Curable composition, cured film, and display device

The curable composition with balanced weight loss ratio and clogP values enhances developability and luminescence intensity, addressing the limitations of existing compositions for semiconductor particle films in display devices.

WO2026235120A1PCT designated stage Publication Date: 2026-11-12SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017332
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-01
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing curable compositions used to form films with semiconductor particles, such as those containing quantum dots, often lack good developability and luminescence intensity, which are crucial for display devices.

Method used

A curable composition comprising semiconductor particles with an organic ligand, a polymerizable compound, and a polymerization initiator, where the weight loss ratio and clogP balance is optimized to achieve a value Z between 115 and 600, enhancing developability and luminescence intensity.

Benefits of technology

The optimized composition results in a cured film with improved developability and luminescence intensity, suitable for use in display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a curable composition capable of forming a cured film having good developability, a cured film formed from the curable composition, and a display device including the cured film. The present invention relates to a curable composition containing semiconductor particles (A), a polymerizable compound (D), and a polymerization initiator (E), in which the semiconductor particles (A) contain an organic ligand (G), and the value Z obtained from formula (1) falls between 115 and 600. Formula (1): Z=X×Y (In formula (1), X represents the 300°C or higher weight loss ratio (%) determined by formula (2) when semiconductor particles (A) containing an organic ligand (G) are heated from 25°C to 600°C at a heating rate of 10°C / min in a nitrogen atmosphere by thermogravimetric analysis. Y represents clogP of the polymerization initiator (E). ) Formula (2): 300°C or higher weight loss ratio X (%)={T1 / (T0+T1)}×100 (In formula (2), T0: weight loss ratio between 100°C and 300°C, based on the weight of the semiconductor particles (A) containing an organic ligand (G) at 100°C, and T1: weight loss ratio between 300°C and 600°C, based on the weight of the semiconductor particles (A) containing an organic ligand (G) at 100°C)
Need to check novelty before this filing date? Find Prior Art

Description

Curable composition, cured film, and display device

[0001] The present invention relates to a curable composition, a cured film, and a display device containing the cured film.

[0002] Patent Document 1 describes a composition, a cured film, and a display device comprising quantum dots (A) and resin (B).

[0003] Japanese Patent Publication No. 2021-105108

[0004] In compositions containing semiconductor particles such as quantum dots, various resins, polymerization initiators, polymerizable compounds, etc., are used, and in some cases, the cured film formed from such a composition is required to have good developability. Therefore, the present invention aims to provide a curable composition capable of forming a cured film with good developability, a cured film formed from the curable composition, and a display device containing the cured film.

[0005] The present invention, which has achieved the above objectives, is as follows: [1] A curable composition comprising semiconductor particles (A), a polymerizable compound (D), and a polymerization initiator (E), wherein the semiconductor particles (A) contain an organic ligand (G), and the value Z obtained from formula (1) satisfies 115 to 600. Z = X × Y …(1) (In equation (1), X represents the weight loss ratio (%) above 300°C, calculated by equation (2), when semiconductor particles (A) containing an organic ligand (G) are heated from 25°C to 600°C in a nitrogen atmosphere at a heating rate of 10°C / min by thermogravimetric analysis. Y represents the clogP of the polymerization initiator (E).) Weight loss ratio above 300°C X (%) = {T1 / (T0 + T1)} × 100 …(2) (In equation (2), T0: Weight loss ratio from 100°C to 300°C, relative to the weight of semiconductor particles (A) containing an organic ligand (G) at 100°C. T1: Weight loss ratio from 300°C to 600°C, relative to the weight of semiconductor particles (A) containing an organic ligand (G) at 100°C.) [2] The curable composition according to [1], wherein the weight loss ratio X at 300°C or higher is 30% or less. [3] The curable composition according to [1] or [2], wherein the clogP of the polymerization initiator (E) is 1 to 25. [4] The curable composition according to any one of [1] to [3], wherein the polymerization initiator (E) contains an oxime compound. [5] The curable composition according to any one of [1] to [4], further comprising a light scattering agent (B). [6] The curable composition according to any one of [1] to [5], further comprising a resin (C). [7] The curable composition according to any one of [1] to [6], wherein the content of the polymerizable compound (D) is 3% by mass or more and 30% by mass or less based on 100% by mass of the total amount of solids in the curable composition.[8] The curable composition according to any one of [1] to [7], wherein the polymerizable compound (D) comprises at least one selected from the group consisting of di(meth)acrylate of ethoxylated bisphenol A, di(meth)acrylate of propoxylated bisphenol A, di(meth)acrylate of ethoxylated bisphenol F, di(meth)acrylate of propoxylated bisphenol F, di(meth)acrylate of ethoxylated bisphenol fluorene, di(meth)acrylate of propoxylated bisphenol fluorene, a compound obtained by monoesterifying pentaerythritol tri(meth)acrylate with succinic acid, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. [9] The curable composition according to any one of [1] to [8], further comprising a polymerization initiator (E), wherein the polymerization initiator (E) comprises an oxime compound.

