Photovoltaic cell, in particular a thin-film photovoltaic cell, and method for manufacturing a photovoltaic cell
A photovoltaic cell with a semiconductor layer of metal oxide nanoparticles in a polymeric matrix enhances mechanical strength and resistance to delamination, addressing the limitations of existing thin-film cells with cost-effective and efficient manufacturing.
Patent Information
- Application Number
- PCT/IB2026/054536
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing thin-film photovoltaic cells face issues with limited fracture energy leading to layer delamination and mechanical failure, particularly during laser ablation, which existing solutions like Atomic Layer Deposition and reinforcement structures are costly, complex, or reduce active surface area.
A photovoltaic cell design with a semiconductor layer composed of metal oxide nanoparticles embedded in a polymeric reinforcing matrix, using low-cost deposition techniques like screen printing, to enhance interfacial resistance and mechanical strength without reducing efficiency.
The solution significantly improves fracture toughness and lamination resistance, reducing the risk of delamination while maintaining efficiency, and is cost-effective with simpler manufacturing processes.
Smart Images

Figure IB2026054536_12112026_PF_FP_ABST
Abstract
Description
[0001] TRANSLATION (RULE 12.3)
[0002] 05 June 2026
[0003] PHOTOVOLTAIC CELL, IN PARTICULAR A THIN-FILM PHOTOVOLTAIC CELL, AND METHOD FOR MANUFACTURING A PHOTOVOLTAIC CELL DESCRIPTION
[0004] Field of Application
[0005] The present invention relates to a photovoltaic cell, in particular a thin-film photovoltaic cell, and a method for manufacturing a photovoltaic cell, according to the preamble of the respective independent claims.
[0006] The photovoltaic cell in question is intended to be connected in series with other photovoltaic cells to form a photovoltaic module adapted to convert solar radiation into electrical energy.
[0007] Therefore, the photovoltaic cell which is the subject of the present invention and the method for manufacturing a photovoltaic cell fall within the field of manufacturing modules for photovoltaic plants.
[0008] State of the Art
[0009] As is known, a photovoltaic module is composed by multiple photovoltaic cells connected in series, which are capable of converting light radiation from the sun into electrical energy.
[0010] In particular, a photovoltaic cell comprises a light-absorbing layer, generally made of a semiconductor material, interposed between a positive electrode and a negative electrode, which allow the generated electric current to flow.
[0011] The photovoltaic cells most widely used on the market in recent decades feature a crystalline silicon absorber layer, fabricated as a wafer, which has a thickness ranging from 100 to 200 pm.
[0012] In order to minimize the amount of material used to create the absorber layer, thin-film photovoltaic cells have been developed, which are provided with an absorber layer provided with a thickness ranging from tens of nanometers to a few micrometers.
[0013] In particular, the absorber layer of the aforementioned thin-film photovoltaic cells can be made of amorphous silicon, cadmium telluride, copper-indium-gallium selenide, gallium arsenide, perovskite, etc.
[0014] Such thin-film photovoltaic cells comprise a substrate of transparent material, for example glass, on which a first layer of conductive material forming a first electrode (positive or negative), the absorber layer and a second layer of conductive material forming a second electrode (of opposite polarity to the first electrode) are sequentially arranged.
[0015] Furthermore, known photovoltaic cells generally comprise additional semiconductor layers arranged respectively between the first electrode and the photo-active layer and between the photo-active layer and the second electrode.
[0016] These semiconductor layers serve to transport charges and generally consist of metal oxide nanoparticles.Furthermore, the first electrode of a photovoltaic cell is generally connected to the second electrode of the next photovoltaic cell, thereby forming a series of photovoltaic cells that produces a higher voltage across its terminals than individual cells, in order to increase the voltage generated by the photovoltaic module and thus reduce its resistive losses.
[0017] The photovoltaic cells described above have proven, in practice, to be not without drawbacks.
[0018] The main drawback lies in the fact that some layers of the cell have a limited fracture energy, as described in particular for perovskite cells by Rolston N. et al. in “Mechanical integrity of solution-processed perovskite solar cells” Extreme Mechanics Letters 9.3 (2016), 353-358.
[0019] The fracture of the layer with the lowest fracture energy leads to delamination of the layers, i.e. their mechanical separation, resulting in the overall failure of the entire photovoltaic cell.
[0020] Specifically, in photovoltaic cells where a semiconductor layer made of nanoparticles is present between the photo-active layer and the second (top) electrode, it has been observed that this semiconductor layer is the most fragile and prone to fracture.
[0021] This issue is most pronounced when the interconnections between photovoltaic cells are monolithic P1-P2-P3 interconnections that involve the laser ablation of one or more layers of the photovoltaic cell itself.
[0022] In fact, laser ablation at P3 removes part of the second electrode, causing, if the layers are not sufficiently cohesive (low interfacial tension resistance) and mechanically stable, local delamination that acts as the initial point of failure for the entire cell. In other words, laser ablation can generate one or more unwanted cracks, which can propagate upon the application of even minimal stress on the photovoltaic cell.
[0023] Consequently, several methods have been developed in the industry to increase the strength of this layer, in order to reduce the risk of premature failure of the photovoltaic cell.
[0024] For example, the process described by Bristow H. et al. in “Mitigating Delamination in Perovskite / Silicon Tandem Solar Modules,” Sol. RRL, 8 (2024), 2400289, involves using a technique called Atomic Layer Deposition (ALD) to deposit the semiconductor layer and the second electrode in a way that increases fracture toughness and interfacial strength.
[0025] However, this latter process has also proven to be not without drawbacks, foremost among which is the fact that the used technique is much more expensive than previously known techniques for the deposition of the nanoparticles of the semiconductor layer.
[0026] Furthermore, another drawback lies in the fact that the Atomic Layer Deposition usable to deposit this semiconductor layer requires specific procedural modifications compared to standard ALD, increasing the complexity of the process.
[0027] Another method is also known, described by Watson B. L. et al. in “Scaffold-reinforced perovskite compound solar cells,” Energy Environ. Sci., 10 (2017), 2500-2508, which involves reinforcing thesemiconductor layer with a planar honeycomb reinforcement structure, which defines hexagonal cells within which the nanoparticles are deposited.
