Method for preparing solid-waste-based molecular sieve catalyst for catalytic pyrolysis of biomass
By using rice husk ash and waste FCC catalyst as raw materials and combining them with specific additives to prepare ZSM-5 catalyst, the problems of catalyst carbon deposition and selectivity were solved, and low-cost, high-efficiency biomass catalytic pyrolysis was achieved.
Patent Information
- Application Number
- PCT/CN2025/105006
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2025-06-27
- Publication Date
- 2026-11-12
AI Technical Summary
In existing biomass catalytic pyrolysis technologies, the pyrolysis intermediates of ZSM-5 catalysts are prone to condensation and carbon deposition, leading to catalyst deactivation, low selectivity and yield of liquid hydrocarbon components, and high cost and serious environmental pollution of traditional hydrothermal synthesis processes.
Using rice husk ash and waste FCC catalyst as raw materials, combined with ammonium chloride, tetrapropylammonium bromide and sodium metasilicate nonahydrate, solid waste-based molecular sieve catalyst ZSM-5 was prepared by solventless crystallization and calcination. Its pore structure and acid sites were controlled to achieve anti-coking performance and aromatic selectivity.
It significantly improves the atom utilization efficiency of the catalyst, reduces production costs, enhances the catalyst's anti-coking properties and aromatic selectivity, and is suitable for industrial applications.
Smart Images

Figure CN2025105006_12112026_PF_FP_ABST
Abstract
Description
A method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis Technical Field
[0001] This invention relates to the field of biomass catalytic conversion and solid waste resource utilization technology, and in particular to a method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis. Background Technology
[0002] With rapid economic development, the excessive consumption of fossil fuels has triggered a severe energy crisis. Developing renewable energy technologies to replace fossil fuels has become an inevitable trend in the evolution of the future energy system. Biomass, as the only carbon-containing renewable resource in nature, has received high attention from countries around the world. Among various biomass utilization technologies, biomass catalytic pyrolysis, through targeted control of the catalytic system, achieves high enrichment of target products in pyrolysis oil, making it a key pathway for the high-value utilization of biomass. In recent years, in the field of biomass catalytic pyrolysis research, ZSM-5 catalysts have become the most widely used catalysts due to their advantages such as strong acidity, tunable pore size, hydrothermal stability, and high selectivity for aromatics. However, the technology for improving the quality of pyrolysis gas through catalytic pyrolysis still faces many challenges, such as the easy condensation and carbon deposition of pyrolysis intermediates, leading to catalyst deactivation; and low selectivity and yield of liquid hydrocarbon components. Currently, the industrial mass production of ZSM-5 molecular sieves is mainly achieved through silica- and aluminate gels under the action of structure-directing agents. For the large-scale production of ZSM-5 catalysts, the product cost is largely constrained by the cost of raw materials. Therefore, developing low-cost, high-performance catalyst mass production technologies is crucial for the industrial-scale promotion of biomass catalytic pyrolysis technology.
[0003] Rice husks, an important byproduct of rice production, are currently mainly utilized through gasification or combustion, transforming them into rice husk ash. Currently, rice husk ash is mostly disposed of through landfill or used as an additive in cement production, with very limited economic benefits. However, it is worth noting that rice husk ash is rich in amorphous SiO2, with a content as high as 85%–98%. Therefore, rice husk ash is an ideal, inexpensive silicon source with the potential to be used as a raw material for the synthesis of ZSM-5 catalysts. On the other hand, fluid catalytic cracking (FCC) units in oil refineries generate large amounts of waste catalysts, which have been listed in the "National Hazardous Waste List (2021 Edition)". Currently, waste FCC catalysts are mainly disposed of through landfill, which undoubtedly causes serious environmental pollution. However, the basic framework of waste FCC catalysts is composed of Y-type zeolite rich in aluminum. Based on this, it can be considered as an aluminum source for the synthesis of ZSM-5 catalysts.
