Method for forming catalyst layer using anion exchange membrane
The direct growth of a catalyst layer on an anion exchange membrane using aqueous solutions addresses the limitations of conventional methods, enhancing interfacial properties and stability, thereby improving water electrolysis performance at room temperature and pressure.
Patent Information
- Application Number
- PCT/KR2023/019060
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2023-11-24
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional catalyst layer formation methods for anion exchange membrane water electrolyzers face challenges in improving interfacial properties and chemical, thermal, and mechanical stability, leading to reduced performance due to the use of ionomers and high temperature/pressure requirements.
A method of directly growing a catalyst layer on an anion exchange membrane using an aqueous reducing agent and metal precursor solutions, without an ionomer or binder, between substrates, allowing for improved interfacial properties and versatility at room temperature and pressure.
This method enhances electrochemical performance by improving interfacial properties within the membrane electrode assembly, reducing interfacial resistance, and maintaining stability, thus improving the overall water electrolysis performance.
Smart Images

Figure KR2023019060_05122024_PF_FP_ABST
Abstract
Description
Method for forming a catalyst layer using an anion exchange membrane
[0001] The present invention relates to a method for forming a catalyst layer in an electrochemical device, and more specifically, to a method for forming a catalyst layer by directly growing the catalyst layer using an anion exchange membrane.
[0002] The most important element that determines the electrolysis performance of an anion exchange membrane water electrolyzer (AEMWE) system may be the membrane electrode assembly (MEA), which may be composed of an anion exchange membrane, a catalyst layer, an ionomer capable of ion exchange, and a gas diffusion layer (GDL).
[0003] In manufacturing membrane electrode assemblies, a powder-type catalyst is used, and ink is prepared by dispersing an ionomer as a binder and the catalyst in a specific solvent. Then, various coating techniques are used to coat a conductive GDL or anion exchange membrane, typically using the CCS (catalyst coated substrate) or CCM (catalyst coated membrane) method.
[0004] A characteristic of membrane electrode assemblies manufactured using CCS or CCM is that the ionomer immobilizes the catalyst on a specific substrate and provides a pathway for ion transport for electrochemical reactions. However, it also prevents exposure of active sites on the catalyst surface and inhibits the release of hydrogen or oxygen gas products produced during electrolysis, thereby degrading the performance of the overall electrolysis device. To address these shortcomings, ionomer-free self-supported electrodes have been developed.
[0005] To manufacture ionomer-free self-supported electrodes, various processes suitable for various conductive supports have been developed, including hydrothermal / solvent synthesis, electroplating, chemical vapor deposition, and chemical corrosion. Self-supported electrodes can not only solve the problems of using ionomers, but also improve the overall water electrolysis performance through improved interfacial properties due to the interaction between the directly grown catalyst layer and the conductive GDL used as a support.
[0006] However, since the interface properties of the anion exchange membrane and the catalyst layer in the membrane electrode assembly are not improved, an additional membrane electrode assembly manufacturing method is required. In addition, since the methods generally used to manufacture self-supporting electrodes are difficult to apply to anion exchange membranes with low chemical, thermal, and mechanical stability, development of a new process is required.
[0007]
[0008] [Prior Art Literature]
[0009] [Patent Document]
[0010] Republic of Korea Patent Publication No. 10-2022-0136465
[0011]
[0012] The purpose of the present invention is to solve problems in conventional catalyst layer forming methods and to provide a catalyst layer forming method applicable to an anion exchange membrane (AEM).
[0013] The purposes of the present invention are not limited to those mentioned above, and other purposes not mentioned will be clearly understood from the description below.
[0014] A method for forming a catalyst layer using an anion exchange membrane according to one embodiment of the present invention comprises the steps of: preparing an anion exchange membrane (AEM) positioned between a first substrate and a second substrate; supplying a reducing agent solution to the first substrate side and supplying a metal precursor solution to the second substrate side; and removing the metal precursor solution supplied to the second substrate side, and then additionally supplying the reducing agent solution supplied to the first substrate side.
