Electrode for hydrogen production by water electrolysis, preparation method therefor, and use thereof in hydrogen production by water electrolysis
By employing a region scanning technique with a moving electrode, a multi-level porous electrode was prepared, solving the problems of high overpotential and safety risks associated with traditional alkaline water electrolysis hydrogen production electrodes. This enabled the preparation of highly active electrodes suitable for large-scale mass production.
Patent Information
- Application Number
- PCT/CN2025/144499
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2025-12-22
- Publication Date
- 2026-11-12
AI Technical Summary
Traditional alkaline water electrolysis for hydrogen production suffers from high electrode overpotential and high energy consumption. Furthermore, conventional bubble template methods pose safety risks and are unsuitable for large-scale production.
By employing a region scanning technique with a moving counter electrode, the electric field distribution is controlled and the working current density is reduced by setting the counter electrode to be covered by an insulating sleeve, thus preparing a multi-level porous electrode. An alloy catalyst is then deposited on the surface of the working electrode using a metal salt plating solution, forming an electrode with a large specific surface area and high activity.
It significantly reduces the electrode oxygen evolution overpotential, improves electrode activity, is suitable for large-scale mass production, and reduces safety risks.
Smart Images

Figure CN2025144499_12112026_PF_FP_ABST
Abstract
Description
Electrolytic water electrolysis hydrogen production electrode, its preparation method and its application in electrolytic water hydrogen production
[0001] Cross-reference information
[0002] This application claims priority to Chinese Patent Application No. 2025105917674, filed on May 9, 2025, entitled "An Electrode for Hydrogen Production by Electrolysis of Water and its Preparation Method and its Application in Hydrogen Production by Electrolysis of Water", the entire contents of which are incorporated herein by reference. Technical Field
[0003] This invention relates to the field of alkaline electrolysis for hydrogen production, specifically to an electrode for hydrogen production by water electrolysis, its preparation method, and its application in hydrogen production by water electrolysis. Background Technology
[0004] Hydrogen production via water electrolysis has garnered significant attention as a clean energy technology for providing green hydrogen. However, the high overpotential of traditional alkaline water electrolysis electrodes leads to high energy consumption, limiting the widespread adoption of green hydrogen technology. Therefore, reducing the energy consumption of alkaline water electrolysis for hydrogen production is crucial.
[0005] Bubble template method is an effective method for electrodeposition preparation of water electrolysis electrodes. It utilizes the formation and evolution of bubbles in a liquid to construct materials with specific microstructures, as shown in CN202210845166.8, CN201910820769.0, and CN202211275336.X. This method can form a porous structure on the electrode material surface, thereby increasing the specific surface area of the electrode and improving its electrocatalytic activity and mass transfer efficiency. However, conventional bubble template methods are usually accompanied by intense hydrogen production and very high operating current densities, posing safety concerns and making them unsuitable for large-scale production. Therefore, it is necessary to provide a new method for preparing electrodes to address these issues. Summary of the Invention
[0006] To address the aforementioned technical problems, the present invention aims to provide an electrode for hydrogen production via water electrolysis, its preparation method, and its application in hydrogen production via water electrolysis. This preparation method can reduce the operating current density, lower safety risks, and is suitable for large-scale batch production. Furthermore, the resulting electrode has the advantages of a large specific surface area and high activity.
[0007] To achieve the above objectives, the present invention provides a method for preparing an electrolytic water hydrogen production electrode, comprising: immersing a working electrode and a counter electrode in a metal salt plating solution; connecting the working electrode to the negative terminal of a power supply and the counter electrode to the positive terminal of the power supply; after energizing the power supply, moving the counter electrode to scan the working electrode, so that metal ions in the metal salt plating solution are reduced on the surface of the working electrode to be plated, depositing to form a metal layer, thereby obtaining the electrolytic water hydrogen production electrode; wherein, an insulating sleeve is provided to cover the outer surface of the counter electrode; one end of the insulating sleeve has an opening so that one outer surface of the counter electrode is not covered, and at least a portion of the insulating sleeve extends beyond the uncovered end of the counter electrode along the direction of the opening; the surface of the working electrode to be plated and the uncovered outer surface of the counter electrode are arranged parallel to each other.
[0008] When energized, under the influence of the electric field, metal ions in the metal salt plating solution are reduced on the working electrode. Based on the aforementioned counter electrode setup, the electric field lines become very dense and the electric field becomes more uniform. Therefore, the working electrode only generates bubbles intensely in the region directly opposite the counter electrode, resulting in the deposition of a multi-level porous electrode.
