Perovskite solar cell, preparation method, tandem cell, photovoltaic system, power generation apparatus, and electric apparatus

By introducing phosphine oxide organic compounds into perovskite solar cells, the oxidation of tin is suppressed, the defect density is reduced, and the tin-lead molar ratio is increased. This solves the problem of Sn2+ oxidation in tin-based perovskite materials and improves the photoelectric conversion efficiency.

WO2026233394A1PCT designated stage Publication Date: 2026-11-12CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/095354
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

In tin-based perovskite materials, Sn2+ is easily oxidized to Sn4+, which leads to an increase in the defect density of the perovskite layer and affects the improvement of photoelectric conversion efficiency.

Method used

Introducing phosphine oxide organic compounds into the perovskite layer inhibits the oxidation of tin. By controlling the coordination of phosphine oxide organic compounds with Sn2+, the defect density is reduced, the tin-lead molar ratio is optimized, and the crystallinity and photoelectric conversion efficiency of the perovskite layer are improved.

Benefits of technology

It effectively suppresses Sn2+ oxidation, reduces perovskite layer defects, improves photoelectric conversion efficiency, and enhances the performance of perovskite solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026095354_12112026_PF_FP_ABST
    Figure CN2026095354_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a perovskite solar cell, a preparation method, a tandem cell, a photovoltaic system, a power generation apparatus, and an electric apparatus. The perovskite solar cell comprises a first electrode, a perovskite layer, and a second electrode, and the perovskite layer is disposed between the first electrode and the second electrode. The perovskite layer comprises an ABX3 perovskite material and a compound represented by formula (1), wherein A comprises a monovalent cation, B comprises tin, and X comprises a monovalent anion.
Need to check novelty before this filing date? Find Prior Art

Description

Perovskite solar cells, fabrication methods, tandem cells, photovoltaic systems, power generation devices, and power consumption devices.

[0001] Related applications

[0002] This application claims priority to Chinese patent application filed on May 8, 2025, with application number 202510585468X, entitled "Perovskite Solar Cell, Preparation Method, Tandem Cell, Photovoltaic System, Power Generation Device and Power Consumption Device", the entire contents of which are incorporated herein by reference. Technical Field

[0003] This application relates to the field of solar cell technology, and in particular to perovskite solar cells, preparation methods, tandem cells, photovoltaic systems, power generation devices, and power consumption devices. Background Technology

[0004] Perovskite solar cells convert solar energy into electrical energy, making them relatively environmentally friendly. In a perovskite solar cell, the perovskite layer absorbs photons, generating electrons and holes. These electrons and holes are then transported to electrodes on either side of the perovskite layer, thus producing a photocurrent. Tin-based perovskite materials, which include tin, offer advantages such as being relatively environmentally friendly and having high photoelectric conversion efficiency. However, the oxidation of tin limits further improvements in the cell's photoelectric conversion efficiency. Summary of the Invention

[0005] The first aspect of this application provides a perovskite solar cell, including a first electrode, a perovskite layer and a second electrode, wherein the perovskite layer is disposed between the first electrode and the second electrode; the perovskite layer includes ABX3 perovskite material and phosphine oxide organic compound shown in formula (1), wherein A includes a monovalent cation, B includes tin element and X includes a monovalent anion;

[0006] In formula (1), R1, R2 and R3 each independently include H, C1-C6 alkyl, C1-C6 alkoxy, amino, methylamino, dimethylamino, mercapto, hydroxyl or halogen, and R1, R2 and R3 are not all hydrogen at the same time.

[0007] In the perovskite solar cell of the first aspect of this application, the introduction of phosphine oxide organic compound can suppress the oxidation of tin, thereby improving the photoelectric conversion efficiency of the perovskite solar cell.

[0008] In some embodiments, the total molar amount of the phosphine oxide organic compound in the perovskite layer is a, and the total molar amount of B is b, with 0.1% ≤ a / b ≤ 5%. A ratio of a / b ≥ 0.1% allows the phosphine oxide organic compound to function effectively, promoting the improvement of the photoelectric conversion efficiency of the perovskite solar cell. A ratio of a / b ≤ 5% reduces the impact of excessive residual phosphine oxide organic compound on the crystal quality of the perovskite layer, which is beneficial for reducing defects in the perovskite layer and further promoting the improvement of the photoelectric conversion efficiency of the perovskite solar cell.

[0009] In some implementations, Sn 2+ The percentage of tin in the total molar amount of the tin element is greater than or equal to 80%. At this point, the tin element in the perovskite layer contains Sn... 2+ A higher proportion of Sn can maintain a low defect density in the perovskite layer, further promoting the improvement of the cell's photoelectric conversion efficiency. Optionally, Sn... 2+ The percentage of the total molar amount of tin is greater than or equal to 90%.

[0010] In some implementations, Sn 4+ The percentage of tin in the total molar amount is less than or equal to 20%. In this case, organophosphorus oxides can more effectively bind with Sn. 2+ Coordination lowers the HOMO energy level of the complex, thereby effectively suppressing Sn. 2+ The oxidation of Sn in the perovskite layer leads to its oxidation. 4+ With a lower proportion, the photoelectric conversion efficiency of perovskite solar cells can be further improved. Optionally, Sn 4+ The percentage of the total molar amount of tin is less than or equal to 10%.

[0011] In some embodiments, one of R1, R2, and R3 is H, or R1, R2, and R3 each independently comprise a C1-C6 alkyl, C1-C6 alkoxy, amino, methylamino, dimethylamino, mercapto, hydroxyl, or halogen. In this case, at least two of R1, R2, and R3 are not H. Compared to the case where two of R1, R2, and R3 are H, the phosphine oxide organic compounds in these embodiments have a lower molecular electrostatic potential minimum and can be used with Sn. 2+ This leads to stronger coordination and further inhibits Sn. 2+ The oxidation process further improves the photoelectric conversion efficiency of perovskite solar cells.

[0012] In some embodiments, R1, R2, and R3 each independently include methyl or methoxy groups.

[0013] In some embodiments, the organophosphorus oxide compound includes one or more of the following compounds (1-1) to (1-4):

[0014] In some embodiments, the band gap of the perovskite layer is 1.1 eV to 1.8 eV. Perovskite layers with band gaps within this range have high visible light absorption, which is beneficial for further improving the photoelectric conversion efficiency of perovskite solar cells.

[0015] In some embodiments, the thickness of the perovskite layer is 200 nm to 1500 nm.

[0016] In some implementations, ABX3 includes ASn x Pb 1-x X3, where 0.5 ≤ x ≤ 1, A includes inorganic monovalent cations, organic monovalent cations, or organic-inorganic mixed cations; X includes inorganic monovalent anions, organic monovalent anions, or organic-inorganic monovalent mixed anions. Tin-lead perovskite materials can achieve a narrower band gap in the perovskite layer, which is beneficial for the development of perovskite solar cells.

[0017] In some embodiments, B further includes lead. Along the thickness direction perpendicular to the perovskite layer, the tin-lead molar ratio at the surface of the perovskite layer is d1, and the tin-lead molar ratio at the cross-section of the perovskite layer is d2, where 0.5 ≤ d2 / d1 ≤ 1. This tin-lead molar ratio represents the molar ratio of tin to lead. Along the thickness direction perpendicular to the perovskite layer, the distance between the cross-section of the perovskite layer and the surface of the perovskite layer is less than 0.5 times the thickness of the perovskite layer. In this case, the tin-lead molar ratio at the cross-section of the perovskite layer in its thickness direction is closer to the tin-lead molar ratio at its surface. This alleviates the problem of tin-lead crystallization rate mismatch, resulting in better crystallinity and fewer defects in the perovskite layer. This, in turn, reduces carrier recombination and improves the photoelectric conversion efficiency of the perovskite solar cell.

[0018] In some embodiments, d1 is 1 to 15. The atomic radius of tin atoms is smaller than that of lead atoms. When the tin-lead molar ratio is large, more tin atoms will replace lead atoms, which may cause distortion of the perovskite crystal structure, affecting the stability of the perovskite layer's spectral absorption and thus limiting the improvement of the photoelectric conversion efficiency of perovskite solar cells. In these embodiments of this application, the introduction of phosphine oxide organic compounds can effectively reduce the tin-lead molar ratio on the surface of the perovskite layer, keeping it at a low level, reducing the risk of perovskite crystal structure distortion, and promoting the improvement of the photoelectric conversion efficiency of perovskite solar cells. Optionally, d1 is 1 to 5.

[0019] In some embodiments, d2 is 0.5–15. A smaller tin-lead molar ratio d2 in the cross-section of the perovskite layer perpendicular to its thickness indicates a smaller tin-lead molar ratio within the perovskite layer. This further reduces the risk of perovskite crystal distortion, allowing the perovskite layer to maintain high stability in spectral absorption, thereby further improving the photoelectric conversion efficiency of the perovskite solar cell. Optionally, d1 is 0.5–5.