[0028] However, even in this latter case, certain drawbacks have been observed.
[0029] A primary drawback lies in the fact that the reinforcement structure significantly reduces the active surface area of the semiconductor layer and thus of the entire device, as part of the surface is occupied by this very structure, which has insulating properties.
[0030] Another drawback is that the fabrication of the reinforcement structure is particularly time-consuming and labor-intensive, requiring a dedicated step for the deposition of the structure, for example, via lithography, followed by the deposition of the nanoparticles.
[0031] Overall, therefore, the solutions listed above are structurally invasive or require particularly complex, labor-intensive, and costly processes for manufacturing the photovoltaic cell itself.
[0032] Presentation of the Invention
[0033] In this context, the problem underlying the present invention is therefore to overcome the drawbacks exhibited by known photovoltaic cells by providing a photovoltaic cell and a method for manufacturing a photovoltaic cell that allow for an increase in the fracture toughness of the photovoltaic cell itself in a simple and cost-effective manner.
[0034] A further objective of the present invention is to provide a photovoltaic cell in which the interfacial resistance between the layers of the structure is greater than in known photovoltaic cells.
[0035] A further object of the present invention is to provide a photovoltaic cell that is durable and provided with reduced degradation over time.
[0036] A further objective of the present invention is to provide a photovoltaic cell and a method for manufacturing a photovoltaic cell that allow for an increase in the mechanical strength of the photovoltaic cell itself without reducing its efficiency.
[0037] Brief Description of the Drawings
[0038] The technical features of the invention, in accordance with the aforementioned objectives, are clearly evident from the content of the claims set forth below and the advantages thereof will become more apparent in the detailed description that follows, made with reference to the attached drawings, which represent some purely illustrative and non-limiting embodiments, wherein:
[0039] - Figure 1 shows a simplified schematic cross-sectional view of a photovoltaic cell that is the subject of the present invention in accordance with a preferred embodiment;
[0040] - Figure 2 shows an illustrative schematic view of a semiconductor layer of the photovoltaic cell; - Figure 3 shows a graph comparing the conversion efficiency between a photovoltaic cell according to a first exemplary embodiment of the present invention and a photovoltaic cell according to a control example;
[0041] - Figure 4 shows a graph comparing the lamination resistance properties between a photovoltaiccell according to the first exemplary embodiment of the present invention and a photovoltaic cell according to the control example;
[0042] - Figures 5a-c show top views under a scanning electron microscope of a photovoltaic cell according to the control example, a photovoltaic cell according to the first exemplary embodiment, and a photovoltaic cell according to a second exemplary embodiment of the present invention subjected to laser ablation.
[0043] Detailed Description of a Preferred Embodiment
[0044] With reference to the accompanying drawings, a photovoltaic cell, in particular a thin-film photovoltaic cell, according to the present invention is shown in its entirety as 1. Such photovoltaic cell 1 is advantageously intended to be connected in series with other photovoltaic cells 1 to form a photovoltaic module.
[0045] In particular, the photovoltaic module comprises multiple photovoltaic cells 1 connected in series in a conventional manner, such that the voltage across the series is equal to the sum of the voltages across the individual photovoltaic cells 1.
[0046] The photovoltaic cell 1 comprises a substrate 2 made of a material that is at least partially transparent and susceptible of being traversed by solar radiation, such as glass, transparent plastic, or transparent metal.
[0047] In particular, the substrate 2 is transparent to at least a part of the solar radiation.
[0048] Furthermore, the photovoltaic cell 1 also comprises a first electrode 3, which is at least partially transparent, disposed on the substrate 2 and susceptible of being traversed by solar radiation coming from the substrate 2.
[0049] Advantageously, the first electrode 3 is made of an electrically conductive material.
[0050] In particular, the first electrode 3 is transparent to at least a part of the solar radiation to which the material of the substrate 2 is transparent, such that at least a part of the solar radiation passing through the substrate 2 is also able to pass through the first electrode 3.
[0051] The photovoltaic cell 1 further comprises a photo-active layer 4, which is disposed on the first electrode 3 and is susceptible of receiving solar radiation for the generation of electric current.
[0052] More in detail, the photo-active layer 4 is provided with a first side 41, which is disposed on the first electrode 3 and is susceptible of receiving solar radiation, and an opposite second side 42, in particular facing in the opposite direction from the first side 41.
[0053] Advantageously, the photo-active layer 4 comprises a solar radiation-absorbing material, in particular a perovskite. For example, the absorbing material is a metal -halide hybrid perovskite.
[0054] More in detail, when the absorber material of the photo-active layer 4 is a metal-halide hybrid perovskite, the latter is a material with a perovskite crystal structure and the chemical formula ABX3, where:A is a cation preferably selected from: methylammonium (MA), formamidinium (FA), cesium (Cs), rubidium (Rb), potassium (K), or other monovalent cations, or a combination thereof;
[0055] B is a divalent metal, preferably selected from: lead (Pb), tin (Sn), or other divalent metals, or a combination thereof;
[0056] X is an anion, most commonly a halogen, preferably selected from: iodine (I), bromine (Br), chlorine (Cl), or a combination thereof.
[0057] Of course, without departing from the scope of the present invention, the photo-active layer 4 may be made of another absorber material, such as cadmium telluride (CdTe), or copper indium gallium selenide (CIGS), or amorphous silicon, or comprising a heterojunction of organic semiconductors, or III-V semiconductor materials, such as gallium arsenide.
[0058] The photovoltaic cell 1 also comprises a second electrode 5, which is disposed on the photo-active layer 4, in particular on the second side 42 of the photo-active layer 4. In particular, the second electrode 5 is arranged to be electrically connected to the first electrode 3 of a further photovoltaic cell connected in series with the photovoltaic cell 1.
[0059] In particular, this electrical series connection between two consecutive photovoltaic cells 1 is of a monolithic type, i.e. with the second and first electrodes 5, 3 in direct contact with each other, without the presence of electrical connectors, such as cables. This monolithic connection advantageously comprises, in a manner known per se, interruption openings Pl, P2 and P3.
[0060] More in detail, the interruption opening Pl is formed on the first electrode 3.
