Phosphorus-carbon composite material powder, negative electrode active material, negative electrode, and secondary battery
The phosphorus-carbon composite material addresses warping and surface issues in electrodes by ensuring optimal particle distribution and chemical bonding, resulting in improved electrode quality and battery performance.
Patent Information
- Application Number
- PCT/JP2026/017271
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional phosphorus-carbon composite materials face issues with warping and surface condition of electrodes in secondary batteries, particularly when applied to current collectors.
A phosphorus-carbon composite material powder with controlled bulk densities and chemical bonding between phosphorus and carbon atoms, produced through high-compressive-force mixing and grinding, which enhances electrode uniformity and reduces warping.
The composite material improves electrode surface smoothness and reduces warping by optimizing particle distribution and stress relief, leading to enhanced performance in secondary batteries.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000027_0000
Abstract
Description
Phosphorus-carbon composite material powder, negative electrode active material, negative electrode, and secondary battery
[0001] The present invention relates to phosphorus-carbon composite material powder, anode active material, anode, and secondary battery.
[0002] For example, as an active material for the negative electrode of a secondary battery, a phosphorus-carbon composite material containing phosphorus atoms and carbon atoms is known, which can be obtained by compounding black phosphorus and carbon raw materials in a ball mill, as disclosed in Patent Document 1.
[0003] Japanese Patent Publication No. 2023-095306
[0004] However, conventional phosphorus-carbon composite materials have room for improvement in terms of the warping and surface condition of electrodes obtained by applying a slurry containing the phosphorus-carbon composite material to a substrate such as a current collector.
[0005] The present invention has been made in view of the above problems, and aims to provide a phosphorus-carbon composite material, etc., that can improve the warping and surface condition of electrodes.
[0006] [1] A phosphorus-carbon composite material powder containing phosphorus atoms and carbon atoms, wherein the bulk density of the phosphorus-carbon composite material powder is 1.4 to 2.7 g / cm³ 3 The bulk density of the phosphorus-carbon composite material powder is 0.18 to 2.0 g / cm³. 3 [1] A phosphorus-carbon composite material powder. [2] The phosphorus-carbon composite material powder according to [1], wherein at least a portion of the phosphorus atoms has a black phosphorus structure. [3] The phosphorus-carbon composite material powder according to [1] or [2], obtained by mixing black phosphorus and a carbon material in a stirring pulverizer. [4] A negative electrode active material comprising the phosphorus-carbon composite material powder according to any one of [1] to [3]. [5] A negative electrode having a negative electrode active material layer comprising the phosphorus-carbon composite material powder according to any one of [1] to [3]. [6] A secondary battery comprising the negative electrode according to [5].
[0007] According to the present invention, a phosphorus-carbon composite material and the like that can improve the warping and surface condition of electrodes are provided.
[0008] FIG. 1 is a schematic diagram showing a lithium secondary battery as an example of a battery. FIG. 2 is a schematic diagram showing an all-solid-state lithium secondary battery as an example of a battery.
[0009] <Phosphorus-Carbon Composite Material> The phosphorus-carbon composite material powder according to the present embodiment is a powder of a phosphorus-carbon composite material containing phosphorus atoms and carbon atoms. In the following description, "phosphorus-carbon composite material" may be abbreviated simply as "P-C composite material", and "phosphorus-carbon composite material powder" may be abbreviated simply as "P-C composite material powder".
[0010] In the phosphorus-carbon composite material powder of the present embodiment, the packed bulk density of the phosphorus-carbon composite material powder is 1.4 to 2.7 g / cm 3 , and the loose bulk density of the phosphorus-carbon composite material powder is 0.18 to 2.0 g / cm 3 .
[0011] The loose bulk density is the density obtained by filling a container with a fixed volume with powder and taking the internal volume of the container as the volume. Specifically, P-C composite material powder is freely dropped using a funnel into a stationary alumina container (diameter: 5 mm, height: 2.5 mm) until the alumina container is full. Thereafter, the mass of the P-C composite material powder in the alumina container is determined. The value obtained by dividing this mass by the volume (internal volume) of the alumina container can be defined as the loose bulk density.
[0012] The loose bulk density of the P-C composite material powder may be 0.19 g / cm 3 or more, may be 0.20 g / cm 3 or more, may be 0.21 g / cm 3 or more, may be 0.22 g / cm 3 or more, and may be 0.23 g / cm 3 or more. The loose bulk density of the P-C composite material powder may be 1.5 g / cm 3 or less, may be 1.2 g / cm 3 or less, may be 1.1 g / cm 3 or less, may be 1.0 g / cm 3 or less, may be 0.7 g / cm 3 or less, may be 0.5 g / cm 3 or less, and may be 0.4 g / cm 3The following is acceptable:
[0013] The bulk density of the heavily loaded material is 102 kgf / cm³. 2 This is the density of P-C composite material powder pressed with a load of 102 kgf / cm². Specifically, 0.1 g of P-C composite material powder is placed in a powder molding die (diameter: 10 mm) and pressed into the die with a hydraulic hand press machine. 2 After applying the load, the thickness (t) of the P-C composite material powder can be calculated, and the value obtained by dividing the mass of the P-C composite material powder by the volume of the P-C composite material powder after pressing can be used as the bulk density of the heavy load.