[0015] The above first substrate and the above second substrate can supply fluid from the outside to the anion exchange membrane.
[0016] The above first substrate and the above second substrate may be a current collector or a gas diffusion layer (GDL).
[0017] The metal of the above metal precursor may have a standard reduction potential that is higher in a positive (+) value than the standard reduction potential of the reducing agent.
[0018] The concentration of the above reducing agent solution may be higher than the concentration of the above metal precursor solution.
[0019] The above reducing agent may be NaBH4.
[0020] The above metal precursor may be a metal chloride.
[0021] The metal of the above metal precursor may be nickel (Ni) or iron (Fe).
[0022]
[0023] The present invention has the effect of growing a catalyst layer directly on an anion exchange membrane (AEM) without using an ionomer or binder, and has the effect of accommodating the low physicochemical properties of the anion exchange membrane (AEM).
[0024] In addition, the present invention has the effect of excellent versatility, as it can be applied regardless of the structural and chemical characteristics of an anion exchange membrane (AEM) under room temperature and pressure conditions rather than high temperature and high pressure conditions.
[0025] In addition, when manufacturing a membrane electrode assembly (MEA) using the present invention, there is an effect of improving the electrochemical performance by improving the interfacial characteristics within the membrane electrode assembly (MEA).
[0026] The technical effects of the present invention are not limited to those mentioned above, and other technical effects not mentioned will be clearly understood by those skilled in the art from the description below.
[0027] Figure 1 is a schematic diagram illustrating a method for forming a catalyst layer using an anion exchange membrane according to one embodiment of the present invention.
[0028] FIG. 2 illustrates a photographic image and an SEM image of a catalyst layer manufactured by a method for forming a catalyst layer using an anion exchange membrane according to one embodiment of the present invention.
[0029] FIG. 3a, FIG. 3b, FIG. 4a and FIG. 4b illustrate the results of EDS analysis of a catalyst layer manufactured by a method for forming a catalyst layer using an anion exchange membrane according to one embodiment of the present invention.
[0030] Figures 5 to 7 illustrate the results of performance analysis of a water electrolysis device using a catalyst layer manufactured by a method for forming a catalyst layer using an anion exchange membrane according to one embodiment of the present invention.
[0031]
[0032] A method for forming a catalyst layer using an anion exchange membrane according to one embodiment of the present invention comprises the steps of: preparing an anion exchange membrane (AEM) positioned between a first substrate and a second substrate; supplying a reducing agent solution to the first substrate side and supplying a metal precursor solution to the second substrate side; and removing the metal precursor solution supplied to the second substrate side, and then additionally supplying the reducing agent solution supplied to the first substrate side.
[0033] The above first substrate and the above second substrate can supply fluid from the outside to the anion exchange membrane.
[0034] The above first substrate and the above second substrate may be a current collector or a gas diffusion layer (GDL).
[0035] The metal of the above metal precursor may have a standard reduction potential that is higher in a positive (+) value than the standard reduction potential of the reducing agent.
[0036] The concentration of the above reducing agent solution may be higher than the concentration of the above metal precursor solution.
[0037] The above reducing agent may be NaBH4.
[0038] The above metal precursor may be a metal chloride.
[0039] The metal of the above metal precursor may be nickel (Ni) or iron (Fe).
[0040]
[0041] Hereinafter, embodiments of the present invention will be described in detail to facilitate easy implementation by those skilled in the art. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein. Furthermore, like reference numbers represent like elements throughout the specification.
[0042]
[0043] Hereinafter, the present invention will be described in detail with reference to the attached drawings.
[0044] A method for forming a catalyst layer using an anion exchange membrane according to one embodiment of the present invention is a method for forming a catalyst layer directly on an anion exchange membrane (AEM), and is a method for forming a catalyst layer by supplying a reducing agent and a metal precursor onto an electrochemical device equipped with an anion exchange membrane (AME).