[0009] Furthermore, during the scanning process of the working electrode by the moving counter electrode, the entire working electrode can be gradually and uniformly deposited with an alloy catalyst coating. This invention employs a moving counter electrode and a region-scanning method to deposit the working electrode, which significantly reduces the operating current density, lowers safety risks, and yields an electrode with advantages such as a large specific surface area and high activity, making it particularly suitable for large-scale batch production.
[0010] Furthermore, the area ratio of the uncovered outer surface of the counter electrode to the surface of the working electrode to be plated is 0.005–0.1:1; the ratio of the axial length of the insulating sleeve to the counter electrode is 1.1–1.3:1. With a smaller counter electrode area and shielding by the insulating sleeve, the electric field lines will be denser and the electric field more uniform.
[0011] Furthermore, the distance between the surface of the working electrode to be plated and the uncovered outer surface of the counter electrode is 0.5 to 10 cm.
[0012] In some alternative implementations, the scanning path is a step-reciprocating, spiral-reciprocating, or Z-shaped path.
[0013] In some alternative embodiments, the scanning speed of the electrodes is 0.01 to 0.1 m / s, preferably 0.02 to 0.06 m / s.
[0014] Furthermore, the current density at the counter electrode is 0.5–5 A / cm². 2 Preferably 3-5A / cm 2 .
[0015] Alternatively, the working electrode may be a nickel mesh, nickel foam, or a perforated nickel plate.
[0016] Optionally, the counter electrode is a nickel block, an iron block, or a nickel-iron alloy block.
[0017] Optionally, the solute in the metal salt plating solution includes one or more combinations of nickel salts, cobalt salts, and iron salts, and the solvent is water.
[0018] Optionally, the concentration of the metal salt plating solution is 10–200 g / L, preferably 70–150 g / L.
[0019] Optionally, a robotic arm is provided with the counter electrode to scan the working electrode by moving the counter electrode. The robotic arm is electrically conductive, and the counter electrode is connected to the positive terminal of the power supply through the robotic arm. For example, in one optional embodiment, the robotic arm fixes the counter electrode with a clamp to precisely control the position of the counter electrode, and scans the counter electrode by moving the robotic arm in the XY axis direction. In some optional embodiments, the step distance of the robotic arm is 0.5 to 10 cm, which means that the robotic arm moves 0.5 to 10 cm in one row before moving to the next row.
[0020] The present invention also provides an electrode for producing hydrogen by water electrolysis, which is prepared by the aforementioned method for preparing electrodes.
[0021] The present invention also provides an application of the aforementioned water electrolysis hydrogen production electrode in water electrolysis hydrogen production. Attached Figure Description
[0022] Figure 1 shows a schematic diagram of a system for preparing an electrolytic water hydrogen production electrode according to one embodiment of the present invention;
[0023] Figure 2 shows a schematic diagram of a system for preparing an electrolytic water hydrogen production electrode according to one embodiment of the present invention;
[0024] Figure 3 shows a SEM image of the water electrolysis hydrogen production electrode in Comparative Example 1 of the present invention;
[0025] Figure 4 shows a SEM image of the water electrolysis hydrogen production electrode in Embodiment 1 of the present invention;
[0026] Figure 5 shows a SEM image of the water electrolysis hydrogen production electrode in Embodiment 1 of the present invention;
[0027] Figure 6 shows the activity test diagram of the water electrolysis hydrogen production electrode in Example 1 and Comparative Example 1 of the present invention.
[0028] Among them, 1-robotic arm; 2-counter electrode; 3-conductive clamp; 4-working electrode; 5-insulating sleeve. Detailed Implementation
[0029] In order to provide a clearer understanding of the technical features, objectives and beneficial effects of the present invention, the technical solution of the present invention will now be described in detail below, but it should not be construed as limiting the scope of implementation of the present invention.
[0030] Example 1
[0031] This embodiment provides a method for preparing an electrode for hydrogen production by water electrolysis, which includes the following steps:
[0032] Provide a power source;
[0033] Provide metal salt plating solution: Dissolve 630g nickel sulfate hexahydrate, 168g ferrous sulfate heptahydrate, 150g boric acid and 6g sodium dodecyl sulfate in 6L deionized water, and adjust the pH of the system to 3.0 using sulfuric acid / ammonia water to obtain the metal salt plating solution.