[0020] In some embodiments, the perovskite solar cell further includes a hole transport layer and / or an electron transport layer; one of the hole transport layer and the electron transport layer is located between the first electrode and the perovskite layer, and the other is located between the second electrode and the perovskite layer.

[0021] A second aspect of this application provides a method for fabricating a perovskite solar cell, comprising the following steps:

[0022] A perovskite precursor solution was prepared by mixing a tin source, a monovalent cation source, a monovalent anion source and the phosphine oxide organic compound shown in formula (1) in a solvent.

[0023] The perovskite precursor solution is applied to the surface of the first electrode and annealed to prepare a perovskite layer.

[0024] A second electrode is fabricated on the surface of the perovskite layer away from the first electrode;

[0025] In formula (1), R1, R2 and R3 each independently include H, C1-C6 alkyl, C1-C6 alkoxy, amino, methylamino, dimethylamino, mercapto, hydroxyl or halogen, and R1, R2 and R3 are not all hydrogen at the same time.

[0026] In some embodiments, the concentration of the phosphine oxide organic compound in the perovskite precursor solution is 1 mg / mL to 400 mg / mL.

[0027] In some embodiments, the annealing temperature is 90°C to 110°C.

[0028] In some embodiments, the annealing process takes 8 to 15 minutes.

[0029] A third aspect of this application provides a tandem solar cell, including a perovskite solar cell of the first aspect or a perovskite solar cell prepared by the preparation method of the second aspect.

[0030] The fourth aspect of this application provides a photovoltaic system, including a perovskite solar cell of the first aspect or a perovskite solar cell prepared by the preparation method of the second aspect.

[0031] The fifth aspect of this application provides a power generation device, including a perovskite solar cell of the first aspect or a perovskite solar cell prepared by the preparation method of the second aspect.

[0032] The sixth aspect of this application provides an electrical device, including a perovskite solar cell of the first aspect or a perovskite solar cell prepared by the preparation method of the second aspect. Attached Figure Description

[0033] To more clearly illustrate the technical solution of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without any creative effort.

[0034] Figure 1 is a schematic diagram of the structure of a perovskite solar cell according to an embodiment of this application.

[0035] Figure 2 shows the appearance of the perovskite precursor solution in Example 1 and Comparative Example 2 of this application before and after exposure to air.

[0036] Figure 3 shows the reaction of compound (1-1) in Example 1 of this application and DMSO in Comparative Example 2 with Sn. 2+ Density of states diagram of the binding.

[0037] The markings in the figure are as follows: 100, perovskite solar cell; 101, first electrode; 102, perovskite layer; 1021, surface; 1022, cross-section; 103, second electrode; 104, hole transport layer; 105, electron transport layer.

[0038] To better describe and illustrate embodiments and / or examples of the inventions disclosed herein, reference may be made to one or more accompanying drawings. Additional details or examples used to describe the drawings should not be considered as limiting the scope of any of the disclosed inventions, the currently described embodiments and / or examples, or the best mode of these inventions as currently understood. Detailed Implementation

[0039] To facilitate understanding of this application, a more complete description will be provided below with reference to the accompanying drawings. Preferred embodiments of this application are shown in the drawings. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of this application.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0041] The "range" disclosed in this application can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the specific range. Ranges defined in this way can include or exclude endpoints. Any endpoint can be included or excluded independently, and they can be combined arbitrarily; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60–120 and 80–110 are listed for a specific parameter, it is expected that ranges of 60–110 and 80–120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are also listed, then the following ranges are all expected: 1–3, 1–4, 1–5, 2–3, 2–4, and 2–5. In this application, unless otherwise stated, the numerical range "a–b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0" and "5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is described as an integer ≥ 2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For instance, when a parameter is described as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0042] In this application, the terms "multiple" or "various" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.

[0043] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0044] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The term "implementation" as used herein has a similar understanding.

[0045] Those skilled in the art will understand that the order in which the steps are written in the methods of various embodiments or examples does not imply a strict execution order and does not constitute any limitation on the implementation process. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if the method may also include step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0046] In this application, unless otherwise stated, A (e.g., B) means that B is a non-limiting example of A, and it is understood that A is not limited to B.

[0047] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0048] Unless otherwise specified, in this application, the term "room temperature" generally refers to 4°C to 30°C, and preferably 25±5°C.

[0049] Unless otherwise stated, the terms used in this application have their common meanings as commonly understood by those skilled in the art. Unless otherwise stated, the numerical values ​​of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art. For example, they can be tested according to the methods given in the embodiments of this application.

[0050] In perovskite solar cells, tin-based perovskite materials, including tin, have advantages such as being relatively environmentally friendly and having high photoelectric conversion efficiency. However, in tin-based perovskite materials, Sn... 2+ It is easily oxidized to Sn 4+ This leads to an increase in defect density in the perovskite layer, affecting carrier transport and diffusion, and thus restricting further improvement in the photoelectric conversion efficiency of the battery.

[0051] Based on this, referring to Figure 1, one embodiment of this application provides a perovskite solar cell 100. The perovskite solar cell 100 includes a first electrode 101, a perovskite layer 102, and a second electrode 103, wherein the perovskite layer 102 is disposed between the first electrode 101 and the second electrode 103; the perovskite layer 102 includes ABX3 perovskite material and phosphine oxide organic compound as shown in formula (1), wherein A includes a monovalent cation, B includes tin, and X includes a monovalent anion;

[0052] In formula (1), R1, R2 and R3 each independently include H, C1-C6 alkyl, C1-C6 alkoxy, amino, methylamino, dimethylamino, mercapto, hydroxyl or halogen, and R1, R2 and R3 are not all hydrogen at the same time.

[0053] In the perovskite solar cell 100 of this embodiment, the introduction of an organic phosphine oxide compound can suppress the oxidation of tin, for example, suppressing the oxidation of Sn. 2+ Oxidized to Sn 4+ This reduces the risk of increased defect density in the perovskite layer, thereby improving the photoelectric conversion efficiency of perovskite solar cells.

[0054] It is understandable that in ABX3 perovskite material, A represents the element at the A site, B represents the element at the B site, and X represents the element at the X site.

[0055] In some embodiments, in the perovskite layer 102, the total molar amount of phosphine oxide organic compounds is a, and the total molar amount of B is b, with 0.1% ≤ a / b ≤ 5%. A ratio of a / b ≥ 0.1% allows the phosphine oxide organic compounds to function effectively, promoting the improvement of the photoelectric conversion efficiency of the perovskite solar cell 100. A ratio of a / b ≤ 5% reduces the impact of excessive residual phosphine oxide organic compounds on the crystal quality of the perovskite layer, which is beneficial for reducing defects in the perovskite layer and further promoting the improvement of the photoelectric conversion efficiency of the perovskite solar cell 100. Optionally, a / b can be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any value within the range of any two of the above values.

[0056] In this application, the perovskite solar cell 100 can be disassembled to obtain the perovskite layer 102, and then the relevant parameters of the perovskite layer 102 can be tested. Optionally, the disassembly method can be as follows: in a clean room, the cell is cut open along the electrode edge using a knife to separate the first electrode and the second electrode, and then the perovskite layer is cleaned with a solvent, such as isopropanol or ethanol, to remove surface residues and contaminants. The separated perovskite layer is then collected using tweezers.

[0057] In this application, the ratio a / b of the total molar amount of phosphorus oxide organic compounds to the total molar amount of B in the perovskite layer 102 can be determined by the following method: elemental analysis using inductively coupled plasma mass spectrometry (ICP-MS). The equipment model is Thermo Fisher iCAP RQ. Sample preparation: The perovskite layer is ground into a homogeneous sample. 0.1 mg of the sample is taken and 0.1 mL of nitric acid and 0.1 mL of hydrofluoric acid are added for microwave digestion. After digestion, the solution is brought to a final volume of 50 mL with nitric acid to ensure complete dissolution of the sample. The total molar amounts of P and B are then measured. The test parameters are: radio frequency power: 1550 W; reaction gas: CCT mode, using ammonia. The ratio of the total molar amount of P to the total molar amount of B is taken as a / b.

[0058] In some embodiments, in the perovskite layer 102, Sn 2+ The percentage of tin in the total molar amount is greater than or equal to 80%. At this point, the tin content in perovskite layer 102 is Sn... 2+ A higher proportion of Sn allows for maintaining a low defect density in the perovskite layer 102, further promoting the improvement of the cell's photoelectric conversion efficiency. Optionally, in the perovskite layer 102, Sn... 2+ The percentage of tin in the total molar amount can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, or any value within the range of any two of the above values. Further optionally, in the perovskite layer 102, Sn... 2+ The percentage of tin in the total molar amount is greater than or equal to 90%.