[0014] The bulk density of the P-C composite material powder is 2.5 g / cm³. 3 The following may be used: 2.3 g / cm³ 3 The following may be used: 2.1 g / cm³ 3 The following may be used: 1.9 g / cm³ 3 The following may be used: 1.8 g / cm³ 3 The following is acceptable:
[0015] The P-C composite material powder according to this embodiment has such light and heavy bulk densities, which makes it possible to reduce warping and improve surface smoothness in electrodes obtained by coating a slurry containing the phosphorus-carbon composite material onto a substrate such as a current collector. Although the mechanism of action is unclear, for example, when making electrodes, if the P-C composite material powder slurry is coated onto a substrate such as a current collector and dried, and the light bulk density of the P-C composite material powder is at an appropriate level, each particle will settle in an optimal location where the repulsive energy between powder particles is minimized, thereby increasing the uniformity of the surface state of the negative electrode active material layer. Furthermore, when the negative electrode active material layer is pressed after coating and drying, if the heavy bulk density of the P-C composite material powder is at an appropriate level, it is thought that the stress on the negative electrode active material layer after pressing will be relieved, and warping of the electrode will be suppressed.
[0016] When the bulk density of the P-C composite material powder is ρPD and the bulk density of the phosphorus-carbon composite material powder is ρUTD, it is preferable that ρPD / ρUTD is 14 or less. The ρPD / ρUTD of the P-C composite material powder may be 14 or less, 12 or less, 11 or less, 10 or less, 9 or less, or 8 or less. The ρPD / ρUTD of the P-C composite material powder may be 1 or more.
[0017] (Angle of Repose) The angle of repose of the P-C composite material powder may be 48.0° or higher, 48.5° or higher, 49.0° or higher, 49.5° or higher, or 50.0° or higher. Alternatively, the angle of repose may be 60.0° or lower, 55.0° or lower, or 53.0° or lower.
[0018] (Particle size distribution of P-C composite material powder) The D50 of the P-C composite material powder can be 1 to 20 μm. D50 may be 1.5 μm or more, 2.0 μm or more, or 5.0 μm or more. D50 may be 17 μm or less, 15 μm or less, 12 μm or less, 11 μm or less, or 10 μm or less. The D90 of the P-C composite material powder can be 15 to 30 μm. D90 may be 16 μm or more, 17 μm or more, 18 μm or more, 19 μm or more, 29 μm or less, 28 μm or less, or 27 μm or less. The D10 of the P-C composite material powder may be 0.01 μm or larger, 0.02 μm or larger, 0.05 μm or larger, 0.1 μm or larger, 0.2 μm or larger, 0.3 μm or larger, 5.0 μm or smaller, 2.0 μm or smaller, 1.0 μm or smaller, 0.7 μm or smaller, or 0.5 μm or smaller.
[0019] In this specification, D10, D50, and D90 refer to the diameters at which 10% of the total volume of particles are smaller than their diameter, 50% of the total volume of particles are smaller than their diameter, and 90% of the total volume of particles are smaller than their diameter, respectively, in the volume-based particle size distribution measured by a laser diffraction particle size analyzer.
[0020] (D90 - D10) / D50 may be 3.0 or greater, 4.0 or greater, 5.0 or greater, 25 or less, 20 or less, or 15 or less. In the calculation of (D90 - D10) / D50, the unit of particle size should be the same for all, for example, all in μm.
[0021] The P-C composite material that constitutes the P-C composite material powder of this embodiment contains phosphorus atoms and carbon atoms.
[0022] In P-C composite materials, the phosphorus atom content is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more. A higher phosphorus content increases the initial charge-discharge capacity of the P-C composite material. Furthermore, in P-C composite materials, the phosphorus atom content is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less. This is because if the phosphorus atom content is too high, the cycle characteristics of the P-C composite material deteriorate. The upper and lower limits of the phosphorus atom content can be arbitrarily combined.
[0023] In P-C composite materials, the carbon content is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more. A higher carbon content improves the cycle characteristics of the P-C composite material. Furthermore, in P-C composite materials, the carbon content is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 50% by mass or less. This is because if the carbon content is too high, the initial charge-discharge capacity of the P-C composite material decreases. The upper and lower limits of the carbon content can be arbitrarily combined.
[0024] P-C composite materials are composed of phosphorus and carbon atoms making up 60% or more of the total mass, and may also contain elements other than phosphorus and carbon atoms. Examples of elements other than phosphorus and carbon atoms included in P-C composite materials include metallic or metalloid elements such as lithium, silicon, germanium, tin, aluminum, magnesium, zinc, niobium, and titanium (however, zinc, niobium, and titanium are transition metal elements), and nonmetallic elements such as nitrogen, oxygen, fluorine, sulfur, and chlorine. These can be used as raw materials in the form of metal oxides, composite metal oxides, metal fluorides, metal sulfides, metal chlorides, silicon dioxide, silicates, titanates, and aluminates.
[0025] When the P-C composite material contains components other than phosphorus atoms and carbon atoms, the content of the other components is preferably 1% by mass or more and 15% by mass or less, more preferably 2% by mass or more and 12% by mass or less, and even more preferably 2.5% by mass or more and 8% by mass or less, relative to the total amount of the other components other than phosphorus atoms and carbon atoms.
[0026] When the proportions of other components are within the above range, the movement of lithium ions is less likely to be inhibited, and the initial capacity of the secondary battery tends to improve.
[0027] The phosphorus atom content, carbon atom content, and other possible atom content in P-C composite materials can be determined by known ICP analysis.
