps with the MD direction of the first and second base layers, and the MD direction overlaps with the TD direction of the first and second base layers, respectively. Then, a laminate film (c) in which pressure-sensitive adhesive layer A was formed as the third pressure-sensitive adhesive layer in the same manner as for the laminate film (a) was overlaid with the pressure-sensitive adhesive layer A facing the third base layer, and the laminate film (c) was left to stand at 40°C for 2 days for aging, thereby obtaining a pressure-sensitive adhesive tape having a first base layer, a first pressure-sensitive adhesive layer, a second base layer, a second pressure-sensitive adhesive layer, a third base layer, and a third pressure-sensitive adhesive layer in this order. In the above-mentioned "(Preparation of Pressure-Sensitive Adhesive Tape)", measurements and calculations were carried out in the same manner as in Example 1, except that the pressure-sensitive adhesive tape was prepared in this manner. The results are shown in Table 5.
[0136] The types of substrates shown in Tables 1 to 6 are as follows: Volara XL-H#0180015 (polyethylene foam, manufactured by Sekisui Chemical Co., Ltd.) Volara XL-H#05002 (polyethylene foam, manufactured by Sekisui Chemical Co., Ltd.) Volara XL-H#018002 (polyethylene foam, manufactured by Sekisui Chemical Co., Ltd.) Volara XL-H#15004 (polyethylene foam, manufactured by Sekisui Chemical Co., Ltd.) Volara XL-H#12003 (polyethylene foam, manufactured by Sekisui Chemical Co., Ltd.) Saran Wrap (registered trademark) (polyvinylidene chloride film, manufactured by Asahi Kasei Home Products Co., Ltd.) Emblem DCDCR-15 (polyvinylidene chloride coated nylon film, manufactured by Unitika Ltd.) Emblet DCKPT-12 (polyvinylidene chloride coated polyester film, manufactured by Unitika Ltd.) Techbarrier LS (transparent silica vapor-deposited high gas barrier film, manufactured by Mitsubishi Chemical Corporation) BR-PET1012 (aluminum-coated polyester film, manufactured by Toray Advanced Film Co., Ltd.) VM-CPP2203 (aluminum-coated unstretched polypropylene film, manufactured by Toray Advanced Film Co., Ltd.) My Foil (aluminum foil, manufactured by UACJ Foil Co., Ltd.) PE Sheet EL (low-density polyethylene film, manufactured by Sekisui Seikei Co., Ltd.) PE Sheet EH (high-density polyethylene film, manufactured by Sekisui Seikei Co., Ltd.) Hishipet PX-40S (polyester-based shrink film, manufactured by Mitsubishi Chemical Corporation) Krehalon ML40-G (multi-layer heat-shrinkable film, manufactured by Kureha Corporation) FE2002 (polyester film, manufactured by Futamura Chemical Co., Ltd.) Hishipet LX-21S (polyester-based shrink film, manufactured by Mitsubishi Chemical Corporation) Krehalon MT500R (polyvinylidene chloride-based shrink film, manufactured by Kureha Corporation) Fancy Wrap FL2 (polyolefin-based shrink film, manufactured by Gunze Limited) Space Clean S7200 (polyester shrink film, manufactured by Toyobo Co., Ltd.) Space Clean S2600 (polyester shrink film, manufactured by Toyobo Co., Ltd.) Foam layer A (obtained in "(Preparation of foam layer A)" below)
[0137] (Preparation of Foam Layer A) 100 parts by weight of n-butyl acrylate and 11 parts by weight of acrylic acid were introduced into a reaction vessel to obtain a monomer component. The monomer component was dissolved in ethyl acetate, and at the reflux point, 0.1 parts by weight of lauroyl peroxide was added as a polymerization initiator. The mixture was refluxed at 70 ° C. for 5 hours to obtain a solution of an acrylic polymer having a weight average molecular weight of 720,000. For 100 parts by weight of the obtained acrylic polymer, 6.3 parts by weight of rosin ester resin P (softening point 140 ° C.) as a tackifier, 0.054 parts by weight of M-A5DT (manufactured by Soken Chemical & Engineering Co., Ltd., aluminum chelate crosslinking agent), and 2.1 parts by weight of Expancel DU120 (manufactured by Nippon Ferrite Co., Ltd., thermally expandable microcapsules) were blended and mixed. The resulting mixture was poured into a mold and left at 120 ° C. for 0.03 hours, and the expansion ratio was 1.5 cm 3 A foam layer A having a molecular weight of 1 / g and a thickness of 100 μm was obtained.