[0034] Working electrode 4: Nickel mesh (200 mesh, plain weave, nickel mesh wire diameter 50μm, thickness 0.2mm, length 40cm, width 40cm);
[0035] A counter electrode 2 is provided: The counter electrode 2 is a nickel block with an area of 3cm×3cm×3cm; an insulating sleeve 5 is provided on the outer surface of the nickel block; one end of the insulating sleeve 5 has an opening so that one outer surface of the counter electrode 2 is not covered; the axial length of the sleeve is 3.3cm, and the ratio of the axial length of the insulating sleeve 5 to that of the counter electrode 2 is 1.1:1, so that at least a portion of the insulating sleeve 5 extends beyond the uncovered end of the counter electrode 2 along the direction of the opening; the counter electrode 2 is connected to a robotic arm 1 in the XY axis direction;
[0036] The working electrode 4 is immersed in a metal salt plating solution using a conductive clamp 3, and the counter electrode 2 is also immersed in the metal salt plating solution using a robotic arm 1. The surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 are arranged relatively parallel to each other (as shown in Figures 1 and 2). The distance between the relatively parallel arrangement of the surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 is 2 cm. The area ratio of the uncovered outer surface of the counter electrode 2 to the surface of the working electrode 4 to be plated is 0.0056:1. The working electrode 4 is connected to the negative terminal of the power supply, and the counter electrode 2 and the robotic arm 1 are connected to the positive terminal of the power supply. The robotic arm 1 is in a conductive state.
[0037] When the power is turned on, the robotic arm 1 drives the counter electrode 2 to perform a step-by-step repeated scan of the working electrode 4. This reduces the metal ions in the metal salt plating solution on the surface of the layer to be plated on the working electrode 4, depositing a metal layer on the entire surface of the working electrode 4, thus obtaining the electrolytic water hydrogen production electrode. The scanning speed is 0.02 m / s; the step distance is 2 cm; and the current density of the counter electrode 2 is 3 A / cm². 2 .
[0038] Example 2
[0039] This embodiment provides a method for preparing an electrode for hydrogen production by water electrolysis, which includes the following steps:
[0040] Provide a power source;
[0041] Provide metal salt plating solution: Dissolve 630g nickel sulfate hexahydrate, 168g ferrous sulfate heptahydrate, 150g boric acid and 6g sodium dodecyl sulfate in 6L deionized water, and adjust the pH of the system to 3.0 using sulfuric acid / ammonia water to obtain the metal salt plating solution.
[0042] Working electrode 4: Nickel mesh (200 mesh, plain weave, nickel mesh wire diameter 50μm, thickness 0.2mm, length 40cm, width 40cm);
[0043] A counter electrode 2 is provided: The counter electrode 2 is a nickel block with an area of 3cm×3cm×3cm; an insulating sleeve 5 is provided on the outer surface of the nickel block; one end of the insulating sleeve 5 has an opening so that one outer surface of the counter electrode 2 is not covered; the axial length of the sleeve is 3.3cm, and the ratio of the axial length of the insulating sleeve 5 to that of the counter electrode 2 is 1.1:1, so that at least a portion of the insulating sleeve 5 extends beyond the uncovered end of the counter electrode 2 along the direction of the opening; the nickel block is connected to a robotic arm 1 in the XY axis direction;
[0044] The working electrode 4 is immersed in a metal salt plating solution using a conductive clamp 3, and the counter electrode 2 is also immersed in the metal salt plating solution using a robotic arm 1. The surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 are arranged relatively parallel to each other (as shown in Figures 1 and 2). The distance between the relatively parallel arrangement of the surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 is 2 cm. The area ratio of the uncovered outer surface of the counter electrode 2 to the surface of the working electrode 4 to be plated is 0.0056:1. The working electrode 4 is connected to the negative terminal of the power supply, and the counter electrode 2 and the robotic arm 1 are connected to the positive terminal of the power supply. The robotic arm 1 is in a conductive state.
[0045] When the power is turned on, the robotic arm 1 drives the counter electrode 2 to perform a step-by-step repeated scan of the working electrode 4. This reduces the metal ions in the metal salt plating solution on the surface of the layer to be plated on the working electrode 4, depositing a metal layer on the entire surface of the working electrode 4, thus obtaining the electrolytic water hydrogen production electrode. The scanning speed is 0.04 m / s; the step distance is 3 cm; and the current density of the counter electrode 2 is 4 A / cm². 2 .
[0046] Example 3
[0047] This embodiment provides a method for preparing an electrode for hydrogen production by water electrolysis, which includes the following steps:
[0048] Provide a power source;
[0049] Provide metal salt plating solution: Dissolve 630g nickel sulfate hexahydrate, 168g ferrous sulfate heptahydrate, 150g boric acid and 6g sodium dodecyl sulfate in 6L deionized water, and adjust the pH of the system to 3.0 using sulfuric acid / ammonia water to obtain the metal salt plating solution.