[0061] Advantageously, the P2 interruption opening is formed at least on the photo-active layer 4. Preferably, the P2 interruption opening is also formed on a semiconductor layer 6 (in particular interposed between the photo-active layer 4 and the second electrode 5), which will be described below. Preferably, the P2 aperture is also formed on an additional semiconductor layer 6’ (in particular interposed between the first electrode 3 and the photo-active layer 4), which will be described below.
[0062] Advantageously, the P3 interruption opening is formed at least on the second electrode 5. Preferably, the P3 interruption opening is also formed on the semiconductor layer 6. Preferably, the P3 interruption opening is also formed on the photo-active layer 4. Preferably, the P3 interruption opening is also formed on the additional semiconductor layer 6’. Therefore, the P3 interruption opening is advantageously formed on all layers except for the second electrode 5.
[0063] Advantageously, the first electrode 3 of a photovoltaic cell 1 is electrically connected to the second electrode 5 of a subsequent photovoltaic cell 1, and preferably, the second electrode 5 of the same photovoltaic cell 1 is electrically connected to the first electrode 3 of a preceding photovoltaic cell 1, to achieve the series connection of the photovoltaic cells 1 of a photovoltaic module.
[0064] Advantageously, the second electrode 5 is made of an electrically conductive material and,preferably, is at least partially transparent, for example in the case where the photovoltaic cell 1 is of the semi-transparent or bifacial type.
[0065] Preferably, the second electrode 5 is preferably formed at least partially, for example at least at 70%, by means of sputtering coating. The photovoltaic cell 1 preferably comprises at least one semiconductor layer 6 interposed between the second electrode 5 and the photo-active layer 4, in particular positioned to connect the latter.
[0066] Advantageously, the photovoltaic cell 1 further comprises at least one additional semiconductor layer 6’ interposed between the first electrode 3 and said photo-active layer 4, in particular positioned in connection between the latter.
[0067] In particular, the aforementioned substrate 2, first electrode 3, photo-active layer 4, semiconductor layer 6, additional semiconductor layer 6’, and second electrode 5 are deposited one on top of the other, forming a layered structure of a type known per se.
[0068] Obviously, without departing from the scope of the present invention, further intermediate layers may be provided between those described above.
[0069] Advantageously, the photovoltaic cell 1 extends predominantly in a thin shape on its own lying plane and is provided with a perimeter edge that delimits its extent on said lying plane.
[0070] Advantageously, each photovoltaic cell 1 extends (preferably in an elongated shape) along an extension direction and extends, transversely to that extension direction, between a first side and a second side, each of which, in particular, is flanked by the corresponding photovoltaic cell 1 of the module.
[0071] One of the two electrodes 3, 5 forms the negative electrode N of the photovoltaic cell 1, while the other forms the positive electrode P of the same photovoltaic cell 1.
[0072] In particular, the negative electrode N and positive electrode P refer to the polarization of the first and second electrodes 3, 5 during normal operation of the photovoltaic cell 1, when the latter is irradiated by solar radiation and produces electrical energy, and is therefore directly polarized.
[0073] More in detail, one of the semiconductor layers 6 and the additional semiconductor layer 6’ is selective for negative charges, i.e., it is arranged to extract electrons (Electron-Transporting Layer, ETL) from the absorber material, and is advantageously positioned at the negative N electrode.
[0074] In particular, one of the semiconductor layers 6 and the additional semiconductor layer 6’ is selective for positive charges, i.e., it is arranged to extract holes (Hole-Transporting Layer, HTL) from the absorber material and is advantageously positioned at the positive electrode P.
[0075] In accordance with the preferred embodiment of the invention, illustrated for example in Figure 1, the photovoltaic cell 1 has a p-i-n structure, in which the first electrode 3 is the positive electrode P and the second electrode 5 is the negative electrode N. Therefore, the semiconductor layer 6 is advantageously selective for negative charges. Advantageously, the additional semiconductor layer 6’is selective for positive charges.
[0076] Differently, according to an alternative embodiment (not shown), the photovoltaic cell 1 has an n-i- p structure, in which the first electrode 3 is the negative N electrode and the second electrode 5 is the positive P electrode. Therefore, in this case, the semiconductor layer 6 is advantageously selective for positive charges. Advantageously, furthermore, the additional semiconductor layer 6’ is selective for negative charges.
[0077] In particular, in a manner that is conventional in itself, the polarity of the first and second electrode 3, 5 (when the photovoltaic cell 1 generates electrical energy) is given by the nature of the photo-active layer 4 and the arrangement of the semiconductor layers 6, 6’, which determine the direction of the current generated by the photo-active layer 4 when the latter is irradiated by solar radiation.
[0078] Functionally, when the photo-active layer 4 is irradiated by solar radiation, the photovoltaic cell 1 is directly polarized and produces electrical energy.
[0079] More in detail, referring for example to Figure 1, which represents a cross-section of a photovoltaic cell 1 with a p-i-n structure, when the photovoltaic cell 1 is exposed to solar radiation, it becomes directly polarized. In particular, electric current flows from the negative N-electrode (which, in the preferred embodiment illustrated in Figure 1, is the second electrode 5) to the opposite positive P electrode (which, in the preferred embodiment illustrated in Figure 1, is the first electrode 3) of the same photovoltaic cell 1 through the photo-active layer 4 and the semiconductor layers 6, 6’.
[0080] In accordance with the idea underlying the present invention, the semiconductor layer 6 is made of a composite material that comprises nanoparticles 7, made of at least one metal oxide, and a reinforcing matrix 8, in which the nanoparticles 7 are partially embedded.
[0081] In particular, the reinforcing matrix 8 is made of a polymeric material comprising a plurality of polymer chains 80 arranged at least in partial interconnection between the nanoparticles 7. Preferably, the polymeric material is an insulating polymer.
[0082] More in detail, as schematically illustrated by way of example in Figure 2, the polymer chains 80 do not completely embed the nanoparticles 7 and, in particular, define only an interconnecting network that allows for an increase in the strength of the semiconductor layer 6.
[0083] The term “interconnection” is to be understood as a connection that is substantially mechanical in nature, which does not involve the formation of strong chemical bonds (e.g., covalent bonds) between the polymer chains 80 and the nanoparticles 7.