[0138] <Evaluation> The pressure-sensitive adhesive tapes obtained in the Examples and Comparative Examples were evaluated by the following methods. The results are shown in Tables 1 to 6.
[0139] (Evaluation of Peel Resistance) (1) Preparation of Housing for Evaluation The obtained pressure-sensitive adhesive tape was cut into a frame shape (outer frame 110 mm × 150 mm, inner frame 90 mm × 130 mm) as shown in Figure 6. A housing having a lid portion 31 (96 × 136 mm, thickness 1 mm) and a main body portion 32 made of SUS304 with a surface 2B finish specified in JIS G 4305 was prepared. The main body portion 32 had a main body bottom of 100 mm × 140 mm and a thickness of 5 mm, and the main body side wall portion, when viewed from the direction facing the main body bottom, had an outer frame of 100 mm × 140 mm and an inner frame of 90 mm × 130 mm, a height of 22 mm in the vertical direction from the main body bottom, and a step (outer frame 97 mm × 137 mm, inner frame 90 mm × 130 mm) located 2 mm from the top of the main body. Lid portion 31 was attached to main body portion 32 by superimposing it on top of it as shown in FIG. 7 via a frame-shaped silicone rubber sheet ("Silicone Rubber Sheet" manufactured by AS ONE Corporation, outer frame 94 × 134 mm, inner frame 92 × 132 mm, thickness 1 mm), and then cut adhesive tape 21 was pressed vertically against the top surface of lid portion 31 under conditions of 23°C and 50% RH, and attached so that each of the four sides of the adhesive tape protruded 5 mm beyond lid portion 31 as shown in FIG. 8. Thereafter, a mold 5 (outer frame 140 mm × 180 mm, inner frame 60 mm × 100 mm, thickness 9 mm, step 6 mm from the top of the mold (outer frame 100.6 mm × 140.6 mm, inner frame 60 mm × 100 mm), circular cutouts with a diameter of 2 mm at the four corners of the outer frame of the step) heated to 60°C was pressed against the surface of the housing covered with lid portion 31 as shown in Figure 9, thereby folding back 5 mm of the adhesive tape 21 protruding from lid portion 31 and attaching it to lid portion 31 and the side wall portion of main body portion 32, thereby producing a housing for evaluation.
[0140] (2) Confirmation of Adhesion of Side Portions After the obtained evaluation casing was left standing for 3 days at 23°C and 50% RH, the adhesion of the sides at the attachment positions of the lid portion 31 and the main body portion 32 was visually confirmed, and peel resistance was evaluated. However, adhesion at the corners was not taken into consideration in this evaluation. A case in which the adhesion of the sides was maintained (no peeling was observed) was rated "Good." On the other hand, if peeling was observed even partially at the sides, in the above-mentioned "(1) Preparation of Evaluation Casing," the periphery of the adhesive tape 21 protruding from the lid portion 31 was folded by 5 mm, and the lid portion 31 was attached to the side wall of the main body portion 32. Immediately after this, the surface of the adhesive tape was pressed with a hand roller to prepare an evaluation casing (hereinafter also referred to as a "hand-roller-pressed casing"). The obtained hand-roller-pressed casing was left standing for 3 days at 23°C and 50% RH, and the adhesion of the sides was similarly confirmed. In the above-mentioned hand roller-pressed housing, the case where the adhesiveness of the side portion was maintained was marked "△", and the case where even a part of the side portion was found to have peeled off was marked "X".