[0059] In some embodiments, in the perovskite layer 102, Sn 4+ The percentage of tin in the total molar amount is less than or equal to 20%. In these embodiments of this application, the organophosphorus oxide compound can more effectively react with Sn. 2+ Coordination lowers the HOMO energy level of the complex, thereby effectively suppressing Sn. 2+ The oxidation of Sn in the perovskite layer 102 further leads to its oxidation. 4+ Having a lower proportion allows for further improvement in the photoelectric conversion efficiency of the perovskite solar cell 100. Optionally, in the perovskite layer 102, Sn 4+The percentage of tin in the total molar amount can be ≤20%, ≤19%, ≤18%, ≤17%, ≤16%, ≤15%, ≤14%, ≤13%, ≤12%, ≤11%, ≤10%, ≤9%, ≤8%, ≤7%, ≤6%, ≤5%, ≤4%, ≤3%, ≤2%, ≤1%, ≤0.5%, ≤0.1%, or any value within the range of any two of the above values. Optionally, in the perovskite layer 102, Sn... 4+ The percentage of tin in the total molar amount is less than or equal to 10%. Further optionally, in the perovskite layer 102, Sn... 4+ The percentage of tin in the total molar amount can be 0.

[0060] Understandably, Sn in the perovskite layer can be tested using X-ray photoelectron spectroscopy (XPS). 2+ and Sn 4+ The percentage of tin in the total molar amount. The XPS model is Thermofisher ESCALAB 250Xi system. Test parameters: energy scan range 0–5000 eV, energy resolution: less than or equal to 0.45 eV, X-ray source: monochromatic Al Kalpha (1468.6 eV), power 150 W.

[0061] It is understood that in formula (1), C1 to C6 alkyl refers to branched or straight-chain alkyl groups containing 1 to 6 carbon atoms, and each time it appears, it can be independently C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl, or C6 alkyl. Suitable choices may include, but are not limited to: methyl, with the structural formula -CH3; ethyl, with the structural formula -CH2CH3; 1-propyl, with the structural formula -CH2CH2CH3; 2-propyl, with the structural formula -CH(CH3)2; 1-butyl, with the structural formula -CH2CH2CH2CH3; 2-methyl-1-propyl, with the structural formula -CH2CH(CH3)2; 2-butyl, with the structural formula -CH(CH3)CH2CH3; 2-methyl-2-propyl, with the structural formula -C(CH3)2CH2CH2CH3. 3; 1-pentyl, structural formula -CH2CH2CH2CH2CH3; 2-pentyl, structural formula -CH(CH3)CH2CH2CH3; 3-pentyl, structural formula -CH(CH2CH3)2; 2-methyl-2-butyl, structural formula -C(CH3)2CH2CH3; 3-methyl-2-butyl, structural formula -CH(CH3)CH(CH3)2; 3-methyl-1-butyl, structural formula -CH2CH2CH(CH3)2; 2-methyl-1- Butyl, with the structural formula -CH2CH(CH3)CH2CH3; 1-hexyl, with the structural formula -CH2CH2CH2CH2CH2CH3; 2-hexyl, with the structural formula -CH(CH3)CH2CH2CH2CH3; 3-hexyl, with the structural formula -CH(CH2CH3)(CH2CH2CH3); 2-methyl-2-pentyl, with the structural formula -C(CH3)2CH2CH2CH3; 3-methyl-2-pentyl, with the structural formula -CH(CH3)CH(CH 3) CH2CH3; 4-methyl-2-pentyl, structural formula -CH(CH3)CH2CH(CH3)2; 3-methyl-3-pentyl, structural formula -C(CH3)(CH2CH3)2; 2-methyl-3-pentyl, structural formula -CH(CH2CH3)CH(CH3)2; 2,3-dimethyl-2-butyl, structural formula -C(CH3)2CH(CH3)2; 3,3-dimethyl-2-butyl, structural formula -CH(CH3)C(CH3)3.

[0062] In formula (1), C1 to C6 alkoxy groups refer to alkoxy groups containing 1 to 6 carbon atoms, and each time they appear, they can be independently C1 alkoxy, C2 alkoxy, C3 alkoxy, C4 alkoxy, C5 alkoxy, and C6 alkoxy groups. Suitable choices may include, but are not limited to: methoxy, with the structural formula -O-CH3; ethoxy, with the structural formula -O-CH2CH3; 1-propoxy, with the structural formula -O-CH2CH2CH3; 2-propoxy, with the structural formula -O-CH(CH3)2; and 1-butoxy, with the structural formula -O-CH2CH2CH2CH3. It is understood that C1 to C6 alkoxy groups can also be groups in which an oxygen atom is introduced into the above C1 to C6 alkyl groups, and the oxygen atom is bonded to the P atom in formula (1).

[0063] In some embodiments, one of R1, R2, and R3 is H, or R1, R2, and R3 each independently comprise a C1-C6 alkyl, C1-C6 alkoxy, amino, methylamino, dimethylamino, mercapto, hydroxyl, or halogen. In this case, at least two of R1, R2, and R3 are not H. Compared to the case where two of R1, R2, and R3 are H, the phosphine oxide organic compounds in these embodiments have a lower molecular electrostatic potential minimum and can be used with Sn. 2+ This leads to stronger coordination and further inhibits Sn. 2+ The oxidation of R1, R2, and R3 further improves the photoelectric conversion efficiency of perovskite solar cells. Optionally, R1, R2, and R3 are not H.

[0064] Alternatively, R1, R2, and R3 may each independently include methyl or methoxy groups.

[0065] In some embodiments, the organophosphorus oxide compound includes one or more of the following compounds (1-1) to (1-4):

[0066] In some embodiments, B also includes lead. In this case, the perovskite layer comprises a tin-lead perovskite material. The tin-lead perovskite material allows the perovskite layer 102 to have a narrower bandgap, which is beneficial for the development of the perovskite solar cell 100. For example, applying the narrow-bandgap perovskite solar cell 100 to a tandem cell can improve the light utilization rate of the tandem cell, thereby improving the photoelectric conversion efficiency of the tandem cell.

[0067] In some implementations, ABX3 includes ASn x Pb 1-x X3, where 0.5≤x≤1, A includes inorganic monovalent cations, organic monovalent cations or organic-inorganic mixed cations; X includes inorganic monovalent anions, organic monovalent anions or organic-inorganic mixed anions.

[0068] Optionally, ASn x Pb 1-x In X3, x can be 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 1, or any value within the range of any two of the above values.

[0069] Optionally, A includes an inorganic monovalent cation, an organic monovalent cation, or a mixed organic-inorganic monovalent cation. For example, the organic monovalent cation includes (NR'1R'2R'3R'4). + (R'1R'2N=CR'3R'4) + (R'1R'2N-C(R'5)=NR'3R'4) + and (R'1R'2N-C(NR'5R'6)=NR'3R'4) + One or more of the following, wherein R'1, R'2, R'3, R'4, R'5, and R'6 are each independently selected from H, substituted or unsubstituted C1-C20 alkyl groups, or substituted or unsubstituted aryl groups. Optionally, the organic monovalent cation includes (H2N=CH-NH2). + (Formamidine cation, abbreviated as: FA) + CH3NH3 + (Methylamine cation, abbreviated as: MA) + The inorganic monovalent cations include one or more of the following: dimethylamine cation, ethylamine cation, propylamine cation, butylamine cation, pentamine cation, hexamine cation, and imidazole cation. For example, inorganic monovalent cations include: Li + Na + K + 、Rb + Cs + Cu + Ag + Au + or Hg + One or more of the following. A may optionally include MA. + FA + Cesium ion (abbreviated as Cs) + ) and rubidium ions (abbreviated as: Rb) + One or more of the following, further optionally MA + or FA + .

[0070] Optionally, in the ABX3 perovskite material, B may also include one or more of zinc, titanium, antimony, bismuth, nickel, iron, cobalt, silver, copper, gallium, germanium, magnesium, calcium, indium, aluminum, manganese, chromium, molybdenum and europium.

[0071] Optionally, in the ABX3 perovskite material, X includes an inorganic monovalent anion, an organic monovalent anion, or a mixed organic-inorganic monovalent anion. X may optionally include one or more of halogen anions and halide-like anions, such as F... - Cl - ,Br - I - SCN - CNO - OCN - OSCN - SH - CN - SeCN - Etc. Further optionally, X includes Br - or I - .

[0072] In some embodiments, the band gap of the perovskite layer 102 is 1.1 eV to 1.8 eV. Perovskite layer 102 with a band gap within this range exhibits high visible light absorption, which is beneficial for further improving the photoelectric conversion efficiency of the perovskite solar cell 100. Optionally, the band gap of the perovskite layer 102 can be 1.1 eV, 1.2 eV, 1.3 eV, 1.4 eV, 1.5 eV, 1.6 eV, 1.7 eV, 1.8 eV, or any value within the range of any two of the above values.

[0073] In some embodiments, the thickness of the perovskite layer 102 is 200 nm to 1500 nm. As an example, the thickness of the perovskite layer 102 can be 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, 1100 nm, 1200 nm, 1300 nm, 1400 nm, 1500 nm, or any value within the range of any two of the above values.

