Display device and manufacturing method therefor

The display device employs a protective member with tailored elastic properties to prevent adhesion failure and buckling at corner curvatures, ensuring the structural integrity of the display device by using materials with specific glass transition temperatures and shrinkage rates.

WO2024248475A1PCT designated stage expired Publication Date: 2024-12-05SAMSUNG DISPLAY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007310
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-29
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Display devices with corner portions face adhesion failure due to deformation of protective members, leading to buckling defects and cracks, especially when applied to curved surfaces.

Method used

A display device design featuring a protective member with a specific elastic modulus and shrinkage rate, applied between the display panel and cover window, to prevent adhesion failure by alleviating strain at corner curvatures, using materials like polyolefin-based or polyester-based resins with a glass transition temperature between 50 to 150 degrees.

Benefits of technology

Prevents buckling and cracks by ensuring proper adhesion and alignment of the display panel and cover window, maintaining the structural integrity of the display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007310_05122024_PF_FP_ABST
    Figure KR2024007310_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A display device according to an embodiment of the present invention comprises: a display panel including a display area; a cover window disposed on the display panel; and a protective member disposed under the display area of the display panel, wherein the protective member has an elastic modulus of 4 GPa or less in a glass transition temperature range, and has a shrinkage rate of 20% or more in a temperature range of 50 degrees to 150 degrees.
Need to check novelty before this filing date? Find Prior Art

Description

Display device and manufacturing method thereof

[0001] The present invention relates to a display device and a method for manufacturing the same.

[0002] As the information society develops, the demand for display devices for displaying images is increasing in various forms. For example, display devices are being used in various electronic devices such as smartphones, digital cameras, laptop computers, navigation systems, and smart televisions.

[0003] As display devices, various types of display devices are used, such as liquid crystal displays (LCDs) and organic light emitting displays (OLEDs). Among these, organic light emitting displays display images using organic light emitting elements that generate light through the recombination of electrons and holes. Organic light emitting displays include a plurality of transistors that provide driving current to the organic light emitting elements.

[0004] As display devices are applied to various electronic devices, display devices with diverse designs are in demand. For example, a display device can display images not only on the front surface but also on the four sides of the front surface, along with the corners positioned between the curved portions.

[0005] The problem to be solved by the present invention is to provide a display device and a manufacturing method thereof that can prevent adhesion failure of a display device having a corner portion.

[0006] The tasks of the present invention are not limited to the tasks mentioned above, and other technical tasks not mentioned will be clearly understood by those skilled in the art from the description below.

[0007] According to one embodiment of the present invention for solving the above problem, a display device includes a display panel including a display area, a cover window disposed on the display panel, and a protective member disposed below the display area of ​​the display panel, wherein the protective member has an elastic modulus of 4 GPa or less in a glass transition temperature range and can have a shrinkage ratio of 20% or more in a temperature range of 50 to 150 degrees.

[0008] The display area may include a flat front portion, curved side portions extending outward from an edge of the front portion and having a curvature, and corner portions disposed between the side portions and having a double curvature.

[0009] The above protective member can be bonded to the entire front portion, the side portions and the corner portions.

[0010] It may further include a first bonding layer disposed between the display panel and the protective member, and a second bonding layer disposed between the display panel and the cover window.

[0011] The glass transition temperature of the above protective member may be in the range of 50 to 150 degrees.

[0012] The above protective member may have an elastic modulus of 0.6 to 0.9 GPa at a temperature range of 74 to 78 degrees.

[0013] The above protective member may include at least one of polyolefin-based, polyvinyl-based, polyethylene-based, and polyester-based resins.

[0014] The thickness of the above protective member may be 25 to 100 μm.

[0015] In addition, a display device according to one embodiment includes a display panel including a display area and a bonding portion spaced apart from the display area, a cover window disposed on the display panel, a first protective member disposed below the display area of ​​the display panel, and a second protective member disposed below the bonding portion of the display panel and spaced apart from the first protective member, wherein a shrinkage ratio of the second protective member may be smaller than a shrinkage ratio of the first protective member.

[0016] The shrinkage ratio of the second protective member and the shrinkage ratio of the first protective member may be shrinkage ratios measured in a temperature range of 50 to 150 degrees.

[0017] The second protective member may have a shrinkage of less than 1% in a temperature range of 50 to 150 degrees.

[0018] The coefficient of thermal expansion of the second protective member may be 30 ppm / ℃ or less in a temperature range of room temperature to 180 degrees.

[0019] The melting point of the above second protective member may be 180 degrees or higher.

[0020] The elastic modulus of the second protective member may be greater than the elastic modulus of the first protective member in a temperature range of 50 degrees to 150 degrees.

[0021] The elastic modulus of the second protective member may be 4.5 GPa or more in a temperature range of 50 degrees to 150 degrees.

[0022] In addition, a method for manufacturing a display device according to one embodiment includes the steps of providing a display panel, a first protective member, and a second protective member, bonding the first protective member and the second protective member to a lower surface of the display panel, aligning a cover window on the display panel and aligning a guide member to a lower surface of the display panel, pressing the cover window, the display panel, and the guide member, heating the first protective member of the display panel through the guide member, and removing the guide member, wherein an elastic modulus of the second protective member may be greater than an elastic modulus of the first protective member.

[0023] The above guide member may include a flat plane portion, curved portions extending outward from an edge of the flat portion and having a curvature, and curved portions disposed between the curved portions and having a double curvature.

[0024] The above guide member includes a first heating member arranged in the above bending portions, and can apply heat to the display panel and the first protective member through the first heating member.

[0025] The above guide member further includes a second heating member arranged in the above bending portions, and can apply heat to the display panel and the first protective member through the first heating member and the second heating member.

[0026] The shrinkage rate of the second protective member may be less than the shrinkage rate of the first protective member in a temperature range of 50 to 150 degrees.

[0027] Specific details of other embodiments are included in the detailed description and drawings.

[0028] A display device and a manufacturing method thereof according to one embodiment can prevent adhesion failure between a display panel and a protective member by deforming the protective member at a corner portion having a curvature of the display device. Accordingly, buckling failure between the display panel and the protective member can be prevented, thereby preventing cracks and disconnection of the display panel.

[0029] The effects according to the embodiments are not limited to those exemplified above, and more diverse effects are included in this specification.

[0030] Figure 1 is a perspective view showing a display device according to one embodiment.

[0031] Figure 2 is a plan view showing a display device according to one embodiment.

[0032] Fig. 3 is a cross-sectional view showing an example of a display panel cut along line Q1-Q1' of Fig. 2.

[0033] FIG. 4 is a plan view schematically illustrating pixels in a display area of ​​a display device according to one embodiment.

[0034] Figure 5 is a cross-sectional view taken along line Q2-Q2' of Figure 4.

[0035] Fig. 6 is a plan view showing a display panel of a display device according to another embodiment.

[0036] Figure 7 is a cross-sectional view taken along line Q3-Q3' of Figure 6.

[0037] Fig. 8 is a cross-sectional view showing another example cut along line Q3-Q3' of Fig. 6.

[0038] Fig. 9 is a flowchart showing a method for manufacturing a display device according to one embodiment.

[0039] Figures 10 to 17 are step-by-step schematic diagrams of a method for manufacturing a display device according to one embodiment.

[0040] Fig. 18 is a graph showing the glass transition temperatures of protective member samples according to one embodiment.

[0041] FIG. 19 is a graph showing the elastic modulus at the glass transition temperature of protective member samples according to one embodiment.

[0042] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the embodiments described in detail below together with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, but may be implemented in various different forms. These embodiments are provided solely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined solely by the scope of the claims.

[0043] When an element or layer is referred to as "on" another element or layer, it includes both cases where it is directly above the other element or layer or where there is another layer or material intervening therebetween. Similarly, when an element or layer is referred to as "below," "left," and "right," it includes both cases where it is directly adjacent to the other element or where there is another layer or material intervening therebetween. Like reference numerals throughout the specification refer to like elements.

[0044] Although terms like "first" and "second" are used to describe various components, these components are not limited by these terms. These terms are used merely to distinguish one component from another. Therefore, it should be understood that a "first" component referred to below may also be a "second" component within the technical scope of the present invention.

[0045] Hereinafter, embodiments will be described with reference to the attached drawings.

[0046] Fig. 1 is a perspective view showing a display device according to one embodiment. Fig. 2 is a plan view showing a display device according to one embodiment.

