Recyclable paper-based packaging laminate, in particular lid laminate for push-through blister packages

A paper layer with a minimum wet strength of 50 kPa and a chemically soluble polymer layer enable effective recycling by maintaining structural integrity and facilitating separation in paper-based packaging laminates.

WO2026233923A1PCT designated stage Publication Date: 2026-11-12HUHTAMAKI FLEXIBLE PACKAGING GERMANY GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/062792
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-05-04
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Paper-based packaging laminates face issues during recycling due to the paper layer disintegrating into fiber components in liquid baths, contaminating recycling processes.

Method used

Incorporating a paper layer with a wet strength of at least 50 kPa and a chemically soluble polymer layer that can be separated using an alkaline solution, allowing the paper layer to maintain its structure and be easily removed from the laminate during recycling.

Benefits of technology

The paper layer retains integrity during recycling, preventing contamination and facilitating efficient separation from the laminate, enhancing recyclability and maintaining the structural integrity of the paper layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026062792_12112026_PF_FP_ABST
    Figure EP2026062792_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A packaging laminate (10) comprises a paper layer (12) and a sealable polymer layer (16), wherein the sealable polymer layer (16) is designed to produce a thermal sealing bond with a polymer surface (34b). According to the invention, it is provided that the paper material (18) of the paper layer (12) has a wet strength according to DIN ISO 3689 of more than 50 kPa.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 1 -

[0002] Recycling-friendly paper-based packaging laminate, especially lid laminate for push-through packaging

[0003] Description

[0004] The present invention relates to a packaging laminate. The packaging laminate comprises a paper layer and a sealable polymer layer, wherein the sealable polymer layer is configured to form a thermal seal with a polymer surface of a connecting body separate from the packaging laminate.

[0005] Such a packaging laminate is known from US 8329309 B2.

[0006] Like the packaging laminate of US 8329309 B2, the packaging laminate of the present invention is also preferably intended for use as a push-through lid laminate for forming a blister pack.

[0007] US patent 6010784 A discloses a packaging laminate for push-through blister packs, which also includes a paper or cardboard layer. This known packaging laminate has a sealable polymer layer made of a hot melt based on ethylene-vinyl acetate (EVA) filled with calcium carbonate particles. The calcium carbonate particles are intended to prevent the sealable polymer layer from clogging. The EVA-based sealant layer is said to provide a particularly good seal when combined with a layer of polytrichlorofluoroethylene.

[0008] Paper-based packaging laminates have recently become preferred for environmental reasons, as paper as a material is generally environmentally friendly and a paper layer significantly reduces the proportion of hydrocarbon-based polymers in the packaging laminate.

[0009] A disadvantage of paper layers in a packaging laminate is their behavior during recycling. In liquid baths, such as those used to clean used packaging laminates, the paper layer is damaged by the liquid in the 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 2 -

[0010] The material is usually broken down into its fiber components, so that the individual fiber components can contaminate process fluids and the desired process step result in the recycling process steps.

[0011] It is therefore an object of the present invention to improve the recyclability of packaging laminates, in particular those for use as lid laminates of blister packaging.

[0012] The present invention solves this problem with regard to a packaging laminate mentioned above by using a paper layer in the packaging laminate made of a paper material that has a wet strength according to DIN ISO 3689 of more than 50 kPa. For the purposes of this application, paper material is defined as any material that meets the paper definition according to DIN 6730.

[0013] By using paper material with the specified minimum wet strength, the paper layer can retain its structure as a paper layer for a period exceeding the usual immersion time of used packaging laminate in liquid baths during standard recycling processes, despite the liquid attack. It therefore does not disintegrate into its fiber components during the typical immersion times of approximately 20 minutes in liquid containers used in recycling processes and can be physically separated from the rest of the packaging laminate as a fiber layer component and removed from the recycling process.

[0014] With increasing wet strength, the paper layer can withstand longer immersion times in a liquid bath or prolonged exposure to liquid without loss of integrity. Therefore, the paper material preferably has a wet strength according to DIN 3689 of more than 55 kPa.