[0141] (Evaluation of Corner Sealing Property Onset Temperature) For the evaluation casing after the above-mentioned "(Evaluation of Peel Resistance)", the temperature of the adhesive tape at the corner of the casing was raised in 5°C increments from 50°C using a vinyl chloride welding machine (hot air sprayer) (manufactured by Fuji Impulse, "NS-300") (heating time at each temperature: 10 seconds, maximum temperature: 100°C), and the lowest temperature at which adhesion of the corner was ensured visually was recorded. Temperature control was performed by adjusting the output of the NS-300 and the distance between the hot air sprayer and the adhesive tape while measuring the temperature using a thermographic camera (manufactured by FLIR Systems, "FLIR i60"). However, if the above-mentioned "(Evaluation of Peel Resistance)" was rated "△" or "×", this evaluation was performed using the above-mentioned hand roller crimped casing after the above-mentioned "(Evaluation of Peel Resistance)".
[0142] (Evaluation of Housing Sealing Property (without Corner Heating)) A small temperature and humidity logger (Maxim Corporation, "iButton Hygrochron DS1923-F5#") was placed inside the housing, and the adhesive tape was cut into the shape of FIG. 10 (the shape of FIG. 6 with 5 mm x 5 mm squares removed from the four corners). Except for this, an evaluation housing was produced in the same manner as in "(Evaluation of Peel Resistance)" above. The obtained housing was left to stand at 40°C for 1 hour, and then left to stand at 65°C and 95% RH for 168 hours, after which the humidity inside the housing was measured. The housing sealing property (without corner heating) was evaluated by marking it as "○" when the humidity inside the housing was 60% or less, and "×" when it exceeded 60%. However, if the above-mentioned "(Evaluation of peel resistance)" resulted in a "△" or "X", a small temperature and humidity logger ("iButton Hygrochron DS1923-F5#" manufactured by Maxim) was placed inside the casing, and a hand roller-pressed casing was produced in the same manner as the above-mentioned "(Evaluation of peel resistance)", except that the adhesive tape was cut into the shape of Figure 10 (the shape of Figure 6 with 5 mm x 5 mm squares removed from the four corners), and this evaluation was carried out using the obtained hand roller-pressed casing.
[0143] (Evaluation of Housing Sealing Property (with Corner Heating)) A housing for evaluation was produced in the same manner as in the above-mentioned "(Evaluation of Peel Resistance)" except that a small temperature and humidity logger (Maxim Corporation, "iButton Hygrochron DS1923-F5#") was placed inside the housing, and the corners of the housing, which had been folded and bonded to the adhesive tape, were further heated for 10 seconds at either 75°C, 85°C, or 95°C. The obtained housing for evaluation was left to stand at 40°C for 1 hour, and then further left to stand in an environment of 65°C and 95% RH for 168 hours, after which the humidity inside the housing was measured. When the corners of the housing were heated at 75 ° C., the humidity inside the housing was 60% or less, as indicated by "◎", when the corners of the housing were heated at 85 ° C., the humidity inside the housing was 60% or less, as indicated by "○", when the corners of the housing were heated at 95 ° C., the humidity inside the housing was 60% or less, as indicated by "△", and when the humidity exceeded 60% in either case, the housing sealability (with corner heating) was evaluated. However, if the result in the above-mentioned "(Evaluation of peel resistance)" was "△" or "×", a small temperature and humidity logger (manufactured by Maxim, "iButton Hygrochron DS1923-F5#") was inserted inside the housing, and the corners of the housing to which the adhesive tape was folded and bonded were further heated at either 75 ° C., 85 ° C., or 95 ° C. for 10 seconds. A hand roller-pressed housing was prepared in the same manner as in the above-mentioned "(Evaluation of peel resistance)", and this evaluation was performed using the obtained hand roller-pressed housing. Even if the evaluation is "X", the pressure-sensitive adhesive tape of the present invention can be used to seal HDDs without any problems.
