Hydrofluorocarbon compounds and their use in integrated circuit manufacturing processes

A gas phase mixture with l-Bromo-l,l-difluoro-A,A-bis(trifluoromethyl)methanamine addresses defects in 3D NAND flash memory devices by minimizing electrical interference and global warming, improving the manufacturing process.

WO2026234224A1PCT designated stage Publication Date: 2026-11-12MERCK PATENT GMBH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063380
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The increasing density of integrated circuit devices leads to electrical interference issues, and the use of low-k insulating materials in 3D NAND flash memory devices results in defects like incomplete etch, bowing, and twisting during channel formation, while traditional etching compounds have high global warming potential.

Method used

A gas phase mixture comprising l-Bromo-l,l-difluoro-A,A-bis(trifluoromethyl)methanamine, along with other compounds, is used to etch and pattern thin films of integrated circuit materials, minimizing defects and reducing global warming potential.

Benefits of technology

The gas phase mixture effectively reduces defects in channel formation and lowers global warming potential, enhancing the manufacturing process of 3D NAND flash memory devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026063380_12112026_PF_FP_ABST
    Figure EP2026063380_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Gas phase mixtures configured to etch a thin film of an integrated circuit material are disclosed. The gas phase mixtures may include a first compound comprising 1-Bromo-1,1-difluoro-N,N-bis(trifluoromethyl)methanamine; and a second compound comprising one or more of: oxygen (O2), argon (Ar), helium (He), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (C5F8), 2,3,3,3-tetrafluoropro-1-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1,1,3,3,3- pentafluoropropene (C3HF5), 1,1,1,3,3,3-hexafluoro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), 1,1,3,3,3-pentafluoro-2-(fluoromethoxy)prop-1- ene (C4H2F6O), sulfur hexafluoride (SF6), and nitrogen trifluoride (NF3). Methods for making 1-Bromo-1,1-difluoro-N,N-bis(trifluoromethyl)methanamine are also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

Attorney Docket No. P25-175-PRI-US01HYDROFLUOROCARBON COMPOUNDS AND THEIR USE IN INTEGRATED CIRCUIT MANUFACTURING PROCESSESTECHNICAL FIELD

[0001] This disclosure generally describes l-Bromo-l,l-difluoro-7V,7V-bis(trifluoromethyl)methanamine, methods of synthesizing the same, and its use in integrated circuit manufacturing processes.BACKGROUND

[0002] Lateral, two-dimensional, geometries of integrated circuit devices continue to decrease in size, and as such, the surface density of these devices continues to increase. With this increased density, the chance of electrical interference, including cross-talk and parasitic capacitance, between adjacent devices increases, thereby leading to decreased overall integrated circuit performance. To reduce the likelihood of this electrical interference, films of low dielectric constant (“low-k”) insulating materials are often placed in the gaps, trenches, vias, and other surface features, between adjacent devices.

[0003] Nevertheless, the placement of low-k insulating materials in the gaps, trenches, and vias, of laterally laid out integrated circuit devices has its limitations too. More specifically, the ability of such low-k insulating materials to eliminate, or reduce, the electrical interference described above may decrease as the distance between adjacent devices is lessened and thus the thickness of the low-k insulating material film between adjacent devices decreases too. Accordingly, manufacturers have begun looking at forming integrated circuit devices not only laterally in two-dimensions, but “vertically” in the third dimension simultaneously too.

[0004] As circuitry is laid out in an increasingly vertical orientation, the number of layers of alternating thin films of integrated circuit materials has increased. For example, three-dimensional NOT AND (“3D NAND”) flash memory devices have gone from 24-layer “stacks” of alternating thin films of integrated circuit materials, to 32-layer stacks, and even to 48-layer stacks of such alternating thin films. More recently, work has begun directed to forming 3D NAND flash memory devicesAttorney Docket No. P25-175-PRI-US01incorporating 96-layer, and 128-layer, stacks of these alternating thin film integrated circuit materials.

[0005] To retain the advantage of moving to three-dimensional vertically laid out circuits, integrated circuit manufacturers require new processes and corresponding materials. One such process, and corresponding set of materials, under review by integrated circuit manufacturers includes the formation of “channels” in 3D NAND flash memory devices. Per the art, a channel is a more or less cylindrical conduit that extends between the bottommost surface of the bottom-layer of alternating thin films of integrated circuit materials in the 3D NAND stack described above, and the opposing outermost surface of the topmost layer of the top-layer of the same stack of alternating thin films integrated circuit materials. Being more or less cylindrical, the channel also has a diameter.

[0006] As the number of layers in the 3D NAND flash memory devices increases, so too does the aspect ratio of the channel. As this aspect ratio increases manufacturers often experience more defects during channel formation including “incomplete etch,” “bowing,” and “twisting.” Incomplete etch occurs when such conduit fails to fully extend between the bottommost surface of the bottom-layer of alternating thin films of integrated circuit materials, and the opposing outermost surface of the topmost layer of the top-layer of the same stack alternating thin films integrated circuit materials. Bowing occurs when the diameter of the conduit is greater than the preferred diameter at some point along the channel, as etching occurs more laterally than vertically at such point. A twisting defect occurs when the channel retains the preferred diameter but extends more laterally than vertically along its preferred, predetermined, path. These defects are to be avoided when etching channels in 3D flash memory devices.

[0007] Besides these issues, 3D NAND flash memory device manufacturers are also focusing on utilizing etching compounds having lower global warming potential than more highly fluorinated compounds. Octafluorocyclobutane (C4F8), for example, is a perfluorocarbon compound that is a greenhouse gas, and has a global warming potential approximately 3200 times greater than carbon dioxide.Octafluorocyclobutane is also a hydrofluorocarbon that may be used to etch the above-described channels. As such, integrated circuit manufacturers are looking for alternative hydrofluorocarbon compounds and mixtures having lower global warmingAttorney Docket No. P25-175-PRI-US01potential than perfluorocarbon compounds, and that also help minimize abovedescribed incomplete etch, bowing, and twisting defects during the etching of channels in 3D NAND flash memory devices.

[0008] The present disclosure is directed to overcoming on or more problems set forth above, and / or other problems associated with the prior art.SUMMARY OF THE INVENTION

[0009] In accordance with a first aspect of the present application, gas phase mixtures configured to etch a thin film of an integrated circuit material are disclosed herein. Such gas phase mixtures may comprise a first compound having the structure:l-Bromo-l,l-difluoro-A,A-bis(trifluoromethyl)methanamine. Such gas phase mixtures may also include a second compound comprising one or more of: oxygen (O2), argon (Ar), helium (He), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1, 1, 3,3,3-pentafluoropropene (C3HF5), 1,1, 1,3,3, 3-hexafhioro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3). In some particular aspects, the second compound can comprise octafluorocyclobutane (C4F8) or hexafluorobutadiene (C4F6).

[0010] In various aspects, the first compound may vary between 1% by volume of the gas phase mixture and being less than, or equal to, 99% by volume of the gas phase mixture configured to etch the thin film of integrated circuit material. In some related aspects, the second compound can comprise greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume ofAttorney Docket No. P25-175-PRI-US01the gas phase mixture, and wherein the first compound and the second compound comprise 100% by volume of the gas phase mixture. Additionally, in some aspects, a ratio of the first compound to the second compound can be between 5:1 and 1:5.

[0011] Beyond the foregoing first and second compounds, gas phase mixtures in accordance with various aspects of the present teachings may additionally include at least one third compound. For example, the third compound can comprise one or more of oxygen (O2), argon (Ar), helium (He), xenon (Xe), krypton (Kr), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-1-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1, 1, 3,3,3-pentafluoropropene (C3HF5), 1,1, 1,3,3, 3-hexafluoro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3). In some aspects, the third compound can comprise greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture, and wherein the first compound, the second compound, and the third compound comprise 100% by volume of the gas phase mixture.

[0012] Gas phase mixtures in accordance with various aspects of the present teachings may be configured to etch a thin film of an integrated circuit material of various compositions. For example, the composition of the thin films of integrated circuit materials gas phase mixtures may be configured to etch include, but are not necessarily limited to, silicon, polysilicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, tungsten, tungsten silicide, a carbon hard mask, a photoresist material, and combinations thereof.