[0015] The wet strength according to DIN 3689 is often also referred to in the literature as 'wet burst strength'. 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 3 -

[0016] Preferably, the paper material of the paper layer has a wet tensile strength in the longitudinal direction of at least 9 N per 15 mm and / or a wet tensile strength in the transverse direction of at least 5 N per 15 mm to provide the desired stability against liquid attack. During papermaking, the fibers are aligned by shaking and rolling. This results in the orientation of the paper fibers across the surface of the paper layer. The longitudinal direction, or grain direction, is the direction in which the paper fibers are oriented. The transverse direction is a direction orthogonal to the longitudinal or grain direction. In the case of roll paper, the longitudinal or grain direction is usually an unwinding direction, or machine direction, orthogonal to the paper roll axis. The transverse direction is then typically a direction on the surface of the paper parallel to the paper roll axis.

[0017] The wet breaking strength is determined as follows:

[0018] - A test strip of the paper material, which has been stored for at least 24 hours at 20 °C and a relative humidity of between 40% and 60%, is prepared with a width of 15 mm.

[0019] - the test strip is completely immersed in deionized water at 20 °C for 5 minutes,

[0020] - Immediately after being removed from the bath of deionized water, the now wet test strip is clamped between two gripping clamps of a tensile testing machine with a clamping distance of 40 mm, - after clamping, the gripping clamps are moved apart exclusively along a spacing direction orthogonal to the width direction of the test strip while measuring the tensile force acting on the clamped wet test strip,

[0021] - The tensile force measured immediately before the test strip tears, divided by the width of the test strip of 15 mm, is the wet tensile strength of the paper material.

[0022] Since wet tensile strength depends solely on the integrity of the wet paper, the lower value is decisive for wet tensile strength; therefore, using the test method described above, this is 5 N per 15 mm. 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 4 -

[0023] Alternatively, the wet tensile strength can be determined according to DIN ISO 3781 (2012-07) with an immersion time of 1 hour for the material sample. Using the test method according to DIN ISO 3781 (2012-07), the paper material exhibits a wet tensile strength of at least 550 N / m in the longitudinal direction and at least 340 N / m transversely to the longitudinal direction. Here, too, the lower of the measured values ​​is the decisive one, i.e., 340 N / m. This corresponds to 5.1 N per 15 mm and deviates by 2% from the value measured above. This is within the measurement accuracy of the test methods used, taking into account any structural homogeneity deviations between different specimens of nominally the same fibrous paper material.

[0024] To achieve the desired wet strength, the paper material of the paper layer can be treated with a wet strength agent. Wet strength agents are also referred to in the literature as 'wet strength enhancers' or 'wet strengthening agents', and in English-language literature as 'wet strength agents'. Wet strength agents are commonly used to treat filter papers for coffee filters and tea bags to ensure that the coffee filters and tea bags do not dissolve during the preparation of the hot beverage. The term 'wet strength agent' or 'wet strength enhancer' is familiar to experts in the relevant technical field. Wet strength agents can be purchased commercially under this term. They may fall under Regulation (EU) 10 / 2011 on "Plastic materials and articles intended to come into contact with foodstuffs".

[0025] Common wet-strength agents include those of the polyamidoamine type. Examples of such agents are polyamine-epichlorohydrin resins (PAE) and polyamidoamine-epichlorohydrin resins (PAAE). PAE and PAAE resins are formaldehyde-free, non-toxic, and tasteless, and are suitable for clean, neutral, and slightly alkaline environments. Other possible wet-strength agents include urea-formaldehyde resins and melamine-formaldehyde resins. Due to its non-toxicity and food-grade properties, PAE or PAAE is preferred among the wet-strength agents mentioned. A material conforming to European Standard 68259P WO is preferred. Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 5 -

[0026] EN13432:2000-12 certified wet-strength agent, which is compostable and therefore biodegradable.