[0084] It was surprisingly found that, in order to ensure the proper electrical functionality of the semiconductor layer 6 while also ensuring sufficient strength, the polymeric material must be present in an amount equal to or less than 10% by weight relative to the weight of the nanoparticles 7, preferably with a minimum amount of 0.01% by weight relative to the weight of the nanoparticles 7. Above this value, in fact, no mechanical benefits are observed, while the efficiency of thephotovoltaic cell 1 drops drastically, as the nanoparticles 7 begin to be increasingly embedded in the insulating reinforcing matrix 8, losing their functionality.
[0085] Advantageously, the polymeric material of the reinforcing matrix 8 is present in the semiconductor layer 6 in an amount between 0.01 to 5% by weight relative to the weight of the nanoparticles 7, preferably between 0.01 to 3% by weight, more preferably between 0.1 to 3% by weight, and even more preferably between 0.1 to 1% by weight.
[0086] In this way, it is possible to easily obtain a semiconductor layer 6, and thus a photovoltaic cell 1, with greater resistance than known photovoltaic cells, significantly reducing the risk of delamination. At the same time, the photovoltaic cell 1 according to the invention advantageously exhibits the same efficiency as known photovoltaic cells.
[0087] In particular, the structure of the semiconductor layer 6 of the photovoltaic cell 1 according to the invention surprisingly allows to reduce the probability that subsequent processing steps, such as sputtering coating of the second electrode 5 and / or laser ablation (as will be seen below), generate cracks or delamination in the semiconductor layer 6 itself due to the introduction of mechanical stresses between the layers.
[0088] Furthermore, the photovoltaic cell 1 according to the invention offers an advantageous reduction in manufacturing time and costs, since, as will be described below, it can be produced substantially using well-known, low-cost techniques, such as screen printing, spin coating, blade coating, and slot die coating, and substantially without the addition of complex additional steps.
[0089] Furthermore, the photovoltaic cell 1 according to the invention advantageously does not require chemical modifications to the nanoparticles 7 and does not alter their properties, making the production process simpler and less expensive.
[0090] According to a preferred embodiment, the nanoparticles have an average diameter between 1 and 80 nm, preferably between 3 and 50 nm.
[0091] More in detail, the nanoparticles 7 are made of at least one semiconductor metal oxide having a bandgap equal to or greater than 2 eV; i.e., in other words, they advantageously possess the characteristics of a wide-bandgap semiconductor.
[0092] Preferably, the semiconductor metal oxide has a work function similar to the conduction band of the photo-active layer 4, i.e., for example, approximately 4 eV, so as to function as an Electron-Transporting Layer (ETL), in particular in the case where the second electrode 5 is the negative N electrode.
[0093] More in detail, the metal oxide semiconductor is a compound defined by the chemical formula MxOy, where M is a metal element and O is oxygen.
[0094] In particular, the aforementioned metal oxide semiconductor is selected from: tin oxide, titanium oxide, zinc oxide, magnesium oxide, niobium oxide.Advantageously, the semiconductor metal oxide may also contain dopants, such as heteroatoms capable of modifying its work function and electrical conductivity. For example, if the metal oxide is zinc oxide, the latter may be doped with aluminum atoms.
[0095] According to a preferred embodiment, the polymer chains 80 of the polymeric material have an average length equal to or greater than three times the diameter of the nanoparticles 7.
[0096] Furthermore, advantageously, the polymer chains 80 of the polymeric material have an average molecular weight equal to or greater than 2000 Da, preferably equal to or greater than 5000 Da, more preferably equal to or greater than 10000 Da, and even more preferably equal to or greater than 20000 Da.
[0097] In this way, it is possible to ensure optimal strength for the semiconductor layer 6. Below a critical value of 2000 Da for the average molecular weight, the strength is still improved, although this property decreases as the molecular weight itself decreases.
[0098] Preferably, the polymeric material of the reinforcing matrix 8 is selected from: polyvinyl alcohol, polyethyleneamine, polyvinylpyrrolidone, poly(sodium 4-styrenesulfonate), poly(n-isopropylacrylamide), sodium polyacrylate, polymethyl methacrylate, polystyrene, and mixtures or copolymers thereof.
[0099] It has in fact been found that the aforementioned polymers or classes of polymers allow for the best performance to be achieved in combination with ease of use in the fabrication of the photovoltaic cell 1, for example by a method described below, which involves dissolving the polymeric material in the same solvent in which the nanoparticles 7 are dispersed.
[0100] Therefore, advantageously, the polymeric material comprises carbon-based macromolecules (polymer chains) with functional groups to make it compatible with the nanoparticles 7 and with the solvent in which they are dispersed.
[0101] In particular, in the case of a polar solvent, such as water, alcohols (ethanol, isopropanol or butanol), or acetone, the polymeric material comprises functional groups formed by heteroatom groups that form dipoles. For example, such functional groups may be hydroxyl, imine, pyrrolyl, sulfonate, acrylamide, or acrylate groups.
[0102] In this case, therefore, the polymeric material is advantageously selected from: polyvinyl alcohol, polyethyleneamine, polyvinylpyrrolidone, poly(sodium 4-styrenesulfonate), poly(n-isopropylacrylamide), sodium polyacrylate, and mixtures or copolymers thereof.
[0103] Furthermore, in the case of a nonpolar solvent, such as toluene, xylene or anisole, the polymeric material comprises functional groups characterized by low dipole moments. For example, such functional groups may be alkyl, benzene, or acrylate groups.
[0104] In such a case, therefore, the polymeric material is advantageously selected from: polymethyl methacrylate, polystyrene, and mixtures or copolymers thereof.Obviously, without departing from the scope of the present invention, it is possible to use any other polymeric material, preferably an insulating polymer, that allows for an increase in the mechanical strength of the semiconductor layer 6 without significantly altering its electronic properties.
[0105] As indicated above, in accordance with the preferred embodiment of the invention, the second electrode 5 is arranged to be electrically connected to the first electrode 3 of a further photovoltaic cell connected in series to the photovoltaic cell 1 by means of a monolithic electrical connection. In this case, an interruption opening P3 is preferably formed on the second electrode 5 itself, in particular by means of laser ablation.