[0004] In previous studies, ZSM-5 catalysts were usually synthesized by hydrothermal crystallization. However, with the advent of the concept of "green chemistry", the traditional hydrothermal synthesis process has revealed the following disadvantages: (1) The hydrothermal synthesis process generates a large amount of waste liquid, which poses a potential threat to the ecological environment; (2) Some raw materials are still present in the waste liquid, resulting in low raw material utilization; (3) Solvents occupy a large amount of space in the reactor, causing a decline in the yield per unit volume of reactor; (4) The hydrothermal reaction pressure is high, which increases equipment costs and safety factors.
[0005] Therefore, developing a green catalyst synthesis route based on industrial solid waste is crucial for the mass production of low-cost catalysts, which can alleviate environmental pressure, reduce production costs, and promote the industrialization of biomass catalytic pyrolysis technology. Summary of the Invention
[0006] In view of the above-mentioned deficiencies of the prior art, in a first aspect of the present invention, a low-cost, high-atom-utilization method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis is provided, comprising the following steps:
[0007] (1) The solid waste raw material is mixed with ammonium chloride (NH4Cl), tetrapropylammonium bromide (TPABr) and sodium metasilicate nonahydrate (Na2SiO3·9H2O) in a certain proportion and ground to obtain a mixed raw material; wherein, the solid waste raw material includes silicon source containing silicon element and aluminum source containing aluminum element;
[0008] (2) The mixed raw materials are placed in a closed environment to carry out a crystallization reaction. After crystallization, a solid product is obtained.
[0009] (3) The obtained solid product was washed and dried to obtain a purified product;
[0010] (4) The purified product was calcined in air to obtain solid waste-based molecular sieve catalyst ZSM-5.
[0011] Preferably, in step (1), the silicon source includes rice husk ash; the aluminum source includes an FCC catalyst.
[0012] The solid waste raw materials used include solid waste with high silicon and aluminum content. From the perspective of green environmental protection and recycling, rice husk ash and FCC catalyst are particularly suitable raw material choices for the preparation of this invention.
[0013] Preferably, in step (1), the mass ratio of solid waste raw material, ammonium chloride, tetrapropylammonium bromide and sodium metasilicate nonahydrate is 1:1.2~1.4:0.6~0.8:3.9~4.1.
[0014] In this process, molecular sieve catalysts with different silicon-to-aluminum ratios can be obtained by adjusting the mass ratio of silicon source to aluminum source in the solid waste raw material, thereby meeting the application requirements under different conditions.
[0015] Preferably, in step (1), a certain proportion of nano-sized calcium carbonate (CaCO3) powder is added to obtain solid waste-based molecular sieve catalysts with different pore sizes.
[0016] More preferably, the particle size of the calcium carbonate powder is <50 nm; the mass ratio of solid waste raw material, ammonium chloride, tetrapropylammonium bromide, sodium metasilicate nonahydrate, and calcium carbonate powder is 1:1.2~1.4:0.6~0.8:3.9~4.1:0.01~0.2.
[0017] In a further preferred embodiment, the solid product obtained by adding nano-sized calcium carbonate powder is first impregnated in 0.1~0.2 mol / L hydrochloric acid, with a mass ratio of hydrochloric acid to solid product of 5~10:1, and then washed with deionized water until neutral.
[0018] Preferably, in step (1), a certain proportion of metal nitrates are added to obtain solid waste-based molecular sieve catalysts with different metal loads.
[0019] More preferably, the mass ratio of the metal nitrate to the solid waste raw material is 0.01~0.1:1.
[0020] This method offers good flexibility. In the initial raw material mixing stage of catalyst preparation, different additives can be added to prepare ZSM-5 molecular sieve catalysts with different pore structures or metal supports.
[0021] Preferably, in step (1), the operation is stopped after grinding until an irritating ammonia odor appears, and the mixed raw materials are obtained.
[0022] Preferably, in step (2), the temperature of the crystallization reaction is 170~190 ℃ and the reaction time is 24~36 h.
[0023] Preferably, in step (3), the solid product is washed with deionized water until neutral; the drying temperature is 100~110 ℃ and the drying time is 12~24 h.
[0024] Preferably, in step (4), the heating rate of the calcination treatment is 10~20 ℃ / min, the calcination temperature is 550~600 ℃, and the calcination time is 4~6 h.
[0025] In a second aspect of the present invention, a solid waste-based molecular sieve catalyst ZSM-5 is provided, which is prepared using the preparation method of the first aspect of the present invention.