[0027] Preferably, the mass fraction of wet strength agent in relation to the total weight of the paper layer is less than 3%, more preferably less than 2% and most preferably less than one percent.

[0028] To further ensure the best possible durability of the paper material as a paper layer under wet conditions, the paper material of the paper layer preferably has a Cobb value according to ISO 535 of no more than 25 g / m². 2 The Cobb value is a measure of the water absorption by the paper material or of the water absorption capacity of the paper material.

[0029] Paper material is therefore particularly suitable as part of a lid laminate for blister packs because it is not only readily biodegradable, but also easily pressed through by consumers, especially when a solid item, such as a tablet, suppository, small part, or similar product, is packaged in a blister pack (also known as a 'blister pack' in the relevant field). For packaging such a solid item, a sufficiently strong and therefore sufficiently thick layer of paper is advantageous to prevent the packaged item from working its way through the paper and detaching from the packaging. Furthermore, it is essential to ensure that even individuals weakened by illness can access the packaged medication, particularly in the case of packaged drugs.For the latter reason, the paper layer should not be too thick.

[0030] In order to combine the aforementioned properties, the paper layer preferably has a basis weight of around 35g / m² in its dry state. 2 up to 65 g / m² 2 The term 'dry state' refers to the state that paper assumes when stored for an extended period, approximately one week, at a temperature of 20°C in a room climate with a relative humidity between 40% and 60%. Absolute dryness is not the determining factor, but rather... 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 6 -

[0031] on dry paper, meaning paper not soaked with liquid.

[0032] For successful recycling of the packaging laminate, especially packaging formed with the laminate, such as push-through packaging, after its use, it is advantageous if the paper material of the paper layer is porous. This allows the fluid used for recycling to penetrate the paper layer completely and reach the underlying polymer layers. A fluid preferably used for recycling is either acidic or alkaline, with alkaline liquids being preferred in current recycling processes.

[0033] The preferred alkaline solution used in recycling is aqueous sodium hydroxide solution with a concentration of no more than 10% by weight. This is used, for example, to clean plastic bottles during recycling. Often, this is aqueous sodium hydroxide solution with a concentration of 5% by weight.

[0034] To increase the recyclability of the packaging laminate and, consequently, of the packaging formed with the packaging laminate, a chemically soluble polymer layer is preferably arranged on the side of the paper layer facing the sealable polymer layer. This allows the paper layer to be easily removed from the rest of the packaging laminate and from the rest of the packaging formed with the packaging laminate by dissolving the chemically soluble polymer layer with aqueous sodium hydroxide solution, at least to the point where the paper layer is no longer bonded to it. Therefore, the chemically soluble polymer layer preferably borders directly on the paper layer.

[0035] Due to the increased wet strength described above, the paper layer, after being separated from the chemically soluble polymer layer, can be removed as a whole, i.e., with the paper layer's structure unchanged, from a sodium hydroxide bath or a collection basin. Decomposition of the paper layer into its fiber components is advantageously not a concern. 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 7 -

[0036] Preferably, the chemically soluble polymer layer is formed such that its layer thickness decreases by at least 1 pm, preferably at least 2 pm, most preferably at least 3 pm, when completely immersed in aqueous sodium hydroxide solution with a concentration of not more than 10% by weight, at a temperature of 50 °C and within 15 minutes.

[0037] This provides a chemically soluble polymer layer which can be dissolved through the paper layer in a sufficiently short time to such an extent that the paper layer separates from the chemically soluble polymer layer or can be separated with minimal force without losing its paper layer structure. This is because, of course, the aforementioned high-strength wet-strength paper material will also dissolve into its fiber components in liquid if it is exposed to the liquid for a sufficiently long time. Preferably, the chemically soluble polymer layer is directly adjacent to the paper layer without any intermediate layers.