[0045]
[0046] A method for forming a catalyst layer using an anion exchange membrane according to one embodiment of the present invention includes the steps of: preparing an anion exchange membrane (AEM) positioned between a first substrate and a second substrate (S100); supplying a reducing agent solution to the first substrate side and supplying a metal precursor solution to the second substrate side (S200); and removing the metal precursor solution supplied to the second substrate side and then additionally supplying the reducing agent solution supplied to the first substrate side (S300). The method may further include supplying deionized water (DI water) to the first substrate side and the second substrate side for washing (S400).
[0047]
[0048] S100 is a step of preparing an anion exchange membrane for growing a catalyst, and may be a step of positioning the anion exchange membrane between the first substrate and the second substrate.
[0049] The above first substrate may supply a fluid from the outside to the anion exchange membrane, and the fluid supplied to the first substrate may be a reducing agent, and may be supplied in the form of a reducing agent aqueous solution, and the reducing agent aqueous solution may use distilled water (DI water) as a solvent.
[0050] The first substrate may be a current collector or a gas diffusion layer (GDL), and the first substrate may be on the cathode side, but is not limited thereto. The current collector may be provided with a flow path through which a fluid may flow, and the current collector may be a conductor, and may be nickel (Ni), titanium (Ti), or stainless steel, but is not limited thereto. The gas diffusion layer (GDL) may be a porous conductor, and examples thereof include, but are not limited to, Ni fiber paper, stainless steel fiber paper, carbon fiber paper, carbon cloth, or Ti mesh.
[0051] The second substrate may supply a fluid from the outside to the anion exchange membrane, and the fluid supplied to the second substrate may be a metal precursor, and may be supplied in the form of a metal precursor aqueous solution, and the metal precursor aqueous solution may use distilled water (DI water) as a solvent.
[0052] The second substrate may be a current collector or a gas diffusion layer (GDL), and the second substrate may be on the anode side, but is not limited thereto. The current collector may be provided with a flow path through which a fluid may flow, and the current collector may be a conductor, and may be nickel (Ni), titanium (Ti), or stainless steel, but is not limited thereto. The gas diffusion layer (GDL) may be a porous conductor, and may be, for example, Ni fiber paper, stainless steel fiber paper, or Ti mesh, but is not limited thereto.
[0053] S100 may provide a membrane electrode assembly (MEA) according to the types of the first substrate and the second substrate, and more specifically, may provide a membrane electrode assembly (MEA) without a catalyst layer.
[0054]
[0055] S200 is a step for forming a catalyst layer on both sides or both surfaces of the anion exchange membrane, and forms a catalyst layer on the anion exchange membrane by utilizing the movement and diffusion of anions.
[0056] S200 may supply the above reducing agent solution, and may supply the metal precursor solution while maintaining the supply of the reducing agent solution after a predetermined period of time has elapsed, until the supply of the reducing agent solution is completed.
[0057] In S200, the reducing agent aqueous solution may be supplied at a predetermined concentration, for a predetermined time, and at a predetermined flow rate. The reducing agent may be NaBH4. At this time, the concentration of the reducing agent aqueous solution may be higher than the concentration of the metal precursor aqueous solution. The concentration of the reducing agent aqueous solution may be 1 M, but is not limited thereto. In addition, the reducing agent aqueous solution may be supplied at a flow rate of 20 mL / min for 20 to 30 minutes (min), and even during the supply of the metal precursor aqueous solution described below, the supply of the reducing agent aqueous solution may be continuously repeated at the predetermined time and flow rate to maintain the supply of the reducing agent aqueous solution.