[0026] In a third aspect of the invention, the application of the solid waste-based molecular sieve catalyst ZSM-5 of the second aspect of the invention is provided, specifically as a catalyst for biomass catalytic pyrolysis reaction.
[0027] Based on the above technical solutions, the design concept and principle of this invention are as follows:
[0028] This invention utilizes a synergistic system based on the "structure-function oriented design principle," selecting solid waste raw materials, ammonium chloride, tetrapropylammonium bromide, and sodium metasilicate nonahydrate as preparation raw materials. The resulting solid waste-based molecular sieve catalyst exhibits excellent anti-coking properties and aromatic selectivity through the directional selection and synergistic effect among the solid waste raw materials, ammonium chloride, tetrapropylammonium bromide, and sodium metasilicate nonahydrate.
[0029] This process uses solid waste as raw material, which is rich in natural aluminosilicates. This not only realizes the resource utilization of solid waste but also provides a physical carrier for subsequent functional regulation due to the natural lattice defects in the raw material. The high silica-alumina ratio of this raw material reduces the density of strongly acidic sites, inhibiting the adsorption of carbon deposition precursors at the source, thereby suppressing carbon deposition and enhancing aromatic selectivity. Ammonium chloride is used as a functional additive. The chloride ions generated by its decomposition at high temperature are used to etch the surface of the raw material, forming a specific microporous-mesoporous coexisting pore structure. This structure is mainly microporous (0~2 nm), and the pore size is highly matched with the aromatic molecules (benzene, toluene, and xylene, kinetic diameter 0.6~0.9 nm), thereby achieving preferential adsorption of aromatics while repelling large molecular intermediate impurities (such as asphaltene, diameter >5 nm) during pyrolysis, reducing the adsorption of carbon deposition precursors at the source. This invention uses tetrapropylammonium bromide as a structure-directing agent. Its cationic groups combine with silica and alumina in the raw materials through electrostatic interactions, directionally guiding the formation of a specific crystal form. This structure has a concentrated pore distribution, allowing only monocyclic aromatic hydrocarbons to pass through while restricting the entry of polycyclic aromatic hydrocarbons or non-aromatic molecules, thereby improving aromatic selectivity. Finally, the main function of sodium metasilicate nonahydrate is to regulate acidic sites and inhibit polymerization. The SiO3 generated from Na2SiO3·9H2O... 2- With skeleton Al 3+ Coordination transforms the catalyst surface acid type from a strong Brønsted acid (Al-OH-Si, leading to excessive olefin polymerization) to a weak Lewis acid (Al... 3+ -O - (Selective adsorption of aromatics). Furthermore, Na2SiO3·9H2O serves as a silicon source and alkaline regulator, generating SiO3... 2- It can neutralize acidic sites in the raw materials and regulate the acid strength on the catalyst surface to a moderate level. This acid distribution can enhance the adsorption of aromatics through π-π interactions and inhibit the strong adsorption of easily carbon-depositing species such as olefins, thereby optimizing the anti-coking performance from the perspective of chemical activity.
[0030] This invention deeply integrates "solid waste resource utilization" with "functionalized catalytic performance". Through the synergistic effect of NH4Cl (green activation), TPABr (structure guidance), and Na2SiO3 (acid regulation), it achieves targeted regulation from "raw material structure → pore morphology → surface chemistry → catalytic performance", thereby improving the anti-coking performance and selectivity of solid waste-based molecular sieve catalysts.
[0031] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0032] This invention provides a method for preparing solid waste-based molecular sieve catalysts for biomass catalytic pyrolysis. Compared with traditional hydrothermal methods, the solvent-free process can significantly improve the atomic utilization efficiency of elements and greatly reduce the raw material cost of the catalyst synthesis process, providing a low-cost solution for the industrial-scale preparation of ZSM-5 molecular sieve catalysts.
[0033] This invention provides a solid waste-based molecular sieve catalyst ZSM-5, which exhibits superior anti-coking performance compared to commercial ZSM-5 molecular sieve catalysts and higher aromatic selectivity during biomass catalytic pyrolysis.