[0038] This offers the advantage that the paper layer can be printed with consumer information, as is mandatory for pharmaceutical packaging, without the printing inks applied to the packaging interfering with later recycling, as they are a substance distinct from the packaging polymer. This is because the printing inks can be removed from the rest of the pharmaceutical packaging along with the paper layer. The pharmaceutical packaging is preferably a blister pack or push-through pack.

[0039] The chemically soluble polymer layer can be a primer layer positioned between the paper layer and the sealable polymer layer, and / or it can be the sealable polymer layer itself. Preferably, the chemically soluble polymer layer, particularly preferably the sealable polymer layer, is applied wet as a dispersion or as a solvent-based varnish. This allows for typical basis weights of less than 5 g / m² for this application method. 2, preferably below 4 g / m³ 2 , more strongly preferred to less than 3 g / m³ 2 to be produced. A minimum application thickness of 0.5 g / m² is required to ensure their effectiveness. 2 , or even better, 0.9 g / m² 2 , recommended.

[0040] Experiments have shown that a suitable chemically soluble polymer layer can be formed from a polymer containing vinyl with a molar fraction of less than 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 8 -

[0041] The polymer layer contains 30% mol of vinyl. Even better, the chemically soluble polymer layer contains vinyl with a mass fraction of less than 25% mol. Both tests have shown that with increasing vinyl content, the polymer containing the vinyl is increasingly protected from hydrolysis, so that chemical dissolution of the polymer with a vinyl content of over 30% mol by the aforementioned sodium hydroxide solution is no longer guaranteed within a timeframe acceptable for the steps of a recycling process.

[0042] Preferably, the chemically soluble polymer layer comprises an ethylene-vinyl acetate with a vinyl molar content of less than 30% mol or is formed from an ethylene-vinyl acetate with a vinyl molar content of less than 30% mol, more preferably less than 25%.

[0043] Alternatively or additionally, the chemically soluble polymer layer can comprise or be a polymer with ester compounds. Ester compounds are susceptible to attack and separation by sodium hydroxide. Preferably, the chemically soluble polymer layer can therefore comprise a polyester and / or a methacrylic acid ester. A suitable polymer is a copolymer of at least one methacrylic acid ester, at least one olefin, and at least one polyester.

[0044] To further protect the goods packaged with the packaging laminate, the packaging laminate can have a barrier layer acting as an oxygen barrier and / or a water vapor barrier. This metal layer can be a polymeric barrier varnish, for example, vinyl alcohol-based, such as polyvinyl alcohol or butenediol-vinyl alcohol copolymer, and / or a metal-based coating, such as a metallization or a metal oxide coating.

[0045] Any material that, at the same layer thickness, offers greater resistance to the migration of oxygen and / or water vapor through the layer than low-density polyethylene (LDPE) is considered a barrier material for forming the barrier layer. In other words, a barrier layer as defined in this application exhibits a lower oxygen transfer rate and / or a lower water vapor transfer rate than an LDPE layer of the same thickness. 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 9 -

[0046] Preferably, the paper layer, which ideally bears a print recognizable to the consumer, is positioned further away from the chemically soluble polymer layer in the packaging laminate than the barrier layer. This ensures a minimum level of accessibility to the chemically soluble polymer layer for the solvent used to dissolve it, preferably sodium hydroxide. The barrier layer is therefore preferably located on the same side of the paper layer as the sealable polymer layer. To enable the chemically soluble polymer layer to either form a strong bond with the sealable polymer layer or, as a sealable polymer layer itself, to bond the packaging laminate to the blister carrier, the barrier layer is positioned between the paper layer and the chemically soluble polymer layer.

[0047] Preferably, the packaging laminate is free of metal foils, which cause problems especially during recycling, as the metal foils have to be separated from the polymer components and disposed of separately.

[0048] In principle, the described packaging laminate is suitable for the production of any type of packaging. Its preferred use is as a lid laminate for creating push-through packaging.