[0028] P-C composite material powder is manufactured by mixing and grinding phosphorus and carbon raw materials under high compressive force using a planetary ball mill or the like, as described later. The inventors conducted a detailed analysis and study of the obtained P-C composite material powder and found that, as will be described in detail later, the negative electrode using the obtained P-C composite material powder exhibited completely different electrochemical properties from a negative electrode using a simple P-C mixture. This revealed that the P-C composite material powder is not simply a mixture of phosphorus and carbon raw material powders, but rather a novel material in which phosphorus atoms and carbon atoms are chemically bonded (covalently bonded) within the P-C composite material, resulting in physical properties different from those of the phosphorus and carbon raw materials.
[0029] Furthermore, confirming the presence or absence of P-C bonding requires advanced analytical techniques, and can be performed using methods such as XPS or NMR, but is not limited to these analytical methods.
[0030] In P-C composite materials, the chemical bond (covalent bond) between phosphorus atoms and carbon atoms can be confirmed, for example, by the appearance of a peak in the 132–136 eV range in the XPS spectrum. The bond between phosphorus atoms and carbon atoms is sometimes simply referred to as a "P-C bond."
[0031] In P-C composite materials, at least some of the phosphorus atoms may have a black phosphorus structure.
[0032] <Method for producing P-C composite material powder> The above-mentioned P-C composite material powder can be produced by a process in which carbon material and phosphorus material are mixed and pulverized while applying a large compressive force, for example, by mixing them in a planetary ball mill.
[0033] The raw materials used are amorphous carbon, graphite, porous carbon, mesocarbon microbeads (MCMB), fullerene, carbon nanotubes, graphene, graphene oxide, and carbon nitride (C). 3 N 4 At least one material selected from the group consisting of amorphous carbon, laminated carbon nanofibers (carbon nanofibers platelets) can be used. All of these carbon materials other than amorphous carbon have a graphite structure.
[0034] Examples of amorphous carbon include carbon black (CB), acetylene black (AB), Ketjenblack, hard carbon, and soft carbon.
[0035] As for fullerenes, C 60 , C 72 , C 84 Examples include:
[0036] Examples of carbon nanotubes include single-walled carbon nanotubes (SWCNTs), multi-walled carbon nanotubes (MWCNTs), cup-stacked carbon nanotubes (CSCNTs), and vapor-grown carbon fiber (VGCF). These have a structure that extends in one axial direction (one-dimensional structure).
[0037] Graphene, graphene oxide, carbon nitride (C 3 N 4 ), stacked carbon nanofibers (carbon nanofibers platelets) have a structure that extends in the planar direction (two-dimensional structure).
[0038] In carbon materials, the edges (edge sites) of the graphite structure are more reactive than other areas. Therefore, it is assumed that most P-C bonds are formed at the edge sites of the carbon material. Consequently, from the viewpoint of facilitating P-C bond formation, it is preferable to use a carbon material that has many edge sites.
[0039] Carbon materials with many edge sites include CSCNTs, graphite, mesocarbon microbeads (MCMBs), graphene, graphene oxide, and carbon nitride (C). 3 N 4 Examples include laminated carbon nanofibers. Among these, graphite is preferred as a carbon material due to its high density and ease of handling.
[0040] Furthermore, any known phosphorus allotrope can be used as the phosphorus material. Among the phosphorus allotropes, black phosphorus is preferred as the phosphorus material because it is the most chemically stable and also a good electrical conductor. When black phosphorus is used as the raw material, at least some of the phosphorus atoms in the resulting phosphorus-carbon composite material powder may have a black phosphorus structure.
[0041] By mixing and pulverizing carbon and phosphorus materials while applying a large compressive force, strong impact forces are applied to the carbon and phosphorus materials. It is believed that this mixing and pulverization of the raw material powders simultaneously causes chemical changes that cannot be obtained with ordinary mixtures. As a result, it is believed that a composite material is obtained in which P-C bonds, which were not present in the raw materials, are formed, and the crystalline state observed in the raw materials is not present.
[0042] Mixing and grinding under high compressive force should be continued until the peaks originating from the raw materials disappear from the XRD profile of the resulting material.
[0043] There are no particular limitations on the processing equipment (grinders) that can perform mixing and grinding while applying a large compressive force, but examples include roller mills, jet mills, hammer mills, pin mills, disc mills, rod mills, ball mills, vibratory mills, attritors, and bead mills. It is especially preferable to use an agitated grinder equipped with a grinding container and a rotating body, as it can perform mixing and grinding simultaneously. Examples of agitated grinders include pin mills, disc mills, rod mills, ball mills, vibratory mills, attritors, and bead mills.
[0044] Furthermore, as the processing apparatus, a media-stirring type pulverizer is preferred because it can mix and pulverize the raw material powder while simultaneously applying strong impact force to the carbon and phosphorus materials. Examples of media-stirring type pulverizers include ball mills, vibratory mills, attritors, and bead mills. Among these, ball mills are particularly preferred from the viewpoint of easily controlling the manufacturing conditions, and planetary ball mills are the most preferred.
[0045] It is believed that mixing in a media-agitating pulverizer such as a planetary ball mill first results in the micronization of the phosphorus material and the decomposition of the carbon material, followed by the formation of P-C bonds.