[0074] In some embodiments, along the direction perpendicular to the thickness of the perovskite layer, the tin-lead molar ratio at the surface of the perovskite layer is d1, and the tin-lead molar ratio at the cross-section of the perovskite layer is d2, where 0.5 ≤ d2 / d1 ≤ 1. The tin-lead molar ratio represents the molar ratio of tin to lead. Along the direction perpendicular to the thickness of the perovskite layer, the distance between the cross-section of the perovskite layer and the surface of the perovskite layer is less than 0.5 times the thickness of the perovskite layer. In this case, the tin-lead molar ratio at the cross-section of the perovskite layer 102 in its thickness direction is closer to the tin-lead molar ratio at its surface. This allows the perovskite layer 102 to have better crystallinity and fewer defects, thereby reducing carrier recombination and improving the photoelectric conversion efficiency of the perovskite solar cell 100. Optionally, d2 / d1 can be 0.5, 0.6, 0.7, 0.8, 0.9, 1, or any value within the range of any two of the above values.

[0075] It is understandable that the distance between the cross section of the perovskite layer and the surface of the perovskite layer represents the distance between the cross section of the perovskite layer and a certain surface of the perovskite layer along the thickness direction of the solar cell.

[0076] It is understandable that a distance of less than 0.5 times the thickness of the perovskite layer between the cross section and the surface of the perovskite layer indicates that, with half the thickness of the perovskite layer as a reference, the cross section and the surface of the perovskite layer are located on the same side of that reference.

[0077] It is understandable that, in the direction perpendicular to the thickness of the perovskite layer 102, the cross-section of the perovskite layer 102 can be understood as the cross-section of the perovskite layer 102. The tin-lead molar ratio of this cross-section can represent the tin-lead molar ratio inside the perovskite layer 102.

[0078] Please refer again to Figure 1, which provides an exemplary view of the surface and cross-section of the perovskite layer 102. In Figure 1, the Z-direction represents the thickness direction of the perovskite layer 102. 1021 represents the surface of the perovskite layer 102 along the thickness direction perpendicular to the thickness direction, and 1022 represents the cross-section of the perovskite layer 102 along the thickness direction perpendicular to the thickness direction. The tin-lead molar ratio d1 represents the molar ratio of tin to lead in surface 1021, and the tin-lead molar ratio d2 represents the molar ratio of tin to lead in cross-section 1022.

[0079] It is understood that, along the thickness direction of the perovskite layer 102, the surface of the perovskite layer 102 can refer to the surface of the perovskite layer 102 near the first electrode 101, or it can refer to the surface of the perovskite layer 102 near the second electrode 103.

[0080] It is also understood that, along the thickness direction of the perovskite layer 102, the cross section of the perovskite layer 102 can represent any cross section perpendicular to the thickness direction of the perovskite layer 102.

[0081] In this application, the tin-lead molar ratio d1 of the surface of the perovskite layer 102 can be obtained by XPS testing of the surface of the perovskite layer 102. The tin-lead molar ratio d2 of the cross-section of the perovskite layer 102 can be obtained by XPS testing of the surface of the perovskite layer 102 after thinning treatment. Optionally, the thinning treatment can be an etching treatment.

[0082] It is understood that XPS testing represents the results within the corresponding test depth. In this application, d1 and d2 obtained by XPS represent the d1 and d2 of the portion with a depth of 50 nm from the test surface. For example, d1 of the surface of the perovskite layer represents the d1 of the portion with a depth of 50 nm from that surface. d2 of the cross-section of the perovskite layer represents the d2 of the portion with a depth of 50 nm from that cross-section.

[0083] It is understood that in this application, the tin-lead molar ratio d1 on the perovskite surface and the tin-lead molar ratio d2 on the cross section of the perovskite layer 102 both represent the ratio of the tin-lead molar ratio on the corresponding surfaces.

[0084] In some implementations, d2 / d1 can be 0.5, 0.6, 0.7, 0.8, 0.9, 1, or any value within the range of any two of the above values.

[0085] In some embodiments, the distance between the cross-section of the perovskite layer 102 and its surface along the thickness direction of the perovskite layer 102 is 0.05 to 0.5 times the thickness of the perovskite layer 102. This thickness multiple can more accurately reflect the relative relationship between the tin-lead molar ratio on the surface and inside of the perovskite layer 102, and also facilitates obtaining and analyzing the cross-section of the perovskite layer 102.

[0086] Please refer again to Figure 1, which exemplarily illustrates the distance between the cross-section of the perovskite layer 102 and its surface, as well as the thickness of the perovskite layer 102. Specifically, along the thickness direction of the perovskite layer 102, the distance between the cross-section of the perovskite layer 102 and its surface is L1, and the thickness of the perovskite layer 102 is L2. The ratio L1 / L2 can represent the multiple of the distance between the cross-section of the perovskite layer 102 and its surface to the thickness of the perovskite layer 102.

[0087] Optionally, the distance between the cross section of the perovskite layer 102 and the surface of the perovskite layer 102 can be 0.05 times, 0.1 times, 0.2 times, 0.3 times, 0.4 times, 0.5 times the thickness of the perovskite layer 102, or any value within the range of any two of the above values.

[0088] In some embodiments, the distance between the cross section of the perovskite layer 102 and the surface of the perovskite layer 102 along the thickness direction of the perovskite layer 102 is 5 nm to 500 nm. Optionally, the distance between the cross section of the perovskite layer 102 and the surface of the perovskite layer 102 can be 5 nm, 10 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, or any value within the range of any two of the above values.

[0089] In some embodiments, d1 is 1 to 15. The atomic radius of tin atoms is smaller than that of lead atoms. When the tin-lead molar ratio is large, more tin atoms will replace lead atoms, which may cause distortion of the perovskite crystal structure, affecting the stability of the spectral absorption of the perovskite layer 102, and thus limiting the improvement of the photoelectric conversion efficiency of the perovskite solar cell 100. In these embodiments of this application, the introduction of phosphine oxide organic compounds can effectively reduce the tin-lead molar ratio on the surface of the perovskite layer 102, keeping the tin-lead molar ratio on the surface of the perovskite layer 102 at a low level, reducing the risk of perovskite crystal structure distortion, and promoting the improvement of the photoelectric conversion efficiency of the perovskite solar cell 100. It is understood that, in the direction perpendicular to the thickness of the perovskite layer 102, the tin-lead molar ratio d1 on the surface of the perovskite layer 102 can be 1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8, 3, 3.2, 3.5, 3.8, 4, 4.2, 4.5, 4.8, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, or any value within the range of any two of the above values. Optionally, d1 is 1 to 5.

[0090] In some embodiments, d2 is 0.5 to 15. In these embodiments of this application, the tin-lead molar ratio d2 of the cross-section of the perovskite layer 102 is small in the direction perpendicular to the thickness of the perovskite layer 102. This indicates that the tin-lead molar ratio inside the perovskite layer 102 is small, which can further reduce the risk of perovskite crystal distortion and maintain high stability of the absorption of the spectrum by the perovskite layer 102, thereby further improving the photoelectric conversion efficiency of the perovskite solar cell 100. Optionally, d2 can be 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, or any value within the range of any two of the above values. Optionally, d1 is 0.5 to 5. In some embodiments, the perovskite solar cell 100 further includes a hole transport layer 104 and / or an electron transport layer 105. Of the hole transport layer 104 and the electron transport layer 105, one is located between the first electrode 101 and the perovskite layer 102, and the other is located between the second electrode 103 and the perovskite layer 102.

[0091] In some embodiments, the electron transport layer 105 is located between the first electrode 101 and the perovskite layer 102, and the hole transport layer 104 is located between the second electrode 103 and the perovskite layer 102.

[0092] Optionally, the perovskite solar cell 100 includes a hole transport layer 104. In this case, the perovskite solar cell 100 includes a first electrode 101, a hole transport layer 104, a perovskite layer 102, and a second electrode 103 stacked sequentially; or the perovskite solar cell 100 includes a first electrode 101, a perovskite layer 102, a hole transport layer 104, and a second electrode 103 stacked sequentially.

[0093] Optionally, the perovskite solar cell 100 includes an electron transport layer 105. In this case, the perovskite solar cell 100 includes a first electrode 101, an electron transport layer 105, a perovskite layer 102, and a second electrode 103 stacked sequentially; or the perovskite solar cell 100 includes a first electrode 101, a perovskite layer 102, an electron transport layer 105, and a second electrode 103 stacked sequentially.

[0094] Optionally, the perovskite solar cell 100 includes a hole transport layer 104 and an electron transport layer 105. In this case, the perovskite solar cell 100 includes a first electrode 101, a hole transport layer 104, a perovskite layer 102, an electron transport layer 105, and a second electrode 103 stacked sequentially; or the perovskite solar cell 100 includes a first electrode 101, an electron transport layer 105, a perovskite layer 102, a hole transport layer 104, and a second electrode 103 stacked sequentially.