[0049] The present application therefore also relates to push-through packaging, comprising a blister carrier with at least one receiving cavity for receiving goods to be packaged and with a lid laminate closing the receiving cavity made of a packaging laminate as described and further developed above, wherein the sealable polymer layer is connected to a polymer surface surrounding the receiving cavity by thermal sealing.

[0050] Preferably, the blister carrier is made from a single material to facilitate recycling. This single material can be polyethylene terephthalate or an olefin-based material, i.e., a material based on polypropylene and / or polyethylene. Even polyvinyl chloride is fundamentally possible as a blister carrier material, although it is not preferred due to its chlorine content. Polyethylene terephthalate is currently being considered as the preferred single material for the blister carrier. 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 10-

[0051] The present invention further relates to the above-described method for separating a thermal seal between the sealable polymer layer of the above-described and further developed packaging laminate, wherein the packaging laminate comprises the above-described chemically soluble polymer layer, and a polymer surface of a connecting body. The connecting body is preferably the above-mentioned blister carrier, but can be any other connecting body.

[0052] The process comprises wetting the chemically soluble polymer layer with an aqueous sodium hydroxide solution with a concentration of no more than 10% and a temperature of 50 °C for a predetermined period of no more than 30 minutes, preferably no more than 15 minutes, and thereby comprises separating the paper layer as a fiber material layer from the bonding body.

[0053] It should be added that the packaging laminate comprises at least one paper layer, although in most applications multiple paper layers will be unnecessary. To minimize the manufacturing effort of the packaging laminate, a preferred embodiment has exactly one paper layer. If the packaging laminate has more than one paper layer, preferably all paper layers are designed according to the above description and preferred embodiments to ensure their separation as a layer from the sealable polymer layer and thus from the packaging produced using the packaging laminate, without any of the paper layers disintegrating into their fiber components.

[0054] The present invention is explained in more detail below with reference to the accompanying drawings. It illustrates:

[0055] Fig. 1 a rough schematic cross-sectional view of a first embodiment of a packaging laminate according to the invention for preferred use as a lid laminate, 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 11 -

[0056] Fig. 2 shows a rough schematic cross-sectional view of a second embodiment of a packaging laminate according to the invention for preferred use as a lid laminate, and

[0057] Fig. 3 shows a rough schematic cross-sectional view through a push-through packaging formed using the packaging laminate of Fig. 1.

[0058] The figures are not to scale.

[0059] In Fig. 1, a first embodiment of a packaging laminate according to the invention is generally designated by 10. The packaging laminate 10 has a paper layer 12 as its base layer, which supports all other layers. The paper layer 12 is part of a base laminate 14 of the packaging laminate 10, which in the first embodiment includes, in addition to the paper layer 12, a sealable polymer layer 16.

[0060] The paper layer 12 is a layer of the commercially available paper material 18, marketed under the trade names 'ROCAL 20T' or 'Cellustraw 40G' by Ahlstrom, headquartered in Helsinki, Finland, and is characterized by a wet burst strength (or wet strength according to DIN ISO 3689) of 56 kPa. The paper material 18 has a basis weight of 40 g / m². 2 Its Cobb value according to ISO 535 is between 17 and 23 g / m². 2 .

[0061] Its wet strength in the longitudinal direction, according to the test conditions specified in the introductory description, is between 10.0 and 11.1 N / 15 mm. The wet strength in the transverse direction is between 5.4 and 6.0 N / 15 mm. For coiled material, the longitudinal direction is the unwinding direction perpendicular to the coil axis, also known as the 'machine direction'. For coiled material, the transverse direction is the direction parallel to the coil axis, also known as the 'cross direction'.

[0062] With these material properties, the paper layer is fundamentally suitable for detaching from the rest of the layer composite by liquid attack, in particular an aqueous alkali, within a reasonable time, i.e., in no more than 30 minutes, preferably about 15 minutes. 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 12 -

[0063] to be detached from the packaging laminate 10 without losing or dissolving its fiber composite as a layer material.