[0034] This invention provides an application of ZSM-5, a solid waste-based molecular sieve catalyst, which has broad prospects as a catalyst in the field of catalytic pyrolysis. Attached Figure Description
[0035] Figure 1 shows the element recovery rate of the solid waste-based molecular sieve catalyst ZSM-5 of the present invention compared with traditional catalyst synthesis technology;
[0036] Figure 2 is the X-ray diffraction (XRD) pattern of the solid waste-based molecular sieve catalyst ZSM-5 in Example 1;
[0037] Figure 3 shows the nitrogen isothermal adsorption-desorption curve and pore size distribution curve of solid waste-based molecular sieve catalyst ZSM-5 in Example 2.
[0038] Figure 4 is the X-ray photoelectron spectroscopy (XPS) spectrum of the solid waste-based molecular sieve catalyst ZSM-5 in Example 3. Embodiments of the present invention
[0039] The present invention is further illustrated below by way of embodiments, but the invention is not limited to the scope of the embodiments described herein. Experimental methods in the following embodiments that do not specify specific conditions were performed according to conventional methods and conditions, or as selected according to the product instructions.
[0040] In the following embodiments:
[0041] The commercial ZSM-5 catalyst was purchased from the catalyst factory of Nankai University (NKF-5 catalyst).
[0042] The rice husks used for rice husk ash came from the processing residue of a rice mill (Nanjing, Jiangsu). The processing residue was calcined at 600 ℃ for 4 h in air to obtain rice husk ash.
[0043] The spent FCC catalyst was supplied by Sinopec Yangzi Petrochemical Company (Jiangsu, China).
[0044] Example 1
[0045] The preparation method of solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis includes the following steps:
[0046] (1) Take 3.0 g rice husk ash, 0.3 g waste FCC catalyst, 13.15 g sodium metasilicate nonahydrate, 2.4 g tetrapropylammonium bromide and 4.3 g ammonium chloride and put them into a mortar and mix them; stop mixing when an irritating ammonia odor appears during the grinding process in the mortar. At this time, the material is in powder form and the mixed raw material is obtained.
[0047] (2) The mixed raw materials were transferred to a sealed reaction vessel and heated in an oven at 170 °C for 24 h. After the crystallization reaction was completed, the mixture was placed in ice water to cool to room temperature to obtain a solid product.
[0048] (3) The solid product was washed with deionized water until the pH was neutral, and then dried in an oven at 100 °C for 24 h to obtain the purified product.
[0049] (4) The purified product was placed in a tube furnace and calcined at 550 °C for 4 h in an air atmosphere to obtain solid waste-based molecular sieve catalyst ZSM-5.
[0050] Example 2
[0051] The preparation method of solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis includes the following steps:
[0052] (1) Take 3.0 g rice husk ash, 0.3 g waste FCC catalyst, 13.15 g sodium metasilicate nonahydrate, 2.4 g tetrapropylammonium bromide, 4.3 g ammonium chloride and 0.33 g nano-sized CaCO3 powder and put them into a mortar and mix them; stop mixing when an irritating ammonia odor appears during the grinding process in the mortar. At this time, the material is in powder form and the mixed raw material is obtained.
[0053] (2) The mixed raw materials were transferred to a sealed reaction vessel and heated in an oven at 170 °C for 24 h. After the crystallization reaction was completed, the mixture was placed in ice water to cool to room temperature to obtain a solid product.
[0054] (3) The solid product was first immersed in 0.1 mol / L hydrochloric acid, with a mass ratio of hydrochloric acid to solid product of 10:1. Then it was washed with deionized water until the pH was neutral. It was then placed in an oven to dry at 100 °C for 24 h to obtain the purified product.
[0055] (4) The purified product was placed in a tube furnace and calcined at 550 °C for 4 h in an air atmosphere to obtain solid waste-based molecular sieve catalyst ZSM-5.
[0056] Example 3
[0057] The preparation method of solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis includes the following steps:
[0058] (1) Take 3.0 g rice husk ash, 0.3 g waste FCC catalyst, 13.15 g sodium metasilicate nonahydrate, 2.4 g tetrapropylammonium bromide, 4.3 g ammonium chloride and 0.24 g zinc nitrate hexahydrate and put them into a mortar and mix them; stop mixing when an irritating ammonia odor appears during the grinding process in the mortar. At this time, the material is in powder form and the mixed raw material is obtained.