[0046] During mixing in a planetary ball mill, manufacturing conditions can be controlled by adjusting the orbital diameter, rotational diameter, orbital speed, the ratio of rotational speed to orbital speed, the amount of media (balls) relative to the raw material (Ball powder ratio), and the mixing time. In particular, from the viewpoint of producing composite materials having the above-mentioned heavy bulk density and light bulk density, it is preferable to increase the orbital diameter. Since the kinetic energy of rotational motion is proportional to the square of the diameter, the orbital diameter has a significant effect on the heavy bulk density, light bulk density, angle of repose, particle size distribution, etc., of the resulting composite material powder. An orbital diameter of 157 mm or more is preferable.
[0047] The balls are a grinding medium for crushing the raw materials and also apply compressive force to the raw materials. The diameter of the balls is the average particle size of the balls. Due to the rotation and revolution of the grinding container itself, the balls flow at high speed inside the grinding container and collide with the raw materials containing carbon and phosphorus materials, causing them to be crushed into smaller particles, form P-C bonds, or change the crystal structure. In the grinding process, it is preferable that the grinding container and the balls do not wear excessively. For this reason, the shape of the balls is preferably spherical or ellipsoidal. Also, if the balls continue to collide, the grinding may stop decreasing in average particle size, or conversely, the average particle size may increase.
[0048] The diameter of the balls should preferably be larger than the average particle size of the composite particles that are ultimately obtained. By using such balls, a large amount of grinding energy can be imparted to the composite material, allowing for the efficient production of composite particles in a short time.
[0049] The diameter of the balls is preferably 0.1 to 10 mm, and more preferably 1 to 10 mm. When the diameter of the balls is within this range, the formation of P-C bonds can be promoted and re-aggregation can be suppressed. The diameters of the balls placed in the grinding container may be uniform or varied.
[0050] Suitable materials for the balls include glass, agate, alumina, zirconia, stainless steel, chrome steel, tungsten carbide, silicon carbide, and silicon nitride. Among these, zirconia is preferred because it has relatively high hardness, making it resistant to wear, and its relatively high specific gravity allows for obtaining large amounts of grinding energy. By using these balls, raw materials can be efficiently ground and ground.
[0051] The weight ratio of balls to raw materials is defined as the ball-raw material ratio. Increasing the ball-raw material ratio allows for more frequent application of strong impact forces to the raw materials, thereby further promoting the formation of P-C bonds. However, if the ball-raw material ratio is too high, the amount of composite material powder produced per unit operation decreases. Therefore, a preferred ball-raw material ratio is 0.5 to 500, more preferably 1 to 200, and even more preferably 10 to 200.
[0052] Furthermore, after the planetary ball mill mixing is complete, the balls are separated from the composite material using a filter or the like.
[0053] Each operating condition in planetary ball mill mixing can be set appropriately within the range in which the composite material powder described above can be obtained.
[0054] <Negative electrode active material> The negative electrode active material of this embodiment includes the P-C composite material powder described above.
[0055] The negative electrode active material may be the P-C composite material powder described above, or it may contain known materials used as negative electrode active materials in addition to the P-C composite material powder. Examples of such materials include (i) carbon materials that can insert and remove lithium ions or sodium ions, (ii) alloy-based negative electrode active material materials that involve the formation of a lithium alloy phase or a sodium alloy phase, (iii) transition metal oxides that undergo decomposition and regeneration reactions (conversion reactions) with lithium ions or sodium ions, and (iv) oxides or composite oxides that have activity as negative electrode active materials.
[0056] (i) Examples of carbon materials include graphite, hard carbon, soft carbon, and carbon nanotubes. There are no particular restrictions on the type of graphite; both natural and artificial graphite can be used. There are no particular restrictions on the shape and form of the graphite particles; various forms such as flakes, lumps, fibers, whiskers, spheres, and fragments can be used.
[0057] (ii) Examples of alloy-based negative electrode active materials include silicon, germanium, tin, aluminum, zinc, magnesium, or alloys thereof.
[0058] (iii) Examples of transition metal oxides include manganese oxide, iron oxide, cobalt oxide, nickel oxide, copper oxide, and magnesium oxide. These oxides may also be composite metal oxides further containing other metals (e.g., lithium).
[0059] (iv) Examples of oxides or composite oxides include titanium dioxide, lithium titanate, and silicon dioxide.
[0060] <Negative Electrode> The negative electrode of this embodiment has a negative electrode active material layer containing the negative electrode active material described above. The negative electrode active material layer may contain a binder in addition to the negative electrode active material. Examples of binders include one or more selected from polyvinylidene fluoride (hereinafter sometimes referred to as PVdF), polyimide, polyamide-imide, styrene-butadiene rubber, carboxymethylcellulose, and acrylic resin. The negative electrode may or may not have a binder for tying the negative electrode active material to the current collector described later, and / or for tying the negative electrode active materials together. The negative electrode active material layer may further contain a conductive additive, a solid electrolyte, etc. Examples of conductive additives include acetylene black and carbon black. Examples of solid electrolytes will be described later. The negative electrode may have a current collector in addition to the negative electrode active material layer. The negative electrode active material layer can be formed on at least one or both surfaces of the current collector. As the material for the current collector, a known configuration can be used, and copper or a copper alloy can be suitably used. An example of a method for manufacturing the negative electrode is to apply a mixture slurry containing the above-mentioned negative electrode active material, a binder as needed, a conductive additive as needed, a solid electrolyte as needed, and a solvent to the surface of a substrate such as a current collector and dry it. Typically, the resulting laminate of the substrate and the negative electrode active material layer is then pressed. Examples of solvents include N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone (NEP), N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), γ-butyrolactone (GBL), sulfolane, and mixtures of these in any proportion. The negative electrode of this embodiment may be for lithium secondary batteries, all-solid-state batteries, or sodium-ion batteries.