[0050] Working electrode 4: Nickel mesh (200 mesh, plain weave, nickel mesh wire diameter 50μm, thickness 0.2mm, length 40cm, width 40cm);
[0051] A counter electrode 2 is provided: The counter electrode 2 is a nickel block with an area of 3cm×3cm×3cm; an insulating sleeve 5 is provided on the outer surface of the nickel block; one end of the insulating sleeve 5 has an opening so that one outer surface of the counter electrode 2 is not covered; the size of the sleeve is 3.3cm, and the ratio of the axial length of the insulating sleeve 5 to that of the counter electrode 2 is 1.1:1, so that at least a portion of the insulating sleeve 5 extends beyond the uncovered end of the counter electrode 2 along the direction of the opening; the nickel block is connected to a robotic arm 1 in the XY axis direction;
[0052] The working electrode 4 is immersed in a metal salt plating solution using a conductive clamp 3, and the counter electrode 2 is also immersed in the metal salt plating solution using a robotic arm 1. The surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 are arranged relatively parallel to each other (as shown in Figures 1 and 2). The distance between the relatively parallel arrangement of the surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 is 2 cm. The area ratio of the uncovered outer surface of the counter electrode 2 to the surface of the working electrode 4 to be plated is 0.0056:1. The working electrode 4 is connected to the negative terminal of the power supply, and the counter electrode 2 and the robotic arm 1 are connected to the positive terminal of the power supply. The robotic arm 1 is in a conductive state.
[0053] When the power is turned on, the robotic arm 1 drives the counter electrode 2 to perform a step-by-step repeated scan of the working electrode 4. This reduces the metal ions in the metal salt plating solution on the surface of the layer to be plated on the working electrode 4, depositing a metal layer on the entire surface of the working electrode 4, thus obtaining the electrolytic water hydrogen production electrode. The scanning speed is 0.06 m / s; the step distance is 4 cm; and the current density of the counter electrode 2 is 5 A / cm². 2 .
[0054] Example 4
[0055] This embodiment provides a method for preparing an electrode for hydrogen production by water electrolysis, which includes the following steps:
[0056] Provide a power source;
[0057] Provide metal salt plating solution: Dissolve 330g nickel sulfate hexahydrate, 88g ferrous sulfate heptahydrate, 150g boric acid and 6g sodium dodecyl sulfate in 6L deionized water, and adjust the pH of the system to 3.0 using sulfuric acid / ammonia water to obtain the metal salt plating solution.
[0058] Working electrode 4: Nickel mesh (200 mesh, plain weave, nickel mesh wire diameter 50μm, thickness 0.2mm, length 40cm, width 40cm);
[0059] A counter electrode 2 is provided: The counter electrode 2 is a nickel block with an area of 3cm×3cm×3cm; an insulating sleeve 5 is provided on the outer surface of the nickel block; one end of the insulating sleeve 5 has an opening so that one outer surface of the counter electrode 2 is not covered; the size of the sleeve is 3.3cm, and the ratio of the axial length of the insulating sleeve 5 to that of the counter electrode 2 is 1.1:1, so that at least a portion of the insulating sleeve 5 extends beyond the uncovered end of the counter electrode 2 along the direction of the opening; the nickel block is connected to a robotic arm 1 in the XY axis direction;
[0060] The working electrode 4 is immersed in a metal salt plating solution using a conductive clamp 3, and the counter electrode 2 is also immersed in the metal salt plating solution using a robotic arm 1. The surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 are arranged relatively parallel to each other (as shown in Figures 1 and 2). The distance between the relatively parallel arrangement of the surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 is 2 cm. The area ratio of the uncovered outer surface of the counter electrode 2 to the surface of the working electrode 4 to be plated is 0.0056:1. The working electrode 4 is connected to the negative terminal of the power supply, and the counter electrode 2 and the robotic arm 1 are connected to the positive terminal of the power supply. The robotic arm 1 is in a conductive state.
[0061] When the power is turned on, the robotic arm 1 drives the counter electrode 2 to perform a step-by-step repeated scan of the working electrode 4. This reduces the metal ions in the metal salt plating solution on the surface of the layer to be plated on the working electrode 4, depositing a metal layer on the entire surface of the working electrode 4, thus obtaining the electrolytic water hydrogen production electrode. The scanning speed is 0.06 m / s; the step distance is 4 cm; and the current density of the counter electrode 2 is 5 A / cm². 2 .