[0106] Furthermore, the interruption opening P3 is also advantageously formed on the semiconductor layer 6.
[0107] In particular, thanks to the semiconductor layer 6 according to the invention, the resistance of the photovoltaic cell 1, even when treated with laser ablation, is significantly improved.
[0108] The following describes some mechanical and efficiency tests performed on certain exemplary embodiments of the present invention.
[0109] In accordance with a first exemplary embodiment of the present invention, the photovoltaic cell 1 comprises a glass substrate 2, a first electrode 3 made of fluorine-doped tin oxide, which acts as the positive electrode, a photo-active layer 4 made of a metal-halide hybrid perovskite, and a second electrode 5 made of indium tin oxide, which acts as the negative electrode.
[0110] Furthermore, the photovoltaic cell 1 according to the first exemplary embodiment comprises two adjacent semiconductor layers 6 with an ETL function, interposed between the photo-active layer 4 and the second electrode 5, of which a first semiconductor layer comprising a C60 fullerene derivative, and a second semiconductor layer comprising nanoparticles 7 of aluminum-doped zinc oxide in a reinforcing matrix 8 of polyvinylpyrrolidone with an average molecular weight of 40 kDa. In particular, the polyvinylpyrrolidone is present in an amount equal to 1% by weight relative to the weight of the nanoparticles 7.
[0111] Furthermore, the photovoltaic cell 1 according to the first exemplary embodiment comprises an additional semiconductor layer 6’ with an HTL function, which is interposed between the photoactive layer 4 and the first electrode 3 and is a p-type high-bandgap semiconductor.
[0112] In accordance with a second exemplary embodiment of the present invention, the photovoltaic cell 1 comprises a glass substrate 2, a first electrode 3 made of fluorine-doped tin oxide, which serves as the positive electrode, a photo-active layer 4 made of a metal-halide hybrid perovskite, and a second electrode 5 made of indium tin oxide, which serves as the negative electrode.
[0113] Furthermore, the photovoltaic cell 1 according to the second exemplary embodiment comprises two adjacent semiconductor layers 6 with an ETL function, interposed between the photo-active layer 4 and the second electrode 5, of which a first semiconductor layer comprising a C60 fullerenederivative, and a second semiconductor layer comprising nanoparticles 7 of aluminum-doped zinc oxide in a reinforcing matrix 8 of polyvinylpyrrolidone with an average molecular weight of 40 kDa. In particular, the polyvinylpyrrolidone is present in an amount equal to 3% by weight relative to the weight of the nanoparticles 7.
[0114] Furthermore, the photovoltaic cell 1 according to the second exemplary embodiment comprises an additional semiconductor layer 6’ with an HTL function, which is interposed between the photoactive layer 4 and the first electrode 3 and is a p-type high-bandgap semiconductor.
[0115] In accordance with a control example, which is not the subject of the present invention, the photovoltaic cell 1 comprises a glass substrate 2, a first electrode 3 made of fluorine-doped tin oxide, which serves as the positive electrode, a photo-active layer 4 made of a metal-halide hybrid perovskite, and a second electrode 5 made of indium tin oxide, which serves as the negative electrode.
[0116] Furthermore, the photovoltaic cell 1 according to the control example comprises two adjacent semiconductor layers 6 with an ETL function, interposed between the photo-active layer 4 and the second electrode 5, of which a first semiconductor layer comprising a derivative of fullerene C60, and a second semiconductor layer comprising only aluminum-doped zinc oxide nanoparticles 7.
[0117] Furthermore, the photovoltaic cell 1 according to the control example comprises an additional semiconductor layer 6’ with an HTL function, which is interposed between the photo-active layer 4 and the first electrode 3 and is a p-type high-bandgap semiconductor.
[0118] The characteristics of the examples described above are abstracted in Table 1 below.
[0119] For each example, multiple photovoltaic cells 1 were connected in series via monolithic interconnections P1-P2-P3 to form a photovoltaic module. The resulting photovoltaic modules were then subjected to measurement of their initial power conversion efficiency.
[0120] Subsequently, each module was laminated using a vacuum lamination process with a polyolefin as the encapsulant and glass as the barrier.
[0121] Table 1 - Layers, in construction sequence, of the photovoltaic cells according to the examples used in the resistance and efficiency tests
[0122]
[0123]
[0124] The lamination process, in particular, was carried out first by placing the photovoltaic module between two layers of encapsulant and on the barrier layer, then heating it to 110 °C, followed by applying a vacuum (or low pressure to evacuate the air), and finally pressing at 1 atm for a minimum of 10 minutes, while maintaining the same temperature of 110 °C.
[0125] Following lamination, the resulting laminated photovoltaic modules were subjected once again to measurement of their final power conversion efficiency.
[0126] The initial power conversion efficiency for the photovoltaic module according to the first implementation example and the comparison example is shown in the graph in Figure 3.
[0127] From this graph, it can be seen that the presence of the reinforcing matrix does not affect the performance of the resulting photovoltaic module.
[0128] Furthermore, the percentage difference between the initial efficiency (before lamination) and the final efficiency (after lamination) for the photovoltaic module according to the first implementation example and the comparison example is shown in the graph in Figure 4.
[0129] From this graph, it can be seen that the presence of the reinforcing matrix 8 in the semiconductor layer advantageously improves lamination resistance, reducing the risk of defects forming in the material.
[0130] Furthermore, the photovoltaic cells obtained from the examples described above were subjected to laser ablation tests of the second electrode 5 to assess the risk of layer delamination and crack formation. The scanning electron microscope images of the ablation lines, obtained for each example with different pulse energies and pulse densities, are shown in Figure 5a-c.
[0131] From this image, it can be observed that as the amount of polymeric material in the semiconductor layer 6 increases, the resistance to delamination also increases. In fact, delamination of the layers is indicated by the presence of a white area around the ablation points, and this is clearly reduced significantly with the addition of the polymeric material of the reinforcing matrix 8.
[0132] The object of the present invention also relates to a method for manufacturing a photovoltaic cell 1, preferably of the type described above, for which the numerical references will be maintained for thesake of simplicity.