[0058] In S200, the metal precursor aqueous solution may be supplied at a predetermined concentration, for a predetermined time, and at a predetermined flow rate. The metal of the metal precursor may have a standard reduction potential that is higher in a positive (+) value than the standard reduction potential of the reducing agent. The metal precursor may be a metal chloride, but is not limited thereto. As an example, the metal of the metal precursor may be nickel (Ni) or iron (Fe). When the metal precursor is a nickel (Ni) precursor, the concentration of the nickel (Ni) precursor aqueous solution may be 0.375 M, and when the metal precursor is an iron (Fe) precursor, the concentration of the iron (Fe) precursor aqueous solution may be 0.125 M, but is not limited thereto. In addition, the reducing agent aqueous solution may be supplied at a flow rate of 20 mL / min for 20 to 30 minutes (min), but is not limited thereto.
[0059]
[0060] S300 is a step of removing the metal precursor solution supplied to the second substrate side, and then additionally adding a reducing agent to reduce the metal supplied to the anion exchange membrane through the metal precursor solution.
[0061] In S300, the reducing agent solution may be supplied at a predetermined concentration, for a predetermined time, and at a predetermined flow rate. The reducing agent may be NaBH4. The concentration of the reducing agent solution may be 1 M, but is not limited thereto. In addition, the reducing agent solution may be supplied at a flow rate of 20 mL / min for 20 to 30 minutes (min), but is not limited thereto.
[0062] In S300, a catalyst layer may be formed on the surface of the anion exchange membrane in the second substrate side direction by supplying the reducing agent solution.
[0063]
[0064] S400 is a step for removing remaining reaction by-products and impurities after the growth and formation of the catalyst layer on the anion exchange membrane is completed.
[0065] S400 can be cleaned using pure distilled water (DI water).
[0066]
[0067] FIG. 1 is a schematic diagram illustrating an example of a method for forming a catalyst layer using an anion exchange membrane according to an embodiment of the present invention. Referring to FIG. 1, a gas diffusion layer (GDL) (corresponding to the 'first substrate' and the 'second substrate') is provided on each of the cathode side and the anode side, and an anion exchange membrane (AEM; Anion exchange membrane) is positioned between the two gas diffusion layers (GDL). Thereafter, an aqueous solution of NaBH4 is supplied as a reducing agent to the cathode side where each flow path is formed, and an aqueous solution of a metal precursor (Ni) is supplied to the anode side. 2+ ion, Fe 3+ ions) is supplied. At this time, BH4 in the supplied NaBH4 aqueous solution - Ions move to the opposite side of the anion exchange membrane and Ni in the metal precursor solution 2+ ions and Fe 3+ A catalyst layer is formed on the anion exchange membrane toward the anode side through a chemical reaction on the surface of the ion and anion exchange membrane. After the catalyst layer is formed, any remaining reaction byproducts and impurities are removed using deionized (DI) water.
[0068]
[0069] Hereinafter, the present invention will be described in more detail through examples.
[0070]
[0071] Example 1. Growth of a catalyst layer on the surface of an anion exchange membrane using a water electrolysis device.
[0072] Ni fiber paper was prepared as the substrate for the cathode electrode and anode electrode and as the gas diffusion layer (GDL), respectively.
[0073]
[0074] Thereafter, referring to FIG. 1, an anion exchange membrane (AEM) is placed between Ni fiber paper (cathode electrode) as a gas diffusion layer (GDL) on the cathode side and Ni fiber paper (anode electrode) as a gas diffusion layer (GDL) on the anode side, and a cathode-side current collector (current collector) with a channel formed thereon and an anode-side current collector (current collector) with a channel formed thereon are placed in opposite directions of the anion exchange membranes of the cathode electrode and the anode electrode, respectively, to assemble a water electrolysis device, and Sustainion® X37-50 is used as the anion exchange membrane. At this time, the cathode electrode and the anode electrode perform the function of a gas diffusion layer (GDL) simultaneously.