[0062] Example 5
[0063] This embodiment provides a method for preparing an electrode for hydrogen production by water electrolysis, which includes the following steps:
[0064] Provide a power source;
[0065] The metal salt plating solution is prepared by dissolving 710.5g nickel sulfate hexahydrate, 189.5g ferrous sulfate heptahydrate, 150g boric acid and 6g sodium dodecyl sulfate in 6L of deionized water and adjusting the pH of the system to 3.0 using sulfuric acid / ammonia water.
[0066] Working electrode 4: Nickel mesh (200 mesh, plain weave, nickel mesh wire diameter 50μm, thickness 0.2mm, length 40cm, width 40cm);
[0067] A counter electrode 2 is provided: The counter electrode 2 is a nickel block with an area of 3cm×3cm×3cm; an insulating sleeve 5 is provided on the outer surface of the nickel block; one end of the insulating sleeve 5 has an opening so that one outer surface of the counter electrode 2 is not covered; the size of the sleeve is 3.3cm, and the ratio of the axial length of the insulating sleeve 5 to that of the counter electrode 2 is 1.1:1, so that at least a portion of the insulating sleeve 5 extends beyond the uncovered end of the counter electrode 2 along the direction of the opening; the nickel block is connected to a robotic arm 1 in the XY axis direction;
[0068] The working electrode 4 is immersed in a metal salt plating solution using a conductive clamp 3, and the counter electrode 2 is also immersed in the metal salt plating solution using a robotic arm 1. The surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 are arranged relatively parallel to each other (as shown in Figures 1 and 2). The distance between the relatively parallel arrangement of the surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 is 2 cm. The area ratio of the uncovered outer surface of the counter electrode 2 to the surface of the working electrode 4 to be plated is 0.0056:1. The working electrode 4 is connected to the negative terminal of the power supply, and the counter electrode 2 and the robotic arm 1 are connected to the positive terminal of the power supply. The robotic arm 1 is in a conductive state.
[0069] When the power is turned on, the robotic arm 1 drives the counter electrode 2 to perform a step-by-step repeated scan of the working electrode 4. This reduces the metal ions in the metal salt plating solution on the surface of the layer to be plated on the working electrode 4, depositing a metal layer on the entire surface of the working electrode 4, thus obtaining the electrolytic water hydrogen production electrode. The scanning speed is 0.06 m / s; the step distance is 4 cm; and the current density of the counter electrode 2 is 5 A / cm². 2 .
[0070] Example 6
[0071] This embodiment provides a method for preparing an electrode for hydrogen production by water electrolysis, which includes the following steps:
[0072] Provide a power source;
[0073] Provide metal salt plating solution: Dissolve 630g nickel sulfate hexahydrate, 168g ferrous sulfate heptahydrate, 150g boric acid and 6g sodium dodecyl sulfate in 6L deionized water, and adjust the pH of the system to 3.0 using sulfuric acid / ammonia water to obtain the metal salt plating solution.
[0074] Working electrode 4: Nickel mesh (200 mesh, plain weave, nickel mesh wire diameter 50μm, thickness 0.2mm, length 40cm, width 40cm);
[0075] A counter electrode 2 is provided: The counter electrode 2 is a nickel block with an area of 3cm×3cm×3cm; an insulating sleeve 5 is provided on the outer surface of the nickel block; one end of the insulating sleeve 5 has an opening so that one outer surface of the counter electrode 2 is not covered; the size of the sleeve is 3.3cm, and the ratio of the axial length of the insulating sleeve 5 to that of the counter electrode 2 is 1.1:1, so that at least a portion of the insulating sleeve 5 extends beyond the uncovered end of the counter electrode 2 along the direction of the opening; the nickel block is connected to a robotic arm 1 in the XY axis direction;
[0076] The working electrode 4 is immersed in a metal salt plating solution using a conductive clamp 3, and the counter electrode 2 is also immersed in the metal salt plating solution using a robotic arm 1. The surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 are arranged relatively parallel to each other (as shown in Figures 1 and 2). The distance between the relatively parallel arrangement of the surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 is 2 cm. The area ratio of the uncovered outer surface of the counter electrode 2 to the surface of the working electrode 4 to be plated is 0.0056:1. The working electrode 4 is connected to the negative terminal of the power supply, and the counter electrode 2 and the robotic arm 1 are connected to the positive terminal of the power supply. The robotic arm 1 is in a conductive state.