[0133] This method comprises a step of arranging a substrate 2 made of at least partially transparent material, a first deposition step, in which a first electrode 3, which is at least partially transparent, is deposited on the substrate 2, and a second deposition step, in which a photo-active layer 4 is deposited on the first electrode 3.
[0134] The method in question further comprises a third deposition step, in which a semiconductor layer 6 is deposited on the photo-active layer 4, and a fourth deposition step, in which a second electrode 5 is deposited on the semiconductor layer 6.
[0135] Preferably, the method in question further comprises an intermediate deposition step, performed between the first deposition step and the second deposition step, in which an additional semiconductor layer 6’ is deposited on the first electrode 3. Therefore, in the second deposition step, the photo-active layer 4 is deposited on the additional semiconductor layer 6’.
[0136] Therefore, within the scope of the present invention, the expression “deposited on” may obviously mean either that the layer is in direct contact with the layer indicated subsequently, or that the layer is arranged indirectly above it, i.e., not necessarily in contact, as intermediate layers may be provided. In particular, the aforementioned deposition steps, with the exception of the third deposition step, may involve known deposition techniques, such as screen printing, spin coating, blade coating, slot die coating, thermal evaporation, sputtering coating, chemical vapor deposition (CVD), atomic layer deposition (ALD), close-space sublimation, pulsed laser deposition (or reactive plasma deposition), or physical or chemical depositions, or even techniques that ensure high precision in the definition of each layer and uniformity across the entire deposition area of the layer itself.
[0137] Preferably, at least the second electrode 5 in the fourth deposition step is formed at least partially, for example at least at 70%, by sputtering coating.
[0138] In particular, the semiconductor layer 6 obtained in the third deposition step, which will be described more in detail below, surprisingly allows for an increase in the cell’s strength while reducing the likelihood that the mechanical stresses introduced by the sputtering coating will cause cracks or delamination in the semiconductor layer 6 itself.
[0139] More in detail, the aforementioned deposition techniques can be employed either individually or in combination with one another.
[0140] Advantageously, the definition of each layer can be achieved by selective deposition of the layer itself or by selective removal, for example through laser devices or mechanical ablation.
[0141] Advantageously, the photo-active layer 4 comprises a material that absorbs solar radiation, in particular a perovskite. For example, the absorbing material is a metal-halide hybrid perovskite. More in detail, when the absorber material of the photo-active layer 4 is a metal-halide hybrid perovskite, the latter is a material with a perovskite crystal structure and the chemical formula ABX3,where:
[0142] A is a cation preferably selected from: methylammonium (MA), formamidinium (FA), cesium (Cs), rubidium (Rb), potassium (K), or other monovalent cations, or a combination thereof;
[0143] B is a divalent metal, preferably selected from one of: lead (Pb), tin (Sn), or other divalent metals, or a combination thereof;
[0144] X is an anion, most commonly a halogen, preferably selected from: iodine (I), bromine (Br), chlorine (Cl), or a combination thereof.
[0145] Of course, without departing from the scope of the present invention, the photo-active layer 4 may be made of another absorber material, such as cadmium telluride (CdTe), or copper indium gallium selenide (CIGS), or amorphous silicon, or which comprises a heterojunction of organic semiconductors, or III-V semiconductor materials, such as gallium arsenide.
[0146] One of the two electrodes 3, 5 forms the negative N electrode of the photovoltaic cell 1, while the other forms the positive P electrode of the same photovoltaic cell 1.
[0147] Furthermore, one of the semiconductor layers 6 and the additional semiconductor layer 6’ is advantageously selective for negative charges, i.e., is arranged to extract electrons (Electron-Transporting Layer, ETL) from the photo-active layer 4, and is advantageously arranged at the negative N-electrode.
[0148] Furthermore, one of the semiconductor layers 6 and the additional semiconductor layer 6’ is advantageously selective for positive charges, i.e., is arranged to extract holes (Hole-Transporting Layer, HTL) from the photo-active layer 4 and is advantageously disposed at the positive P electrode. In particular, in accordance with the preferred embodiment of the invention, the first electrode 3 forms the positive electrode P of the photovoltaic cell 1 and the second electrode 5 forms the negative electrode N of the photovoltaic cell 1, advantageously resulting in a p-i-n structure. Therefore, the semiconductor layer 6 is advantageously selective for negative charges. Furthermore, the additional semiconductor layer 6’ is advantageously selective for positive charges.
[0149] Alternatively, in accordance with an alternative embodiment (not shown), in photovoltaic cell 1, the first electrode 3 is the negative N electrode and the second electrode 5 is the positive P electrode. Therefore, in this case, the semiconductor layer 6 is advantageously selective for positive charges. Furthermore, the additional semiconductor layer 6’ is advantageously selective for negative charges. In accordance with the underlying concept of the present invention, the third deposition step involves a stage of arrangement of a solvent. In particular, the solvent may be polar or nonpolar.
[0150] In accordance with a first embodiment of the method, the solvent is polar and is advantageously selected from: water, acetone, alcohols, and mixtures thereof. Preferably, the polar solvent is an alcohol, such as ethanol, isopropanol, or butanol.
[0151] According to a second embodiment of the method, the solvent is nonpolar and is advantageouslyselected from: toluene, xylene, anisole, and mixtures thereof.
[0152] The third deposition step of the method according to the invention further comprises a stage of dispersion of nanoparticles 7, made of a metal oxide, in the solvent. Advantageously, therefore, the nanoparticles 7 are dispersed in the aforementioned solvent.
[0153] In particular, the nanoparticles 7 have an average diameter between 1 and 80 nm, preferably between 3 and 50 nm.
[0154] More in detail, the nanoparticles 7 are made of at least one semiconductor metal oxide having a bandgap equal to or greater than 2 eV; i.e., in other words, they advantageously possess the characteristics of a wide-bandgap semiconductor.
[0155] Preferably, the semiconductor metal oxide has a work function similar to the conduction band of the photo-active layer 4, i.e., for example, approximately 4 eV, so as to function as an Electron-Transporting Layer (ETL), in particular in the case where the second electrode 5 is the negative N electrode.
[0156] More in detail, the metal oxide semiconductor is a compound defined by the chemical formula MxOy, where M is a metal element and O is oxygen.