[0013] Methods of etching a thin film of an integrated circuit material are also disclosed herein. In accordance with various aspects of the present disclosure, methods of etching a thin film of an integrated circuit material may include the step of contacting a surface of the thin film of the integrated circuit material with a plasmaAttorney Docket No. P25-175-PRI-US01comprising reactive ions generated by subjecting a gas phase mixture configured to etch the thin film of the integrated circuit material to a plasma generating device, thereby removing a portion of the thin film of the integrated circuit material. The gas phase mixture configured to etch the thin film may comprise a first compound comprising:p pl-Bromo-l,l-difluoro-A,A-bis(trifluoromethyl)methanamine. Such gas phase mixtures may also include a second compound comprising one or more of oxygen (O2), argon (Ar), helium (He), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1, 1, 3,3,3-pentafluoropropene (C3HF5), 1,1, 1,3,3, 3-hexafluoro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3). In some particular aspects, the second compound can comprise octafluorocyclobutane (C4F8) or hexafluorobutadiene (C4F6).

[0014] The composition of thin films etched according to methods of the present teachings include, but is not necessarily limited to, silicon, polysilicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, tungsten, tungsten silicide, a carbon hard mask, a photoresist material, and combinations thereof.

[0015] In certain aspects, the thin film can comprise a first film and a second film. For example, in some aspects, the first film and the second film can eachAttorney Docket No. P25-175-PRI-US01independently comprise silicon, silicon dioxide, silicon nitride, polysilicon, or a masking material. By way of example, the first film can comprise silicon dioxide and the second film can comprise silicon nitride, and the gas phase mixture can have an etch selectivity for silicon dioxide compared to silicon nitride of greater than or equal to about 1. By way of further example, in some aspects, the first film can comprise silicon dioxide or silicon nitride and the second film can comprise a masking material, and the gas phase mixture can have an etch selectivity for silicon dioxide compared to the masking material of greater than or equal to about 1 or the gas phase mixture can have an etch selectivity for silicon nitride compared to the masking material of greater than or equal to about 1. In certain aspects, the masking material can comprise polysilicon, a metal mask, a carbon hard mask, or a photoresist material.

[0016] Methods of patterning a thin film of an integrated circuit material are also disclosed herein. In accordance with various aspects of the present disclosure, methods of patterning a thin film of an integrated circuit material may include the step of contacting a surface of the thin film with a plasma comprising reactive ions generated by subjecting a gas phase mixture configured to etch the thin film of the integrated circuit material to a plasma generating device, thereby removing a portion of the thin film and generating a pattern in the thin film of the integrated circuit material. In such methods, at least a portion of the thin film can be disposed between confronting surfaces of a substrate and a masking material layer, wherein the masking material layer comprises an aperture defined therein exposing a portion of the surface of the thin film. In this method, the gas phase mixture may comprise a first compound comprising:l-Bromo-l,l-difluoro-A,A-bis(trifluoromethyl)methanamine. Such gas phase mixtures may also include a second compound comprising one or more of: oxygen (O2), argon (Ar), helium (He), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F),Attorney Docket No. P25-175-PRI-US01octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (CsFe), hexafluorocyclopropane (CsFe), 1, 1,3, 3, 3-pentafluoropropene (C3HF5), 1,1, 1,3,3, 3-hexafluoro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3).

[0017] The composition of the substrate according to methods of the present teachings include, but is not necessarily limited to, silicon, silicon oxide, silicon dioxide, silicon nitride, tantalum, tantalum nitride, titanium nitride, aluminum oxide, copper, tungsten carbonitride, molybdenum, polysilicon, a carbon hard mask, a photoresist material, and a combination thereof. Likewise, the composition of the thin film patterned according to methods of the present teachings include, but is not necessarily limited to, silicon, polysilicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, tungsten, tungsten silicide, a carbon hard mask, a photoresist material, and combinations thereof.

[0018] In various aspects, the masking material can comprise polysilicon, a metal mask, a carbon hard mask, or photoresist material, all by way of non-limiting example.

[0019] Methods of synthesizing l-Bromo-l,l-difluoro-7V,7V-bis(trifluorom ethyl) methanamine are also disclosed herein. In accordance with various aspects of the present disclosure, the compound may be formed by reacting bis(trifluoromethyl)amide anion with dibromodifluoromethane in the presence of a trimethyl(trifluoromethyl)silane catalyst. For example, in certain aspects, the trimethyl(trifluoromethyl)silane catalyst can be dropwise added to a solution of the bis(trifluoromethyl)amide anion and dibromodifluoromethane. In some aspects, this reaction can be performed at a temperature in a range from about -50°C to about 50°C, preferably at about 0°C.

[0020] In some aspects, bis(trifluoromethyl)amide anions can be provided by reacting A,7V-bis(trifluoromethyl)trifluoromethanesulfonamide with potassiumAttorney Docket No. P25-175-PRI-US01fluoride. By way of example, this reaction can be performed with dimethylacetamide as the solvent. In certain aspects this reaction can be performed at a temperature in a range from about -70°C to about 40°C, preferably at about -10°C.

[0021] In some aspects, the l-Bromo-l,l-difluoro-7V,7V-bis(trifluorom ethyl) methanamine formed from the reaction of bis(trifluoromethyl)amide anion and dibromodifluoromethane can be recovered via condensation. In some related aspects, the condensate can be purified, for example, via spinning band distillation.

[0022] These and other aspects of the present teachings are set forth herein.BRIEF DESCRIPTION OF THE DRAWINGS

[0023] FIG. l is a side elevation view of a multi-layer stack of alternating thin films of integrated circuit materials in a 3D NAND flash memory device depicting: (1) defect free channels etched through the stack; (2) examples of bowing and twisting in channels extending through the stack; and (3) an example of an incomplete etch that fails to extend through the stack.

[0024] FIG. 2 is a flowchart depicting a method configured to etch a thin film of an integrated circuit material with the compounds and gas phase mixtures disclosed herein.

[0025] FIG. 3 is a cross-sectional diagram of a wafer that may be utilized in the method configured to etch a thin film of an integrated circuit material depicted in FIG. 2.

[0026] FIG. 4 is a flowchart depicting a method configured to pattern a thin film of an integrated circuit material with the compounds and gas phase mixtures disclosed herein.

[0027] FIG. 5A is cross-sectional diagram of a wafer that may be utilized in the method configured to etch a thin film of an integrated circuit material depicted in FIG. 4 before patterning occurs.

[0028] FIG. 5B is a cross-sectional diagram of a wafer that may be utilized in the method configured to etch a thin film of an integrated circuit material depicted in FIG. 4 during the patterning process.Attorney Docket No. P25-175-PRI-US01

[0029] FIG. 5C is a cross-sectional diagram of a wafer that may be utilized in the method configured to etch a thin film of an integrated circuit material depicted in FIG. 4 depicting a pattern generated in the thin film of integrated circuit material.

[0030] FIGS. 6A-D are cross-sectional SEM images of trenches etched using an octafluorocyclobutane (C4F8) mixture (FIG. 6A) and an hexafluorobutadiene (C4F6) mixture (FIG. 6B) in comparison to trenches etched utilizing a gas phase mixture comprising 1-Bromo-l, l-difluoro-A,A-bis(trifluoromethyl)methanamine disclosed herein under two different process conditions (FIGS. 6C-D).DETAILED DESCRIPTION

[0031] Example embodiments will be described more fully with reference to the accompanying drawings. Example embodiments are provided so that this disclosure will be thorough, and will fully convey the scope to those who are skilled in the art. Numerous specific details are set forth such as examples of specific compositions, components, devices, and methods, to provide a thorough understanding of embodiments of the present disclosure. It will be apparent to those skilled in the art that specific details need not be employed, that example embodiments may be embodied in many different forms and that neither should be construed to limit the scope of the disclosure. In some example embodiments, well-known processes, well-known device structures, and well-known technologies are not described in detail.

[0032] The terminology used herein is for the purpose of describing particular example embodiments only and is not intended to be limiting. As used herein, the singular forms “a,” “an,” and “the” may be intended to include the plural forms as well, unless the context clearly indicates otherwise. The terms “comprises,” “comprising,” “including,” and “having,” are inclusive and therefore specify the presence of stated features, elements, compositions, steps, integers, operations, and / or components, but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof. Although the open-ended term “comprising” is to be understood as a non-restrictive term used to describe and claim various embodiments set forth herein, in certain aspects, the term may alternatively be understood to instead be a more limiting and restrictive term, such as “consisting of’ or “consisting essentially of.” Thus, for anyAttorney Docket No. P25-175-PRI-US01given embodiment reciting compositions, materials, components, elements, features, integers, operations, and / or process steps, the present disclosure also specifically includes embodiments consisting of, or consisting essentially of, such recited compositions, materials, components, elements, features, integers, operations, and / or process steps. In the case of “consisting of,” the alternative embodiment excludes any additional compositions, materials, components, elements, features, integers, operations, and / or process steps, while in the case of “consisting essentially of,” any additional compositions, materials, components, elements, features, integers, operations, and / or process steps that materially affect the basic and novel characteristics are excluded from such an embodiment, but any compositions, materials, components, elements, features, integers, operations, and / or process steps that do not materially affect the basic and novel characteristics can be included in the embodiment.