[0077] When the power is turned on, the robotic arm 1 drives the counter electrode 2 to perform a step-by-step repeated scan of the working electrode 4. This reduces the metal ions in the metal salt plating solution on the surface of the layer to be plated on the working electrode 4, depositing a metal layer on the entire surface of the working electrode 4, thus obtaining the electrolytic water hydrogen production electrode. The scanning speed is 0.04 m / s; the step distance is 4 cm; and the current density of the counter electrode 2 is 5 A / cm². 2 .
[0078] Example 7
[0079] This embodiment provides a method for preparing an electrode for hydrogen production by water electrolysis, which includes the following steps:
[0080] Provide a power source;
[0081] Provide metal salt plating solution: Dissolve 42g nickel sulfate hexahydrate, 11.2g ferrous sulfate heptahydrate, 150g boric acid and 6g sodium dodecyl sulfate in 6L deionized water, and adjust the pH of the system to 3.0 using sulfuric acid / ammonia water to obtain the metal salt plating solution.
[0082] Working electrode 4: Nickel mesh (200 mesh, plain weave, nickel mesh wire diameter 50μm, thickness 0.2mm, length 40cm, width 40cm);
[0083] A counter electrode 2 is provided: The counter electrode 2 is a nickel block with an area of 3cm×3cm×3cm; an insulating sleeve 5 is provided on the outer surface of the nickel block; one end of the insulating sleeve 5 has an opening so that one outer surface of the counter electrode 2 is not covered; the size of the sleeve is 3.3cm, and the ratio of the axial length of the insulating sleeve 5 to that of the counter electrode 2 is 1.1:1, so that at least a portion of the insulating sleeve 5 extends beyond the uncovered end of the counter electrode 2 along the direction of the opening; the nickel block is connected to a robotic arm 1 in the XY axis direction;
[0084] The working electrode 4 is immersed in a metal salt plating solution using a conductive clamp 3, and the counter electrode 2 is also immersed in the metal salt plating solution using a robotic arm 1. The surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 are arranged relatively parallel to each other (as shown in Figures 1 and 2). The distance between the relatively parallel arrangement of the surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 is 2 cm. The area ratio of the uncovered outer surface of the counter electrode 2 to the surface of the working electrode 4 to be plated is 0.0056:1. The working electrode 4 is connected to the negative terminal of the power supply, and the counter electrode 2 and the robotic arm 1 are connected to the positive terminal of the power supply. The robotic arm 1 is in a conductive state.
[0085] When the power is turned on, the robotic arm 1 drives the counter electrode 2 to perform a step-by-step repeated scan of the working electrode 4. This reduces the metal ions in the metal salt plating solution on the surface of the layer to be plated on the working electrode 4, depositing a metal layer on the entire surface of the working electrode 4, thus obtaining the electrolytic water hydrogen production electrode. The scanning speed is 0.06 m / s; the step distance is 4 cm; and the current density of the counter electrode 2 is 5 A / cm². 2 .
[0086] Example 8
[0087] This embodiment provides a method for preparing an electrode for hydrogen production by water electrolysis, which includes the following steps:
[0088] Provide a power source;
[0089] Provide metal salt plating solution: Dissolve 819g nickel sulfate hexahydrate, 218.4g ferrous sulfate heptahydrate, 150g boric acid and 6g sodium dodecyl sulfate in 6L deionized water, and adjust the pH of the system to 3.0 using sulfuric acid / ammonia water to obtain the metal salt plating solution.
[0090] Working electrode 4: Nickel mesh (200 mesh, plain weave, nickel mesh wire diameter 50μm, thickness 0.2mm, length 40cm, width 40cm);
[0091] A counter electrode 2 is provided: The counter electrode 2 is a nickel block with an area of 3cm×3cm×3cm; an insulating sleeve 5 is provided on the outer surface of the nickel block; one end of the insulating sleeve 5 has an opening so that one outer surface of the counter electrode 2 is not covered; the size of the sleeve is 3.3cm, and the ratio of the axial length of the insulating sleeve 5 to that of the counter electrode 2 is 1.1:1, so that at least a portion of the insulating sleeve 5 extends beyond the uncovered end of the counter electrode 2 along the direction of the opening; the nickel block is connected to a robotic arm 1 in the XY axis direction;
[0092] The working electrode 4 is immersed in a metal salt plating solution using a conductive clamp 3, and the counter electrode 2 is also immersed in the metal salt plating solution using a robotic arm 1. The surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 are arranged relatively parallel to each other (as shown in Figures 1 and 2). The distance between the relatively parallel arrangement of the surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 is 2 cm. The area ratio of the uncovered outer surface of the counter electrode 2 to the surface of the working electrode 4 to be plated is 0.0056:1. The working electrode 4 is connected to the negative terminal of the power supply, and the counter electrode 2 and the robotic arm 1 are connected to the positive terminal of the power supply. The robotic arm 1 is in a conductive state.