[0064] The sealable polymer layer 16 is preferably either an ethylene-vinyl acetate copolymer applied as a heat-seal dispersion with a molar vinyl content preferably less than 25%, or a copolymer of methacrylic acid ester, olefin, and polyester applied as a heat-seal lacquer. The heat-seal dispersion is commercially available under the trade name 'Adcote 37R972 E-42' from the Dow Chemical Group. The heat-seal lacquer is available under the trade name 'Degacryl® HS 4315 E' from Evonik Industries AG.

[0065] Both of the aforementioned sealable polymer layers are chemically soluble in an aqueous sodium hydroxide solution with a concentration of 5% by weight to such an extent that the paper layer 12 can be separated from the sealable polymer layer 16 within 15 minutes. This means that in these 15 minutes or less, enough material from the sealable polymer layer 16 is dissolved by the 5% sodium hydroxide solution to eliminate the adhesion between the paper layer 12 and the sealable polymer layer 16.

[0066] As is typical for flowable lacquers and dispersions, the sealable polymer layer 16 has a mass per unit area in the single-digit g / m² range. 2 -area applied directly to the paper layer 12. In the first embodiment shown in Fig. 1, the sealable polymer layer 16 is applied directly to a surface 12a of the paper layer 12.

[0067] Because the paper layer 12 is porous, the sodium hydroxide solution can penetrate the paper layer 12 completely during recycling, i.e., after use of the packaging laminate 10 or the push-through packaging 30 formed with it (see Fig. 3), and thus chemically attack and dissolve the sealable polymer layer 16 across its entire surface on the side facing the paper layer 12. This makes the wet-strength paper layer 12 detachable from the sealable polymer layer 16. 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 13-

[0068] The free surface 16a of the sealable polymer layer 16, which is facing away from the paper layer 12 and is also the free surface 14a of the base laminate 14 of the packaging laminate 10, is designed to produce a seal connection with a polymer, in this case polyethylene terephthalate.

[0069] On the opposite surface 14b of the base laminate 14, which is also the surface 12b of the paper layer 12 facing away from the sealable polymer layer 16, a printed layer 20 is provided, which is protected from external influences by an overprint varnish 22. Preferably, the overprint varnish 22 is also soluble or at least permeable to the aforementioned sodium hydroxide solution in the specified concentration.

[0070] Figure 2 shows a cross-sectional view of a second embodiment of a packaging laminate according to the invention. Identical and functionally equivalent components and component sections as in the first embodiment are provided with the same reference numerals in the second embodiment, but increased by the number 100.

[0071] The second embodiment will only be described below insofar as it differs from the first embodiment, to whose description reference is otherwise expressly made for the purpose of explaining the second embodiment.

[0072] In the second embodiment, the sealable polymer layer 116 is not applied directly to a surface 112a of the paper layer 112, but rather with the intermediate arrangement of further layers.

[0073] A primer layer 124 is applied to the surface 112a of the paper layer 112. In the second embodiment, this primer layer is chemically soluble in aqueous sodium hydroxide solution with a concentration of no more than 10% mol, preferably 5% mol, under the conditions mentioned above. This, in turn, makes it possible to separate the paper layer 112 as a whole from the remaining packaging laminate 110 or from the remaining base laminate 114 without breaking the paper layer 112 into its fiber components. - 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 14 -

[0074] gen. In the second embodiment, therefore, the primer layer 124 is the chemically soluble polymer layer mentioned in the introductory description.

[0075] On the side of the primer layer 124 facing away from the paper layer 112, a metallization layer 126 is deposited as a bamere layer 128 using a vacuum vapor deposition process. Instead of or in addition to a metallization layer, the bamere layer 128 can also comprise or be a metal oxide layer. This significantly reduces the migration of oxygen and water vapor through the packaging laminate 110 and thus protects products packaged by the packaging laminate 110 from oxidation and water vapor.

[0076] On the side of the bamere layer 128 facing away from the primer layer 124, a further primer layer 130 can be arranged to increase the adhesion of the sealable polymer layer 116 to the bamere layer 128.