[0033] Any method steps, processes, and operations described herein are not to be construed as necessarily requiring their performance in the particular order discussed or illustrated, unless specifically identified as an order of performance. It is also to be understood that additional or alternative steps may be employed, unless otherwise indicated.

[0034] When a component, element, or layer is referred to as being “on,” “engaged to,” “connected to,” or “coupled to” another element or layer, it may be directly on, engaged, connected, or coupled to the other component, element, or layer, or intervening elements or layers may be present. In contrast, when an element is referred to as being “directly on,” “directly engaged to,” “directly connected to,” or “directly coupled to” another element or layer, there may be no intervening elements or layers present. Other words used to describe the relationship between elements should be interpreted in a like fashion (e.g., “between” versus “directly between,” “adjacent” versus “directly adjacent,” etc.). As used herein, the term “and / or” includes any and all combinations of one or more of the associated listed items.

[0035] Although the terms first, second, third, etc. may be used herein to describe various steps, elements, components, regions, layers and / or sections, these steps, elements, components, regions, layers and / or sections should not be limited by these terms, unless otherwise indicated. These terms may be only used to distinguish one step, element, component, region, layer or section from another step, element,Attorney Docket No. P25-175-PRI-US01component, region, layer, or section. Terms such as “first,” “second,” and other numerical terms when used herein do not imply a sequence or order unless clearly indicated by the context. Thus, a first step, element, component, region, layer, or section discussed below could be termed a second step, element, component, region, layer, or section without departing from the teachings of the example embodiments.

[0036] Spatially or temporally relative terms, such as “before,” “after,” “inner,” “outer,” “beneath,” “below,” “lower,” “above,” “upper,” and the like, may be used herein for ease of description to describe one element or feature's relationship to another element(s) or feature(s) as illustrated in the figures. Spatially or temporally relative terms may be intended to encompass different orientations of the device or system in use or operation in addition to the orientation depicted in the figures.

[0037] Throughout this disclosure, the numerical values represent approximate measures or limits to ranges to encompass minor deviations from the given values and embodiments having about the value mentioned as well as those having exactly the value mentioned. Other than in the working examples provided at the end of the detailed description, all numerical values of parameters (e.g., of quantities or conditions) in this specification, including the appended claims, are to be understood as being modified in all instances by the term “about” whether or not “about” actually appears before the numerical value. “About” indicates that the stated numerical value allows some slight imprecision (with some approach to exactness in the value; approximately or reasonably close to the value; nearly). If the imprecision provided by “about” is not otherwise understood in the art with this ordinary meaning, then “about” as used herein indicates at least variations that may arise from ordinary methods of measuring and using such parameters. For example, “about” may comprise a variation of less than or equal to 5%, optionally less than or equal to 4%, optionally less than or equal to 3%, optionally less than or equal to 2%, optionally less than or equal to 1%, optionally less than or equal to 0.5%, and in certain aspects, optionally less than or equal to 0.1%.

[0038] In addition, disclosure of ranges includes disclosure of all values and further divided ranges within the entire range, including endpoints and sub-ranges given for the ranges. Thus, ranges are, unless specified otherwise, inclusive of endpoints and include disclosure of all distinct values and further divided ranges within the entire range. Disclosure of values and ranges of values for specific parameters (such asAttorney Docket No. P25-175-PRI-US01temperatures, molecular weights, weight percentages, etc.) are not exclusive of other values and ranges of values useful herein. It is envisioned that two or more specific exemplified values for a given parameter may define endpoints for a range of values that may be claimed for the parameter. For example, if Parameter X is exemplified herein to have value A and also exemplified to have value Z, it is envisioned that Parameter X may have a range of values from about A to about Z. Similarly, it is envisioned that disclosure of two or more ranges of values for a parameter (whether such ranges are nested, overlapping, or distinct) subsume all possible combination of ranges for the value that might be claimed using endpoints of the disclosed ranges. For example, if Parameter X is exemplified herein to have values in the range of 1-10, or 2-9, or 3-8, it is also envisioned that Parameter X may have other ranges of values including 1-9, 1-8, 1-3, 1-2, 2-10, 2-8, 2-3, 3-10, and 3-9.

[0039] As used herein, the terms “composition” and “material” are used interchangeably to refer broadly to a substance containing at least the preferred chemical constituents, elements, or compounds, but which may also comprise additional elements, compounds, or substances, including trace amounts of impurities, unless otherwise indicated.

[0040] Various aspects of the disclosure will now be described with reference to the drawings and tables disclosed herein, if applicable, with like reference numbers referring to like elements, unless specified otherwise. As described above, to retain the advantage of moving to three-dimensional vertically laid out circuitry, integrated circuit manufacturers require new processes and corresponding materials. One such process under review is the formation of channels during the creation of 3D flash memory devices having minimal formation of defects such as incomplete etch, bowing, and twisting. Turning now to FIG. 1, a side elevation view of a multi-layer stack 10 of alternating thin films of integrated circuit materials 12 utilized in a 3D flash memory device is depicted. As represented there, a channel 14 can extend between the bottommost surface 16 of the bottom-layer 18 of the alternating thin films of integrated circuit materials 12 in the multi-layer stack 10, and the opposing outermost surface 20 of the top-layer 22 of the alternating thin films of integrated circuit materials 12 in the multi-layer stack 10. Without intending to be limiting, the alternating thin films of integrated circuit materials 12 in such stack 10 are oftenAttorney Docket No. P25-175-PRI-US01comprised of a layer of silicon nitride (i.e., SisN^ followed by a layer of silicon dioxide (i.e., SiCh).

[0041] As is additionally shown in FIG. 1, defects may occur during the creation of the channel 14 in 3D flash memory devices. One such defect is an incomplete etch defect 24. More specifically, and as is described above, the incomplete etch defect 24 occurs when the channel 14 fails to fully extend between the bottommost surface 16 of the bottom-layer 18 of the alternating thin films of integrated circuit materials 12 in the multi-layer stack 10, and the opposing topmost surface 20 of the top-layer 22 of the alternating thin films of integrated circuit materials 12 in the multi-layer stack 10.

[0042] Another defect integrated circuit manufacturers may experience during the creation of the channel 14 in 3D flash memory devices includes a bowing defect 26.As represented in FIG. 1, the bowing defect 26 occurs when the diameter of the channel 14 is greater than the preferred, predetermined, diameter of the channel 14 at some point along the channel 14 extending between the bottommost surface 16 of the bottom-layer 18 of the alternating thin films of integrated circuit materials 12 in the multi-layer stack 10, and the opposing outermost surface 20 of the top-layer 22 of the alternating thin films of integrated circuit materials 12 in the multi-layer stack 10. The thickness of each layer of the alternating thin films of integrated circuit materials 12 in the multi-layer stack 10 may be as little as a single nanometer, and possibly may be two, three, four, five, or more, microns in thickness.

[0043] Finally, another defect that may occur in the formation of the channel 14 in 3D flash memory devices is a twisting defect 28. As seen in FIG. 1, the twisting defect 28 occurs when the channel 14 retains the preferred diameter, but at least some portion of the channel 14 extends more laterally, than vertically, relative to its preferred path 30. As was also described above, manufacturers are simultaneously looking to utilize hydrofluorocarbon compounds having lower global warming potential than more traditionally utilized perfluorocarbon compounds, such as octafluorocyclobutane, during the etching of such channels 14.

[0044] In a first aspect of the present disclosure, novel and non-obvious gas phase mixtures configured to have lower global warming potential, which may be used for etching and / or patterning thin films, such as thin films of integrated circuit materialsAttorney Docket No. P25-175-PRI-US0112 in the multi-layer stack 10, are provided herein. More specifically, such gas phase mixtures may comprise a first compound corresponding in structure to:p p1-Bromo-l, l-difluoro-A,A-bis(trifluoromethyl)methanamine. An exemplary synthesis of 1-Bromo-l, l-difluoro-A,A-bis(trifluoromethyl)methanamine has been described by Sundermeyer et al. (D. Sohn, W. Sundermeyer, Chem. Ber. 1982, 115, 3334-3339), which is incorporated by reference in its entirety. As will be described in more detail below, 1-Bromo-l, l-difluoro-A,A-bis(trifluoromethyl)methanamine can also be prepared according to novel methods of synthesis in accordance with various aspects of the present teachings.