[0093] When the power is turned on, the robotic arm 1 drives the counter electrode 2 to perform a step-by-step repeated scan of the working electrode 4. This reduces the metal ions in the metal salt plating solution on the surface of the layer to be plated on the working electrode 4, depositing a metal layer on the entire surface of the working electrode 4, thus obtaining the electrolytic water hydrogen production electrode. The scanning speed is 0.06 m / s; the step distance is 4 cm; and the current density of the counter electrode 2 is 5 A / cm². 2 .
[0094] Example 9
[0095] This embodiment provides a method for preparing an electrode for hydrogen production by water electrolysis, which includes the following steps:
[0096] Provide a power source;
[0097] Provide metal salt plating solution: Dissolve 630g nickel sulfate hexahydrate, 168g ferrous sulfate heptahydrate, 150g boric acid and 6g sodium dodecyl sulfate in 6L deionized water, and adjust the pH of the system to 3.0 using sulfuric acid / ammonia water to obtain the metal salt plating solution.
[0098] Working electrode 4: Nickel mesh (200 mesh, plain weave, nickel mesh wire diameter 50μm, thickness 0.2mm, length 40cm, width 40cm);
[0099] A counter electrode 2 is provided: The counter electrode 2 is a nickel block with an area of 3cm×3cm×3cm; an insulating sleeve 5 is provided on the outer surface of the nickel block; one end of the insulating sleeve 5 has an opening so that one outer surface of the counter electrode 2 is not covered; the size of the sleeve is 3.3cm, and the ratio of the axial length of the insulating sleeve 5 to that of the counter electrode 2 is 1.1:1, so that at least a portion of the insulating sleeve 5 extends beyond the uncovered end of the counter electrode 2 along the direction of the opening; the nickel block is connected to a robotic arm 1 in the XY axis direction;
[0100] The working electrode 4 is immersed in a metal salt plating solution using a conductive clamp 3, and the counter electrode 2 is also immersed in the metal salt plating solution using a robotic arm 1. The surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 are arranged relatively parallel to each other (as shown in Figures 1 and 2). The distance between the relatively parallel arrangement of the surface of the working electrode 4 to be plated and the uncovered outer surface of the counter electrode 2 is 2 cm. The area ratio of the uncovered outer surface of the counter electrode 2 to the surface of the working electrode 4 to be plated is 0.0056:1. The working electrode 4 is connected to the negative terminal of the power supply, and the counter electrode 2 and the robotic arm 1 are connected to the positive terminal of the power supply. The robotic arm 1 is in a conductive state.
[0101] When the power is turned on, the robotic arm 1 drives the counter electrode 2 to perform a step-by-step repeated scan of the working electrode 4. This reduces the metal ions in the metal salt plating solution on the surface of the layer to be plated on the working electrode 4, depositing a metal layer on the entire surface of the working electrode 4, thus obtaining the electrolytic water hydrogen production electrode. The scanning speed is 0.2 m / s; the step distance is 4 cm; and the current density of the counter electrode 2 is 5 A / cm². 2 .
[0102] Comparative Example 1
[0103] Electrolysis of water to produce hydrogen electrode: nickel mesh (200 mesh, plain weave, nickel mesh wire diameter 50μm, thickness 0.2mm, length 40cm, width 40cm).
[0104] Performance evaluation:
[0105] (I) Morphological characterization: The electrode structure was characterized by field emission scanning electron microscopy (SEM) using a Hitachi S4800 microscope with magnifications of X100 and X1000.
[0106] Figure 3 shows a SEM image (magnification x 100) of the water electrolysis hydrogen production electrode in Comparative Example 1 of the present invention; Figure 4 shows a SEM image (magnification x 100) of the water electrolysis hydrogen production electrode in Example 1 of the present invention; Figure 5 shows a SEM image (magnification x 1000) of the water electrolysis hydrogen production electrode in Example 1 of the present invention.
[0107] As can be seen from Figures 3, 4 and 5, Embodiment 1 of the present invention can obtain a uniform multi-level porous electrode, which has a large active area.
[0108] (II) Electrode Activity Test: A three-electrode system was used for testing at room temperature. The electrolyte was 1M KOH. The working electrode was the water electrolysis hydrogen production electrode (1cm × 1cm) from the aforementioned examples and comparative examples. The counter electrode was a platinum sheet electrode, and the reference electrode was a saturated calomel electrode. Polarization curves and solution resistance were measured using linear voltammetry and electrochemical impedance spectroscopy.