[0075] Thereafter, a 1 M NaBH4 aqueous solution is supplied to the cathode-side current collector at 20 ml / min for 30 min, and then, while maintaining the supply of the NaBH4 aqueous solution, a metal precursor mixed aqueous solution (total 16 mL, final NiCl2 concentration: 0.375 M, final FeCl3 concentration: 0.125 M) containing 3 mL of NiCl2·6H2O (2 M) and 1 mL of FeCl3·6H2O (2 M) in 12 mL of deionized water is supplied to the anode-side current collector at 20 ml / min for 30 min. Thereafter, all of the mixed aqueous solution remaining on the anode-side current collector is removed, and a 1 M NaBH4 aqueous solution is additionally supplied to the cathode-side current collector at 20 ml / min for 30 min. Afterwards, in order to remove the reaction byproducts and impurities remaining in the cathode-side current collector and the anode-side current collector, DI water is supplied to wash them respectively.
[0076]
[0077] Example 2. Growth of a catalyst layer on the surface of an anion exchange membrane using a water electrolysis device.
[0078] The same procedure as in Example 1 was performed, but fumasep® FAA-3-50 was used as the anion exchange membrane.
[0079]
[0080] Example 3. Growth of a catalyst layer on the surface of an anion exchange membrane using a water electrolysis device.
[0081] The same procedure as in Example 1 was performed, but fumasep® FAS-50 was used as the anion exchange membrane.
[0082]
[0083] Example 4. Growth of a catalyst layer on the surface of an anion exchange membrane using a water electrolysis device.
[0084] The same procedure as in Example 1 was performed, but PiperION AEM (PiperION Anion Exchange Membrane, 80 microns) was used as the anion exchange membrane.
[0085]
[0086] Measurement example. Surface analysis
[0087] In order to observe whether a catalyst was formed on the anion exchange membrane through the above Examples 1 to 4, the photographic images and SEM analysis results of the anion exchange membranes before and after catalyst growth according to the above Examples 1 to 4 are shown in FIG. 2. In FIG. 2, the anion exchange membrane in Example 1 is indicated as "Sustatinion X37-50", the anion exchange membrane in Example 2 as "FAA-3-50", the anion exchange membrane in Example 3 as "FAS-50", and the anion exchange membrane in Example 4 as "PiperION". Before catalyst growth is indicated as "Before", and after catalyst growth is indicated as "After", and the bottommost image of each is an SEM image after catalyst growth.
[0088] Referring to Fig. 2, it can be confirmed that a catalyst was directly grown on each of the anion exchange membranes in Examples 1 to 4 through color change (see After), and it can be confirmed that a catalyst layer having a nanosheet form perpendicular to the surface was formed through the SEM image (bottom image).
[0089]
[0090] Measurement example. EDS analysis
[0091] EDS analysis of the surface and cross-section of the anion exchange membrane manufactured in Example 1 was performed, and the EDS analysis images are shown in FIGS. 3a to 4b.
[0092] Fig. 3a is a surface EDS image of the anion exchange membrane manufactured in Example 1, and Fig. 3b illustrates the results of surface EDS spectrum analysis of the anion exchange membrane manufactured in Example 1. The results of elemental analysis according to the surface EDS analysis of the anion exchange membrane manufactured in Example 1 are summarized in Table 1 below.
[0093] Elementwt.%Atomic%C K9.5430.19O K9.0914.48Fe L20.3013.82Ni l64.0741.51Total100.00100.00
[0094]
[0095] Fig. 4a is a cross-sectional EDS image of the anion exchange membrane manufactured in Example 1, and Fig. 4b illustrates the results of a cross-sectional EDS spectrum analysis of the anion exchange membrane manufactured in Example 1. The results of the elemental analysis according to the cross-sectional EDS analysis of the anion exchange membrane manufactured in Example 1 are summarized in Table 2 below.
[0096] Elementwt.%Atomic%C K43.7872.47N K1.191.7O K7.779.66Fe L9.793.48Ni l37.4712.69Total100.00100.00
[0097]
[0098] Referring to FIGS. 3a to 4b, Tables 1 and 2, it can be confirmed that the metal elements are uniformly distributed in the catalyst layer at a ratio equal to the concentration of the metal precursor aqueous solution used, and further, in the case of the cross-section, it can be confirmed that the metal ions diffuse inward from the surface of the anion exchange membrane by several micrometers, so that a diffusion layer can also be formed inside the anion exchange membrane. This indirectly demonstrates a strong interaction between the catalyst layer and the anion exchange membrane.