[0045] Such gas phase mixtures configured to etch a thin film of an integrated circuit material additionally include at least one second compound besides the first compound, 1-Bromo-l, l-difluoro-A,A-bis(trifluoromethyl)methanamine. For example, gas phase mixtures in accordance with the present teaching may include at least one second compound comprising oxygen (O2), argon (Ar), helium (He), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2, 3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1,1,3,3,3-pentafluoropropene (C3HF5), 1,1, 1,3,3, 3-hexafluoro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3). These second compounds, like the first compound described above, may also function as materials that contribute to etching thin films as described herein.

[0046] Besides the first and second compounds described above, such gas phase mixtures often include at least one third compound comprising oxygen (O2), argon (Ar), helium (He), xenon (Xe), krypton (Kr), and nitrogen (N2). Oxygen is customarily used as a material that limits the creation of fluoropolymers generated when reactive ions of the first and second compounds described and depicted aboveAttorney Docket No. P25-175-PRI-US01recombine a polymer at some point along the channel 14 of the alternating thin films of integrated circuit materials 12 in the multi-layer stack 10. Such buildup of fluoropolymer at the bottom of the channel 14 may help lead to the incomplete etch defect 24 described above. Alternatively, such buildup of fluoropolymer at differing points along the channel 14 may also help lead to the formation of the bowing defect 26 as well as the twisting defect 28.

[0047] As described before, the at least one third compound may also be selected from argon (Ar), helium (He), xenon (Xe), krypton (Kr), and nitrogen (N2). Such compounds often act as carrier gases for the etching process, and more importantly act to help transfer energy to, and ionize, the first compounds and second compounds described before.

[0048] In a preferred embodiment of this aspect of the disclosure, the first compound comprises greater than, or equal to, about 1% by volume of this gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture. In a more preferred embodiment, the first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 90% by volume of the gas phase mixture. In a further preferred embodiment, the first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 80% by volume of the gas phase mixture. In a further preferred embodiment, the first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 70% by volume of the gas phase mixture. In another preferred embodiment, the first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 60% by volume of the gas phase mixture. In an additional preferred embodiment, the first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 50% by volume of the gas phase mixture.

[0049] The at least one second compound, and the at least one third compound, make up the balance of the % volumes described just above. More specifically, when the first compound ranges between 1% and 99% of the volume of the gas phase mixture, then the at least one second compound alone, or together with the at least one third compound, ranges between 99% and 1% by volume of the gas phase mixture. In the instance that the first compound comprises greater than, or equal to, about 10% byAttorney Docket No. P25-175-PRI-US01volume of this gas phase mixture, and less than or equal to about 80% by volume of the gas phase mixture, then the at least one second compound alone, or together with the at least one third compound, ranges between 90% and 20% by volume of the gas phase mixture. Additionally, in another example, in the instance that the first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 50% by volume of the gas phase mixture, then the at least one second compound alone, or together with the at least one third compound, ranges between 90% and 50% by volume of the gas phase mixture.Generally, the ratio of the first compound to the second compound is between 5:1 and 1 :5 in this gas phase mixture.

[0050] As described before, the gas phase mixtures described in this first aspect of the present disclosure are configured to etch thin films of integrated circuit materials. In many instances, this thin film of integrated circuit material includes silicon, polysilicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, or where appropriate, combinations thereof. However, the gas phase mixtures described in this first aspect of the present disclosure may also find usefulness in etching other thin film materials including, but not necessarily limited to, gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, tungsten, tungsten silicide, a carbon hard mask, a photoresist material, and combinations thereof, too.

[0051] In operation, the compounds and gas phase mixtures depicted and described above find usefulness in many integrated circuit manufacturing processes including, but not limited to, etching a thin film, for example, a thin film of an integrated circuit material circuit material 12 in the multi-layer stack 10 depicted in FIG. 1, in a plasma-enhanced etching process. Accordingly in a second aspect of the present disclosure, and as represented in FIG. 2, a flowchart depicting a method configured to etch a thin film of an integrated circuit material with the compounds and gas phase mixtures disclosed herein is disclosed. As seen in a step 110, a wafer comprising a thin film of an integrated circuit material disposed thereon may be positioned inside a plasma-enhanced etching tool reaction chamber.Attorney Docket No. P25-175-PRI-US01

[0052] Turning now to FIG. 3, a cross-sectional diagram of an exemplary wafer 210 that may be utilized in step 110, as well as any remaining steps of the process depicted in FIG. 2, is disclosed. As seen therein, the wafer may be comprised of a substrate 212 having a thin film of an integrated circuit material 214 disposed thereon. The composition of the substrate 212 according to methods of the present teachings include, but is not necessarily limited to, silicon, silicon oxide, silicon dioxide, silicon nitride, tantalum, tantalum nitride, titanium nitride, aluminum oxide, copper, tungsten carbonitride, molybdenum, polysilicon, a carbon hard mask, a photoresist material, and a combination thereof. In some exemplary instances, the substrate 212 comprises one of either silicon (e.g., monocrystalline silicon) or polysilicon. In many instances, the thin film of integrated circuit material 214 comprises silicon, polysilicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, and where appropriate, combinations thereof. For example, in some instances the thin film of integrated circuit material 214 will either be one of silicon or polysilicon. In most instances the thin film of integrated circuit material 214 will either be one of silicon dioxide or silicon nitride.

[0053] Additionally, or alternatively, the thin film of integrated circuit material 214 disposed on the wafer 210 may also include gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, a carbon hard mask material, a photoresist material, and combinations thereof, too. Additionally, the thin film of integrated circuit material 214 comprises a surface 216 that may be contacted with a plasma comprising reactive ions of the gas phase mixture that is configured to etch the thin film of integrated circuit material 214. Although not shown in FIG. 3, it is contemplated herein that the wafer may include more than one thin film of integrated circuit material, for example, alternating thin films of the same and / or different material as described herein, disposed on a substrate.

[0054] Now turning back to FIG. 2, and while still reviewing FIG. 3, in step 112 a gas phase mixture configured to etch the thin film of integrated circuit material 214Attorney Docket No. P25-175-PRI-US01may be flowed into the plasma-enhanced etching tool chamber. Such gas phase mixtures may comprise a first compound corresponding in structure to:p p1 -Bromo- 1 , 1 -difluoro-A,A-bis(trifluoromethyl)m ethanamine.

[0055] Such gas phase mixture configured to etch a thin film of an integrated circuit material can additionally include at least one second compound besides the first compound listed above. More clearly, such gas phase mixture includes at least one second compound comprising oxygen (O2), argon (Ar), helium (He), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (CsFe), hexafluorocyclopropane (CsFe), 1, 1, 3,3,3-pentafluoropropene (C3HF5), 1,1, 1,3,3, 3-hexafluoro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3). These second compounds, like the first compound described above, may also function as materials that contribute to etching thin films as described herein.

[0056] Besides the first and second compounds described above, such gas phase mixtures often include at least one third compound comprising oxygen (O2), argon (Ar), helium (He), xenon (Xe), krypton (Kr), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (CsFe), hexafluorocyclopropane (CsFe), 1, 1, 3,3,3-pentafluoropropene (C3HF5), 1,1, 1,3,3, 3-hexafluoro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3). Oxygen is customarily used as a material that limits the creation of fluoropolymers generated when reactive ions of the first and second compounds described and depicted aboveAttorney Docket No. P25-175-PRI-US01recombine a polymer at some point along the channel 14 of the alternating thin films of integrated circuit materials 12 in the multi-layer stack 10. Such buildup of fluoropolymer at the bottom of the channel 14 may help lead to the incomplete etch defect 24 described above. Alternatively, such buildup of fluoropolymer at differing points along the channel 14 may also help lead to the formation of the bowing defect 26 as well as the twisting defect 28.

[0057] As described before, the at least one third compound may also be selected from argon, helium, xenon, krypton, and nitrogen. Such compounds often act as carrier gases for the etching process, and more importantly act to help transfer energy to, and ionize, the first compounds and second compounds described before.