[0109] Figure 6 shows the activity test results of the water electrolysis hydrogen production electrode in Example 1 and the water electrolysis hydrogen production electrode in Comparative Example 1. As can be seen from Figure 6, the electrode prepared by the method of the present invention has very high activity and can significantly reduce the oxygen evolution overpotential of the electrode.
[0110] Table 1 shows the electrolysis results of water at a current density of 0.1 A / cm². 2 and 0.3A / cm 2 The corresponding voltage.
[0111] Table 1
[0112] As shown in Table 1, the electrodes prepared by the method of the present invention can significantly reduce the oxygen evolution overpotential. Furthermore, increasing the counter electrode current density during the preparation of the water electrolysis hydrogen production electrode can further reduce the oxygen evolution overpotential. Comparative Example 1, however, uses a current density of 0.3 A / cm². 2 The voltage exceeds 2.0V, and the electrode plates are severely corroded and damaged.
Claims
1. A method for preparing an electrode for hydrogen production by water electrolysis, wherein, include: The working electrode and the counter electrode are immersed in a metal salt plating solution; The working electrode is connected to the negative terminal of the power supply, and the counter electrode is connected to the positive terminal of the power supply. After the power supply is turned on, the counter electrode is moved to scan the working electrode, so that the metal ions in the metal salt plating solution are reduced on the surface of the layer to be plated on the working electrode, and a metal layer is deposited to form a metal layer, thus obtaining an electrolytic water hydrogen production electrode. The outer surface of the counter electrode is covered with an insulating sleeve; one end of the insulating sleeve has an opening so that one outer surface of the counter electrode is not covered, and at least a portion of the insulating sleeve extends beyond the uncovered end of the counter electrode along the direction of the opening; the surface of the working electrode to be plated and the uncovered outer surface of the counter electrode are arranged parallel to each other.
2. The method for preparing an electrolytic water electrolysis hydrogen production electrode according to claim 1, wherein, The scanning speed of the counter electrode is 0.01–0.1 m / s; and / or, The current density of the counter electrode is 0.5–5 A / cm². 2 .
3. The method for preparing an electrolytic water electrolysis hydrogen production electrode according to claim 2, wherein, The scanning speed of the counter electrode is 0.02–0.06 m / s; and / or, The current density of the counter electrode is 3-5 A / cm. 2 .
4. The method for preparing an electrolytic water electrolysis hydrogen production electrode according to claim 1, wherein, The area ratio of the outer surface of the counter electrode not covered by the insulating sleeve to the surface of the working electrode to be plated is 0.005 to 0.1:1; and / or, The ratio of the axial length of the insulating sleeve to that of the counter electrode is 1.1 to 1.3:1; and / or, The distance between the surface of the working electrode to be plated and the uncovered outer surface of the counter electrode is 0.5 to 10 cm.
5. The method for preparing an electrolytic water electrolysis hydrogen production electrode according to claim 1, wherein, The counter electrode is connected to a robotic arm, which is electrically conductive to move the counter electrode to scan the working electrode; wherein the stepping distance of the robotic arm is 0.5 to 10 cm.
6. The method for preparing an electrolytic water electrolysis hydrogen production electrode according to claim 1, wherein, The scanning path can be a step-reciprocating pattern, a spiral reciprocating pattern, or a Z-shaped pattern.
7. The method for preparing an electrolytic water electrolysis hydrogen production electrode according to claim 1, wherein, The working electrode is a nickel mesh, nickel foam, or perforated nickel plate; and / or, The counter electrode is a nickel block, an iron block, or a nickel-iron alloy block.
8. The method for preparing an electrolytic water electrolysis hydrogen production electrode according to claim 1, wherein, The solute in the metal salt plating solution includes one or more of nickel salts, cobalt salts, and iron salts.
9. The method for preparing an electrolytic water electrolysis hydrogen production electrode according to claim 1, wherein, The concentration of the metal salt plating solution is 10–200 g / L.
10. The method for preparing an electrolytic water electrolysis hydrogen production electrode according to claim 1, wherein, The concentration of the metal salt plating solution is 70–150 g / L.
11. An electrode for producing hydrogen through water electrolysis, wherein, The method for preparing an electrolytic water hydrogen production electrode according to any one of claims 1 to 10 is used.
12. The application of the water electrolysis hydrogen production electrode according to claim 11 in water electrolysis hydrogen production.