[0099]
[0100] Comparative Example 1. Fabrication of a water electrolysis device using a catalyst coated substrate (CCS).
[0101] Comparative Example 1-1. Synthesis of anode catalyst and preparation of anode electrode
[0102] To prepare an anode catalyst, a mixed metal solution (total 16 mL, final NiCl2 6H2O (2 M) 3 mL and final FeCl3 6H2O (2 M) 1 mL were added to 12 mL of deionized water (DI water) for 30 mL of a 1 M NaBH4 solution, and stirred for 5 minutes to prepare a mixed solution. After confirming that the color of the mixed solution had changed to transparent, centrifugation was performed to separate the solid catalyst, and the separated catalyst was washed using distilled water (DI water) and ethanol, and then freeze-dried for one day (24 hours) to obtain the final anode catalyst.
[0103] To prepare an anode catalyst ink, 50 mg of the obtained anode catalyst was added to a solvent mixture of 4.94 mL of distilled water (DI water), 4.94 mL of anhydrous 2-propanol, and 0.12 mL of FAA-3-SOLUT-10 (for binder and ionomer use), and the anode catalyst was uniformly dispersed through ultrasonic treatment to prepare an anode catalyst ink.
[0104] The manufactured anode catalyst ink was spray-coated on Ni fiber paper as an electrode substrate and gas diffusion layer (GDL) at 2 mg / cm. 2 It was coated with a quantity of .
[0105]
[0106] Comparative Example 1-2. Preparation of an anion exchange membrane (AEM)
[0107] Sustainion® X37-50 was prepared as an anion exchange membrane.
[0108]
[0109] Comparative Example 1-3. Cathode Electrode Manufacturing
[0110] As a cathode catalyst, 20 wt% Pt / C was prepared, and 50 mg of the prepared Pt / C was uniformly dispersed in a solvent containing 6 mL of distilled water (DI water), 3 mL of anhydrous 2-propanol, and 1 mL of Nafion 117 solution by ultrasonic treatment to prepare a cathode catalyst ink. The cathode catalyst ink was spray-coated on carbon fiber paper at a concentration of 2 mg / cm. 2 The cathode electrode was manufactured by coating with a quantity of .
[0111]
[0112] Comparative Example 1-4. Fabrication of a Water Electrolysis Device
[0113] An anode electrode (Comparative Example 1-1) and a cathode electrode (Comparative Example 1-3) were placed with an anion exchange membrane (Sustainion® X37-50) (Comparative Example 1-2) between them, and a current collector was placed in which each path was formed in the direction of the anode electrode and the cathode electrode that did not come into contact with the anion exchange membrane, thereby manufacturing a water electrolysis device.
[0114]
[0115] Comparative Example 2. Fabrication of a water electrolysis device using a catalyst coated membrane (CCM).
[0116] Comparative Example 2-1. Synthesis of anode catalyst and preparation of anion exchange membrane (AEM).
[0117] To prepare an anode catalyst, a mixed metal solution (total 16 mL, final NiCl2 6H2O (2 M) 3 mL and final FeCl3 6H2O (2 M) 1 mL were added to 12 mL of deionized water (DI water) for 30 mL of a 1 M NaBH4 solution, and stirred for 5 minutes to prepare a mixed solution. After confirming that the color of the mixed solution had changed to transparent, centrifugation was performed to separate the solid catalyst, and the separated catalyst was washed using distilled water (DI water) and ethanol, and then freeze-dried for one day (24 hours) to obtain the final anode catalyst.
[0118] To prepare an anode catalyst ink, 50 mg of the obtained anode catalyst was added to a solvent mixture of 4.94 mL of distilled water (DI water), 4.94 mL of anhydrous 2-propanol, and 0.12 mL of FAA-3-SOLUT-10 (for binder and ionomer use), and the anode catalyst was uniformly dispersed through ultrasonic treatment to prepare an anode catalyst ink.