[0095] The electron transport material of the electron transport layer 105 in this application is a common electron transport layer material in the art, and this application does not limit its type. Optionally, the electron transport material of the electron transport layer 105 may include, but is not limited to, one or more of the following materials and their derivatives: fullerenes and their derivatives, imide compounds, metal oxides, metal sulfides, metal fluorides, cyano-containing polyphenylacetylene, boron-containing polymers, copper bath, red phenanthroline, aluminum hydroxyquinoline, oxadiazole compounds, and quinone compounds. Among them, fullerenes and their derivatives include one or more of fullerene C60, fullerene C70, PCBM ([6,6]-phenyl-C61-butyrate methyl ester), and [6,6]-phenyl-C71-butyrate methyl ester (PC71BM); imide compounds include one or more of perylene imide materials, naphthylimide materials, phthalimide, succinimide, N-bromosuccinimide, glutarimide, or maleimide; the metal element in the metal oxide may be... Including one or more of Mg, Ni, Cd, Zn, In, Pb, Mo, W, Sb, Bi, Cu, Hg, Ti, Ag, Mn, Fe, V, Sn, Zr, Sr, Ga, and Cr, such as one or more of tin oxide (SnO2), zinc oxide (ZnO), and titanium oxide; metal sulfides such as indium sulfide or zinc sulfide; and metal fluorides such as one or more of lithium fluoride (LiF), sodium fluoride, magnesium fluoride (MgF2), and calcium fluoride (CaF2).

[0096] In some embodiments, the thickness of the electron transport layer 105 is 5 nm to 100 nm. Within this range, the thickness of the electron transport layer 105 can provide good electron transport for the perovskite solar cell 100 while maintaining a relatively small thickness, thus promoting the thinner and lighter design of the perovskite solar cell. Optionally, the thickness of the electron transport layer 105 can be 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, or any value within the range of any two of the above values.

[0097] In some embodiments, the perovskite solar cell 100 further includes a hole-blocking layer, not shown in the figure. The hole-blocking layer is located between the electron transport layer 105 and the first electrode 101. The hole-blocking layer can block the transport of holes toward the first electrode 101, reducing the recombination of electrons and holes at non-ideal locations, and further improving the photoelectric conversion efficiency of the perovskite solar cell 100. Optionally, the hole-blocking layer includes, but is not limited to, the following materials: 2,9-dimethyl-4,7-biphenyl-1,10-o-phenanthroline (BCP), SnO2, ZnO, CeO.x And so on, where x is the number of oxygen atoms. Furthermore, the thickness of the hole-blocking layer can be selected from 0.5 nm to 20 nm. For example, the thickness of the hole-blocking layer can be 0.5 nm, 1 nm, 5 nm, 10 nm, 15 nm, 20 nm, or any value within the range of any two of the above values.

[0098] The hole transport material of the hole transport layer 104 in this application is a common hole transport layer material in the art, and this application does not limit its type. The hole transport material of the hole transport layer 104 may include, but is not limited to, one or more of the following materials and their derivatives: poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (abbreviated as: PTAA), 2,2',7,7'-tetratetra[N,N-di(4-methoxyphenyl)amino]-9,9'-spirodifluorene (abbreviated as: Spiro-OMeTAD), poly(3,4-ethylenedioxythiophene):polystyrene sulfonic acid (abbreviated as: PEDOT:PSS), poly(3-hexylthiophene) (abbreviated as: P3HT), and triphenylamine with a triphenylene core (abbreviated as: H101). Materials that can transport holes and block electrons include 3,4-ethylenedioxythiazole-methoxytriphenylamine (EDOT-OMeTPA), N-(4-aniline)carbazole-spirobisfluorene (CzPAF-SBF), polythiazole, nickel oxide, molybdenum oxide (MoO3), cuprous iodide (CuI), cuprous oxide (CuO), [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz), and [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz).

[0099] Optionally, the thickness of the hole transport layer 104 is 1 nm to 100 nm. Within this range, the thickness of the hole transport layer 104 can provide good hole transport for the perovskite solar cell 100 while maintaining a relatively small thickness, thus promoting the lightweight and thin design of the perovskite solar cell. Optionally, the thickness of the hole transport layer 104 can be 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, or any value within the range of any two of the above values.

[0100] In some embodiments, the perovskite solar cell 100 further includes an electron blocking layer, which is not shown in the figures. The electron blocking layer is located between the hole transport layer 104 and the corresponding electrode. The electron blocking layer can block the transport of electrons toward the corresponding electrode of the hole transport layer 104, reduce the recombination of electrons and holes at non-ideal locations, and further improve the photoelectric conversion efficiency of the perovskite solar cell 100.

[0101] In some embodiments, the perovskite solar cell 100 further includes a hole-blocking layer, which is not shown in the figures. The hole-blocking layer is located between the electron transport layer 105 and the corresponding electrode. The hole-blocking layer can block the transport of holes toward the corresponding electrode of the electron transport layer 105, reducing the recombination of electrons and holes at non-ideal locations, and further improving the photoelectric conversion efficiency of the perovskite solar cell 100. Exemplarily, the material of the hole-blocking layer can be tin oxide, copper bath (2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, BCP), etc.

[0102] In some embodiments, the first electrode 101 can be a metal electrode, a metal-nonmetal hybrid electrode, a transparent electrode, etc., and the second electrode 103 can be a metal electrode, a metal-nonmetal hybrid electrode, or a transparent electrode. At least one of the first electrode 101 and the second electrode 103 is a transparent electrode for light incident. In some embodiments, one of the first electrode 101 and the second electrode 103 is a transparent electrode, and the other is a metal electrode. By configuring the transparent electrode and the metal electrode, a conventional perovskite solar cell or an inverted perovskite solar cell can be obtained.

[0103] It is understandable that, for a standard perovskite solar cell, a standard perovskite solar cell includes a first electrode 101, an electron transport layer 105, a perovskite layer 102, a hole transport layer 104, and a second electrode 103 stacked sequentially. The first electrode 101 is a transparent electrode used for light incident, and the second electrode 103 can be a metal electrode, a metal-nonmetal hybrid electrode, a transparent electrode, etc. For an inverted perovskite solar cell, an inverted perovskite solar cell includes a second electrode 103, a hole transport layer 104, a perovskite layer 102, an electron transport layer 105, and a first electrode 101 stacked sequentially. The second electrode 103 is a transparent electrode used for light incident, and the first electrode 101 can be a metal electrode, a metal-nonmetal hybrid electrode, a transparent electrode, etc.

[0104] Optionally, the material of the transparent electrode includes transparent conductive oxides, including but not limited to one or more of fluorine-doped tin oxide (FTO), indium tin oxide (ITO), aluminum-doped zinc oxide (AZO), boron-doped zinc oxide (BZO), indium zinc oxide (IZO), and indium tungsten oxide (IWO). Optionally, the thickness of the transparent electrode is 100 nm to 1000 nm. More preferably, the thickness of the transparent electrode is 300 nm to 800 nm.

[0105] Optionally, the material of the metal electrode includes one or more of Au, Ag, Cu, Al, Ni, Cr, Bi, Pt, Mg, Mo, W, and their alloys. In the metal-nonmetal hybrid electrode, the metal material includes one or more of Au, Ag, Cu, Al, Ni, Cr, Bi, Pt, Mg, Mo, W, and their alloys, and the nonmetal material includes C. Optionally, the thickness of the metal electrode or the metal-nonmetal hybrid electrode is 20 nm to 200 nm; alternatively, the thickness of the metal electrode or the metal-nonmetal hybrid electrode is 60 nm to 100 nm; further alternatively, the thickness of the metal electrode or the metal-nonmetal hybrid electrode is 70 nm to 90 nm.

[0106] Understandably, the perovskite solar cell 100 also includes a substrate for supporting the perovskite solar cell 100. The substrate includes a glass substrate and a flexible substrate. The material of the flexible substrate may be, but is not limited to, transparent organic polymer materials. Further, the material of the flexible substrate may be a mixture of one or more of the following materials in different proportions: including but not limited to polyvinyl alcohol (PVA), polyester (PET), polyimide (PI), polyethylene naphthalate (PEN), polydimethylsiloxane (PDMS), etc.

[0107] Understandably, other functional layers, such as buffer layers, can be introduced into the perovskite solar cell 100 as needed.

[0108] In some embodiments, the perovskite solar cell 100 may be provided with a buffer layer of suitable energy level, which can play one or more of the following roles: reducing the energy level barrier, promoting energy level matching, improving carrier extraction efficiency, passivating interface defect states, protecting the light absorption layer, suppressing the oxidative decomposition of the cell by water molecules and oxygen, improving photoelectric conversion efficiency, and improving the stability of the perovskite solar cell 100. Depending on the location of the buffer layer, the type of buffer layer may include four types: a buffer layer between the hole transport layer 104 and the anode, a buffer layer between the electron transport layer 105 and the cathode, a buffer layer between the hole transport layer 104 and the perovskite layer 102, and a buffer layer between the electron transport layer 105 and the perovskite layer 102. Materials that can be used for the buffer layer in the perovskite solar cell 100 may include, but are not limited to, Cu2O, NiO, AZO, TiO2, etc.