[0059] (2) The mixed raw materials were transferred to a sealed reaction vessel and heated in an oven at 170 °C for 24 h. After the crystallization reaction was completed, the mixture was placed in ice water to cool to room temperature to obtain a solid product.
[0060] (3) The solid product was washed with deionized water until the pH was neutral, and then dried in an oven at 100 °C for 24 h to obtain the purified product.
[0061] (4) The purified product was placed in a tube furnace and calcined at 550 °C for 4 h in an air atmosphere to obtain solid waste-based molecular sieve catalyst ZSM-5.
[0062] Example 4
[0063] This embodiment characterizes the solid waste-based molecular sieve catalyst ZSM-5 prepared in Example 1 to study its performance.
[0064] Atom recovery rate is an important indicator for measuring the efficiency of atom utilization in chemical reactions or catalyst synthesis. It reflects the proportion of atoms from reactants that are retained in the final product. Atom recovery rate is calculated based on the chemical formula of the reactants and the amount of each substance used, determining the amount of each type of atom.
[0065] The silicon and aluminum content in the raw materials and catalysts was accurately determined using inductively coupled plasma mass spectrometry (ICP-OES / MS), and the results are shown in Figure 1. As can be seen from Figure 1, the atomic recovery rate of the traditional hydrothermal method is lower than that of the solvent-free method of this invention, indicating that this process has higher atomic utilization efficiency.
[0066] The crystal structure of the solid waste-based molecular sieve catalyst ZSM-5 was obtained by X-ray diffraction, and the results are shown in Figure 2. Figure 2 shows that the synthesized solid waste-based molecular sieve catalyst has the same diffraction peaks as the commercial ZSM-5 molecular sieve, indicating that the target product was successfully prepared.
[0067] Performance testing was conducted on the solid waste-based molecular sieve catalyst ZSM-5. A straw biomass catalytic pyrolysis experiment was carried out in a self-made fixed-bed reactor. Before the experiment, N2 was introduced into the reactor at a rate of 400 mL / min for 10 min to ensure an inert atmosphere. The straw and catalyst were separated by quartz wool and loaded together in a quartz basket for ex-situ catalytic pyrolysis. The mass of the straw was 1.0 g, and the mass of the catalyst was 2.0 g. Before the experiment, the tubular furnace was preheated to 550 °C, and then the quartz basket containing the sample was rapidly moved into the isothermal zone. To ensure complete reaction, the entire reaction process lasted for 10 min. The liquid product was collected using an ice-water bath condensation system, with each condenser containing 15 mL of ethanol, and placed in a mixture of isopropanol and liquid nitrogen (-40 °C).
[0068] The products were qualitatively and quantitatively analyzed by GC-MS, and the total yield of BTX (benzene, toluene, xylene) was found to be 49.4 mg / g, of which benzene: 20.2 mg / g; toluene: 16.7 mg / g; and xylene: 12.5 mg / g.
[0069] Example 5
[0070] This embodiment studies the properties of the solid waste-based molecular sieve catalyst ZSM-5 prepared by adding nano-sized calcium carbonate powder to regulate the pore structure in Example 2.
[0071] The pore structure of the solid waste-based molecular sieve catalyst ZSM-5 was determined using nitrogen isothermal adsorption-desorption testing, and the results are shown in Figure 3. Figure 3(a) shows that the nitrogen isothermal adsorption-desorption curve of the synthesized solid waste-based molecular sieve catalyst ZSM-5 belongs to type IV adsorption-desorption curves, indicating that the catalyst has a pore structure with both micropores and mesopores. Figure 3(b) shows the pore size distribution curve of the synthesized solid waste-based molecular sieve catalyst ZSM-5, which is highly concentrated, mainly around 0.7 nm and 2.6 nm, consistent with the results of nitrogen isothermal adsorption-desorption testing. Detailed pore structure parameters of the molecular sieve catalyst were obtained by fitting and calculating using the Brunauer-Emmett-Teller (BET) method, and its specific surface area is 351.99 m². 2 / g, total pore volume is 0.517 cm³ 3 / g.