[0119] The manufactured anode catalyst ink was spray-coated on an anion exchange membrane (Sustainion® X37-50) at 2 mg / cm 2 It was coated with a quantity of .
[0120]
[0121] Comparative Example 2-2. Preparation of Anode Electrode
[0122] Ni fiber paper was prepared as an anode electrode and a gas diffusion layer (GDL).
[0123]
[0124] Comparative Example 2-3. Cathode Electrode Manufacturing
[0125] As a cathode catalyst, 20 wt% Pt / C was prepared, and 50 mg of the prepared Pt / C was uniformly dispersed in a solvent containing 6 mL of distilled water (DI water), 3 mL of anhydrous 2-propanol, and 1 mL of Nafion 117 solution by ultrasonic treatment to prepare a cathode catalyst ink. The cathode catalyst ink was spray-coated on carbon fiber paper at a concentration of 2 mg / cm. 2 The cathode electrode was manufactured by coating with a quantity of .
[0126]
[0127] Comparative Example 2-4. Fabrication of a Water Electrolysis Device
[0128] An anode electrode (Comparative Example 2-2) was placed on the side of the anion exchange membrane coated with the anode catalyst, and a cathode electrode (Comparative Example 2-3) was placed on the side not coated with the anode catalyst, with an anion exchange membrane (Sustainion® X37-50) (Comparative Example 2-1) coated with the anode catalyst interposed therebetween, and a current collector having respective flow paths formed in the direction of the anode electrode and cathode electrode that are not in contact with the anion exchange membrane was placed to manufacture a water electrolysis device.
[0129]
[0130] Measurement example. Fabrication of an anion exchange membrane electrolysis device.
[0131] Measurement Example 1. Cathode Electrode Manufacturing
[0132] As a cathode catalyst, 20 wt% Pt / C was prepared, and 50 mg of the prepared Pt / C was uniformly dispersed in a solvent containing 6 mL of distilled water (DI water), 3 mL of anhydrous 2-propanol, and 1 mL of Nafion 117 solution by ultrasonic treatment to prepare a cathode catalyst ink. The cathode catalyst ink was spray-coated on carbon fiber paper at a concentration of 2 mg / cm. 2 The cathode electrode was manufactured by coating with a quantity of .
[0133]
[0134] Measurement Example 2. Fabrication of a water electrolysis device for performance evaluation.
[0135] In the electrolysis device in which the anion exchange membrane according to Examples 1 to 4 was grown, the Ni fiber paper as the gas diffusion layer (GDL) on the cathode side was removed, and the cathode electrode manufactured in Measurement Example 1 was introduced to manufacture the electrolysis device. The main configurations of the electrolysis devices in Examples 1 to 4 are summarized in Table 3 below.
[0136] Distinction Cathode (GDL) Anion exchange membrane and Anode (GDL) Measurement example 2-1 Measurement example 1 Example 1 Measurement example 2-2 Measurement example 1 Example 2 Measurement example 2-3 Measurement example 1 Example 3 Measurement example 2-4 Measurement example 1 Example 4
[0137]
[0138] Experimental Example. Evaluation of the Performance of Water Electrolysis Using an Anion Exchange Membrane
[0139] For the electrolysis devices according to the above Measurement Example 2 and Table 3, electrolysis performance evaluation (1M KOH, 50°C) was performed, and the results of the electrolysis performance evaluation are shown in Fig. 5. Fig. 5 (a) shows a current-voltage curve, and Fig. 5 (b) shows a Nyquist plot for impedance analysis. In Fig. 5, the electrolysis device of Measurement Example 2-1 (Example 1) was indicated as "Sustainion X37-50", the electrolysis device of Measurement Example 2-2 (Example 2) was indicated as "FAA-3-50", the electrolysis device of Measurement Example 2-3 (Example 3) was indicated as "FAS-50", and the electrolysis device of Measurement Example 2-4 (Example 4) was indicated as "PiperION", respectively. At this time, in the electrolysis performance evaluation, 1M KOH was supplied to the anode side only at 5 mL / min, and the temperature (T) was 50°C.