[0058] In a preferred embodiment of this aspect of the disclosure, the at least one first compound comprises greater than, or equal to, about 1% by volume of this gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture. In a more preferred embodiment, the at least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 90% by volume of the gas phase mixture. In a further preferred embodiment, the at least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 80% by volume of the gas phase mixture. In a further preferred embodiment, the at least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 70% by volume of the gas phase mixture. In another preferred embodiment, the at least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 60% by volume of the gas phase mixture. In an additional preferred embodiment, the at least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 50% by volume of the gas phase mixture.

[0059] The at least one second compound, and the at least one third compound, make up the balance of the % volumes described just above. More specifically, when the at least one first compound ranges between 1% and 99% of the volume of the gas phase mixture, then the at least one second compound alone, or together with the at least one third compound, ranges between 99% and 1% by volume of the gas phase mixture. In the instance that the least one first compound comprises greater than, orAttorney Docket No. P25-175-PRI-US01equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 80% by volume of the gas phase mixture, then the at least one second compound alone, or together with the at least one third compound, ranges between 90% and 20% by volume of the gas phase mixture. Additionally, in another example, in the instance that the least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 50% by volume of the gas phase mixture, then the at least one second compound alone, or together with the at least one third compound, ranges between 90% and 50% by volume of the gas phase mixture. Generally, the ratio of the first compound to the second compound between 5:1 and 1:5 in this gas phase mixture.

[0060] As described before, the gas phase mixtures described in this first aspect of the present disclosure are configured to etch thin films of integrated circuit materials. In many instances, this thin film of integrated circuit material includes silicon, polysilicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, or where appropriate, combinations thereof. However, the gas phase mixtures described in this first aspect of the present disclosure may also find usefulness in etching other thin film materials including, but not necessarily limited to, gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, tungsten, tungsten silicide, a carbon hard mask, a photoresist material, and combinations thereof, too.

[0061] While still reviewing FIG. 2, in view of FIG. 3, in step 114 a plasma generating device electronically coupled with the plasma-enhanced etching tool reaction chamber may be turned on, and thereby generate a plasma comprising reactive ions of the gas phase mixture configured to etch the thin film of integrated circuit material 214 inside the plasma-enhanced etching tool’s reaction chamber. In step 116 depicted in FIG. 2, the surface 216 of FIG. 3 may be contacted with the plasma comprising reactive ions of the gas phase mixture configured to etch the thin film of integrated circuit material 214, thereby removing a portion of that thin film 214 disposed on the wafer 210.Attorney Docket No. P25-175-PRI-US01

[0062] In accordance with a third aspect of the invention disclosed herein, a method of pattering a thin film of an integrated circuit material is disclosed. Turning now to FIG. 4, while also reviewing FIGS. 5A-5C, at step 310 a wafer 410 may be positioned inside a plasma-enhanced etching tool reaction chamber. As represented in each of FIGS. 5A-5C, the wafer 410 may be comprised of a substrate 420 having a thin film of an integrated circuit material 430 disposed thereon between opposing surfaces 440 of the substrate 420 and a masking material layer 450.

[0063] The composition of the substrate 420 according to methods of the present teachings include, but is not necessarily limited to, silicon, silicon oxide, silicon dioxide, silicon nitride, tantalum, tantalum nitride, titanium nitride, aluminum oxide, copper, tungsten carbonitride, molybdenum, polysilicon, a carbon hard mask, a photoresist material, and a combination thereof. For example, substrate 420 can comprise one of either silicon (e.g., monocrystalline silicon) or polysilicon. In many instances the thin film of integrated circuit material 430 comprises silicon, polysilicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, and where appropriate, combinations thereof. For example, in some instances the thin film of integrated circuit material 430 will either be one of silicon or polysilicon. In most instances the thin film of integrated circuit material 430 will either be one of silicon dioxide or silicon nitride.

[0064] Additionally, or alternatively, the thin film of integrated circuit material 430 disposed between the opposing surfaces 440 comprises gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, and combinations thereof, too. In addition, the masking material layer 450 may comprise polysilicon, a metal mask, a carbon hard mask, a photoresist material, and combinations thereof. Finally, and as is seen in FIG. 5A, the masking material layer 450 comprises one or more apertures 460 at least partially defined therethrough. In another instance, the one or more apertures 460 may be defined fully through the masking material layer 450. As is understood by a person having ordinary skill in the art, the apertures 460 will define a pattern in the thin film of integrated circuit material 430 after etching.Attorney Docket No. P25-175-PRI-US01

[0065] Turning back to FIG. 4, and while still reviewing FIGS. 5A and 5B, in step 312 a gas phase mixture configured to etch the thin film of integrated circuit material 430 may be flowed into the plasma-enhanced etching tool chamber. Such gas phase mixtures may comprise a first compound corresponding in structure to:1 -Bromo- 1 , 1 -difluoro-A,A-bis(trifluoromethyl)m ethanamine.

[0066] Such gas phase mixture configured to etch a thin film of an integrated circuit material can additionally include at least one second compound besides l-Bromo-1,1-difluoro-A,A-bis(trifluoromethyl)methanamine. More clearly, such gas phase mixture can include at least one second compound comprising oxygen (O2), argon (Ar), helium (He), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1,1,3,3,3-pentafluoropropene (C3HF5), 1, 1,1, 3,3,3-hexafluoro-2 -methoxy -2-(trifluoromethyl)propane (C5H3F9O), 1, 1,3,3, 3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3). These second compounds, like the first compounds described above may also function as materials that contribute to etching thin films as described herein.

[0067] Besides the first and second compounds described above, such gas phase mixtures often include at least one third compound comprising oxygen (O2), argon (Ar), helium (He), xenon (Xe), krypton (Kr), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1,1,3,3,3-pentafluoropropene (C3HF5), 1,1, 1,3,3, 3-hexafluoro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2-(fluoromethoxy)prop-l-Attorney Docket No. P25-175-PRI-US01ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3). Oxygen is customarily used as a material that limits the creation of fluoropolymers generated when reactive ions of the first and second compounds described and depicted above recombine a polymer at some point along the channel 14 of the alternating thin films of integrated circuit materials 12 in the multi-layer stack 10. Such buildup of fluoropolymer at the bottom of the channel 14 may help lead to the incomplete etch defect 24 described above. Alternatively, such buildup of fluoropolymer at differing points along the channel 14 may also help lead to the formation of the bowing defect 26 as well as the twisting defect 28.

[0068] As described before, the at least one third compound may also be selected from argon, helium, xenon, krypton, and nitrogen. Such compounds often act as carrier gases for the etching process, and more importantly act to help transfer energy to, and ionize, the first compounds and second compounds described before.

[0069] In a preferred embodiment of this aspect of the disclosure, the at least one first compound comprises greater than, or equal to, about 1% by volume of this gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture. In a more preferred embodiment, the at least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 90% by volume of the gas phase mixture. In a further preferred embodiment, the at least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 80% by volume of the gas phase mixture. In a further preferred embodiment, the at least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 70% by volume of the gas phase mixture. In another preferred embodiment, the at least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 60% by volume of the gas phase mixture. In an additional preferred embodiment, the at least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 50% by volume of the gas phase mixture.

[0070] The at least one second compound, and the at least one third compound, make up the balance of the % volumes described just above. More specifically, when the at least one first compound ranges between 1% and 99% of the volume of the gasAttorney Docket No. P25-175-PRI-US01phase mixture, then the at least one second compound alone, or together with the at least one third compound, ranges between 99% and 1% by volume of the gas phase mixture. In the instance that the least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 80% by volume of the gas phase mixture, then the at least one second compound alone, or together with the at least one third compound, ranges between 90% and 20% by volume of the gas phase mixture. Additionally, in another example, in the instance that the least one first compound comprises greater than, or equal to, about 10% by volume of this gas phase mixture, and less than or equal to about 50% by volume of the gas phase mixture, then the at least one second compound alone, or together with the at least one third compound, ranges between 90% and 50% by volume of the gas phase mixture. Generally, the ratio of the first compound to the second compound between 5:1 and 1 :5 in this gas phase mixture.

[0071] As described before, the gas phase mixtures described in this first aspect of the present disclosure are configured to etch thin films of integrated circuit materials. In many instances, this thin film of integrated circuit material includes silicon, polysilicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, or where appropriate, combinations thereof. However, the gas phase mixtures described in this first aspect of the present disclosure may also find usefulness in etching other thin film materials including, but not necessarily limited to, gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, tungsten, tungsten silicide, a carbon hard mask, a photoresist material, and combinations thereof, too.