[0157] In particular, the aforementioned metal oxide semiconductor is selected from: tin oxide, titanium oxide, zinc oxide, magnesium oxide, niobium oxide.
[0158] Advantageously, the semiconductor metal oxide may also contain dopants, such as heteroatoms capable of modifying its work function and electrical conductivity. For example, if the metal oxide is zinc oxide, the latter may be doped with aluminum atoms.
[0159] The third deposition step of the method according to the invention further comprises a stage of dissolution of a polymeric material in the aforementioned solvent. Preferably, the polymeric material is an insulating polymer.
[0160] In particular, the dissolution stage of the polymeric material occurs after the dispersion step of the nanoparticles 7, but may also occur before the latter.
[0161] Therefore, advantageously, the polymeric material comprises carbon-based macromolecules (i.e., polymer chains 80) with functional groups to make it compatible with the nanoparticles 7 and with the solvent in which they are dispersed.
[0162] In particular, according to the first embodiment of the method, in which the solvent is polar, the polymeric material is a polymer soluble in the polar solvent and comprises at least one functional group provided with dipole-forming heteroatoms. For example, such functional groups may be hydroxyl, imine, pyrrolyl, sulfonate, acrylamide, or acrylate groups.
[0163] In this case, the polymeric material is, for example, selected from: polyvinyl alcohol, polyethyleneamine, polyvinylpyrrolidone, poly(sodium 4-styrenesulfonate), poly(n-isopropylacrylamide), sodium polyacrylate, and mixtures or copolymers thereof.Furthermore, in accordance with the second embodiment of the method, in which the solvent is nonpolar, the polymeric material is a polymer soluble in the nonpolar solvent and comprises low-dipole functional groups, for example one of: alkyl groups, benzene groups, and acrylate groups. In this case, therefore, the polymeric material is, for example, selected from: polymethyl methacrylate, polystyrene, and mixtures or copolymers thereof.
[0164] Advantageously, the polymeric material is dissolved in the solvent in an amount equal to or less than 10% by weight relative to the weight of the nanoparticles 7, preferably with a minimum amount of 0.01% by weight relative to the weight of the nanoparticles 7.
[0165] In particular, the polymeric material is dissolved in the solvent in an amount comprising 0.01 to 5% by weight relative to the weight of the nanoparticles 7, preferably comprising 0.01 to 3% by weight, more preferably comprising 0.1 to 3% by weight, and even more preferably comprising 0.1 to 1% by weight.
[0166] The third deposition step of the method according to the invention further comprises a stage of spreading the mixture comprising the solvent, the nanoparticles, and the polymeric material onto the photo-active layer 4.
[0167] In particular, the spreading step may be performed using any suitable deposition method, for example those described above, such as for example screen printing, spin coating, blade coating, and slot die coating.
[0168] The third deposition step of the method according to the invention further comprises a stage of evaporation of the solvent to form the semiconductor layer 6 that comprises a reinforcing matrix 8 made of the polymeric material, preferably the insulating polymer, in which the nanoparticles 7 are partially embedded and at least partially interconnected by polymer chains 80 of the polymeric material.
[0169] In this way, it is possible to obtain, in a simple, fast, and low-cost manner, a photovoltaic cell 1 that is more resistant to delamination without losing efficiency.
[0170] Advantageously, the polymeric material comprises polymer chains 80 with an average length equal to or greater than three times the diameter of the nanoparticles 7.
[0171] Furthermore, advantageously, the polymer chains 80 of the polymeric material have an average molecular weight equal to or greater than 2000 Da, preferably equal to or greater than 5000 Da, more preferably equal to or greater than 10000 Da, and even more preferably equal to or greater than 20000 Da.
[0172] In this way, it is possible to ensure optimal strength for the semiconductor layer 6. Below a critical value of 2000 Da for the average molecular weight, the strength is still improved, although this property decreases as the molecular weight itself decreases.
[0173] Advantageously, the method comprises one or more removal steps, at least partially intermediatebetween the (deposition) steps described above, in which a portion of one or more layers is removed to form interruption openings Pl, P2 and P3, in order to create, if necessary and preferably in a manner known per se, one or more monolithic interconnections with one or more other photovoltaic cells 1.
[0174] In particular, the aforementioned layers comprise: the first electrode 3, the photo-active layer 4, the second electrode 5, the semiconductor layer 6, and advantageously the additional semiconductor layer 6’.
[0175] In particular, this removal step involves the use of removal techniques such as, for example, laser ablation or chemical removal following partial masking of the area affected by the process.
[0176] Advantageously, the removal step involves, in particular between the first deposition step and the second deposition step, the removal by means of laser ablation of a portion of the first electrode 3 to form the Pl interruption opening.
[0177] Advantageously, the removal step involves, in particular between the second deposition step and the fourth deposition step, preferably between the third deposition step and the fourth deposition step, the removal by means of laser ablation of at least a portion of the photo-active layer 4, preferably also of the semiconductor layer 6, and preferably also of the additional semiconductor layer 6, to form the P2 intermption opening.
[0178] Advantageously, the removal step comprises, in particular after the fourth deposition step, the removal by means of laser ablation of at least a portion of the second electrode 5, in particular to form the P3 intermption opening. Furthermore, the removal step advantageously involves the removal by means of laser ablation of a portion of the semiconductor layer 6, in particular to form the P3 intermption opening. Optionally, the removal step advantageously involves the removal by means of laser ablation of a portion of the photo-active layer 4, in particular to form the P3 intermption opening.
[0179] As seen above, the semiconductor layer 6 surprisingly exhibits improved resistance to mechanical stresses caused by the removal step thanks to the presence of the reinforcing matrix 8.
[0180] Obviously, the photovoltaic cell 1 obtained by this method may have any additional feature, in particular in terms of shapes and materials, of the photovoltaic cell 1 described above.
[0181] The photovoltaic cell 1 thus conceived and the method for manufacturing a photovoltaic cell 1 therefore achieve the intended objectives.