[0109] Another embodiment of this application provides a method for preparing a perovskite solar cell 100. The method includes the following steps: mixing a tin source, a monovalent cation source, a monovalent anion source, and a phosphine oxide organic compound as shown in formula (1) in a solvent to prepare a perovskite precursor solution. Applying the perovskite precursor solution to the surface of a first electrode 101 and annealing it to prepare a perovskite layer 102. Preparing a second electrode 103 on the surface of the perovskite layer 102 away from the first electrode 101.

[0110] In formula (1), R1, R2 and R3 each independently include H, C1-C6 alkyl or C1-C6 alkoxy, and R1, R2 and R3 are not all hydrogen at the same time.

[0111] Optionally, one of R1, R2, and R3 is H, or R1, R2, and R3 each independently include a C1-C6 alkyl group, a C1-C6 alkoxy group, an amino group, a methylamino group, a dimethylamino group, a mercapto group, a hydroxyl group, or a halogen. Optionally, none of R1, R2, and R3 are H.

[0112] Optionally, the tin source includes tin-containing halides. More optionally, the tin source includes tin iodide (SnI2).

[0113] Optionally, the monovalent cation source may include AX as described above, and the selection of the monovalent cation is as defined above. For example, the monovalent cation source may include one or more of CsI, FAI, MAI, and MACl.

[0114] Optionally, the solvent for preparing the perovskite precursor solution may include one or more of N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and chlorobenzene.

[0115] In some embodiments, the feedstock for the perovskite precursor solution also includes a lead source. Optionally, the lead source includes a lead halide. For example, the lead source includes lead iodide (PbI2).

[0116] In some embodiments, the concentration of the phosphine oxide organic compound in the perovskite precursor solution is from 1 mg / mL to 400 mg / mL. For example, the concentration of the phosphine oxide organic compound in the perovskite precursor solution can be 1 mg / mL, 1.5 mg / mL, 2 mg / mL, 2.5 mg / mL, 5 mg / mL, 10 mg / mL, 20 mg / mL, 30 mg / mL, 40 mg / mL, 50 mg / mL, 60 mg / mL, 80 mg / mL, 100 mg / mL, 150 mg / mL, 200 mg / mL, 250 mg / mL, 300 mg / mL, 350 mg / mL, 400 mg / mL, or any value within the range of any two of the above values.

[0117] Understandably, when the phosphine oxide organic compound is a liquid, considering the volatility of liquids, the concentration of the phosphine oxide organic compound in the perovskite precursor solution can be relatively high. When the phosphine oxide organic compound is a solid, the concentration of the phosphine oxide organic compound in the perovskite precursor solution can be relatively low.

[0118] For example, when the phosphine oxide organic compound is in liquid form, the concentration of the phosphine oxide organic compound in the perovskite precursor solution can be from 50 mg / mL to 400 mg / mL. For example, when the phosphine oxide organic compound is compound (1-1), the concentration of the phosphine oxide organic compound in the perovskite precursor solution can be from 50 mg / mL to 400 mg / mL.

[0119] For example, when the phosphine oxide organic compound is in solid form, the concentration of the phosphine oxide organic compound in the perovskite precursor solution can be from 1 mg / mL to 3 mg / mL. For example, when the phosphine oxide organic compound is one or more of compounds (1-2), (1-3), and (1-4), the concentration of the phosphine oxide organic compound in the perovskite precursor solution can be from 1 mg / mL to 3 mg / mL.

[0120] In some embodiments, applying the perovskite precursor solution to the surface of the first electrode 101 includes spin-coating the perovskite precursor solution onto the surface of the first electrode 101. Optionally, the spin-coating speed is 2000 rpm to 4000 rpm. For example, the spin-coating speed can be 2000 rpm, 2200 rpm, 2500 rpm, 2800 rpm, 3000 rpm, 3200 rpm, 3500 rpm, 3800 rpm, 4000 rpm, or any value within the range of any two of the above values.

[0121] In some embodiments, the annealing temperature is 90°C to 110°C. For example, the annealing temperature can be 90°C, 92°C, 95°C, 98°C, 100°C, 102°C, 105°C, 108°C, 110°C, or any value within the range of any two of the above values.

[0122] In some embodiments, the annealing time is 8 min to 15 min. Optionally, the annealing time can be 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, or any value within the range of any two of the above values.

[0123] Another embodiment of this application provides a tandem solar cell. The tandem solar cell includes the perovskite solar cell 100 described above or the perovskite solar cell 100 prepared by the above method. The tandem solar cell can be formed by stacking two or more cells with different band gaps, and is used to absorb light of different wavelengths, thereby broadening the absorption spectrum of the tandem solar cell and improving its photoelectric conversion efficiency.

[0124] In some embodiments, the tandem solar cell further includes a first light-absorbing layer disposed between the first electrode and the second electrode, the first light-absorbing layer having a different band gap than the perovskite layer. Thus, by providing a perovskite layer and a first light-absorbing layer with different band gaps, the tandem solar cell can effectively absorb light of different wavelengths, broadening the spectral range of absorbed light and improving the photoelectric conversion efficiency of the tandem solar cell.

[0125] In some embodiments, the first light-absorbing layer is located on the side of the perovskite layer facing the first electrode. In other embodiments, the first light-absorbing layer is located on the side of the perovskite layer facing the second electrode. In some embodiments, the first light-absorbing layer comprises a layer of the following compounds: a first perovskite material, crystalline silicon, copper zinc tin sulfide, copper zinc tin selenide, copper zinc tin selenide sulfide, copper indium gallium selenide, copper indium gallium diselenide, or copper indium selenide. These materials can absorb light of different wavelengths with the light-absorbing layer, thereby broadening the spectral range of light absorption in multi-junction solar cells and improving the photoelectric conversion efficiency of multi-junction solar cells. In this application, the definition of the first perovskite material is the same as the above-mentioned perovskite material types, but the specific composition differs to obtain a first light-absorbing layer with a different bandgap, used to absorb light of different wavelengths with the perovskite light-absorbing layer, broadening the absorption spectral range of multi-junction solar cells and improving the photoelectric conversion efficiency of multi-junction solar cells.

[0126] In some embodiments, the band gap of the first light-absorbing layer is larger than that of the perovskite layer, such as a band gap greater than 1.80 eV. In other embodiments, the band gap of the perovskite layer is 1.2 eV to 1.6 eV, and the band gap of the first light-absorbing layer is 1.65 eV to 2.2 eV. The band gap configuration of the first light-absorbing layer and the perovskite layer effectively absorbs both short-wavelength and long-wavelength light, improving the photoelectric conversion efficiency of the tandem solar cell.

[0127] In some embodiments, the tandem solar cell includes a first electrode, an optional hole transport layer, a perovskite layer, an optional electron transport layer, a recombination layer, an optional first hole transport layer, a first light absorption layer, an optional first electron transport layer, and a second electrode, all stacked together. Alternatively, the tandem solar cell includes a first electrode, an optional electron transport layer, a perovskite layer, an optional hole transport layer, a recombination layer, an optional first electron transport layer, a first light absorption layer, an optional first hole transport layer, and a second electrode, all stacked together. Thus, the presence of the hole transport layer and / or the electron transport layer facilitates the extraction and transport of electrons or holes generated by the perovskite layer or the first light absorption layer, enhancing the extraction and transport effect of electrons and holes and improving the performance of the tandem solar cell.

[0128] In this application, the tandem solar cell may simultaneously include a first hole transport layer, a first electron transport layer, a hole transport layer, and an electron transport layer, or it may include only one or more of the first hole transport layer, the first electron transport layer, the hole transport layer, and the electron transport layer; no limitation is made here. The definitions and material selections of the corresponding hole transport layer or electron transport layer are as described above and will not be repeated here.

[0129] In the case where a first hole transport layer, a first electron transport layer, an electron transport layer, and a hole transport layer are simultaneously present, taking a stacked battery structure including a first electrode, a hole transport layer, a perovskite layer, an electron transport layer, a recombination layer, a first hole transport layer, a first light absorption layer, a first electron transport layer, and a second electrode as an example, the first electrode, the hole transport layer, the perovskite layer, and the electron transport layer constitute a first battery unit, and the first hole transport layer, the first light absorption layer, the first electron transport layer, and the second electrode constitute a second battery unit. The recombination layer is used to recombine and annihilate electrons generated from the perovskite layer and holes generated from the first light absorption layer that are transported toward the recombination layer, so as to achieve low-ohmic tunnel recombination between the first battery unit containing the perovskite layer and the second battery unit containing the first light absorption layer.

[0130] In the case where a first hole transport layer, a first electron transport layer, an electron transport layer, and a hole transport layer are simultaneously present, taking a stacked battery structure including a first electrode, an electron transport layer, a perovskite layer, a hole transport layer, a recombination layer, a first electron transport layer, a first light absorption layer, a first hole transport layer, and a second electrode as an example, the first electrode, the electron transport layer, the perovskite layer, and the hole transport layer constitute a first battery unit, and the first electron transport layer, the first light absorption layer, the first hole transport layer, and the second electrode constitute a second battery unit. The recombination layer is used to recombine and annihilate holes generated from the perovskite layer and electrons generated from the first light absorption layer that are transported toward the recombination layer, so as to achieve low-ohmic tunnel recombination between the first battery unit containing the perovskite layer and the second battery unit containing the first light absorption layer.