[0061] <Lithium-ion secondary battery> The lithium-ion secondary battery of this embodiment includes the negative electrode described above.
[0062] A suitable example of a lithium secondary battery using the negative electrode active material of this embodiment includes a positive electrode and a negative electrode, a separator sandwiched between the positive electrode and the negative electrode, and an electrolyte placed between the positive electrode and the negative electrode.
[0063] Figure 1 is a schematic diagram showing an example of a lithium secondary battery. For example, a cylindrical lithium secondary battery 10 is manufactured as follows.
[0064] First, as shown in the partially enlarged view of Figure 1, a pair of strip-shaped separators 1, a strip-shaped positive electrode 2 having a positive electrode lead 21 at one end, and a strip-shaped negative electrode 3 having a negative electrode lead 31 at one end are stacked in the order of separator 1, positive electrode 2, separator 1, negative electrode 3, and then wound to form an electrode group 4.
[0065] The positive electrode 2, as an example, has a positive electrode active material layer 2a containing a positive electrode active material (hereinafter referred to as CAM) and a positive electrode current collector 2b on which the positive electrode active material layer 2a is formed on one surface. Such a positive electrode 2 can be manufactured by first preparing a positive electrode mixture containing CAM, a conductive material, and a binder, and then supporting the positive electrode mixture on one surface of the positive electrode current collector 2b to form the positive electrode active material layer 2a.
[0066] The negative electrode 3 is as described above, and may be a negative electrode having a negative electrode active material layer containing the P-C composite material powder described above on a current collector, or an electrode having a negative electrode active material layer containing the P-C composite material powder described above but without a current collector.
[0067] Next, the electrode group 4 and an insulator (not shown) are placed in the battery can 5, the bottom of the can is sealed, the electrode group 4 is impregnated with electrolyte 6, and the electrolyte is placed between the positive electrode 2 and the negative electrode 3. Furthermore, the top of the battery can 5 is sealed with a top insulator 7 and a sealing body 8 to manufacture the lithium secondary battery 10.
[0068] As for the shape of the electrode group 4, for example, a columnar shape can be given such that the cross-sectional shape when the electrode group 4 is cut perpendicular to the winding axis is a circle, an ellipse, a rectangle, or a rectangle with rounded corners.
[0069] Furthermore, the shape of the lithium secondary battery having such an electrode group 4 can be one of those specified in IEC 60086, a battery standard established by the International Electrotechnical Commission (IEC), or JIS C 8500. For example, cylindrical or prismatic shapes can be used.
[0070] Furthermore, lithium secondary batteries are not limited to the wound configuration described above; they may also have a stacked configuration in which a stacked structure of positive electrode, separator, negative electrode, separator is repeatedly stacked. Examples of stacked lithium secondary batteries include so-called coin-type batteries, button-type batteries, or paper-type (or sheet-type) batteries.
[0071] For the positive electrode, separator, negative electrode, and electrolyte that constitute the lithium secondary battery, for example, the configuration, materials, and manufacturing methods described in
[0113] to
[0140] of WO2022 / 113904A1 can be used.
[0072] <All-Solid-State Lithium Secondary Battery> Next, we will explain the all-solid-state lithium secondary battery having the negative electrode described above, while describing the configuration of the all-solid-state lithium secondary battery.
[0073] Figure 2 is a schematic diagram showing an example of an all-solid-state lithium secondary battery. The all-solid-state lithium secondary battery 1000 shown in Figure 2 has a laminate 100 having a positive electrode 110, a negative electrode 120, and a solid electrolyte layer 130, and an outer casing 200 that houses the laminate 100. The all-solid-state lithium secondary battery 1000 may also have a bipolar structure in which the CAM and the negative electrode active material are arranged on both sides of the current collector. A specific example of a bipolar structure is the structure described in JP-A-2004-95400.
[0074] The positive electrode 110 comprises a positive electrode active material layer 111 and a positive electrode current collector 112. The positive electrode active material layer 111 contains the CAM and solid electrolyte described above. The positive electrode active material layer 111 may also contain a conductive material and a binder.
[0075] The negative electrode 120 comprises a negative electrode active material layer 121 and a negative electrode current collector 122. The negative electrode active material layer 121 contains the aforementioned negative electrode active material. The negative electrode active material layer 121 may also contain a solid electrolyte and a conductive material.
[0076] (Solid Electrolyte) As the solid electrolyte contained in the positive electrode active material layer 111, the solid electrolyte layer 130, etc., a solid electrolyte having lithium ion conductivity and used in known all-solid-state lithium secondary batteries can be used. Examples of such solid electrolytes include inorganic electrolytes and organic electrolytes. Examples of inorganic electrolytes include oxide-based solid electrolytes, sulfide-based solid electrolytes, and hydride-based solid electrolytes. Examples of organic electrolytes include polymer-based solid electrolytes. Examples of each electrolyte include compounds described in WO2020 / 208872A1, US2016 / 0233510A1, US2012 / 0251871A1, and US2018 / 0159169A1, and for example, the following compounds.