[0047] Referring to FIGS. 1 and 2, the display device (10) according to one embodiment may include various devices that display a screen or image. For example, the display device (10) according to the embodiments of the present specification may be applied to various home appliances such as a mobile phone, a tablet PC, a PDA (Personal Digital Assistant), a PMP (Portable Multimedia Player), a television, a game console, a wristwatch-type electronic device, a head-mounted display, a monitor of a personal computer, a notebook computer, an automobile navigation system, an automobile dashboard, a digital camera, a camcorder, an external billboard, an electronic display, a medical device, an inspection device, a refrigerator, a washing machine, or an Internet of Things device, in addition to a smartphone.

[0048] In this specification, the short side of the display device (10) on a planar surface may extend in a direction parallel to a first direction (DR1), and the long side of the display device (10) may extend in a direction parallel to a second direction (DR2). For example, the first direction (DR1) and the second direction (DR2) may intersect each other so as to be perpendicular to each other, and the first direction (DR1) on a planar surface may be a horizontal direction of the display device (10), and the second direction (DR2) may be a vertical direction of the display device (10) on a planar surface. The third direction (DR3) may be a direction perpendicular to the first direction (DR1) and the second direction (DR2), for example, the third direction (DR3) may be a thickness direction of the display device (10).

[0049] The display device (10) may include a display area (DA) and a non-display area (NDA).

[0050] The display area (DA) can display an image. The display area (DA) can include pixels and / or light-emitting areas. The display area (DA) can include a front portion (FS), side portions (SS: SS1, SS2, SS3, SS4), and corner portions (CS: CS1, CS2, CS3, CS4). The front portion (FS), side portions (SS: SS1, SS2, SS3, SS4), and corner portions (CS: CS1, CS2, CS3, CS4) can be substantially included in a cover window (CW) described below.

[0051] The front portion (FS) may be substantially flat over the entire area, but is not limited thereto, and may include a convex or concave shape in the thickness direction (third direction (DR3)) at least in a portion of the area. The front portion (FS) may include a rectangular shape having a short side in the first direction (DR1) and a long side in the second direction (DR2). The front portion (FS) may have a shape in which corners thereof are rounded in a plan view. The front portion (FS) may have a polygonal shape in which corners thereof are rounded in a plan view. For example, as illustrated in FIG. 1, the front portion (FS) may have a rectangular shape in which corners thereof are rounded, but is not limited thereto.

[0052] The side portions (SS: SS1, SS2, SS3, SS4) may extend outward from the edge of the front portion (FS) and may be bent at a predetermined angle. For example, the side portion (SS) may be bent at an angle greater than or equal to 90 degrees and less than 180 degrees with respect to the front portion (FS). When the front portion (FS) includes a rectangular shape in plan view, the side portion (SS) may include a first side portion (SS1) and a third side portion (SS3) extending from the front portion (FS) in one and the other direction (DR1), and may include a second side portion (SS2) and a fourth side portion (SS4) extending in one and the other direction (DR2). The first and third side portions (SS1, SS3) may be regarded as a pair of first side portions, and the second and fourth side portions (SS2, SS4) may be regarded as a pair of second side portions. The first to fourth side sections (SS1, SS2, SS3, SS4) may be substantially identical in function or configuration except for their positions.

[0053] Each side surface of the side surface (SS: SS1, SS2, SS3, SS4) may include, but is not limited to, a round shape in plan view. For example, one side and the other side of the second direction (DR2) of the first side surface (SS1) may include, but is not limited to, a round shape in plan view.

[0054] The first to fourth side portions SS1, SS2, SS3, and SS4 extend from the front portion FS and include a predetermined curvature and may include a round shape. The first to fourth side portions SS1, SS2, SS3, and SS4 may include a shape that is convex toward the outside of the display device (10). For example, the first side portion SS1 may include a first curvature, the second side portion SS2 may include a second curvature, the third side portion SS3 may include a third curvature, and the fourth side portion SS4 may include a fourth curvature. Each of the first to fourth curvatures may be the same, but is not limited thereto, and the first to fourth curvatures may be different from each other, or only some of the first to fourth curvatures may be the same. In some embodiments, the first curvature and the third curvature may be the same. In some embodiments, the second curvature and the fourth curvature may be the same.

[0055] The portion between adjacent side portions (SS: SS1, SS2, SS3, SS4) that are bent outward from the front portion (FS) of the display device (10) is defined as a corner portion (CS). The first to fourth side portions (SS1, SS2, SS3, SS4) may be spaced apart from each other at least in some areas with a certain interval. Corner portions (CS: CS1, CS2, CS3, CS4) may be arranged in the areas where the first to fourth side portions (SS1, SS2, SS3, SS4) are spaced apart.

[0056] For example, a first corner portion (CS1) may be disposed between a first side portion (SS1) and a second side portion (SS2), a second corner portion (CS2) may be disposed between a second side portion (SS2) and a third side portion (SS3), a third corner portion (CS3) may be disposed between a third side portion (SS3) and a fourth side portion (SS4), and a fourth corner portion (CS4) may be disposed between a fourth side portion (SS4) and the first side portion (SS1). The first corner portion (CS1) may connect the first and second side portions (SS1, SS2) to each other. The second corner portion (CS2) may connect the second and third side portions (SS2, SS3) to each other. The third corner portion (CS3) may connect the third and fourth side portions (SS3, SS4) to each other. The fourth corner portion (CS4) can connect the fourth and first side portions (SS4, SS1) to each other. The first to fourth corner portions (CS1, CS2, CS3, CS4) can be substantially identical in function or configuration except for their positions.

[0057] Each of the first to fourth corner portions (CS1, CS2, CS3, CS4) includes all curvatures of the adjacent side portions and may include a round shape. For example, the first corner portion (CS1) may be disposed between the first side portion (SS1) and the second side portion (SS2). In this case, the first corner portion (CS1) may include a double curvature including the first curvature of the first side portion (SS1) and the second curvature of the second side portion (SS2). For example, the curvature of the first corner portion (CS1) may change from the first curvature to the second curvature. At the first boundary between the first corner portion (CS1) and the first side portion (SS1), the curvature of the first corner portion (CS1) may correspond to the first curvature. At the second boundary between the first corner portion (CS1) and the second side portion (SS2), the curvature of the first corner portion (CS1) may correspond to the second curvature. Between the first boundary and the second boundary, the curvature of the first corner portion (CS1) may correspond to a curvature between the first and second curvatures. The description of the first corner portion (CS1) described above may also be applied to the second to fourth corner portions (CS2, CS3, CS4). However, the present invention is not limited thereto. The first and second curvatures may be the same, and the entire first corner portion (CS1) may have the same curvature.

[0058] Pixels can be arranged on the front (FS) and side (SS) portions of the display device (10), as well as the corner portions (CS), and a screen can be displayed. Accordingly, when viewing the display device (10) from the front, the user can perceive that the entire area of ​​the display device (10) is being displayed. In other words, the user can perceive that there is virtually no bezel, and can be provided with a more immersive screen.

[0059] A non-display area (NDA) may not be displayed. The non-display area (NDA) may not include pixels or light-emitting areas. Signal lines or scan drivers for driving pixels or light-emitting areas may be arranged in the non-display area (NDA). The non-display area (NDA) may be arranged to surround the display area (DA). The non-display area (NDA) may be arranged on the outer side of the front side (FS) and the side side (SS) and the outer side of the corner side (CS). The non-display area (NDA) may constitute a bezel area of ​​the display device (10).

[0060] Fig. 3 is a cross-sectional view showing an example of a display panel cut along line Q1-Q1' of Fig. 2.

[0061] Referring to FIG. 3, the display device (10) may include a protective member (PRL), a substrate (SUB), a display layer (DISL), a sensor layer (SENL), and / or a cover window (CW).

[0062] The substrate (SUB) may be made of an insulating material such as a polymer resin or glass. For example, the substrate (SUB) may include polyimide. In this case, the substrate (SUB) may be a flexible substrate (SUB) that can be bent, folded, rolled, etc. The substrate (SUB) provides a space where other components placed thereon can be positioned, and may serve to support other components placed thereon.

[0063] A display layer (DISL) may be arranged on a substrate (SUB). The display layer (DISL) may include a display area (DA) and a non-display area (NDA). In the display area (DA) of the display layer (DISL), not only light-emitting areas but also scan lines, data lines, power lines, etc. for driving light-emitting elements may be arranged. In the non-display area (NDA) of the display layer (DISL), a scan driving circuit for outputting scan signals to the scan lines, and fan-out lines for connecting the data lines and the driving circuit may be arranged.

[0064] The display layer (DISL) may include a pixel circuit layer in which thin film transistors, as described below, are formed, a light-emitting element layer in which light-emitting elements that emit light are arranged in light-emitting areas, and an encapsulating layer for encapsulating the light-emitting element layer.