[0077] Since the primer layer 124 is already a chemically soluble polymer layer, the person skilled in the art has more freedom in choosing the sealable polymer layer 116. In the second embodiment, the sealable polymer layer 116 need not be a chemically soluble polymer layer.

[0078] The advantage of the packaging laminate presented in the present application lies in the fact that the paper layer, i.e., paper layer 12 or 112, can be physically separated from the at least one polymer layer of the packaging laminate without the paper layer disintegrating into its fiber components. At the time of recycling, the at least one polymer layer, in particular the sealable polymer layer, is generally thermally sealed to a connecting element, such as a blister carrier 34 (see Fig. 3), so that after the paper layer is separated from the sealable polymer layer in the recycling process, a sufficiently pure polymer remains, which, with suitable material selection, can be recycled particularly easily.

[0079] The embodiments shown in Figures 1 and 2 are merely examples. With a suitable choice of material for the sealable polymer layer 116, the primer layer 130 can be designed to be sealed. (See also: 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 15-)

[0080] be dispensable if the material of the sealable polymer layer 116 adheres sufficiently to the barrier layer 128.

[0081] Fig. 3 shows, by way of example, a rough schematic cross-section of a push-through packaging 30 formed with the participation of the packaging laminate 10 of Fig. 1. Those skilled in the art will immediately see that instead of the packaging laminate 10, the packaging laminate 110 of Fig. 2 can also be thermally sealed with the blister carrier 34.

[0082] To facilitate its recycling, the blister carrier 34 is made of a single material, in the illustrated embodiment of polyethylene terephthalate.

[0083] The blister carrier 34 has typical depressions 34c for this packaging form, which form packaging spaces 36 in which a packaged product 38, such as a tablet or a capsule, can be received in a manner known per se.

[0084] On the blister carrier 34, the surface 34a faces away from the lid laminate 32, which closes the cavities 34c. The opposite surface 34b of the blister carrier 34, which is made of a flat, usually deep-drawn, monomaterial, serves to create a thermal seal with the sealable polymer layer 16 of the packaging laminate 10, which serves as the lid laminate 32. Since the surface 34b of the blister carrier 34 completely surrounds the cavities 34c of the blister carrier 34, the packaging space 36 of each cavity 34c is sealed by the creation of the seal between the lid laminate 32 and the surface 34b of the blister carrier 34.

[0085] The lid laminate 32 can be pressed through manually even by weakened persons, whereby the packaged product 38 usually serves as a pressing aid in order to exert a surface load on the lid laminate 32 locally exceeding the burst strength of the lid laminate 32.

[0086] When recycling the push-through packaging 30 after use, the sealable polymer layer 16 sealed with the blister carrier 34 remains with the blister carrier 34. 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 16-

[0087] bound, while the paper layer 12 and all layers applied on the side of the paper layer 12 facing away from the sealable polymer layer 16 are detached and disposed of with the paper layer 12 from the used push-through packaging 30.

Claims

68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 17- Claims 1. Packaging laminate (10; 110) comprising a paper layer (12; 112) and a sealable polymer layer (16; 116), wherein the sealable polymer layer (16; 116) is configured to form a thermal seal with a polymer surface (34b), characterized in that the paper material (18; 118) of the paper layer (12; 112) has a wet strength according to DIN ISO 3689 of more than 50 kPa.