[0131] For example, the composite layer comprises one or more of metallic materials, transparent conductive oxides, and carbon materials. Further, the transparent conductive oxide layer comprises, but is not limited to, one or more of FTO (fluorine-doped tin oxide), ITO (indium tin oxide), AZO (aluminum-doped zinc oxide), BZO (boron-doped zinc oxide), IZO (indium zinc oxide), IGZO (indium gallium zinc oxide), and ATO (antimony tin oxide). Further, the metallic materials include, but are not limited to, one or more of gold, copper, silver, platinum, aluminum, and iron. Further, the carbon materials include one or more of graphite, graphene, and carbon nanotubes.

[0132] In some embodiments, the thickness of the composite layer is 0.1 nm to 200 nm. For example, it can be 0.1 nm, 0.8 nm, 1 nm, 2 nm, 10 nm, 30 nm, 50 nm, 90 nm, 100 nm, 130 nm, 150 nm, 160 nm, 200 nm, or within the range of any two of the above point values ​​as end values.

[0133] In some embodiments, the tandem solar cell includes a first electrode, an optional hole transport layer, a perovskite layer, an optional electron transport layer, a third electrode, an insulating layer, a fourth electrode, an optional first hole transport layer, a first light absorption layer, an optional first electron transport layer, and a second electrode, all stacked together. Alternatively, the tandem solar cell includes a first electrode, an optional hole transport layer, a perovskite layer, an optional electron transport layer, a third electrode, an insulating layer, a fourth electrode, an optional first electron transport layer, a first light absorption layer, an optional first hole transport layer, and a second electrode, all stacked together. Thus, the presence of the hole transport layer and / or the electron transport layer facilitates the extraction and transport of electrons or holes generated by the perovskite layer or the first light absorption layer, enhancing the extraction and transport effect of electrons and holes and improving the performance of the tandem solar cell. Thus, the first electrode, perovskite layer, and third electrode form the first sub-cell (if there is a hole transport layer or electron transport layer, the corresponding transport layer is also included here), and the fourth electrode, first light-absorbing layer, and second electrode form the second sub-cell (if there is a first hole transport layer or first electron transport layer, the corresponding transport layer is also included here). The first and second sub-cells are isolated in the circuit by an insulating layer. Each cell has two electrodes, for a total of four electrodes. The circuits of the two sub-cells are independent of each other, forming a four-terminal multi-junction solar cell. This allows for adjustment of the current in the tandem solar cell.

[0134] Furthermore, since the third and fourth electrodes are located in the middle of the stacked cell, in order to further increase the light energy utilization rate of the stacked cell and allow the remaining light after absorption by one sub-cell to enter the next sub-cell, the third and fourth electrodes can be set as light-transmitting electrodes. In some embodiments, the material of the insulating layer includes, but is not limited to, glass or insulating adhesive. Further, the glass is transparent glass; further, the insulating adhesive is a transparent adhesive.

[0135] It is understood that other functional layers, such as buffer layers and hole-blocking layers, can be introduced into the tandem solar cell as needed, and this is not limited here. Another embodiment of this application provides a photovoltaic system. This photovoltaic system includes the perovskite solar cell 100 described above or the perovskite solar cell 100 prepared by the above method.

[0136] Another embodiment of this application provides a power generation device. The power generation device includes the perovskite solar cell 100 described above or the perovskite solar cell 100 prepared by the above method.

[0137] Another embodiment of this application provides an electrical device. This electrical device includes the perovskite solar cell 100 described above or the perovskite solar cell 100 prepared by the above method. The type of power generation device may include, but is not limited to, integrated power generation. The location of the power generation device may include, but is not limited to, the roof of a vehicle, the back panel, etc.

[0138] Furthermore, the aforementioned electrical devices may include mobile devices, such as mobile phones and laptops, electric vehicles, electric trains, ships and satellites, power generation systems, etc., but are not limited to these.

[0139] To make the technical problems, technical solutions, and beneficial effects solved by this application clearer, the application will be further described in detail below with reference to embodiments and accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit this application or its applications. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0140] Where specific techniques or conditions are not specified in the examples, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0141] Example 1

[0142] The fabrication method of the perovskite solar cell in this embodiment includes:

[0143] S101: Preparation of perovskite precursor solution: In a glove box under nitrogen atmosphere, 0.085 mmol CsI, 1.615 mmol FAI, 0.85 mmol PbI2 and 0.85 mmol SnI2, as well as compound (1-1) (abbreviated as DMPO), were dissolved in 1 mL of DMF to prepare a CsI solution with a molar concentration of 1.7 mol / L. 0.05 FA 0.95 Pb 0.5 Sn 0.5 The I3 perovskite precursor solution was heated and stirred at 60°C for 2 hours, then filtered and set aside for later use.

[0144] S102: A PEDOT:PSS aqueous solution was spin-coated onto the FTO surface at 7000 rpm and heated at 140 °C for 20 min on a hot stage to obtain a hole transport layer with a thickness of 100 nm.

[0145] S103: A perovskite precursor solution was spin-coated onto the surface of the hole transport layer at 3000 rpm, followed by annealing at 100 °C for 10 min and cooling to room temperature to obtain a perovskite layer with a thickness of 1000 nm.

[0146] S104: C60 with a thickness of 30 nm, BCP with a thickness of 7 nm, and Cu with a thickness of 60 nm are sequentially deposited on the surface of the perovskite layer at a deposition rate of 0.1 A / s.

[0147] Examples 2-8

[0148] Compared with Example 1, the preparation methods of Examples 2-8 are largely the same, except that the types and / or amounts of the phosphine oxide organic compounds added are different, as shown in Table 1. It is understood that different amounts of phosphine oxide organic compounds result in different a / b ratios in the perovskite layer, where a represents the total molar amount of phosphine oxide organic compounds in the perovskite layer, and b represents the total molar amount of B in the ABX3 perovskite material in the perovskite layer.

[0149] Comparative Example 1

[0150] The preparation method of Comparative Example 1 is roughly the same as that of Example 1, except that no phosphine oxide organic compound is added.

[0151] Comparative Example 2

[0152] The difference between Comparative Example 2 and Example 1 is that compound (1-1) was replaced with the same concentration of dimethyl sulfoxide (DMSO).

[0153] Test case

[0154] (1) The tin-lead molar ratio d1 on the surface of the perovskite layer of the perovskite solar cells in Examples 1, 6, 7 and Comparative Example 2 was tested using XPS. Then, a certain depth was etched, and the tin-lead molar ratio d2 on the corresponding surface was measured again, and d2 / d1 was calculated. The results are shown in Table 1.

[0155] Test method:

[0156] S01: Clean the surface: Use ultraviolet ozone or solvent to clean the perovskite layer to make the surface of the perovskite sample free of contamination, and then dry it.

[0157] S02: XPS Instrument Preparation

[0158] Calibration: The XPS instrument was calibrated using a standard sample (metallic silver).

[0159] Vacuum: Ensure the analysis chamber is in a high vacuum state to reduce background signal interference.

[0160] S03: Surface Analysis

[0161] Initial scan: A full-spectrum scan of the perovskite sample surface is performed to obtain overall information on surface elements.

[0162] Fixed-point analysis: Ten points were selected for fixed-point analysis, focusing on the Sn and Pb signals. The test result is the average of the results from the ten points.

[0163] S04: In-depth analysis

[0164] Angle variation: By changing the incident angle of X-rays (angle-resolved XPS), information at different depths can be acquired. Smaller incident angles are beneficial for detecting more surface information, while larger incident angles can detect deeper components.

[0165] Sputtering etching: The sample is etched layer by layer using an ion gun, and XPS scanning is performed after each layer. The etching rate and etching time need to be precisely controlled according to the properties of the sample and the required depth.

[0166] S05: Data Acquisition

[0167] Elemental spectra: XPS spectra of Sn and Pb were acquired for each depth layer.

[0168] Peak fitting: The spectral peaks of Sn and Pb are fitted to determine the binding energy and peak area of ​​each element.

[0169] S06: Molar ratio calculation

[0170] Peak area ratio: Based on the fitted peak areas, the atomic ratio of Sn and Pb at each depth is calculated. Considering the difference in atomic mass between Sn and Pb, the atomic ratio is further converted into a molar ratio.

[0171] (2) The appearance of the perovskite precursor solutions in Example 1 and Comparative Example 2 before and after exposure to air for 1 hour was compared, and the results are shown in Figure 2. In Figure 2, (a) shows the appearance of the perovskite precursor solutions before exposure to air, and (b) shows the appearance of the perovskite precursor solutions after exposure to air for 1 hour. In Figure 2, the transparent bottle labeled 1 contains the perovskite precursor solution from Comparative Example 2, and the transparent bottle labeled 2 contains the perovskite precursor solution from Example 1. As can be seen from Figure 2, after exposure to air, the perovskite precursor solution in Comparative Example 2 turned red, while the perovskite precursor solution in Example 1 hardly changed color. This indicates that the perovskite precursor solution in Example 1 has better antioxidant properties than that in Comparative Example 2, and can extend the experimental window.