[0140] Referring to Figure 5, it can be confirmed that the water electrolysis reaction operates normally regardless of the type of anion exchange membrane (see Figure 5 (a)), and it can be confirmed that all anion exchange membranes have the same equivalent circuit (see Figure 5 (b)).
[0141]
[0142] The electrolysis performance evaluation was performed on the electrolysis device of the above measurement example 2-1 (exemplary example 1) and the electrolysis devices of the above comparative examples 1 and 2, and the electrolysis performance evaluation results are shown in Figs. 6 and 7. In Figs. 6 and 7, the electrolysis device of measurement example 2-1 (exemplary example 1) is "AEMEW m-ccm ", the electrolysis device of comparative example 1 is "AEMEW c-ccs ", the electrolysis device of comparative example 2 is "AEMEW c-ccm " were respectively indicated. At this time, in the electrolysis performance evaluation, 1M KOH was supplied to the anode side only at 5 mL / min for the electrolyte, and the temperature (T) was 50°C.
[0143]
[0144] Referring to FIG. 6, it can be confirmed that the same current density can be obtained at a lower potential when using the process according to Measurement Example 2-1 (Example 1) of the present invention compared to the general method (Comparative Examples 1 and 2), which means that the electrolysis performance is improved (see (a) of FIG. 6). In addition, when looking at the impedance of the electrolysis device (electrolysis), the value of the first x-axis intercept in each semicircle represents the sum of the resistance value of the entire electrolysis device and the interfacial resistance of each component for the junction interface, and therefore, it can be confirmed that the interfacial resistance is reduced when using the method according to Measurement Example 2-1 (Example 1) compared to the existing method (Comparative Examples 1 and 2), which helps improve the performance of the electrolysis device (see (b) of FIG. 6).
[0145]
[0146] Referring to Fig. 7, in the long-term stability test, when using the process according to Measurement Example 2-1 (Example 1) of the present invention, a high current density (@ 1000 mAcm) -2 ) can confirm stable electrolysis performance.
[0147]
[0148] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.
Claims
1. A step of preparing an anion exchange membrane (AEM) positioned between the first substrate and the second substrate; A step of supplying a reducing agent solution to the first substrate side and supplying a metal precursor solution to the second substrate side; and A step of removing the metal precursor aqueous solution supplied to the second substrate side and then additionally supplying the reducing agent aqueous solution supplied to the first substrate side. Method for forming a catalyst layer using an anion exchange membrane.
2. In paragraph 1, The above first substrate and the above second substrate supply fluid from the outside to the anion exchange membrane. Method for forming a catalyst layer using an anion exchange membrane.
3. In paragraph 1, The above first description and the above second description, Whether it is a current collector or a gas diffusion layer (GDL), Method for forming a catalyst layer using an anion exchange membrane.
4. In paragraph 1, The metal of the above metal precursor has a standard reduction potential that is higher in a positive (+) value than the standard reduction potential of the reducing agent. Method for forming a catalyst layer using an anion exchange membrane.
5. In paragraph 1, The concentration of the above reducing agent solution is higher than the concentration of the above metal precursor solution. Method for forming a catalyst layer using an anion exchange membrane.
6. In paragraph 1, The reducing agent is NaBH4. Method for forming a catalyst layer using an anion exchange membrane.
7. In paragraph 1, The above metal precursor is a metal chloride, Method for forming a catalyst layer using an anion exchange membrane.
8. In paragraph 6, The metal of the above metal precursor is nickel (Ni) or iron (Fe). Method for forming a catalyst layer using an anion exchange membrane.
Citation Information
Patent Citations
Composition for promoting osteoblast proliferation or differentiation comprsing Sparassis crispa extract as an active ingredient
KR1020220124401A
Device for the production of hydrogen
WO2020260370A1