[0077] (Oxide-based solid electrolytes) Examples of oxide-based solid electrolytes include perovskite-type oxides, NASICON-type oxides, LISICON-type oxides, and garnet-type oxides. Specific examples of each oxide include compounds described in WO2020 / 208872A1, US2016 / 0233510A1, and US2020 / 0259213A1, and examples of the following compounds.
[0078] As perovskite-type oxides, Li a La 1-a TiO 3 Li-La-Ti oxides such as (0 < a < 1), Li b La 1-b TaO 3 Li-La-Ta oxides such as (0 < b < 1) and Li c La 1-c NboO 3 Examples include Li-La-Nb oxides such as (0 < c < 1).
[0079] As for NASICON-type oxides, Li 1+d Al d Ti 2-d (PO 4 ) 3 Examples include (0 ≤ d ≤ 1). NASICON-type oxides are Li m M 1 n M 2 oP p O q (In the formula, M 1 This is one or more elements selected from the group consisting of B, Al, Ga, In, C, Si, Ge, Sn, Sb, and Se. 2 (I) is an oxide represented by , where m, n, o, p, and q are arbitrary positive numbers.
[0080] As for LISICON-type oxides, Li 4 M 3 O 4 -Li 3 M 4 O 4 (M 3 is one or more elements selected from the group consisting of Si, Ge, and Ti. 4 (The element is one or more elements selected from the group consisting of P, As, and V.) Examples include oxides represented by ( ).
[0081] As for garnet-type oxides, Li 7 La 3 Zr 2 O 12 Examples include Li-La-Zr oxides such as LLZ. The oxide-based solid electrolyte may be a crystalline material or an amorphous material.
[0082] (Sulfide-based solid electrolytes) Examples of sulfide-based solid electrolytes include Li 2 S-P 2 S 5 based compound, Li 2 S-SiS 2 based compound, Li 2 S-GeS 2 based compound, Li 2 S-B 2 S 3 system compound, LiI-Si 2 S-P 2 S 5 system compound, LiI-Li 2 S-P 2 O 5 system compound, LiI-Li 3 PO 4 -P 2 S5 -based compound and Li 10 GeP 2 S 12 -based compounds, and the like can be exemplified.
[0083] It should be noted that in the present specification, the expression "-based compound" referring to a sulfide-based solid electrolyte is used as a general term for solid electrolytes mainly containing raw materials such as "Li 2 S" and "P 2 S 5 " described before the "-based compound". For example, Li 2 S-P 2 S 5 -based compounds include solid electrolytes mainly containing Li 2 S and P 2 S 5 , and further containing other raw materials. The proportion of Li 2 S-P 2 S 5 S contained in the -based compound is, for example, 50 to 90 mass% relative to the entire Li 2 S-P 2 S 2 S 5 -based compound. The proportion of P contained in the Li 2 S-P 2 S 5 S contained in the -based compound is, for example, 10 to 50 mass% relative to the entire Li 2 S 5 S-P 2 S 2 S 5 -based compound. In addition, the proportion of other raw materials contained in the Li 2 S-P 2 S 5 S-based compound is, for example, 0 to 30 mass% relative to the entire Li 2 S-P 2 S 5 -based compound. Furthermore, the Li 2 S-P 2 S 5 -based compounds also include solid electrolytes with different mixing ratios of Li 2 S and P 2 S 5 .
[0084] Li 2 S-P 2 S 5As for system compounds, Li 2 S-P 2 S 5 Li 2 S-P 2 S 5 -LiI, Li 2 S-P 2 S 5 -LiCl, Li 2 S-P 2 S 5 - LiBr, Li 2 S-P 2 S 5 -LiI-LiBr, Li 2 S-P 2 S 5 -Li 2 O, Li 2 S-P 2 S 5 -Li 2 O-LiI and Li 2 S-P 2 S 5 -Z m S n Examples include: (m and n are positive numbers. Z is Ge, Zn, or Ga.)
[0085] Li 2 S-SiS 2 As for system compounds, Li 2 S-SiS 2 Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 - LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 -LiI, Li 2 S-SiS 2 -P 2 S 5 -LiI, Li 2 S-SiS 2 -P 2 S 5 -LiCl, Li 2 S-SiS 2 -Li 3 PO 4 Li2 S-SiS 2 -Li 2 SO 4 and Li 2 S-SiS 2 -Li x MO y Examples include: (x and y are positive numbers. M is P, Si, Ge, B, Al, Ga, or In.)
[0086] Li 2 S-GeS 2 As for system compounds, Li 2 S-GeS 2 and Li 2 S-GeS 2 -P 2 S 5 These are some examples. Also, a typical compositional formula for allozyldite-type sulfide solid electrolytes is Li 6 PS 5 X (where X is a halogen element such as Cl, Br, I), and a specific example is Li 6 PS 5 Cl, Li 6 PS 5 Br, Li 6 PS 5 Examples include I.
[0087] The sulfide-based solid electrolyte may be a crystalline material or an amorphous material.
[0088] (Hydride-based solid electrolytes) Examples of hydride-based solid electrolyte materials include LiBH 4 LiBH 4 -3KI, LiBH 4 -PI 2 LiBH 4 -P 2 S 5 LiBH 4 -LiNH 2 ,3LiBH 4 -LiI, LiNH 2 Li 2 AlH 6 Li(NH 2 ) 2 I, Li 2 NH, LiGd(BH 4 ) 3 Cl, Li2 (BH 4 ) (NH 2 ), Li 3 (NH 2 ) I and Li 4 (BH 4 ) (NH 2 ) 3 These are some examples.