[0065] A sensor layer (SENL) may be placed on the display layer (DISL). The sensor layer (SENL) may include sensor electrodes. The sensor layer (SENL) may detect the touch of a person or object using the sensor electrodes.

[0066] A cover window (CW) may be disposed on the sensor layer (SENL). The cover window (CW) may be attached to the sensor layer (SENL) by a transparent adhesive such as an optically clear adhesive (OCA) or an optically clear resin (OCR). The cover window (CW) may be an inorganic material such as glass, or an organic material such as a plastic or a polymer material. The cover window (CW) may include the front portion (FS), side portions (SS: SS1, SS2, SS3, SS4), and corner portions (CS: CS1, CS2, CS3, CS4) described above. In some embodiments, the cover window (CW) may cover the display layer (DISL) without being disposed on the bonding portion (BON). In some embodiments, the cover window (CW) may cover the entire area of ​​the display layer (DISL) without covering any area of ​​the bonding portion (BON).

[0067] The protective member (PRL) protects the lower surface of the display panel (300) from the outside and can maintain the shape of the display panel (300). In some embodiments, the protective member (PRL) may be a rigid layer to prevent the shape of the display panel (300) from being deformed during the manufacturing process of the display device (10).

[0068] Fig. 4 is a plan view schematically illustrating pixels in a display area of ​​a display device according to one embodiment. Fig. 5 is a cross-sectional view taken along line Q2-Q2' of Fig. 4.

[0069] Referring to FIG. 4, the display area DA of the display panel 300 may include a plurality of pixels PX. Each of the plurality of pixels PX may include a plurality of light-emitting areas EA1, EA2, EA3, and EA4. For example, each of the plurality of pixels PX may include a first light-emitting area EA1, a second light-emitting area EA2, a third light-emitting area EA3, and a fourth light-emitting area EA4. The first light-emitting area EA1, the second light-emitting area EA2, the third light-emitting area EA3, and the fourth light-emitting area EA4 may emit different colors, but the present invention is not limited thereto. For example, the first light-emitting area EA1 may emit red light, the third light-emitting area EA3 may emit blue light, and the second light-emitting area EA2 and the fourth light-emitting area EA4 may emit green light.

[0070] Referring to FIG. 5, a cross-sectional structure of a pixel (PX) is examined. A first bonding layer (401) may be disposed on a protective member (PRL), and a substrate (SUB) may be disposed on the first bonding layer (401). A display layer (DISL) including a pixel circuit layer (PCL), a light emitting element layer (EML), and an encapsulation layer (TFEL) may be disposed on the substrate (SUB), and a sensor layer (SENL) including driving electrodes (TE), sensing electrodes (RE), and touch connection electrodes (BE) may be disposed on the display layer (DISL).

[0071] The protective member (PRL) can protect the lower surface of the display panel (300) from the outside and help maintain the shape of the display panel (300). In some embodiments, the protective member (PRL) can serve to maintain the shape of the display panel (300) during the manufacturing process of the display device (10).

[0072] The first bonding layer (401) can serve to bond the protective member (PRL) to another configuration. Therefore, the first bonding layer (401) is made of a material that can bond to the protective member (PRL), and the lower surface of the first bonding layer (401) can be in direct contact with the upper surface of the protective member (PRL) and bonded to the upper surface of the protective member (PRL). The first bonding layer (401) can be an adhesive layer or an adhesive layer. The first bonding layer (401) can include, but is not limited to, an optically transparent material made of silicone, such as a silicone-based optically clear adhesive (OCA).

[0073] The substrate (SUB) may include a flexible substrate capable of bending, folding, rolling, and / or stretching as described above.

[0074] A pixel circuit layer (PCL) may be arranged on a substrate (SUB). The pixel circuit layer (PCL) may include first thin film transistors (ST1). The pixel circuit layer (PCL) may include a first thin film transistor (ST1), a pixel connection electrode (ANDE1), a buffer layer (BF1), a gate insulating layer (130), a first interlayer insulating layer (141), a second interlayer insulating layer (142), a first planarization layer (150), and a second planarization layer (160).

[0075] A buffer layer (BF1) may be disposed on the substrate (SUB). The buffer layer (BF1) may be formed of a silicon nitride layer, a silicon oxynitride layer, a silicon oxide layer, a titanium oxide layer, or an aluminum oxide layer.

[0076] A first thin film transistor (ST1) may be arranged on the buffer layer (BF1). The first thin film transistor (ST1) may include a first active layer (ACT1), a first gate electrode (G1), a first source electrode (S1), and a first drain electrode (D1).

[0077] A first active layer (ACT1) of a first thin film transistor (ST1) may be disposed on a buffer layer (BF1). The first active layer (ACT1) may include a silicon semiconductor such as polycrystalline silicon, single crystal silicon, low-temperature polycrystalline silicon, or amorphous silicon. The first active layer (ACT1) overlapping the first gate electrode (G1) in the third direction (DR3) may be defined as a channel region. The first active layer (ACT1) not overlapping the first gate electrode (G1) in the third direction (DR3) may be defined as a conductive region. The conductive region of the first active layer (ACT1) may be a silicon semiconductor doped with ions or impurities to have conductivity.

[0078] A gate insulating layer (130) may be disposed on the first active layer (ACT1) of the first thin film transistor (ST1). The gate insulating layer (130) may be formed of an inorganic film, for example, a silicon nitride layer, a silicon oxynitride layer, a silicon oxide layer, a titanium oxide layer, or an aluminum oxide layer.

[0079] A first gate electrode (G1) of a first thin film transistor (ST1) and a first capacitor electrode (CAE1) may be disposed on the gate insulating layer (130). The first gate electrode (G1) of the first thin film transistor (ST1) may overlap the first active layer (ACT1) in the third direction (DR3). The first capacitor electrode (CAE1) may overlap the second capacitor electrode (CAE2) in the third direction (Z-axis direction). The first gate electrode (G1) and the first capacitor electrode (CAE1) may be formed as a single layer or multiple layers made of any one of molybdenum (Mo), aluminum (Al), chromium (Cr), gold (Au), titanium (Ti), nickel (Ni), neodymium (Nd), and copper (Cu), or an alloy thereof.

[0080] A first interlayer insulating layer (141) may be disposed on the first gate electrode (G1) and the first capacitor electrode (CAE1). The first interlayer insulating layer (141) may be formed of an inorganic film, for example, a silicon nitride layer, a silicon oxynitride layer, a silicon oxide layer, a titanium oxide layer, or an aluminum oxide layer. The first interlayer insulating layer (141) may include a plurality of inorganic films.

[0081] A second capacitor electrode (CAE2) may be disposed on the first interlayer insulating layer (141). The second capacitor electrode (CAE2) may overlap the first capacitor electrode (CAE1) in the third direction (DR3). Since the first interlayer insulating layer (141) has a predetermined permittivity, a capacitor may be formed by the first capacitor electrode (CAE1), the second capacitor electrode (CAE2), and the first interlayer insulating layer (141). The second capacitor electrode (CAE2) may be formed as a single layer or multiple layers made of any one of molybdenum (Mo), aluminum (Al), chromium (Cr), gold (Au), titanium (Ti), nickel (Ni), neodymium (Nd), and copper (Cu), or an alloy thereof.

[0082] A second interlayer insulating layer (142) may be disposed on the second capacitor electrode (CAE2). The second interlayer insulating layer (142) may be formed of an inorganic film, for example, a silicon nitride layer, a silicon oxynitride layer, a silicon oxide layer, a titanium oxide layer, or an aluminum oxide layer.

[0083] A first source electrode (S1) and a first drain electrode (D1) of a first thin film transistor (ST1) may be disposed on the second interlayer insulating layer (142). The first source electrode (S1) and the first drain electrode (D1) may be formed as a single layer or multiple layers made of any one of molybdenum (Mo), aluminum (Al), chromium (Cr), gold (Au), titanium (Ti), nickel (Ni), neodymium (Nd), and copper (Cu), or an alloy thereof.

[0084] A first source electrode (S1) of a first thin film transistor (ST1) can be connected to a conductive region disposed on one side of a channel region of a first active layer (ACT1) through a contact hole penetrating through a gate insulating layer (130), a first interlayer insulating layer (141), and a second interlayer insulating layer (142). A first drain electrode (D1) of the first thin film transistor (ST1) can be connected to a conductive region disposed on the other side of the channel region of the first active layer (ACT1) through a contact hole penetrating through a gate insulating layer (130), a first interlayer insulating layer (141), and a second interlayer insulating layer (142).