[0072] Example 6
[0073] This embodiment characterizes the solid waste-based molecular sieve catalyst ZSM-5 prepared by loading metal in Example 3.
[0074] The chemical valence states of the metals loaded on the solid waste-based molecular sieve catalyst ZSM-5 were analyzed using X-ray photoelectron spectroscopy, and the results are shown in Figure 4. Figure 4 shows that the peaks near the binding energies of 1022 eV and 1045 eV correspond to the 2p 3 / 2 and 2p 1 / 2 orbitals of Zn, respectively. It can be seen from the figure that Zn mainly exists on the surface of the solid waste-based molecular sieve catalyst ZSM-5 in the form of ZnO.
[0075] Example 7
[0076] To study the anti-coking performance of solid waste-based molecular sieve catalyst ZSM-5, this example collected the catalyst after catalytic pyrolysis reaction in Example 4. The carbon deposition of solid waste-based molecular sieve catalyst ZSM-5 and commercial ZSM-5 was quantitatively analyzed by TG-DSC.
[0077] TG-DSC test results show that the carbon deposition of the catalyst prepared in this invention is only 3.6 wt.%. In contrast, the carbon deposition of commercial ZSM-5 reaches 8.9 wt.%, which is 2.47 times that of the catalyst of this invention.
[0078] The reason why this invention exhibits improved anti-coking performance is that, through the regulation of the silicon-aluminum structure of solid waste raw materials and the synergistic modification of ammonium chloride and TPABr, the synthesized ZSM-5 catalyst has a multi-level pore structure with both micropores and mesopores. This gives it multiple advantages, including "micropore size matching aromatic molecules, mesoporous structure accelerating molecule mass transfer within the catalyst, and the catalyst's weak acidity inhibiting macromolecular polymerization and carbon deposition." Compared with the commercial ZSM-5, which relies solely on micropore sieving, this invention achieves a breakthrough improvement in anti-coking performance while maintaining high aromatic selectivity.
[0079] This invention utilizes a catalyst synthesized through pore size sieving and acidity regulation to reduce irreversible carbon deposition at its source. Subsequently, continuous catalytic pyrolysis tests were conducted on the catalyst. After 72 hours of continuous reaction, the aromatic yield of the catalyst from this invention decreased by only 4.3% (from 85.2% to 81.5%), while the yield of commercial ZSM-5 decreased by 15.7% after only 24 hours. The results are shown in Table 1.
[0080] Table 1: Test results of continuous catalytic pyrolysis reaction
[0081]
[0082] To address the problems of catalyst deactivation due to carbon deposition from pyrolysis intermediates and low selectivity and yield of liquid hydrocarbon components in traditional catalysts, this invention systematically solves the above-mentioned defects through three innovative mechanisms: "raw material selection, multi-level pore structure design, and precise control of acid-base sites".
[0083] This invention, through the regulation of the silicon-aluminum structure of solid waste raw materials and the synergistic modification with ammonium chloride and TPABr, synthesizes a ZSM-5 catalyst with a multi-level pore composite structure where micropores and mesopores coexist. This overcomes mass transfer limitations and inhibits carbon deposition. This unique structure has multiple advantages: "micropore size matches aromatic molecules, and the mesoporous structure provides a rapid diffusion channel for macromolecular pyrolysis intermediates, accelerating molecular mass transfer within the catalyst and preventing excessive residence of molecules in the micropores, which leads to condensation and carbon deposition."
[0084] Secondly, the mesopores act as a buffer space for carbon deposition, transferring carbon deposits to regions with less impact on active sites. Through the regulation of acid site distribution, the acidity of the catalyst is significantly reduced. Its weak acidity inhibits the polymerization of macromolecules and carbon deposition. Simultaneously, it retains an appropriate number of weak acid sites to promote C-C bond breaking and facilitate the decomposition of biomass macromolecules into light hydrocarbons. Compared to the mechanism of commercial ZSM-5, which relies solely on microporous sieving, this catalyst achieves a breakthrough improvement in anti-coking performance while maintaining high aromatic selectivity.