[0144] (Evaluation of Housing Sealant Property (with Corner Heating, Long-Term)) Using adhesive tapes obtained in the same manner as those adhesive tapes for which the evaluation result of the above-mentioned "(Evaluation of Housing Sealant Property (with Corner Heating))" was "◎", "◯", or "△", the humidity inside the housing was measured in the same manner as the above-mentioned "(Evaluation of Housing Sealant Property (with Corner Heating))", except that the heating temperature of the corners of the housing was changed to the temperature at which the humidity inside the housing became 60% or less in the above-mentioned "(Evaluation of Housing Sealant Property (with Corner Heating))" and the standing time in an environment of 65°C and 95% RH was changed to 336 hours. Here, the above "temperature at which the humidity inside the housing became 60% or less in the "(Evaluation of Housing Sealant Property (with Corner Heating))"" means 75°C for those for which the evaluation result of the above-mentioned "(Evaluation of Housing Sealant Property (with Corner Heating))" was "◎", 85°C for those for which the evaluation result was "◯", and 95°C for those for which the evaluation result was "△". The housing sealing ability (with corner heating, for a long period of time) was evaluated based on the following criteria: when the humidity inside the housing was 50% or less, it was marked "◎", when it was more than 50% but not more than 60%, it was marked "◯", and when it was more than 60%, it was marked "×". Note that even if the evaluation is "×", the pressure-sensitive adhesive tape of the present invention can be used to seal HDDs without any problems.
[0145]
[0146]
[0147]
[0148]
[0149]
[0150]
[0151] According to the present invention, it is possible to provide an adhesive tape having excellent barrier properties and L-shaped bend application properties. Also, according to the present invention, it is possible to provide a method for manufacturing a hard disk drive that has excellent sealing properties even when the housing is sealed from the outside by using the adhesive tape. Furthermore, according to the present invention, it is possible to provide a hard disk drive sealing structure that is sufficiently sealed even when the housing is sealed from the outside.
[0152] tn Thickness of the nth layer from the outermost surface (n = 1, 2 ...) h n b: Sum of thicknesses from the outermost layer to the nth layer (n=1, 2, ...) b: Bending width λ: Distance from the neutral axis of the adhesive tape to the outermost surface 0: Lid of HDD 01: Top surface 02: Lid corner 1: Main body of HDD 11: Bottom of main body 12: Side wall of main body 13: Corner of main body 2: Adhesive tape 21: Adhesive tape used in evaluation of peel resistance 22: Adhesive tape used in evaluation of housing sealability (no corner heating) 31: Lid of HDD used in evaluation of peel resistance 32: Main body of HDD used in evaluation of peel resistance 4: Mold 41: Upper surface of bottom of mold 42: Lower surface of bottom of mold 43: Side wall of mold 5: Mold used in evaluation of peel resistance
Claims
1. Water vapor permeability at 40°C and 90% RH is 7.5 g / (m 2 ·day) or less, and the bending stiffness at 25°C at a bending width of 2.0 mm in at least one of the MD direction and the TD direction is 1.0 N·mm 2 or less, and a 180° peel strength from SUS at 23° C. is 5.0 N / 25 mm or more.
2. In at least one of the MD and TD directions, the bending stiffness at 25°C at a bending width of 2.0 mm is 0.45 N mm 2 The adhesive tape according to claim 1, wherein:
3. The adhesive tape according to claim 1 or 2, which has a 10% heat shrinkage temperature of 95°C or less in at least one of the MD and TD directions.
4. The adhesive tape according to claim 1, 2 or 3, wherein the adhesive tape has two or more layers, the two or more layers including at least a first base layer and a first adhesive layer, and all of the two or more layers of the adhesive tape satisfy a product of the tensile storage modulus and thickness at 25°C of 200 MPa mm or less.
5. The first base layer has a water vapor permeability of 40 g / (m 2 5. The adhesive tape according to claim 4, wherein the adhesion is 0.05-0.5% (day) or less.
6. The adhesive tape according to claim 4 or 5, wherein the first base layer contains a foam.
7. The adhesive tape of claim 6, wherein said foam comprises a polyolefin foam.
8. An adhesive tape according to claim 4, 5, 6 or 7, wherein the first base layer has a 10% heat shrinkage temperature of 95°C or less in at least one of the MD and TD directions.
9. The adhesive tape according to claim 8, wherein the first base layer has a 10% heat shrinkage temperature of 95° C. or less in both the MD and TD directions.