[0085] A first planarization layer (150) may be disposed on the first source electrode (S1) and the first drain electrode (D1) to level the steps caused by the thin film transistors. The first planarization layer (150) may be formed of an organic film such as an acrylic resin, an epoxy resin, a phenolic resin, a polyamide resin, or a polyimide resin.

[0086] A pixel connection electrode (ANDE1) may be arranged on the first planarization layer (150). The pixel connection electrode (ANDE1) may be connected to the first source electrode (S1) or the first drain electrode (D1) of the first thin film transistor (ST1) through a contact hole penetrating the first planarization layer (150). The pixel connection electrode (ANDE1) may be formed as a single layer or multiple layers made of any one of molybdenum (Mo), aluminum (Al), chromium (Cr), gold (Au), titanium (Ti), nickel (Ni), neodymium (Nd), and copper (Cu), or an alloy thereof.

[0087] A second planarization layer (160) may be disposed on the pixel connection electrode (ANDE1). The second planarization layer (160) may be formed of an organic film such as an acrylic resin, an epoxy resin, a phenolic resin, a polyamide resin, or a polyimide resin.

[0088] A barrier layer (161) may be disposed on the second planarization layer (160). The barrier layer (161) may be formed of a silicon nitride layer, a silicon oxynitride layer, a silicon oxide layer, a titanium oxide layer, or an aluminum oxide layer.

[0089] An emission layer (EML) is arranged on the pixel circuit layer (PCL). The emission layer (EML) may include emission elements (170) and banks (180).

[0090] Each of the light-emitting elements (170) may include a pixel electrode (171), a light-emitting layer (172), and a common electrode (173). Each of the light-emitting regions (EA1, EA2, EA3, and EA4) represents a region in which the pixel electrode (171), the light-emitting layer (172), and the common electrode (173) are sequentially laminated, and holes from the pixel electrode (171) and electrons from the common electrode (173) are combined with each other in the light-emitting layer (172) to emit light. In this case, the pixel electrode (171) may be an anode electrode, and the common electrode (173) may be a cathode electrode. The first light-emitting region (EA1) and the fourth light-emitting region (EA4) may be substantially the same as the third light-emitting region (EA3).

[0091] The pixel electrode (171) may be placed on the barrier layer (161). The pixel electrode (171) may be connected to the pixel connection electrode (ANDE1) through a contact hole penetrating the barrier layer (161) and the second planarization layer (160).

[0092] In a top emission structure that emits light in the direction of the common electrode (173) based on the light-emitting layer (172), the pixel electrode (171) can be formed with a laminated structure of aluminum and ITO (ITO / Al / ITO) in which ITO having a high work function, aluminum for reflecting light, and ITO having high adhesive strength are laminated.

[0093] The bank (180) serves to define the light-emitting areas (EA1, EA2, EA3, EA4) of the display pixels. To this end, the bank (180) may be formed to expose a portion of the pixel electrode (171) on the barrier layer (161). The bank (180) may cover the edge of the pixel electrode (171). The bank (180) may be formed of an organic film such as an acrylic resin, an epoxy resin, a phenolic resin, a polyamide resin, or a polyimide resin.

[0094] A light-emitting layer (172) may be disposed on the pixel electrode (171). The light-emitting layer (172) may include an organic material and emit light of a predetermined color. For example, the light-emitting layer (172) may include a hole transport layer, an organic material layer, and an electron transport layer. The organic material layer may include a host and a dopant. The organic material layer may include a material that emits a predetermined light, and may be formed using a phosphorescent material or a fluorescent material.

[0095] A common electrode (173) may be disposed on the light-emitting layer (172). The common electrode (173) may cover the light-emitting layer (172). The common electrode (173) may be a common layer formed commonly across the display pixels. A capping layer may be formed on the common electrode (173).

[0096] In the upper light-emitting structure, the common electrode (173) serves to lower the resistance and can be formed with a thin thickness of a transparent conductive material (TCO) such as ITO or IZO that can transmit light, or an alloy of magnesium (Mg), silver (Ag), or magnesium (Mg) and silver (Ag) that has a low work function.

[0097] An encapsulation layer (TFEL) may be formed on the light emitting element layer (EML). The encapsulation layer (TFEL) may include at least one inorganic film to prevent oxygen or moisture from penetrating into the light emitting element layer (EML). In addition, the encapsulation layer (TFEL) may include at least one organic film to protect the light emitting element layer (EML) from foreign substances (particles). In some embodiments, the encapsulation layer (TFEL) may include a stacked structure of at least one inorganic film and at least one organic film.

[0098] For example, the thin film encapsulation layer (TFEL) may include a first encapsulation inorganic film (191) disposed on a common electrode (173), an encapsulation organic film (192) disposed on the first encapsulation inorganic film (191), and a second encapsulation inorganic film (193) disposed on the encapsulation organic film (192). The first encapsulation inorganic film (191) and the second encapsulation inorganic film (193) may be formed as a multi-film in which one or more inorganic films of a silicon nitride layer, a silicon oxynitride layer, a silicon oxide layer, a titanium oxide layer, and an aluminum oxide layer are alternately laminated. The organic film may be an acrylic resin, an epoxy resin, a phenolic resin, a polyamide resin, or a polyimide resin.

[0099] A sensor layer (SENL) is arranged on the encapsulation layer (TFEL). The sensor layer (SENL) may include driving electrodes (TE), sensing electrodes (RE), and touch connection electrodes (BE).

[0100] A first touch inorganic film (TINS1) may be disposed on the encapsulation layer (TFEL). The first touch inorganic film (TINS1) may be formed of a silicon nitride layer, a silicon oxynitride layer, a silicon oxide layer, a titanium oxide layer, or an aluminum oxide layer.

[0101] Touch connection electrodes (BE) may be arranged on the first touch inorganic film (TINS1). The touch connection electrodes (BE) may be formed with a laminated structure of aluminum and ITO (ITO / Al / ITO).

[0102] A second touch inorganic film (TINS2) may be disposed on the touch connection electrodes (BE). The second touch inorganic film (TINS2) may be formed of a silicon nitride layer, a silicon oxynitride layer, a silicon oxide layer, a titanium oxide layer, or an aluminum oxide layer.

[0103] Drive electrodes (TE) and sensing electrodes (RE) may be arranged on the second touch inorganic film (TINS2). In order to prevent or reduce a decrease in brightness of light emitted from the light-emitting areas (EA1, EA2, EA3, EA4) by being blocked by the drive electrodes (TE) and sensing electrodes (RE), the drive electrodes (TE) and sensing electrodes (RE) do not overlap with the light-emitting areas (EA1, EA2, EA3, EA4). The drive electrodes (TE) and sensing electrodes (RE) may also be formed of a laminated structure of aluminum and titanium (Ti / Al / Ti).

[0104] A touch organic film (TINS3) may be disposed on the driving electrodes (TE) and the sensing electrodes (RE). The touch organic film (TINS3) may be an acrylic resin, an epoxy resin, a phenolic resin, a polyamide resin, or a polyimide resin.

[0105] The cover window (CW) described above may be disposed on the display panel (300). The cover window (CW) may be adhered to the display panel (300) through a second bonding layer (402) disposed between the display panel (300) and the cover window (CW). The second bonding layer (402) may include an acrylic-based optically clear adhesive (OCA). Therefore, the second bonding layer (402) may be optically transparent. The upper surface of the second bonding layer (402) is in direct contact with the lower surface of the cover window (CW) and may have the same area and shape as the lower surface of the cover window (CW).

[0106] Meanwhile, a protective member (PRL) may be placed at the rear of the display panel (300). The protective member (PRL) overlaps the display area (DA) of the display panel (300) to protect the lower surface of the display panel (300) from the outside and maintain the shape of the display panel (300).

[0107] As described above, the display device (10) may include side portions and corner portions having curvatures. The corner portions of the display device (10) have a double curvature having curvatures of both the left and right sides and the upper and lower sides, and therefore, the display device (10) of this shape may be deformed by the protective member (PRL) and the display layer (DISL). For example, in a process of attaching the protective member (PRL) to the display layer (DISL), the protective member (PRL) and the display layer (DISL) may be deformed to be aligned with each other at the corner portions having the double curvatures. Due to this deformation of the protective member (PRL), wrinkles may be formed on the deformed surface of the protective member (PRL). To remove these wrinkles, heat is applied in a process of bonding the display panel (300) and the protective member (PRL). Buckling may occur due to the difference in elastic modulus and shrinkage rate between the protective member (PRL) and the display panel (300), causing the protective member (PRL) to detach from the display panel (300) and generate air bubbles. If buckling occurs in the protective member (PRL), cracks may occur in the display panel (300), causing wires to be disconnected and resulting in display defects.