2. Packaging laminate (10; 110) according to claim 1 , characterized in that the paper material (18; 118) of the paper layer (12; 112) has a wet tensile strength in the longitudinal direction of at least 9 N per 15 mm and / or a wet tensile strength in the transverse direction of at least 5 N per 15 mm, wherein the wet tensile strength is determined according to the following specifications: - a test strip of the paper material (18; 118) which has been stored for at least 24 h at 20 °C and a relative humidity of between 40% and 60% is prepared with a width of 15 mm, - the test strip is completely immersed in deionized water at 20 °C for 5 minutes, - After being removed from the bath of deionized water, the now wet test strip is immediately clamped between two gripping clamps of a tensile testing machine with a clamping distance of 40 mm, - After clamping, the gripping clamps are moved apart exclusively along a spacing direction orthogonal to the width direction of the test strip, while measuring the tensile force acting on the clamped wet test strip. - The tensile force measured immediately before tearing of the test strip, divided by the width of the test strip of 15 mm, is the wet tensile strength of the paper material (18; 118).68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 18- 3. Packaging laminate (10; 110) according to claim 1 or 2, characterized in that the paper material (18; 118) of the paper layer (12; 112) is treated with a wet strength agent.

4. Packaging laminate (10; 110) according to one of the preceding claims, characterized in that the paper material (18; 118) of the paper layer (12; 112) has a Cobb value according to ISO 535 of not more than 25 g / m² 2 exhibits.

5. Packaging laminate (10; 110) according to one of the preceding claims, characterized in that the paper layer (12; 112) has a basis weight in the range of 35 g / m² in the dry state. 2 up to 65 g / m² 2 exhibits.

6. Packaging laminate (10; 110) according to one of the preceding claims, characterized in that the paper material (18; 118) of the paper layer (12; 112) is porous.

7. Packaging laminate (10; 110) according to one of the preceding claims, characterized in that a chemically soluble polymer layer (16; 124) is arranged on the side (12a; 112a) of the paper layer (12; 112) facing the sealable polymer layer (16; 116), the thickness of which decreases by at least 1 pm within 15 minutes when the packaging laminate is completely immersed in aqueous sodium hydroxide solution with a concentration of not more than 10% by weight and a temperature of 50 °C.

8. Packaging laminate (10; 110) according to claim 7, characterized in that the chemically soluble polymer layer (16; 124) is a primer layer (124) arranged between the paper layer (12; 112) and the sealable polymer layer (16; 116) and / or the sealable polymer layer (16). 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 19- 9. Packaging laminate (10; 110) according to claim 7 or 8, characterized in that the chemically soluble polymer layer (16; 124) is formed from a polymer which has vinyl with a molar fraction of less than 30% mol.

10. Packaging laminate (10; 110) according to claim 9, characterized in that the chemically soluble polymer layer (16; 124) comprises an ethylene vinyl acetate with a vinyl molar content of less than 30% mol.

11. Packaging laminate (10; 110) according to one of claims 7 to 10, characterized in that the chemically soluble polymer layer (16; 124) comprises or is a polymer with ester compounds.

12. Packaging laminate (10; 110) according to one of the preceding claims, characterized in that the packaging laminate (10; 110) has a barrier layer (128) as an oxygen barrier and / or as a water vapor barrier.

13. Use of a packaging laminate (10; 110) as a lid laminate (32) to form a push-through package (30).

14. Push-through packaging (30), comprising a blister carrier (34) with at least one receiving cavity (34c) for receiving a product (38) to be packaged and with a lid laminate (32) closing the receiving cavity (34c) made of a packaging laminate (10; 110) according to one of claims 1 to 12, wherein the sealable polymer layer (16; 116) is connected to a polymer surface (34b) surrounding the receiving cavity (34c) by thermal sealing.

15. Method for separating a thermal seal between the sealable polymer layer (16; 116) of a packaging laminate (10; 110) according to one of claims 1 to 12, wherein the packaging laminate (10; 110) is the 68259P WO Huhtamaki Flexible Packaging Germany GmbH & Co. KG - 20 - features of claim 7, and a polymer surface (34b) of a connecting body (34), comprising wetting the chemically soluble polymer layer (16; 124) of the packaging laminate (10; 110) with an aqueous sodium hydroxide solution having a concentration of not more than 10% mol and a temperature of 50 °C for a predetermined period of time of not more than 30 minutes and thereby separating the paper layer (12; 112) as a fiber material layer from the connecting body (34).