[0072] Moving on, in step 314 a plasma generating device electronically coupled with the plasma-enhanced etching tool reaction chamber may be turned on, and thereby generate a plasma comprising reactive ions of the gas phase mixture configured to etch the thin film of integrated circuit material 430 inside the plasma-enhanced etching tool’s reaction chamber. In step 316 depicted in FIG. 4, the one or more apertures 460 represented in FIGS. 5 A and 5B may be contacted with the plasma comprising reactive ions of the gas phase mixture configured to etch the thinAttorney Docket No. P25-175-PRI-US01film of integrated circuit material 430, thereby removing any remaining masking material layer 450 and thus fully defining the one or more apertures 460 through the entirety of the masking material layer 450 and thereby exposing a surface 470 of the thin film of integrated circuit material 430 consistent in shape and size to the aperture 460 from which it is associated.

[0073] In step 318, as is represented in FIG. 4, the surface 470 of FIG. 5B may be contacted with the plasma comprising reactive ions of the gas phase mixture configured to etch the thin film of integrated circuit material 430, thereby removing a portion of that thin film 430 disposed on the wafer 410. As seen in FIG. 5C, the removal of this material 430 in step 318 generated a pattern 480 in the thin film of integrated circuit material 430. As a person having ordinary skill in the dry etching arts understands, the pattern 480 generated in this process is consistent in shape and size with the aperture 460 from which it is coupled in the masking material layer 440.Some common patterns 480 etched into the thin film of integrated circuit material 430 include gaps, trenches, vias that may subsequently be backfilled with a low-k material. Alternatively, the pattern 480 may comprise a channel 14 of a 3D flash memory device depicted above in FIG. 1.

[0074] Use of the gas phase mixtures described herein advantageously result in thin film etching and patterning with desirable selectivity. For example, where the thin film comprises silicon dioxide or silicon nitride, the gas phase mixture can have an etch selectivity for the thin film to the masking material layer (e.g., metal mask, carbon hard mask, photoresist) of greater than or equal to about 1.Synthesis of 1 -Bromo- 1, l-difluoro-A,A-bis(trifluoromethyl)methanamine

[0075] In a fourth aspect of the present disclosure, improved methods of synthesis of l-Bromo-l,l-difluoro-A,A-bis(trifluoromethyl)methanamine are provided herein. In particular, exemplary methods of synthesis in accordance with various aspects of the present teachings can provide increased yield and better scalability relative to known methods as described, for example, by Sundermeyer et al. (D. Sohn, W.Sundermeyer, Chem. Ber. 1982, 115, 3334-3339), which is incorporated by reference in its entirety.Attorney Docket No. P25-175-PRI-US01

[0076] In accordance with various aspects of the present teachings, l-Bromo-1,1-difluoro-7V,7V-bis(trifluoromethyl)methanamine can be prepared by reacting bis(trifluoromethyl)amide anion with dibromodifluoromethane in the presence of a trimethyl(trifluoromethyl)silane. An exemplary general reaction formula according to various aspects of the present teachings is shown below:CBrgFg[TMS-CF3Jr hK N(CFA- . » .CF3

[0077] It has been surprisingly discovered that the trimethyl(trifluoromethyl)silane catalyst (TMS-CF3) can be effective to accelerate the reaction between the bis(trifluoromethyl)amide anion ([N(CF3)2)]') and dibromodifluoromethane (CBr2F2) by orders of magnitude relative to the reaction in the absence of the catalyst (e.g., the production of l-Bromo-l,l-difluoro-A,A-bis(trifluoromethyl)methanamine can occur in seconds as opposed to hours and even days as with known processes).

[0078] The TMS-CF3 catalyzed reaction of bis(trifluoromethyl)amide anion with dibromodifluoromethane can be performed in a variety of solvents. By way of nonlimiting example, such solvents can include, but are not necessarily limited to, dimethylacetamide (DMA), dimethylformamide (DMF), N-methyl-2 -pyrrolidone (NMP), tetrahydrofuran (THF), 1,4-di oxane, dimethoxy ethane (glyme), bis(2-methoxyethyl) ether (diglyme), diethyl ether, and methyl tert-butyl ether (MTBE).

[0079] The TMS-CF3 catalyzed reaction of bis(trifluoromethyl)amide anion with dibromodifluoromethane can also be performed in a variety of reaction conditions. By way of example, the reaction of bis(trifluoromethyl)amide anion with dibromodifluoromethane in the presence of the trimethyl(trifluoromethyl)silane catalyst can be performed at a temperature in a range from about -50°C to about 50°C, preferably at about 0°C, in order to produce a volatile product containing 1-Bromo-l,l-difluoro-A,A-bis(trifluoromethyl)methanamine. In certain aspects, such a highly volatile product can be collected via condensation, and optionally, the l-Bromo-1,1-difluoro-A,A-bis(trifluoromethyl)methanamine can be further purified, via spinning band distillation, all by way of non-limiting example.Attorney Docket No. P25-175-PRI-US01

[0080] Bis(trifluoromethyl)amide anions for use in the above-catalyzed reaction with dibromodifluoromethane can be obtained from any source or generated by any reaction known in the art or hereafter developed. For example, in certain aspects of the present teachings, the bis(trifluoromethyl)amide anions can initially be formed by reacting a precursor such as 7V,7V-bis(trifluoromethyl)trifluoromethanesulfonamide with potassium fluoride (KF) within a solvent (e.g., DMA), with the byproduct trifluoromethanesulfonyl fluoride (F3CSO2F) being optionally removed (e.g., via condensation) as shown in the reaction formula below.DMAf ,CF3 -1O ’C*RT © @ FjC-S-N + KF - ► K N(CF3)2O CFS. F3CSO2F

[0081] Though potassium fluoride (KF) serves as a source of fluoride ions in the exemplary generation of bis(trifluoromethyl)amide anion depicted above, it will be appreciated that the present teachings are not so limited. Various sources of fluoride ions can be utilized in accordance with the present teachings such as potassium fluoride, sodium fluoride, rubidium fluoride, cesium fluoride, quaternary ammonium fluorides (e.g., tetramethylammonium fluoride), and tris(dimethylamino)sulfonium difluorotrimethylsilicate (TASF), all by way of non-limiting example. Likewise, a person skilled in the art would appreciate that a variety of solvents can be utilized including, but not necessarily limited to, DMA (as depicted in the exemplary reaction above), DMF, NMP, THF, 1,4-di oxane, glyme, diglyme, diethyl ether, and MTBE, all by way of non-limiting example. Additionally, it will be appreciated that the formation of bis(trifluoromethyl)amide anion with dibromodifluoromethane can also be performed in a variety of reaction conditions. By way of non-limiting example, the bis(trifluoromethyl)trifluoromethane-sulfonamide can be reacted with potassium fluoride at a temperature in a range from about -70°C to about 40°C, preferably at about -10°C.

[0082] Working Example 1 - Synthesis of l-Bromo-l,l-difluoro-7V,7V-bis(trifluoromethyl)m ethanamine:

[0083] In a 250 mL round bottom flask (NS 29 Young PTFE valve) dry powdered KF (5.02 g, 86.4 mmol) in dimethylacetamide (75 mL) was treated at -10°C over 30 min with 7V,7V-bis(trifluoromethyl)trifluoromethanesulfonamide (26.93 g, 94.2 mmol)Attorney Docket No. P25-175-PRI-US01to generate bis(trifluoromethyl)amide anions. After stirring for 1.5 h, the byproduct trifluoromethanesulfonyl fluoride was condensed into a cooling trap.

[0084] Then, dibromodifluoromethane (17.9 g, 85,3 mmol) was added at 0°C over 5 min, followed by dropwise addition of trimethyl(trifluoromethyl)silane (0.327 g, 2.30 mmol). During the catalyst addition, a colorless precipitate formed. The reaction mixture was stirred for 20 h at room temperature, and the highly volatile product was transferred into a Young flask by condensation. Crude yield: 19.2 g (68.0 mmol, 79%; 89% purity by GLC). The condensed product was further purified by spinning band distillation, and exhibited the following characteristics (bp. 34.5 °C, 99% purity by GLC):19F NMR (470.6 MHz, CDC13): 8 = -27.7 (sept, 2F, JFF = 13.7 Hz, CF2Br), -54.5 (t, 6F, JFF = 13.7 Hz, NCF3) ppm.13C NMR (125.8 MHz, CDCI3): 5 = 117.8 (q, JCF = 271.3 Hz, N(CF3)2),106.6 (t, 4 JCF = 312.8 Hz, CF2Br) ppm.13C{19F} NMR (125.8 MHz, CDCI3): 6 = 117.8 (s, N(CF3)2),106.6 (s, CF2Br) ppm.