[0089] (Polymer-based solid electrolytes) Examples of polymer-based solid electrolytes include organic polymer electrolytes such as polyethylene oxide-based polymer compounds and polymer compounds containing one or more selected from the group consisting of polyorganosiloxane chains and polyoxyalkylene chains. In addition, so-called gel-type products in which a non-aqueous electrolyte is held in a polymer compound can also be used. Two or more solid electrolytes can be used in combination as long as the effects of the invention are not impaired.
[0090] The laminated body 100 may have an external terminal 113 connected to the positive electrode current collector 112 and an external terminal 123 connected to the negative electrode current collector 122. In addition, the all-solid-state lithium secondary battery 1000 may have a separator between the positive electrode 110 and the negative electrode 120.
[0091] The all-solid-state lithium secondary battery 1000 further includes an insulator (not shown) that insulates the laminate 100 from the outer casing 200 and a seal (not shown) that seals the opening 200a of the outer casing 200.
[0092] The outer casing 200 can be a container formed from a highly corrosion-resistant metal material such as aluminum, stainless steel, or nickel-plated steel. Alternatively, the outer casing 200 can be a container made by processing a laminate film with corrosion-resistant treatment applied to at least one side into a bag shape.
[0093] Examples of the shape of the all-solid-state lithium secondary battery 1000 include coin-shaped, button-shaped, paper-shaped (or sheet-shaped), cylindrical, rectangular, or laminated (pouch-shaped).
[0094] Although the all-solid-state lithium secondary battery 1000 is shown in one example configuration having a single laminate 100, this embodiment is not limited to this configuration. The all-solid-state lithium secondary battery 1000 may also have a configuration in which the laminate 100 is used as a unit cell, and multiple unit cells (laminated 100) are sealed inside the outer casing 200.
[0095] For all-solid-state lithium secondary batteries, for example, the configuration, materials, and manufacturing methods described in
[0141] to
[0181] of WO2022 / 113904A1 can be used.
[0096] [Other Batteries] The above P-C composite material powder, negative electrode active material, and negative electrode can also be applied to secondary batteries other than lithium-ion secondary batteries and all-solid-state lithium-ion secondary batteries. For example, they can be applied to sodium secondary batteries and all-solid-state sodium secondary batteries. In the above lithium secondary batteries and all-solid-state secondary batteries, sodium-containing metal oxides such as sodium cobalt oxide and sodium iron phosphate can be used as the positive electrode active material instead of lithium oxide, and if a solid electrolyte is used, a sodium ion conductive solid electrolyte can be used.
[0097] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0098] ≪Example 1≫ [Manufacturing process for P-C composite material powder] Black phosphorus as the phosphorus material and natural graphite as the carbon material were weighed in a mass ratio of phosphorus:carbon = 6:4 (total amount 1.25g), and mixed using a planetary ball mill under the following conditions to obtain the P-C composite material powder of Example 1. (Ball mill mixing conditions) Apparatus: Planetary ball mill: Retsch PM-200 Orbital diameter: 157 mm Orbital speed: 350 rpm Rotation speed: Half the orbital speed and in the opposite direction of rotation Container: ZrO 2 50 mL container media: ZrO 2 8mm diameter ball, 90g Atmosphere: Argon gas filled Sample amount: 1.25g as a mixture of raw materials Ball / raw material ratio: 72 (by weight) Mixing time: 12 hours
[0099] (Composition) Given the extremely high airtightness of the container used during the manufacturing process described above, it can be determined that the content of each atom in the P-C composite material powder is equal to the ratio of the raw materials.
[0100] (Negative Electrode Active Material Compatibility) The obtained P-C composite material powder was charged with lithium metal as the counter electrode at a charging rate of 0.2C. As a result, the average charging potential of the P-C composite material powder relative to the capacity (mAh / g) during charging was 0.1V or higher, confirming that the obtained P-C composite material powder is a material that intercepts lithium ions when lithium (alkali metal) is used as the counter electrode and a voltage of 0.1V or higher is applied. A charging potential of 0.1V or higher means that a mechanism different from the 0V potential at which metallic lithium is deposited occurred, i.e., lithium ions were intercepted. Furthermore, a two-stage charging process, such as in P-C mixtures where Li ions are first charged to P only and then to C, was not observed.
[0101] (Bulk density when lightly packed) P-C composite material powder was allowed to free-fall into an alumina container (diameter: 5 mm, height: 2.5 mm) using a funnel until the container was full. The mass of the P-C composite material powder in the alumina container was then determined. The value obtained by dividing this mass by the volume (internal volume) of the alumina container was defined as the bulk density when lightly packed.
[0102] (Heavy-duty bulk density) A powder molding die (diameter: 10 mm) containing 0.1 g of P-C composite material powder was pressed into the die using a hydraulic hand press at a density of 102 kgf / cm². 2 After applying the load, the total length (h) of the mold was measured. The thickness (t) of the P-C composite material powder after pressing was calculated from the difference between the total length (h) of the mold and the total length (H) of the empty powder molding die. The bulk density of the heavy load was calculated by dividing the mass of the P-C composite material powder by the volume of the P-C composite material powder after pressing (the product of the thickness (t) of the P-C composite material powder and the area of the powder molding die).