[0085] This invention establishes a clear causal link between "raw material selection and auxiliary agent effect" and "anti-carbon deposition and high selectivity" performance, rather than being a random experimental result. Multi-dimensional characterization using BET, XRD, XPS, and other methods fully demonstrates the rationality and advancement of the technical solution.
[0086] In summary, the raw materials for the synthesized catalyst of this invention are derived from common industrial solid waste, reducing catalyst production costs. Furthermore, it overcomes the dependence on liquid-phase reaction media in traditional hydrothermal methods, constructing a solvent-free, all-solid-phase reaction system. In catalytic pyrolysis reactions using the synthesized ZSM-5 molecular sieve catalyst, its anti-coking performance is superior to commercial ZSM-5 molecular sieve catalysts. Simultaneously, thanks to optimized pore structure, aromatic selectivity is significantly improved. The molecular sieve catalyst preparation method proposed in this invention is low-cost and environmentally friendly. Compared to traditional hydrothermal processes, it increases raw material utilization and reduces pollutant emissions, providing an economical and efficient solution for the industrial-scale synthesis of ZSM-5 molecular sieve catalysts to produce aromatic-rich biofuels, while simultaneously achieving high-value utilization of solid waste.
[0087] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.
Claims
1. A method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis, characterized in that, Includes the following steps: (1) Mix and grind the solid waste raw material with ammonium chloride, tetrapropylammonium bromide and sodium metasilicate nonahydrate in a certain proportion to obtain a mixed raw material; wherein, the solid waste raw material includes silicon source containing silicon element and aluminum source containing aluminum element; (2) The mixed raw materials are placed in a closed environment to carry out a crystallization reaction. After crystallization, a solid product is obtained. (3) The obtained solid product was washed and dried to obtain a purified product; (4) The purified product was calcined in air to obtain solid waste-based molecular sieve catalyst ZSM-5.
2. The method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis according to claim 1, characterized in that: In step (1), the silicon source includes rice husk ash; the aluminum source includes FCC catalyst; and the mass ratio of solid waste raw material, ammonium chloride, tetrapropylammonium bromide and sodium metasilicate nonahydrate is 1:1.2~1.4:0.6~0.8:3.9~4.
1.
3. The method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis according to claim 1, characterized in that: In step (1), a certain proportion of nano-sized calcium carbonate (CaCO3) powder is added to obtain solid waste-based molecular sieve catalysts with different pore sizes; the particle size of the calcium carbonate powder is <50 nm; the mass ratio of solid waste raw material, ammonium chloride, tetrapropylammonium bromide, sodium metasilicate nonahydrate, and calcium carbonate powder is 1:1.2~1.4:0.6~0.8:3.9~4.1:0.01~0.2; the solid product obtained by adding nano-sized calcium carbonate powder is first impregnated in 0.1~0.2 mol / L hydrochloric acid, the mass ratio of hydrochloric acid to solid product is 5~10:1, and then washed with deionized water until neutral.
4. The method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis according to claim 1, characterized in that: In step (1), a certain proportion of metal nitrates are added to obtain solid waste-based molecular sieve catalysts with different metal loads; the mass ratio of the metal nitrates to the solid waste raw materials is 0.01~0.1:
1.
5. The method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis according to claim 1, characterized in that: In step (1), the operation is stopped after grinding until a pungent ammonia odor appears, and the mixed raw materials are obtained.
6. The method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis according to claim 1, characterized in that: In step (2), the temperature of the crystallization reaction is 170~190 ℃ and the reaction time is 24~36 h.
7. The method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis according to claim 1, characterized in that: In step (3), the solid product is washed with deionized water until neutral; the drying temperature is 100~110 ℃ and the drying time is 12~24 h.
8. The method for preparing a solid waste-based molecular sieve catalyst for biomass catalytic pyrolysis according to claim 1, characterized in that: In step (4), the heating rate of the calcination treatment is 10~20 ℃ / min, the calcination temperature is 550~600 ℃, and the calcination time is 4~6 h.
9. A solid waste-based molecular sieve catalyst ZSM-5, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 8.
10. An application of the solid waste-based molecular sieve catalyst ZSM-5 as described in claim 9, characterized in that: It is used as a catalyst in biomass catalytic pyrolysis reactions.