[0108] According to one embodiment, the protective member (PRL) may include a material having elasticity so that strain concentrated at the corners can be alleviated. The protective member (PRL) may include a material that shrinks in a specific temperature environment so as to facilitate adhesion to the side and corner portions having a curvature of the display device (10). For example, the protective member (PRL) may include any one of polyolefin-based, polyvinyl-based, polyethylene-based, and polyester-based resins. The protective member (PRL) may include an elongated polyester, for example, polyethylene terephthalate (PET).

[0109] The protective member (PRL) has a predetermined thickness and can support and protect the display panel (300). The thickness of the protective member (PRL) may be 100 μm or less, for example, 25 to 100 μm.

[0110] When heat is applied to the protective member (PRL), the protective member (PRL) may shrink. The protective member (PRL) may have a shrinkage rate of 20% or more in a temperature range of 50 degrees to 150 degrees. For example, the protective member (PRL) may exhibit a shrinkage rate of 30% or more when heated at a temperature of 85 degrees for about 10 minutes. If the protective member (PRL) has a shrinkage rate of less than 20% in a temperature range of 50 degrees to 150 degrees, bending may occur at the corner of the display device (10), causing buckling between the display device (10) and the protective member (PRL). Therefore, the protective member (PRL) preferably has a shrinkage rate of 20% or more in a temperature range of 50 degrees to 150 degrees to prevent buckling, and more preferably has a shrinkage rate of 30% or more. In some embodiments, the protective member (PRL) has a shrinkage ratio of greater than 30% in a temperature range of 50 to 150 degrees Celsius, which can more effectively remove or smooth out wrinkles caused by buckling.

[0111] The protective member (PRL) shrinks and may cause other layers bonded to the upper or lower surface of the protective member (PRL) to shrink together. In addition, when the protective member (PRL) shrinks, the intermolecular distance in the shrinking portion becomes smaller, so the intermolecular distance in the portion of the protective member (PRL) that shrinks due to heat may be smaller than the intermolecular distance in the portion that does not shrink due to heat. Therefore, the protective member (PRL) that shrinks due to heat may have a higher density per unit volume than the protective member (PRL) that does not shrink due to heat.

[0112] In addition, the protective member (PRL) may have a glass transition temperature (Tg) in the range of 50 degrees to 150 degrees. The protective member (PRL) may have an elastic modulus of 4 GPa or less in the glass transition temperature (Tg) range, for example, a temperature range of 50 degrees to 150 degrees. When the elastic modulus of the protective member (PRL) is 4 GPa or less, the protective member (PRL) may have flexibility when heat is applied, thereby preventing bending due to curvature at the corner of the display device (10) and preventing the occurrence of a non-bonded portion. In some embodiments, the protective member (PRL) may exhibit an elastic modulus of 3.6 GPa at room temperature (25 degrees). In some embodiments, the protective member (PRL) may exhibit a glass transition temperature of from 74 degrees to 78 degrees and may have an elastic modulus of no greater than 2.5 GPa, preferably from 0.6 to 0.9 GPa, in the temperature range of from 74 degrees to 78 degrees.

[0113] Therefore, the protective member (PRL) according to one embodiment can satisfy the following characteristic conditions.

[0114] 1) Glass transition temperature: 50 to 150 degrees

[0115] 2) Elastic modulus: 4 GPa or less (temperature range from 50 to 150 degrees)

[0116] 3) Shrinkage: 20% or more (temperature range 50 to 150 degrees)

[0117] As described above, according to one embodiment, by using a protective member (PRL) that satisfies the above-described characteristic conditions, buckling, in which a bond separates from the display panel (300) and bubbles are generated, can be prevented, and cracks and short circuits of the display panel (300) can be improved.

[0118] Fig. 6 is a plan view showing a display panel of a display device according to another embodiment. Fig. 7 is a cross-sectional view taken along line Q3-Q3' of Fig. 6.

[0119] Referring to FIGS. 6 and 7, the present embodiment is different from the embodiments of FIGS. 1 to 5 described above in that a first protective member (PRL1) is disposed in the display area (DA) of the display panel (300) and a second protective member (PRL2) is disposed in the bonding portion (BON) of the display panel (300).

[0120] A display device (10) according to one embodiment may include a display panel (300). The display panel (300) may include a display area (DA) and a bonding portion (BON). The bonding portion (BON) may be spaced apart from the display area (DA) and may be disposed on a substrate (SUB) extending from the display area (DA). The bonding portion (BON) may be disposed on the back surface of the display area (DA) by bending a flexible substrate (SUB). The bonding portion (BON) may include a driving circuit (DIC). The driving circuit (DIC) may serve to transmit a driving signal from an external device to the display area (DA).

[0121] The rear side of the substrate (SUB) may include a first protective member (PRL1) overlapping the display area (DA) and a second protective member (PRL2) overlapping the bonding portion (BON). The first protective member (PRL1) and the second protective member (PRL2) may be spaced apart from each other. The first protective member (PRL1) supports the display area (DA) and protects the lower surface of the display panel (300) from the outside, and the second protective member (PRL2) supports the bonding portion (BON) and protects the lower surface of the bonding portion (BON) from the outside.

[0122] The first protective member (PRL2) may be the protective member (PRL) described in FIGS. 1 to 5 . The second protective member (PRL2) may include a heat-resistant resin. For example, the second protective member (PRL2) may include a polyester-based or polyimide-based resin. Polyethylene terephthalate (PET) may be an example of a polyester-based resin.

[0123] The above-described driving circuit (DIC) can be mounted on the bonding portion (BON) of the substrate (SUB) through a compression process. Since heat is applied to the bonding portion (BON) during the compression process, the second protective member (PRL2) can have heat resistance that is not damaged by the heat. If the second protective member (PRL2) is damaged by heat, the alignment of the driving circuit (DIC) and the bonding portion (BON) terminals may be misaligned, resulting in a driving failure.

[0124] In one embodiment, the second protective member (PRL2) may be heat-resistant and have a low coefficient of thermal expansion (CTE). The coefficient of thermal expansion of the second protective member (PRL2) may be 30 ppm / °C or less at a temperature from room temperature to 180 degrees. In some embodiments, the coefficient of thermal expansion of the second protective member (PRL2) may be 30 ppm / °C or less at a temperature selected from the range of room temperature to a melting point temperature of the material of the second protective member (PRL2). A lower coefficient of thermal expansion means a smaller change in volume due to a temperature increase. Since the second protective member (PRL2) has a low coefficient of thermal expansion of 30 ppm / °C or less, it can prevent deformation due to heat during a pressing process of the driving circuit (DIC), thereby preventing the alignment of the driving circuit (DIC) from being misaligned.

[0125] The melting point of the second protective member (PRL2) may be 180 degrees or higher. The melting point is the temperature at which a state change occurs from a solid to a liquid. A higher melting point indicates better heat resistance. By having a melting point of 180 degrees or higher, the second protective member (PRL2) can prevent damage to the second protective member (PRL2) due to heat during the compression process of the driving circuit (DIC).

[0126] The second protective member (PRL2) may have a shrinkage ratio lower than that of the first protective member (PRL1). In one embodiment, the shrinkage ratio of the second protective member (PRL2) may be 1% or less in a temperature range of 50 to 150 degrees. The first protective member (PRL1) should have a large shrinkage ratio in order to adhere well to the lower surface of the substrate (SUB), for example, a curved side surface and a corner surface. Conversely, the second protective member (PRL2) should have a small shrinkage ratio in order to withstand the heat applied during the pressing process of the driving circuit (DIC) while adhered to the lower surface of the substrate (SUB) and to prevent misalignment between the driving circuit (DIC) and the terminals.

[0127] Specifically, when the second protective member (PRL2) shrinks, other layers adhered to the upper surface of the second protective member (PRL2) may shrink together. In this case, during the pressing process of the above-described driving circuit (DIC), the substrate (SUB) may shrink together with the second protective member (PRL2), which may cause misalignment between the terminals of the driving circuit (DIC) and the substrate (SUB). The second protective member (PRL2) has a shrinkage rate of 1% or less in a temperature range of 50 degrees to 150 degrees, thereby preventing misalignment between the terminals of the driving circuit (DIC) and the substrate (SUB) during the pressing process of the driving circuit (DIC). For example, within a process margin in which the driving circuit (DIC) is aligned with the terminals of the substrate (SUB), a shrinkage rate of 1% or less may be allowed for the second protective member (PRL2).