[0085] The foregoing description of the embodiments has been provided for purposes of illustration and description. It is not intended to be exhaustive or to limit the disclosure. Individual elements or features of a particular embodiment are generally not limited to that particular embodiment, but, where applicable, are interchangeable and can be used in a selected embodiment, even if not specifically shown or described. The same may also be varied in many ways. Such variations are not to be regarded as a departure from the disclosure, and all such modifications are intended to be included within the scope of the disclosure.Patterning Methods

[0086] All patterning tests were conducted with a PlasmaTherm APEX SLR ICP 200mm reaction chamber. The plasma generating device electronically coupled with the reaction chamber is an inductively coupled plasma generator having a 2 MHz top electrode source and a 13.56 MHz biased bottom electrode / susceptor. The top electrode power may be varied between 0 watts (“W”) and about 2000 W, while theAttorney Docket No. P25-175-PRI-US01bottom electrode / susceptor power can be varied between 0 W and about 600 W. The temperature of the bottom electrode / susceptor may be varied between about -40°C and 250°C to evaluate the effect of reduced temperature on pattern formation. The pressure of the reaction chamber may be varied between about 1 mTorr and 100 mTorr, and the flow rate of the gas phase mixture configured to etch the thin films of integrated circuit material may be varied between 1 and 500 standard cubic centimeters per minute (“seem”). Oxygen, argon, or oxygen and argon are typically flowed into the reaction chamber as part of the gas phase mixture configured to etch a thin film of an integrated circuit material, while up to three other gases may be simultaneously flowed into the reaction chamber along with oxygen and / or argon to help generate a pattern in a thin film of an integrated circuit material.

[0087] Working Example 2 - Use of 1 -Bromo- l,l-difhroro-A,7V-bis(trifluoromethyl)m ethanamine (referred to as C3BrF8N below) to Generate a Trench:p p

[0088] Based on a blanket wafer screening DOE several process conditions were selected for a patterned SiO? wafer etch and compared to octafluorocyclobutane (C4F8) and hexafluorobutadiene (C4F6) under Best Known Method (“BKM”) conditions. BKM is a term of art.

[0089] The below table shows C4F8 BKM conditions:RF Bias Press 02 Ar C4F8 Etch Time [W] [W] [mtorr] [seem] [seem] [seem] [min]600 600 5 3 36 21 3

[0090] The below table shows C4F6 BKM conditions:RF Bias Press 02 Ar C4F6 Etch Time [W] [W] [mtorr] [seem] [seem] [seem] [min]600 600 5 7 36 33 6Attorney Docket No. P25-175-PRI-US01

[0091] The table below shows two process conditions with l-Bromo-l,l-difluoro- 7V,7V-bis(trifluoromethyl)methanamine (C3BrF8N) run on patterned SiO? wafers:Etch RF Bias Press 02 Ar C3F6O Wafer Time [W] [W] [mtorr] [seem] [seem] [seem] [min] C3BrF8N1000 600 5 0 5 30 3 P4C3BrF8N1000 600 5 5 5 30 3P5All patterned etches from the table above were carried out at a chamber temperature of 60°C and an electrode temperature of 25°.

[0092] The table below shows an etch profile comparison of the two process conditions of l-Bromo-l,l-difluoro-A,A-bis(trifluoromethyl)m ethanamine (i.e., C3BrF8N P4 and C3BrF8N P4). CD in the all the tables below is defined as Critical Dimension, a term of art.C4F8 BKM C4F6 BKM C3BrF8N P4 C3BrF8N P5 ER [nm / min] 305 234 367 383 PR THK [nm] 344 255 131 0 A PR (nm) 756 845 969 1100 Selectivity 1.21 1.66 1.09 1.01 Hole CD [nm] 388 340 635 599 BTM CD [nm] 260 288 440 437 PTN Depth [nm] 916 1405 1100 1150BTM / TOP 0.67 0.85 0.69 0.73

[0093] The data shows that l-Bromo-l,l-difluoro-N,N- bis(trifluoromethyl)m ethanamine demonstrates higher pattern SiO? etch rates than C4F8 and C4F6 but with reduced selectivity and up to 10% improved bottom / top CD ratio over C4F8. Performance can likely be improved through further optimization.

[0094] Cross-sectional SEM images of trenches generated by the C4F8 BKM, C4F6 BKM, and P4 and P5 processes with l-Bromo-l, l -difluoro- A- bis(trifluoromethyl)m ethanamine are seen in FIGS. 6A-D, respectively. The SEM images demonstrate very high etch rates, straight sidewalls and no excessive polymer formation on the film surface.

[0095] The above description is meant to be representative only, and thus modifications may be made to the aspects of the invention disclosed herein withoutAttorney Docket No. P25-175-PRI-US01departing from the scope of the disclosure. Thus, these modifications fall within the scope of the present disclosure and are intended to fall within the appended claims.

Claims

Attorney Docket No. P25-175-PRI-US01CLAIMSWhat is claimed is:

1. A gas phase mixture configured to etch a thin film of an integrated circuit material, comprising:a first compound comprising:F F / N - ( - F / \Br — V FF F1 -Bromo- 1, l-difluoro-7V,7V-bis(trifluoromethyl)methanamine; anda second compound comprising one or more of: oxygen (O2), argon (Ar), helium (He), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1,1,3,3,3-pentafluoropropene (C3HF5), 1, 1,1, 3,3,3-hexafluoro-2 -methoxy -2-(trifluoromethyl)propane (C5H3F9O), 1, 1,3,3, 3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3).

2. The gas phase mixture according to claim 1, wherein the thin film comprises silicon, polysilicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, tungsten, tungsten silicide, a carbon hard mask, a photoresist material, and combinations thereof.Attorney Docket No. P25-175-PRI-US013. The gas phase mixture according to claim 1 or claim 2, wherein the first compound comprises greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture.

4. The gas phase mixture according to claim 3, wherein the second compound comprises greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture, and wherein the first compound and the second compound comprise 100% by volume of the gas phase mixture.

5. The gas phase mixture according to claim 4, wherein a ratio of the first compound to the second compound is between 5:1 and 1:5.

6. The gas phase mixture according to any one of the previous claims, wherein the second compound comprises octafluorocyclobutane (C4F8) or hexafluorobutadiene (C4F6).

7. The gas phase mixture according to any of the previous claims, further comprising a third compound comprising one or more of oxygen (O2), argon (Ar), helium (He), xenon (Xe), krypton (Kr), nitrogen (N2), octafluorocyclobutane (CdFs), hexafluorobutadiene (C4Fe), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1, 1, 3,3,3-pentafluoropropene (C3HF5), 1,1, 1,3,3, 3-hexafluoro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2FeO), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3).

8. The gas phase mixture according to claim 7, wherein the third compound comprises greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture, and wherein the first compound, the second compound, and the third compound comprise 100% by volume of the gas phase mixture.Attorney Docket No. P25-175-PRI-US019. A method of etching a thin film of an integrated circuit material, comprising:contacting a surface of the thin film of the integrated circuit material with a plasma comprising reactive ions generated by subjecting a gas phase mixture configured to etch the thin film of the integrated circuit material to a plasma generating device, thereby removing a portion of the thin film of the integrated circuit material;wherein the gas phase mixture comprises a first compound comprising:N - ( - F / \Br — Fp p1 -Bromo- 1, l-difluoro-A,A-bis(trifluoromethyl)methanamine; anda second compound comprising one or more of: oxygen (O2), argon (Ar), helium (He), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1, 1, 3,3,3- pentafluoropropene (C3HF5), 1,1, 1,3,3, 3-hexafhioro-2-methoxy-2- (trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2- (fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3).

10. The method according to claim 9, wherein the thin film comprises silicon, polysilicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, tungsten, tungsten silicide, a carbon hard mask, a photoresist material, and combinations thereof.Attorney Docket No. P25-175-PRI-US0111. The method according to claim 9 or claim 10, wherein the first compound comprises greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture.

12. The method according to claim 11, wherein the second compound comprises greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture, and wherein the first compound and the second compound comprise 100% by volume of the gas phase mixture.

13. The method according to claim 12, wherein a ratio of the first compound to the second compound is between 5:1 and 1:5.