10. The adhesive tape has the first base layer, the first adhesive layer, the second base layer, and the second adhesive layer in this order, the first base layer contains a foam, and the first base layer has a water vapor transmission rate of 40 g / (m2) at 40° C. and 90% RH. 2 10. The pressure-sensitive adhesive tape according to claim 4, wherein the product of the average tensile storage modulus at 25°C in the MD and TD directions and the thickness of the first base material layer is 50 MPa mm or less, and the second base material layer has a 10% heat shrinkage temperature of 95°C or less in at least one of the MD and TD directions.
11. The adhesive tape according to claim 4, 5, 6, 7, 8, 9 or 10, further comprising an inorganic layer.
12. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or 11, which has a thickness of 0.20 mm or more.
13. A method for manufacturing a hard disk drive having a body portion with a hard disk and a cover portion, comprising a step of attaching an adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12 to the body portion and the cover portion to seal the hard disk drive.
14. A method for manufacturing a hard disk drive according to claim 13, wherein the step of sealing the hard disk drive comprises folding and attaching the adhesive tape from the lid portion to the main body portion, and then thermally shrinking the adhesive tape.
15. A method for manufacturing a hard disk drive as described in claim 14, wherein the main body includes a main body bottom and a main body side wall protruding upward from the outer periphery of the main body bottom, the lid is structured to be attached onto the main body side wall of the main body, and the process of sealing the hard disk drive includes a process (I) of folding and attaching the adhesive tape from the lid to the main body side wall, and a process (II) of thermally shrinking the adhesive tape after the process (I).
16. A method for manufacturing a hard disk drive as described in claim 15, wherein the main body has a main body corner on a surface of the main body side wall to which the lid is attached, and the lid has a lid corner that contacts the main body corner, and in step (I), the adhesive tape is folded and attached at least from the lid corner to the main body corner, and in step (II), the portion of the adhesive tape attached from the lid corner to the main body corner is thermally shrunk.
17. A method for manufacturing a hard disk drive as claimed in claim 15 or 16, wherein in step (I), the lid is attached onto the main body side wall, the adhesive tape is attached to the outer periphery of the upper surface of the lid so that a portion of the adhesive tape is located outside the outer periphery of the upper surface of the lid, a mold including a mold bottom and a mold side wall protruding downward from the outer periphery of the mold bottom is pressed against the upper surface of the lid and the lower surface of the mold bottom so that they face each other, the adhesive tape is folded so that the portion of the adhesive tape not in contact with the upper surface of the lid is located between the mold side wall and the main body side wall, and the adhesive tape is attached to the main body side wall, thereby bonding the main body and the lid.
18. A method for manufacturing a hard disk drive as set forth in claim 17, wherein the mold is heated to 35° C. or higher and 60° C. or lower when the top surface of the lid and the bottom surface of the mold are pressed against each other so that they face each other.
19. A method for manufacturing a hard disk drive as described in claim 15, 16, 17 or 18, wherein in step (I), the adhesive tape is frame-shaped having a shape corresponding to the outer peripheral edge of the upper surface of the lid portion, and the outer frame of the frame-shaped adhesive tape is attached so as to be positioned outside the outer peripheral edge of the upper surface of the lid portion.
20. A method for manufacturing a hard disk drive as claimed in claim 15, 16, 17, 18 or 19, wherein in step (II), the adhesive tape is thermally shrunk by 10% or more in at least one of the MD and TD directions, and the adhesive tape is thermally shrunk at a temperature of 95°C or less.
21. A hard disk drive sealing structure comprising a body and a lid, the body and the lid being secured together by a heat-shrunk adhesive tape.
Citation Information
Patent Citations
Hermetic sealing vessel and hermetic sealing method
JP1996161881A
Sealing method of electronic component
JP2007141292A
Adhesive sheet, and magnetic disc device
JP2019073711A
Pressure sensitive adhesive sheet and pressure sensitive adhesive sheet having release liner
JP2023011339A
Multilayer foam sheet and adhesive tape
JP2023051882A