[0128] The second protective member (PRL2) may have a higher elastic modulus than the first protective member (PRL1). As the elastic modulus increases, the strain may be smaller even when the pulling stress increases. In other words, the second protective member (PRL2) may exhibit a characteristic of becoming stiffer as the elastic modulus increases. The second protective member (PRL2) may have a characteristic of having a high elastic modulus to prevent misalignment between the terminals of the substrate (SUB) arranged thereon and the driving circuit (DIC).

[0129] In one embodiment, the second protective member (PRL2) may have an elastic modulus of 4.5 GPa or more at a process temperature, for example, in a temperature range of 50 to 150 degrees Celsius. In some embodiments, the elastic modulus of the second protective member (PRL2) may be 4.5 to 5.5 GPa. When the elastic modulus of the second protective member (PRL2) is 4.5 GPa or more, the strain (or deformation) of the second protective member (PRL2) may be reduced, and thus the deformation of the substrate (SUB) bonded on the second protective member (PRL2) may also be reduced. Accordingly, misalignment between terminals formed on the substrate (SUB) and the driving circuit (DIC) may be prevented, thereby preventing driving failure.

[0130] Therefore, the second protective member (PRL2) according to one embodiment can satisfy the following characteristic conditions.

[0131] 1) Thermal expansion coefficient: 30ppm / ℃ or less (temperature range from room temperature to 180 degrees)

[0132] 2) Elastic modulus: 4.5 GPa or more (temperature range 50 to 150 degrees)

[0133] 3) Shrinkage: Less than 1% (temperature range 50 to 150 degrees)

[0134] 4) Melting point: 180 degrees or higher

[0135] As described above, according to one embodiment, by using a second protective member (PRL2) that satisfies the above-described characteristic conditions, the alignment of the driving circuit (DIC) and the bonding portion (BON) terminals can be prevented from being misaligned during the bonding process of the driving circuit (DIC), thereby improving driving failure.

[0136] Fig. 8 is a cross-sectional view showing another example cut along line Q3-Q3' of Fig. 6.

[0137] Referring to FIG. 8, this embodiment is different from the embodiments of FIGS. 1 to 7 described above in that one protective member (PRL) is placed at the rear of the display area (DA) and bonding portion (BON) of the display panel (300).

[0138] A display device (10) according to one embodiment may include a protective member (PRL) overlapping a display area (DA) and a bonding portion (BON) on the rear side of a substrate (SUB) of a display panel (300). The protective member (PRL) may be arranged to extend from the display area (DA) of the display panel (300) to the bonding portion (BON). The protective member (PRL) may support the display area (DA) and the bonding portion (BON) and protect the lower surface of the display panel (300) from the outside.

[0139] As described above, the protective member (PRL) used in the display area (DA) requires a low coefficient of thermal expansion and modulus, and the protective member (PRL) used in the bonding portion (BON) requires a low coefficient of thermal expansion and a high melting point. This embodiment exemplifies a case where the display device (10) is manufactured using a low-temperature process in which the bonding process temperature of the driving circuit (IC) is 50 degrees or less.

[0140] In one embodiment, a single protective member (PRL) is provided at the rear of the display panel (300) to simplify the structure and process. The protective member (PRL) may satisfy the following characteristics.

[0141] 1) Thermal expansion coefficient: 30ppm / ℃ or less (temperature range from room temperature to 180 degrees)

[0142] 2) Elastic modulus: 2.5 GPa or less (temperature range from 50 to 150 degrees)

[0143] 3) Shrinkage: 20% or more (temperature range 50 to 150 degrees)

[0144] 4) Melting point: 180℃ or higher

[0145] Fig. 9 is a flowchart showing a method for manufacturing a display device according to one embodiment.

[0146] Referring to FIG. 9, a method for manufacturing a display device (10) may include a step (S100) of providing a display panel (300), a first protective member (PRL1), and a second protective member (PRL2), a step (S200) of bonding the first protective member (PRL1) and the second protective member (PRL2) to the display panel (300), a step (S300) of aligning a cover window (CW) on the display panel (300) and aligning a guide member (HG) under the display panel (300), a step (S400) of pressing the cover window (CW), the display panel (300), and the guide member (HG), a step (S500) of heating the first protective member (PRL1) of the display panel (300) through the guide member (HG), and a step (S600) of removing the guide member (HG).

[0147] Figures 10 to 17 are step-by-step schematic diagrams of a method for manufacturing a display device according to one embodiment.

[0148] Hereinafter, a method for manufacturing a display device (10) will be described in detail together with the drawings shown in FIGS. 10 to 17 in conjunction with the flowchart of FIG. 9.

[0149] Referring to FIG. 10, a display panel (300), a first protective member (PRL1), and a second protective member (PRL2) are provided. (S100) The first protective member (PRL1) and the second protective member (PRL2) can be aligned respectively at the rear of the display panel (300).

[0150] The first protective member (PRL1) may be the protective member (PRL) described in FIGS. 1 to 5 described above, and the second protective member (PRL2) may be the second protective member (PRL2) described in FIGS. 6 and 7 described above. For example, the first protective member (PRL1) may have a shrinkage ratio of 20% or more in a temperature range of 50 degrees to 150 degrees, a glass transition temperature (Tg) in a range of 50 degrees to 150 degrees, and an elastic modulus of 4 GPa or less in a temperature range of 50 degrees to 150 degrees. In addition, the second protective member (PRL2) may have a thermal expansion coefficient of 30 ppm / ℃ or less in a temperature range of room temperature to 180 degrees, a melting point of 180 degrees or more, and a shrinkage ratio of 1% or less in a temperature range of 50 degrees to 150 degrees. In some embodiments, the second protective member (PRL2) may have a coefficient of thermal expansion of 30 ppm / °C or less at a temperature selected from a melting point range at room temperature, and may have a shrinkage of 1% or less at a first temperature selected from a temperature range of 50 to 150 degrees. In some embodiments, the first temperature selected from the temperature range may correspond to a glass transition temperature of the second protective member (PRL2).

[0151] Next, a first protective member (PRL1) and a second protective member (PRL2) are bonded to the display panel (300). (S200) The first protective member (PRL1) can be bonded to the rear of the display area (DA) of the display panel (300), and the second protective member (PRL2) can be bonded to the rear of the bonding portion (BON) of the display panel (300). The bonding of the first protective member (PRL1) and the display panel (300) may be preliminary bonding, and may be completely bonded in the bonding process described later. A first bonding layer may be disposed on each of the upper surfaces of the first protective member (PRL1) and the second protective member (PRL2), so that the first protective member (PRL1) and the second protective member (PRL2) can be attached to the rear of the display panel (300). The first bonding layer may be, for example, a pressure-sensitive adhesive (PSA).

[0152] Next, referring to FIGS. 11 and 12, a cover window (CW) is aligned on a display panel (300), and a guide member (HG) is aligned under the display panel (300). (S300) The cover window (CW) and the display panel (300) are the same as described above, and thus a description thereof is omitted. For example, the cover window (CW) may have a front portion ('FS' in FIG. 2), a side portion ('SS' in FIG. 2), and a corner portion ('CS' in FIG. 2) described in FIG. 2. In some embodiments, the cover window (CW) is aligned on an upper surface of the display area (DA), and the guide member (HG) is aligned on a lower surface of the display area (DA), so that the cover window (CW) and the guide member (HG) may be pressed against the display area (DA). In some embodiments, the cover window (CW) and the guide member (HG) may not cover an upper surface and a lower surface of the bonding portion (BON), respectively.

[0153] As illustrated in FIG. 12, the guide member (HG) may have a shape similar to that of the cover window (CW). Specifically, the guide member (HG) may include a base portion (BS), a flat portion (FFS), a curved portion (SO: SO1, SO2, SO3, SO4), and a convex portion (CO: CO1, CO2, CO3, CO4). In some embodiments, the guide member (HG) may have substantially the same shape as the cover window (CW), and the area of ​​the guide member (HG) may be smaller than that of the cover window (CW). In a state where the cover window (CW), the guide member (HG), and the display panel (300) are pressed, the guide member (HG) may be fitted into a space formed by the inner surface of the cover window (CW) with the display panel (300) therebetween.

[0154] The base portion (BS) may correspond to a body that serves as a base for the flat portion (FFS), the curved portion (SO), and the convex portion (CO). The base portion (BS) may constitute the lower portion of the guide member (HG).

[0155] The flat portion (FFS) is a substantially flat area that may correspond to the front surface of the cover window (CW). The flat portion (FFS) may have a rectangular shape having a short side in the first direction (DR1) and a long side in the second direction (DR2). The flat portion (FFS) may have a shape with rounded corners on the plane.