Claims
CLAIMS1. Photovoltaic cell (1), in particular a thin-film photovoltaic cell, which comprises:- a substrate (2) made of at least partially transparent material susceptible of being traversed by solar radiation;- a first electrode (3), at least partially transparent, which is disposed on said substrate (2) and is susceptible of being traversed by said solar radiation coming from said substrate (2);- a photo-active layer (4), which is disposed on said first electrode (3) and is susceptible of receiving said solar radiation for the generation of electric current;- a second electrode (5), which is disposed on said photo-active layer (4);- at least one semiconductor layer (6) interposed between said second electrode (5) and said photo-active layer (4);wherein one of said first electrode (3) and second electrode (5) is a negative electrode (N), and the other of said first electrode (3) and second electrode (5) is a positive electrode (P);wherein said second electrode (5) is arranged to be electrically connected to the first electrode (3) of a further photovoltaic cell connected in series to the photovoltaic cell (1) by means of a monolithic series electrical connection, which has interruption openings Pl, P2 and P3;wherein said semiconductor layer (6) is made of a composite material comprising:- nanoparticles (7) made of at least one metal oxide, and- a reinforcing matrix (8), in which said nanoparticles (7) are partially embedded, made with a polymeric material that comprises a plurality of polymer chains (80) arranged at least in partial interconnection between said nanoparticles (7);wherein the polymeric material is present in an amount equal to or less than 10% by weight relative to the weight of said nanoparticles (7), with a minimum amount of 0.01% by weight relative to the weight of said nanoparticles (7).
2. Photovoltaic cell (1) according to claim 1, characterized in that said nanoparticles have an average diameter between 1 and 80 nm, and that the polymer chains (80) have an average length equal to or greater than three times the diameter of said nanoparticles (7).
3. Photovoltaic cell (1) according to claim 1 or 2, characterized in that the polymer chains (80) of said polymeric material have an average molecular weight equal to or greater than 2000 Da.
4. Photovoltaic cell (1) according to any of the preceding claims, characterized in that the polymeric material of said reinforcing matrix (8) is an insulating polymer;said polymeric material selected from: polyvinyl alcohol, polyethyleneamine, polyvinylpyrrolidone, poly(sodium 4-styrenesulfonate), poly(n-isopropylacrylamide), sodium polyacrylate, polymethyl methacrylate, polystyrene, and mixtures or copolymers thereof.
5. Photovoltaic cell (1) according to any of the preceding claims, characterized in that thepolymeric material of said reinforcing matrix (8) is present in said semiconductor layer (6) in an amount between 0.01 to 5% by weight relative to the weight of said nanoparticles (7), preferably between 0.01 and 3% by weight, more preferably between 0.1 and 3% by weight, and most preferably between 0.1 and 1% by weight.
6. Photovoltaic cell (1) according to any of the preceding claims, characterized in that said nanoparticles (7) are made of at least one semiconductor metal oxide having a band gap equal to or greater than 2 eV selected from: tin oxide, titanium oxide, zinc oxide, magnesium oxide, niobium oxide.
7. Photovoltaic cell (1) according to any of the preceding claims, characterized in that said photoactive layer (4) comprises an absorber material, which is a perovskite.
8. Photovoltaic cell (1) according to any of the preceding claims, characterized in that said monolithic series electrical connection is obtained by removing a portion of one or more of said layers (3, 4, 5, 6) by means of laser ablation to form said interruption openings Pl, P2, and P3.
9. Photovoltaic cell (1) according to any of the preceding claims, characterized in that an interruption opening P3 of said interruption openings Pl, P2 and P3 is formed on said second electrode (5) itself, in particular by means of laser ablation.
10. Photovoltaic cell (1) according to claim 9, characterized in that said interruption opening P3 is also formed on said semiconductor layer (6).
11. Photovoltaic cell (1) according to any of the preceding claims, characterized in that said second electrode (5) is formed at least partially by means of sputtering coating.
12. Method for manufacturing a photovoltaic cell (1), which method comprises:- a step of arranging a substrate (2) of at least partially transparent material;- a first deposition step, in which a first electrode (3), at least partially transparent, is deposited on said substrate (2);- a second deposition step, in which a photo-active layer (4) is deposited on said first electrode (3);- a third deposition step, in which a semiconductor layer (6) is deposited on said photo-active layer (4);- a fourth deposition step, in which a second electrode (5) is deposited on said semiconductor layer (6);- one or more removal steps, at least partially intermediate between said deposition steps, in which a portion of one or more of said layers (3, 4, 5, 6) is removed to form Pl, P2, and P3 interruption openings, to create one or more monolithic interconnections with one or more other photovoltaic cells (1);wherein one of said first electrode (3) and second electrode (5) is a negative (N) electrode, and theother of said first electrode (3) and second electrode (5) is a positive (P) electrode;said method being characterized in that said third deposition step comprises:- a stage of arrangement of a solvent;- a stage of dispersion of nanoparticles (7), made of a metal oxide, in said solvent;- a stage of dissolution of a polymeric material in said solvent;- a stage of spreading the mixture comprising said solvent, said nanoparticles and said polymeric material onto said photo-active layer (4);- a stage of evaporation of said solvent to form said semiconductor layer (6) which comprises a reinforcing matrix (8) made of said polymeric material, in which the nanoparticles (7) are partially embedded and at least partially interconnected by polymeric chains (80) of the polymeric material.
13. Method for manufacturing a photovoltaic cell (1) according to claim 12, characterized in that said solvent is a polar solvent and said polymeric material is a polymer soluble in said polar solvent and comprising at least one functional group provided with dipole-forming heteroatoms.
14. Method for manufacturing a photovoltaic cell (1) according to claim 12, characterized in that said solvent is a nonpolar solvent and said polymeric material is a polymer soluble in said nonpolar solvent and comprising low-dipole functional groups, for example comprised of: alkyl groups, benzene groups, acrylate groups.
15. Method for manufacturing a photovoltaic cell (1) according to any of claims 12 to 13, characterized in that said removal step involves laser ablation.
16. A method for manufacturing a photovoltaic cell (1) according to any one of claims 12 to 15, characterized in that said removal step comprises removing, by means of laser ablation, a portion of said second electrode (5) to form an interruption opening P3.
17. A method for manufacturing a photovoltaic cell (1) according to any of claims 12 to 16, characterized in that at least the second electrode (5) in said fourth deposition step is formed at least partially by sputtering coating.