14. The method according to any one of claims 9 to 13, wherein the second compound comprises octafluorocyclobutane (C4F8) or hexafluorobutadiene (C4F6).

15. The method according to any one of claims 9 to 14, further comprising a third compound comprising one or more of: oxygen (O2), argon (Ar), helium (He), xenon (Xe), krypton (Kr), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1,1, 3, 3, 3 -pentafluoropropene (C3HF5), 1, 1,1, 3,3,3-hexafluoro-2 -methoxy -2-(trifluoromethyl)propane (C5H3F9O), 1, 1,3,3, 3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3).

16. The method according to claim 15, wherein the third compound comprises greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture, and wherein the first compound, the second compound, and the third compound comprise 100% by volume of the gas phase mixture.Attorney Docket No. P25-175-PRI-US0117. The method according to any one of claims 9 to 16, wherein the thin film comprises a first film and a second film.

18. The method according to claim 17, wherein the first film and the second film each independently comprise silicon, silicon dioxide, silicon nitride, polysilicon, or a masking material.

19. The method according to claim 18, wherein the first film comprises silicon dioxide and the second film comprises silicon nitride, and the gas phase mixture has an etch selectivity for silicon dioxide compared to silicon nitride of greater than or equal to about 1.

20. The method according to claim 18, wherein the first film comprises silicon dioxide or silicon nitride and the second film comprises a masking material, and the gas phase mixture has an etch selectivity for silicon dioxide compared to the masking material of greater than or equal to about 1 or the gas phase mixture has an etch selectivity for silicon nitride compared to the masking material of greater than or equal to about 1.

21. The method according to claim 20, wherein the masking material comprises poly silicon, a metal mask, a carbon hard mask, or a photoresist material.

22. A method of patterning a thin film of integrated circuit material, comprising:contacting a surface of the thin film with a plasma comprising reactive ions generated by subjecting a gas phase mixture configured to etch the thin film of the integrated circuit material to a plasma generating device, thereby removing a portion of the thin film and generating a pattern in the thin film of the integrated circuit material,wherein at least a portion of the thin film is disposed between confronting surfaces of a substrate and a masking material layer, wherein the masking material layer comprises an aperture defined therein exposing a portion of the surface of the thin film; andwherein the gas phase mixture comprises a first compound comprising:Attorney Docket No. P25-175-PRI-US011 -Bromo- 1, I -di fl uoro-N,Af-bi s(tri fluoromethyl )methan amine; anda second compound comprising one or more of: oxygen (O2), argon (Ar), helium (He), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1, 1, 3,3,3- pentafhroropropene (C3HF5), 1,1, 1,3,3, 3-hexafhroro-2-methoxy-2- (trifluoromethyl)propane (C5H3F9O), 1, 1,3,3, 3-pentafluoro-2- (fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3).

23. The method according to claim 22, wherein the substrate is selected from the group consisting of silicon, silicon oxide, silicon dioxide, silicon nitride, tantalum, tantalum nitride, titanium nitride, aluminum oxide, copper, tungsten carbonitride, molybdenum, polysilicon, a carbon hard mask, a photoresist material, and a combination thereof.

24. The method according to claim 22 or claim 23, wherein the thin film comprises silicon, silicon oxide, silicon dioxide, silicon carbide, silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, gallium nitride, aluminum gallium nitride, gallium arsenide, aluminum gallium arsenide, indium phosphide, indium aluminum arsenide, indium gallium arsenide, silicon germanium, silicon hydrogen bromide, zinc selenide, indium tin oxide, lead zirconium titanate, molybdenum, polysilicon, tungsten, tungsten silicide, a carbon hard mask, a photoresist material, and combinations thereof.Attorney Docket No. P25-175-PRI-US0125. The method according to any one of claims 22 to 24, wherein the first compound comprises greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture.

26. The method according to claim 25, wherein the second compound comprises greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture, and wherein the first compound and the second compound comprise 100% by volume of the gas phase mixture.

27. The method according to claim 26, wherein a ratio of the first compound to the second compound is between 5:1 and 1:5.

28. The method according to any one of claims 22 to 27, wherein the second compound comprises octafluorocyclobutane (C4F8) or hexafluorobutadiene (C4F6).

29. The method according to any one of claims 22 to 28, wherein the masking material comprises polysilicon, a metal mask, a carbon hard mask, or a photoresist material.

30. The method according to any one of claims 22 to 29, further comprising a third compound comprising one or more of: oxygen (O2), argon (Ar), helium (He), xenon (Xe), krypton (Kr), nitrogen (N2), octafluorocyclobutane (C4F8), hexafluorobutadiene (C4F6), carbonyl fluoride (COF2), difluoromethane (CH2F2), trifluoromethane (CHF3), carbon tetrafluoride (CF4), methyl fluoride (CH3F), octafluorocyclopentene (CsFs), 2,3,3,3-tetrafluoropro-l-ene (C3H2F4), hexafluoropropene (C3F6), hexafluorocyclopropane (C3F6), 1, 1, 3,3,3-pentafhroropropene (C3HF5), 1,1, 1,3,3, 3-hexafhroro-2-methoxy-2-(trifluoromethyl)propane (C5H3F9O), l,l,3,3,3-pentafluoro-2-(fluoromethoxy)prop-l-ene (C4H2F6O), sulfur hexafluoride (SFe), and nitrogen trifluoride (NF3).

31. The method according to claim 30, wherein the third compound comprises greater than or equal to about 1% by volume of the gas phase mixture, and less than or equal to about 99% by volume of the gas phase mixture, and wherein the firstAttorney Docket No. P25-175-PRI-US01compound, the second compound, and the third compound comprise 100% by volume of the gas phase mixture.

32. The method according to any one of claims 22 to 31, wherein the thin film comprises silicon dioxide or silicon nitride and the gas phase mixture has an etch selectivity for the thin film to the masking material of greater than or equal to about 1.

33. The method according to any one of claims 22 to 31, wherein the thin film comprises a first film and a second film.

34. The method according to claim 33, wherein the first film and the second film each independently comprise silicon, silicon dioxide, silicon nitride, polysilicon, or a masking material.

35. The method according to claim 34, wherein the first film comprises silicon dioxide and the second film comprises silicon nitride, and the gas phase mixture has an etch selectivity for silicon dioxide compared to silicon nitride of greater than or equal to about 1.

36. The method according to claim 34, wherein the first film comprises silicon dioxide or silicon nitride and the second film comprises a masking material, and the gas phase mixture has an etch selectivity for silicon dioxide compared to the masking material of greater than or equal to about 1 or the gas phase mixture has an etch selectivity for silicon nitride compared to the masking material of greater than or equal to about 1.

37. The method according to claim 36, wherein the masking material comprises poly silicon, a metal mask, a carbon hard mask, or a photoresist material.

38. A process for making l-Bromo-l,l-difluoro-A,A-bis(trifluorom ethyl) methanamine, comprising:reacting bis(trifluoromethyl)amide anion with dibromodifluoromethane in the presence of atrimethyl(trifhioromethyl)silane catalyst to provide l-Bromo-1,1-difluoro-7V,7V-bis(trifluoromethyl)methanamine.Attorney Docket No. P25-175-PRI-US0139. The process according to claim 38, further comprising reacting 7V,7V-bis(trifluoromethyl)trifluoromethanesulfonamide with potassium fluoride to provide the bis(trifluoromethyl)amide anion.

40. The process according to claim 39, wherein 7V,7V-bis(trifluoromethyl)trifluoromethanesulfonamide is reacted with potassium fluoride at a temperature in a range from about -70°C to about 40°C, preferably at about -10°C.

41. The process according to any one of claims 37 to 40, wherein dimethylacetamide is the solvent in the one or more reacting steps.

42. The process according to any one of claims 37 to 41, wherein bis(trifluoromethyl)amide anion is reacted with dibromodifluoromethane at a temperature in a range from about -50°C to about 50°C, preferably at about 0°C.

43. The process according to any one of claims 37 to 42, further comprising adding dropwise the trimethyl(trifluoromethyl)silane catalyst to a solution of the bis(trifluoromethyl)amide anion and dibromodifluoromethane.

44. The process of according to any one of claims 37 to 43, further comprising recovering the l-Bromo-l,l-difluoro-7V,7V-bis(trifluoromethyl)methanamine formed from the reaction of bis(trifluoromethyl)amide anion and dibromodifluoromethane via condensation.

45. The process of claim 44, further comprising purifying the condensate via spinning band distillation.