[0156] The curved portions (SO: SO1, SO2, SO3, SO4) may extend outward from the edge of the flat portion (FFS) and may be bent at a predetermined angle. When the flat portion (FFS) has a rectangular shape in plan view, the curved portion (SO) may include a first curved portion (SO1) and a third curved portion (SO3) extending from the flat portion (FFS) in one direction (DR1) and the other side, and may include a second curved portion (SO2) and a fourth curved portion (SO4) extending in one direction (DR2) and the other side. The first to fourth curved portions (SO1, SO2, SO3, SO4) may correspond to the first to fourth side portions (SS1, SS2, SS3, SS4) of the cover window (CW) described above. The first to fourth bending portions (SO1, SO2, SO3, SO4) extend from the flat portion (FFS) and include a predetermined curvature and may include a round shape.

[0157] Among the portions that are bent outwardly from the flat portion (FFS) of the guide member (HG), the portions between adjacent bends (SO: SO1, SO2, SO3, SO4) are defined as a double bend (CO). The first to fourth bends (SO1, SO2, SO3, SO4) may be spaced apart from each other at least in some areas with a certain interval. In the areas where the first to fourth bends (SO1, SO2, SO3, SO4) are spaced apart, double bends (CO: CO1, CO2, CO3, CO4) may be arranged.

[0158] For example, a first bend section (CO1) may be arranged between the first bend section (SO1) and the second bend section (SO2), a second bend section (CO2) may be arranged between the second bend section (SO2) and the third bend section (SO3), a third bend section (CO3) may be arranged between the third bend section (SO3) and the fourth bend section (SO4), and a fourth bend section (CO4) may be arranged between the fourth bend section (SO4) and the first bend section (SO1). The first to fourth bend sections (CO1, CO2, CO3, CO4) may correspond to the corner sections (CS: CS1, CS2, CS3, CS4) of the cover window (CW) described above.

[0159] The first to fourth convex portions (CO1, CO2, CO3, CO4) include convex curvatures that include curvatures of adjacent convex portions (SO), and may include a round shape. For example, the first convex portion (CO1) may be positioned between the first convex portion (SO1) and the second convex portion (SO2). In this case, the first convex portion (CO1) may include convex curvatures that include the first curvature of the first convex portion (SO1) and the second curvature of the second convex portion (SO2). For example, the valley of the first convex portion (CO1) may change from the first curvature to the second curvature. At the first boundary between the first convex portion (CO1) and the first convex portion (SO1), the curvature of the first convex portion (CO1) may correspond to the first curvature. At the second boundary between the first bend (CO1) and the second bend (SO2), the curvature of the first bend (CO1) corresponds to the second curvature. Between the first boundary and the second boundary, the curvature of the first bend (CO1) may correspond to a curvature between the first curvature and the second curvature.

[0160] The above-described guide member (HG) is formed in a shape similar to that of the cover window (CW), and as described below, presses the display panel (300) from below the display panel (300) to firmly adhere and adhere the first protective member (PRL1) adhered to the rear of the display panel (300) to the back surface of the display panel (300).

[0161] The guide member (HG) may further include a heating element (HT). The heating element (HT) functions to radiate heat and may include components that radiate heat, such as a coil or an infrared irradiation device. The heating element (HT) may be positioned in each of the bending portion (SO) and the convex portion (CO) of the guide member (HG).

[0162] Specifically, the heating unit (HT) may include a first heating unit (HT1) disposed in the bend section (CO) and a second heating unit (HT2) disposed in at least a portion of the bend section (SO). The first heating unit (HT1) may be disposed in each of the bend sections (CO). For example, the first heating unit (HT1) may be disposed in each of the first to fourth bend sections (CO1, CO2, CO3, CO4). The area of ​​the first heating unit (HT1) may be the same as, but is not limited to, the area of ​​each of the first to fourth bend sections (CO1, CO2, CO3, CO4) and may be larger or smaller. The second heating unit (HT2) may be disposed in each of the bend sections (SO). The second heating unit (HT2) may be disposed in at least a portion of each of the bend sections (SO). For example, the second heating unit (HT2) may be arranged at a point where the first to fourth bending units (SO1, SO2, SO3, SO4) and the flat portion (FFS) meet. The second heating unit (HT2) may be arranged in a form that entirely surrounds the flat portion (FFS).

[0163] Next, referring to FIGS. 13 to 15, the cover window (CW), the display panel (300), and the guide member (HG) are pressed (S400). Specifically, the cover window (CW) can press toward the display panel (300) in front of the display panel (300), and the guide member (HG) can press toward the display panel (300) in the rear of the display panel (300).

[0164] When the cover window (CW) and the guide member (HG) are pressed from the upper and lower portions of the display panel (300), the display panel (300) can be adhered to the lower surface of the cover window (CW) in accordance with the shape of the cover window (CW). In this case, the cover window (CW) has a pressure-sensitive adhesive (PSA) applied to the lower surface, and the upper surface of the display panel (300) and the lower surface of the cover window (CW) can be adhered to the upper surface by the pressure-sensitive adhesive (PSA). As described above, the cover window (CW) includes a front portion (FS), side portions (SS: SS1, SS2, SS3, SS4), and corner portions (CS: CS1, CS2, CS3, CS4), and the flat display panel (300) can be adhered to the front portion (FS), side portions (SS), and corner portions (CS) of the cover window (CW).

[0165] In addition, when the guide member (HG) presses on the rear of the display panel (300), the first protective member (PRL1) bonded to the lower surface of the display panel (300) may have strain applied to the side surface (SS) and the corner surface (CS) of the cover window (CW) having a curvature. For example, when the first protective member (PRL1) is pressed between the cover window (CW) and the guide member (HG), the first protective member (PRL1) may be deformed along the shape of the side surface (SS) and the corner surface (CS) of the cover window (CW). The deformation of the first protective member (PRL1) on the corner surface (CS) causes the first protective member (PRL1) to bend, which may cause wrinkles to form on the deformed surface of the first protective member (PRL1) at the corner surface (CS). In the present embodiment, the deformation of the first protective member (PRL1) can be relieved through heating of the guide member (HG) described later.

[0166] Next, the first protective member (PRL1) of the display panel (300) is heated through the guide member (HG). (S500) In this step, the first protective member (PRL1) may be subjected to heat and contracted by the heating of the guide member (HG).

[0167] Specifically, heat can be applied to the heating unit (HT) of the guide member (HG) to increase the temperature of the first protective member (PRL1). The heating unit (HT) can apply heat in a temperature range of about 50 to 150 degrees. As described above, the first protective member (PRL1) has a shrinkage rate of 20% or more in a temperature range of 50 to 150 degrees, and thus can shrink when the temperature rises. Since the first protective member (PRL1) is bonded to the display panel (300) by a bonding layer, when the first protective member (PRL1) shrinks, the display panel (300) bonded thereto also shrinks, so that the entire display device (10) can shrink in an area corresponding to a corner (CS) of the display device (10), that is, a corner of the cover window (CW).

[0168] Since the side surface of the display device (10) adjacent to each corner portion is bent downward through the aforementioned pressing step, the corner portion can shrink in a direction in which the intermolecular distance of the first protective member (PRL1) becomes narrower. Accordingly, the corner portion can shrink in the same direction as the center direction of the direction in which the adjacent side surface of the display device (10) is bent.

[0169] As shown in Fig. 15, the display panel (300) and the first protective member (PRL1) may be subject to strain at each corner due to the pressurizing step described above, but as the first protective member (PRL1) contracts through heating of the guide member (HG), the display panel (300) may also contract to relieve the strain.

[0170] In this way, by heating the guide member (HG), the corner portion of the display device (10) can be contracted, thereby reducing the difference between the shape and curvature of the lower surface of the cover window (CW) placed on the upper surface of the display panel (300) and the shape and curvature of the upper surface of the display panel (300).

[0171] Referring to FIG. 16, the guide member (HG) is removed (S600). In this step, the guide member (HG) can be detached after the cover window (CW) and the display panel (300) are bonded. Accordingly, a display device (10) according to one embodiment can be manufactured.

[0172] Fig. 17 is a perspective view showing a guide member according to another embodiment.

[0173] Referring to FIG. 17, in this embodiment, the guide member (HG) is different from the above-described FIG. 12 in that the second heating member arranged in the bending portion (SO: SO1, SO2, SO3, SO4) is omitted.

[0174] The side portion of the display device (10) may have a curvature in one direction so that the stainless steel applied to the display panel (300) and the first protective member (PRL1) may be insufficient. The guide member (HG) may omit the second heating member that applies heat to an area corresponding to the side portion of the display device (10), thereby simplifying the complex structure of the guide member (HG).