[0103] (Angle of Repose) The measurement was performed in accordance with JIS R 9301-2-2. 0.5 g of P-C composite material powder was dropped onto a horizontal substrate from a funnel set so that the height of the nozzle tip was 30 mm. The base angle was calculated from the diameter and height of the resulting conical deposit, and the angle of repose was determined from this base angle. The angle of repose was calculated using the following formula: θ = arc tan(2h / D) where θ = angle of repose, h = height of the cone (distance between the substrate and the nozzle tip of the funnel) (mm), and D = diameter of the cone (mm).
[0104] (Particle Size Distribution) A sample of 0.005 g of P-C composite material powder was placed in a beaker with 10 g of deionized water. The sample was dispersed in an ultrasonic cleaner for 1 minute, and then placed in a particle size distribution measurement cell immersed in a 0.2 wt% aqueous solution of sodium hexametaphosphate. The particle size distribution was measured while stirring. A Shimadzu SALAD-2300 was used to measure the particle size distribution. D50, D90, and D10 were determined from the volume-based particle size distribution. The results are shown in Table 1.
[0105] <<Example 2>> A P-C composite material powder was obtained using the same method as in Example 1, except that hard carbon was used instead of natural graphite as the carbon material. In the same manner as in Example 1, lithium ion absorption, light bulk density, heavy bulk density, angle of repose, and particle size distribution were measured.
[0106] <<Example 3>> A P-C composite material powder was obtained in the same manner as in Example 2, except that a planetary ball mill with an orbital diameter of 300 mm, the Retsch PM-400, was used as the planetary ball mill apparatus. In the same manner as in Example 1, lithium ion absorption, light bulk density, heavy bulk density, angle of repose, and particle size distribution were measured.
[0107] <<Comparative Example 1>> A P-C composite material powder was obtained in the same manner as in Example 1, except that a planetary ball mill with an orbital diameter of 141 mm, the Retsch PM-100, was used as the planetary ball mill apparatus, and the mixing time was set to 1 hour. In the same manner as in Example 1, lithium ions were absorbed, and the light bulk density, heavy bulk density, angle of repose, and particle size distribution were measured.
[0108] <<Comparative Example 2>> A P-C composite material powder was obtained using the same method as in Comparative Example 1, except that hard carbon was used instead of natural graphite as the carbon material. In the same manner as in Example 1, lithium ion absorption, light bulk density, heavy bulk density, angle of repose, and particle size distribution were measured.
[0109] <<Comparative Example 3>> A P-C composite material powder was obtained in the same manner as in Comparative Example 1, except that the mixing time in the planetary ball mill was changed from 1 hour to 12 hours. In the same manner as in Example 1, lithium ion absorption, light bulk density, heavy bulk density, angle of repose, and particle size distribution were measured.
[0110] (Evaluation of the negative electrode) (Method for manufacturing the negative electrode) (1) Preparation of the negative electrode P-C composite material powder, conductive material, and binder were weighed and a mixture of [P-C composite material powder]:[conductive material]:[binder] = 80:10:10 (mass ratio) was prepared. The materials used were as follows: Binder: polyvinylidene fluoride PVdF Kureha KF Polymer #1100 (manufactured by Kureha Corporation) Conductive material: acetylene black, Denka Black HS100 (manufactured by Denka Corporation) The above mixture and solvent (NMP (N-methyl-2-pyrrolidone)) were kneaded using an agate mortar to prepare a negative electrode slurry. At this time, the slurry concentration was adjusted so that the content of the negative electrode active material (total of P-C composite material powder, conductive material, and binder) in the negative electrode slurry was 30 to 60% by mass. The negative electrode slurry was applied to a copper foil current collector using a doctor blade, and then the solvent was removed by air drying at 120°C for 1 hour to obtain a laminate. The obtained laminate was then pressurized at 10 MPa for 10 seconds, and then vacuum dried at 120°C for 12 hours to obtain the negative electrode. The preparation of the negative electrode slurry and the negative electrode described above were carried out in a glove box under an argon atmosphere.
[0111] (Electrode warping) The prepared negative electrode was punched out to a diameter of φ15 mm, placed on a glass plate, and the height of the floating edge of the negative electrode was measured with a ruler.
[0112] (Electrode surface condition) The surface condition of the negative electrode was observed visually to confirm the presence or absence of patterns.
[0113] As shown in Tables 1 and 2, it was confirmed that P-C composite material powders with specific light and heavy bulk densities improved the warpage and surface condition of electrodes containing phosphorus-carbon composite materials.
[0114] 100...Laminate, 120...Negative electrode, 121...Negative electrode active material layer, 130...Solid electrolyte layer.
Claims
1. A phosphorus-carbon composite material powder containing phosphorus atoms and carbon atoms, wherein the bulk density of the phosphorus-carbon composite material powder is 1.4 to 2.7 g / cm³. 3 The bulk density of the phosphorus-carbon composite material powder is 0.18 to 2.0 g / cm³. 3 This is a phosphorus-carbon composite material powder.
2. The phosphorus-carbon composite material powder according to claim 1, wherein at least a portion of the phosphorus atoms have a black phosphorus structure.
3. The phosphorus-carbon composite material powder according to claim 1 or 2, wherein the phosphorus-carbon composite material powder is obtained by mixing black phosphorus and a carbon material in a stirring-type pulverizer.
4. A negative electrode active material comprising the phosphorus-carbon composite material powder described in claim 1 or 2.
5. A negative electrode having a negative electrode active material layer containing the phosphorus-carbon composite material powder described in claim 1 or 2.
6. A secondary battery comprising the negative electrode described in claim 5.