[0172] (3) The perovskite precursor solutions from Examples 1-8 and Comparative Examples 1-2 were exposed to air, and the time required for each perovskite precursor solution to completely change color was tested. The results are shown in Table 2.

[0173] (4) The photoelectric conversion efficiency of the perovskite solar cells in Examples 1-8 and Comparative Examples 1-2 was tested. The test method was as follows:

[0174] Using Keithley 2400SMU, AM1.5G solar irradiation at 100mW / cm 2 Under the light source, the battery performance was tested, and the photoelectric conversion efficiency was calculated as follows: PCE=Pout / Pin=Voc×Jsc×(Vmpp×Jmpp) / (Voc×Jsc) / Pin=Voc×Jsc×FF / Pin

[0175] Where Pout, / Pin, Vmpp, Jmpp, Voc, and Jsc represent the battery's operating output power, incident light power, battery's maximum power point voltage, battery's maximum power point current, open-circuit voltage, and short-circuit current, respectively. The photoelectric conversion efficiency test results are shown in Table 2.

[0176] (5) The electrostatic potential minimum values ​​of compound (1-1) in Example 1 and DMSO in Comparative Example 2 were calculated using Gaussian 16 software, basis set, and functional combination M062X / def2tzvp. The results showed that the electrostatic potential minimum value of compound (1-1) was -57.8 kcal / mol, and the electrostatic potential minimum value of DMSO was -52.7 kcal / mol, indicating that compound (1-1) can react with Sn. 2+ It forms a strong coordination.

[0177] (6) Calculate Sn 2+ +DMSO and Sn 2+ The density of states plot of compound (1-1) is shown in Figure 3. In Figure 3, (a) corresponds to DMSO, and (b) corresponds to compound (1-1). As can be seen from Figure 3, Sn... 2+ + The highest occupied state energy level of the compound (1-1) complex is lower than that of Sn. 2+ The highest occupied state energy level of the +DMSO complex, Sn 2+ The (1-1) complex of compound + is less likely to lose electrons, which is beneficial for inhibiting Sn. 2+ Oxidation.

[0178] Table 1

[0179] In Table 1, the multiples represent the ratio of the distance between the cross-section of the perovskite layer and the surface of the perovskite layer to the thickness of the perovskite layer. d1 is the tin-lead molar ratio at the surface of the perovskite layer, and d2 is the tin-lead molar ratio at the cross-section of the perovskite layer. As can be seen from Table 1, the tin-lead molar ratio at the surface of the perovskite layer in Examples 1, 6, and 7 is less than that in Comparative Example 2. This reduces the risk of perovskite crystal structure distortion and promotes the improvement of photoelectric conversion efficiency of perovskite solar cells. Simultaneously, the cross-sectional area d2 / d1 of the perovskite layer in Examples 1, 6, and 7 is greater than that in Comparative Example 2 and closer to 1, indicating that the perovskite layer has better crystallinity and uniformity. Combined with Table 2, it can be seen that the perovskite solar cells in Examples 1, 6, and 7 have higher photoelectric conversion efficiency.

[0180] Table 2

[0181] As shown in Table 2, the perovskite precursor solution exhibits higher oxidation resistance when it contains an appropriate proportion of phosphine oxide organic compounds. Furthermore, perovskite solar cells demonstrate higher photoelectric conversion efficiency when the perovskite layer includes an appropriate proportion of phosphine oxide organic compounds.

[0182] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0183] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A perovskite solar cell, comprising a first electrode, a perovskite layer, and a second electrode, wherein the perovskite layer is disposed between the first electrode and the second electrode; the perovskite layer comprises ABX3 perovskite material and a phosphine oxide organic compound of formula (1), wherein, A includes monovalent cations, B includes tin, and X includes monovalent anions. In formula (1), R1, R2 and R3 each independently include H, C1-C6 alkyl, C1-C6 alkoxy, amino, methylamino, dimethylamino, mercapto, hydroxyl or halogen, and R1, R2 and R3 are not all hydrogen at the same time.

2. The perovskite solar cell according to claim 1, wherein, In the perovskite layer, the total molar amount of the phosphine oxide organic compound is a, and the total molar amount of B is b, where 0.1% ≤ a / b ≤ 5%.

3. The perovskite solar cell according to any one of claims 1 to 2, wherein, The perovskite layer satisfies one or two of the following conditions: (1)Sn 2+ The percentage of the total molar amount of tin is greater than or equal to 80%; (2)Sn 4+ The percentage of the total molar amount of tin is less than or equal to 20%.

4. The perovskite solar cell according to claim 3, wherein, The perovskite layer satisfies one or two of the following conditions: (1)Sn 2+ The percentage of the total molar amount of tin is greater than or equal to 90%; (2)Sn 4+ The percentage of the total molar amount of tin is less than or equal to 10%.

5. The perovskite solar cell according to any one of claims 1 to 4, wherein, One of R1, R2, and R3 is H, or R1, R2, and R3 each independently include C1-C6 alkyl, C1-C6 alkoxy, amino, methylamino, dimethylamino, mercapto, hydroxyl, or halogen.

6. The perovskite solar cell according to any one of claims 1 to 5, wherein, R1, R2, and R3 each independently include either methyl or methoxy groups.

7. The perovskite solar cell according to any one of claims 1 to 6, wherein, The phosphine oxide organic compound includes one or more of the following compounds (1-1) to (1-4):

8. The perovskite solar cell according to any one of claims 1 to 7, wherein, The band gap of the perovskite layer is 1.1 eV to 1.8 eV.

9. The perovskite solar cell according to any one of claims 1 to 8, wherein, The thickness of the perovskite layer is 200 nm to 1500 nm.

10. The perovskite solar cell according to any one of claims 1 to 9, wherein, ABX3 includes ASn x Pb 1- x X3, where 0.5≤x≤1, A includes inorganic monovalent cations, organic monovalent cations or organic-inorganic mixed cations; X includes inorganic monovalent anions, organic monovalent anions or organic-inorganic mixed anions.

11. The perovskite solar cell according to any one of claims 1 to 10, wherein, B also includes lead, wherein the tin-lead molar ratio at the surface of the perovskite layer is d1 along the direction perpendicular to the thickness of the perovskite layer, and the tin-lead molar ratio at the cross-section of the perovskite layer is d2, 0.5≤d2 / d1≤1, and the tin-lead molar ratio represents the molar ratio of tin and lead; and the distance between the cross-section of the perovskite layer and the surface of the perovskite layer along the direction perpendicular to the thickness of the perovskite layer is less than 0.5 times the thickness of the perovskite layer.

12. The perovskite solar cell according to claim 11, wherein, The tin-lead molar ratio satisfies one or more of the following characteristics: (1) d1 is 1 to 15; it can be 1 to 5. (2) d2 is 0.5 to 15; it can be 0.5 to 5.

13. The perovskite solar cell according to any one of claims 1 to 12, wherein, The perovskite solar cell further includes a hole transport layer and / or an electron transport layer; one of the hole transport layer and the electron transport layer is located between the first electrode and the perovskite layer, and the other is located between the second electrode and the perovskite layer.

14. A method for fabricating a perovskite solar cell, comprising the following steps: A perovskite precursor solution was prepared by mixing a tin source, a monovalent cation source, a monovalent anion source and the phosphine oxide organic compound shown in formula (1) in a solvent. The perovskite precursor solution is applied to the surface of the first electrode and annealed to prepare a perovskite layer. A second electrode is fabricated on the surface of the perovskite layer away from the first electrode; In formula (1), R1, R2 and R3 each independently include H, C1-C6 alkyl, C1-C6 alkoxy, amino, methylamino, dimethylamino, mercapto, hydroxyl or halogen, and R1, R2 and R3 are not all hydrogen at the same time.

15. The preparation method according to claim 14, wherein, In the perovskite precursor solution, the concentration of the phosphine oxide organic compound is 1 mg / mL to 400 mg / mL.

16. The preparation method according to any one of claims 14-15, wherein, The annealing process satisfies one or more of the following characteristics: (1) The annealing temperature is 90℃~110℃; (2) The annealing time is 8 min to 15 min.

17. A tandem solar cell, comprising a perovskite solar cell according to any one of claims 1 to 13 or a perovskite solar cell prepared by the preparation method according to any one of claims 14 to 16.

18. A photovoltaic system comprising a perovskite solar cell according to any one of claims 1 to 13 or a perovskite solar cell prepared by the preparation method according to any one of claims 14 to 16.

19. A power generation device comprising a perovskite solar cell according to any one of claims 1 to 13 or a perovskite solar cell prepared by the preparation method according to any one of claims 14 to 16.

20. An electrical device comprising a perovskite solar cell according to any one of claims 1 to 13 or a perovskite solar cell prepared by the preparation method according to any one of claims 14 to 16.