[0175] Fig. 18 is a graph showing the glass transition temperature of protective member samples according to one embodiment. Fig. 19 is a graph showing the elastic modulus at the glass transition temperature of protective member samples according to one embodiment.

[0176] The glass transition temperature and elastic modulus were measured using a Perkin Elmer dynamic mechanical analyzer (DMA) under conditions of a heating rate of 2°C / min and a frequency of 2 Hz.

[0177] The protective member samples shown in Fig. 18 or Fig. 19 are as follows.

[0178] Sample 1: MD-stretched 75 ㎛ thick PET with an elastic modulus of 4.5 GPa.

[0179] Sample 2: 75㎛ thick PET with elastic modulus of 4.5GPa and TD elongation

[0180] Sample 3: MD-stretched 50 ㎛ thick PET with an elastic modulus of 1.6 GPa

[0181] Sample 4: 50㎛ thick PET with elastic modulus of 1.6GPa and TD elongation

[0182] Sample 5: MD-stretched 50 μm thick PET with an elastic modulus of 3.6 GPa.

[0183] Sample 6: 50㎛ thick PET with elastic modulus of 3.6GPa and TD elongation

[0184] Here, MD (machine direction) stretching indicates stretching in the length direction of the film, and TD (transverse direction) stretching indicates stretching in the width direction of the film.

[0185] In Fig. 18, the horizontal axis represents temperature, and the vertical axis represents tangent delta (tan d), which is the ratio of the storage modulus value to the loss modulus value. The glass transition temperature of the samples may be the temperature at which the tangent delta value is maximum (or in the range).

[0186] Referring to FIG. 18, the glass transition temperatures of samples 5 and 6 are in the range of about 70 to 80 degrees, and the glass transition temperatures of samples 1 to 4 are in the range of about 105 to 115 degrees.

[0187] That is, it was confirmed that the protective members according to Samples 1 to 6 exhibited glass transition temperatures in the range of 50 to 150 degrees and thus could be used as protective members of the display device (10) of the present embodiment. In particular, the protective members according to Samples 3 to 6 exhibited a low modulus of 4 GPa or less and thus were suitable for use in the first protective member (PRL1) overlapping the display area (DA) of the display device (10), and the protective members according to Samples 1 and 2 exhibited a high modulus of 4.5 GPa or more and thus were suitable for use in the second protective member (PRL2) overlapping the bonding portion (BON) of the display device (10).

[0188] Also, referring to FIG. 19, Samples 3 and 4 exhibit an elastic modulus of about 0.6 to 0.9 GPa at a glass transition temperature of about 75 degrees. That is, it was confirmed that the protective member according to the present embodiment exhibits an elastic modulus of 2.5 GPa or less in the glass transition temperature range. Therefore, the protective members according to Samples 3 and 4 exhibit a low elastic modulus of 2.5 GPa or less, and thus may be suitable for use in a first protective member (PRL1) overlapping a display area (DA) of a display device (10).

[0189] Hereinafter, an experimental example of a display device according to the above-described embodiment is disclosed.

[0190] <Experimental example: Lighting evaluation of heterogeneous protective materials and appearance evaluation of bonding parts>

[0191] A PET film having a modulus of 4.5 GPa was attached to the lower surface of each of the display area and bonding portion of the display panel using an acrylic PSA, and combined with a cover window to manufacture a display device of a comparative example.

[0192] A PET film having a modulus of 2.5 GPa was attached to the lower surface of the display area of ​​the display panel using an acrylic PSA, a PET film having a modulus of 4.5 GPa was attached to the lower surface of the bonding portion, and the display device of the embodiment was manufactured by combining it with a cover window.

[0193] The lighting evaluation of the display devices of the comparative examples and examples described above was performed, and after bonding the driving circuit, an external inspection was performed to check for cracks or short circuits in the bonding portion, and the results are shown in Table 1 below.

[0194] Lighting ratio (%) Appearance inspection comparison Example 100 No occurrence Example 100 No occurrence

[0195] Referring to Table 1 above, in the example in which a PET film having a low elastic modulus of 2.5 GPa was attached to the lower surface of the display area, the display panel operated normally as in the comparative example, and no cracks or short circuits occurred in the bonding portion. Through this result, it was confirmed that a quality display device can be manufactured even if different types of protective members having different elastic moduli are placed on the display area and bonding portion of the display panel.

[0196] Although embodiments of the present invention have been described with reference to the attached drawings, those skilled in the art will appreciate that the present invention can be implemented in other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood to be illustrative in all respects and not restrictive.

Claims

1. A display panel including a display area; a cover window arranged on the above display panel; and A protective member is included which is positioned below the display area of ​​the display panel, A display device wherein the above protective member has an elastic modulus of 4 GPa or less in the glass transition temperature range and a shrinkage ratio of 20% or more in the temperature range of 50 to 150 degrees.

2. In paragraph 1, The above display area is, Flat front; Side portions extending outwardly from the edge of the front portion and having a curve and being bent; and A display device disposed between the above side portions and including corner portions having a double curvature.

3. In paragraph 2, A display device in which the above protective member is adhered to the entire front part, the side parts and the corner parts.

4. In paragraph 1, A first bonding layer disposed between the display panel and the protective member; and A display device further comprising a second bonding layer disposed between the display panel and the cover window.

5. In paragraph 1, A display device wherein the glass transition temperature of the above protective member is in the range of 50 to 150 degrees.

6. In paragraph 1, The above protective member is a display device having an elastic modulus of 0.6 to 0.9 GPa at a temperature range of 74 to 78 degrees.

7. In paragraph 1, The above protective member is a display device including at least one of polyolefin-based, polyvinyl-based, polyethylene-based and polyester-based resins.

8. In paragraph 1, A display device wherein the thickness of the above protective member is 25 to 100㎛.

9. A display panel including a display area and a bonding portion spaced apart from the display area; A cover window disposed on the above display panel; A first protective member disposed below the display area of ​​the display panel; and A second protective member is disposed below the bonding portion of the display panel and is spaced apart from the first protective member. A display device wherein the shrinkage ratio of the second protective member is smaller than the shrinkage ratio of the first protective member.

10. In paragraph 9, A display device in which the shrinkage ratio of the second protective member and the shrinkage ratio of the first protective member are shrinkage ratios measured in a temperature range of 50 to 150 degrees.

11. In paragraph 9, The second protective member is a display device having a shrinkage of 1% or less in a temperature range of 50 to 150 degrees.

12. In paragraph 9, A display device in which the coefficient of thermal expansion of the second protective member is 30 ppm / ℃ or less in a temperature range of room temperature to 180 degrees.

13. In paragraph 9, An indicator device wherein the melting point of the second protective member is 180 degrees or higher.

14. In paragraph 9, An indicator device wherein the elastic modulus of the second protective member is greater than the elastic modulus of the first protective member in a temperature range of 50 degrees to 150 degrees.

15. In paragraph 9, A display device wherein the elastic modulus of the second protective member is 4.5 GPa or more in a temperature range of 50 to 150 degrees.

16. A step of providing a display panel, a first protective member and a second protective member; A step of bonding a first protective member and a second protective member to the lower surface of the above display panel; A step of aligning a cover window on the display panel and aligning a guide member under the display panel; A step of pressurizing the cover window, the display panel and the guide member; A step of heating the first protective member of the display panel through the guide member; and A step of removing the above guide member is included, A method for manufacturing a display device, wherein the elastic modulus of the second protective member is greater than the elastic modulus of the first protective member.

17. In paragraph 16, The above guide absence is, flat surface; Curved portions extending outwardly from the edge of the above-mentioned flat portion and having a curvature; and A method for manufacturing a display device including curved portions having a double curvature and arranged between the above curved portions.

18. In paragraph 17, The above guide member includes a first heating member arranged in the above bending sections, A method for manufacturing a display device, wherein heat is applied to the display panel and the first protective member through the first heating unit.

19. In paragraph 18, The above guide member further includes a second heating member arranged in the above bends, A method for manufacturing a display device, wherein heat is applied to the display panel and the first protective member through the first heating unit and the second heating unit.

20. In paragraph 17, A method for manufacturing a display device, wherein the shrinkage ratio of the second protective member is smaller than the shrinkage ratio of the first protective member in a temperature range of 50 to 150 degrees.

Citation Information

Patent Citations

  • Lower protect film for display panel and display device comprising the same

    KR1020150085352A

  • Resin sheet and use thereof

    KR1020160073956A

  • Device for adjusting multidirection of vehicle seat

    KR1020210126849A

  • Questionnaire security system and method by multi-authorization

    KR102202109B1

  • KR20230059942A