[10] A cured film formed from the curable composition according to any one of [1] to [9]. A display device comprising the cured film described in

[11] and

[10] .

[0006] According to the present invention, it is possible to provide a curable composition capable of forming a cured film with good developability, a cured film formed from the curable composition, and a display device containing the cured film.

[0007] <<Curable Composition>> The curable composition comprises semiconductor particles (A), a polymerizable compound (D), and a polymerization initiator (E), and preferably includes at least one selected from a light scattering agent (B), a resin (C), an antioxidant (Fa), a leveling agent (H), and a solvent (J) as needed.

[0008] In this specification, unless otherwise specified, the compounds exemplified as components may be used individually or in combination of two or more. Furthermore, when using multiple types of components, unless otherwise specified, the content should be adjusted by the total amount of all components used.

[0009] The curable composition is characterized in that the value Z obtained from formula (1) is between 115 and 600. Z = X × Y …(1) (In equation (1), X represents the weight loss ratio (%) above 300°C, calculated by equation (2), when semiconductor particles (A) containing an organic ligand (G) are heated from 25°C to 600°C in a nitrogen atmosphere at a heating rate of 10°C / min by thermogravimetric analysis. Y represents the clogP of the polymerization initiator (E).) Weight loss ratio above 300°C X (%) = {T1 / (T0 + T1)} × 100 …(2) (In equation (2), T0: Weight loss ratio from 100°C to 300°C, relative to the weight of semiconductor particles (A) containing an organic ligand (G) at 100°C. T1: Weight loss ratio from 300°C to 600°C, relative to the weight of semiconductor particles (A) containing an organic ligand (G) at 100°C.)

[0010] The value Z is obtained from the product of the weight loss ratio X above 300°C and Y, represented by the clogP of the polymerization initiator (E). It represents the degree of influence of the balance between hydrophobicity and hydrophilicity of the semiconductor particles (A) containing the organic ligand (G) and the degree of hydrophobicity of the polymerization initiator (E), and is considered an evaluation parameter for developability. From the viewpoint of good developability, the value Z is preferably 115 to 550, more preferably 115 to 500, even more preferably 115 to 450, even more preferably 115 to 350, even more preferably 115 to 250, and particularly preferably 115 to 200. In addition, the value Z can be considered not only as an evaluation parameter for developability but also for luminescence intensity, and the value Z is most preferably 115 to 190. When the value Z satisfies the above range, both developability and luminescence intensity can be improved. The reason why the curable composition of the present invention provides the above effects is not necessarily clear, but the inventors speculate as follows. In other words, when the value Z is within the above range, the balance between hydrophobicity and hydrophilicity in the curable composition is appropriately maintained, resulting in good solubility in the developer. Furthermore, when the value Z is within the above range, the dispersibility of the semiconductor particles (A) can be improved, which tends to improve the luminescence intensity.

[0011] <Semiconductor Particle (A)> Semiconductor particle (A) is preferably a light-emitting inorganic semiconductor particle that absorbs primary light and emits light of a different wavelength than the primary light, and more preferably the light-emitting inorganic semiconductor particle absorbs primary light and emits green or red light, and even more preferably it converts the wavelength of blue light, which is the primary light, to the wavelength of red light or the wavelength of green light.

[0012] In this specification, "blue" refers to all light that is perceived as blue (all light with intensity in the blue wavelength range, for example, 380 nm to 495 nm), and is not limited to light of a single wavelength. "Green" refers to all light that is perceived as green (all light with intensity in the green wavelength range, for example, 495 nm to 585 nm), and is not limited to light of a single wavelength. "Red" refers to all light that is perceived as red (all light with intensity in the red wavelength range, for example, 585 nm to 780 nm), and is not limited to light of a single wavelength.

[0013] Examples of semiconductor particles (A) include quantum dots and particles composed of compounds having a perovskite crystal structure (hereinafter referred to as "perovskite compounds"), with quantum dots being preferred. Quantum dots are luminescent inorganic semiconductor nanoparticles with a particle size of 1 nm to 100 nm (preferably 1 nm to 50 nm, more preferably 1 nm to 30 nm), which utilize the band gap of the semiconductor to absorb ultraviolet light or visible light (e.g., blue light) and emit light.

[0014] Examples of quantum dots include CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, HgS, HgSe, HgTe, CdHgTe, CdSeS, CdSeTe, CdSte, ZnSeS, ZnSeTe, ZnSte, HgSeS, HgSeTe, HgSte, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSte, CdHgSeS, CdHgSte, CdHgSte, HgZnSeS, HgZn Examples include compounds of group 12 elements and group 16 elements such as SeTe and HgZnSte; compounds of group 13 elements and group 15 elements such as GaN, GaP, GaAs, AlN, AlP, AlAs, InN, InP, InAs, GaNP, GaNAs, GaPAs, AlNP, AlNAs, AlPAs, InNP, InNAs, InPAs, GaAlNP, GaAlNAs, GaAlPAs, GaInNP, GaInNAs, GaInPAs, InAlNP, InAlNAs, InAlPAs; and compounds of group 14 elements and group 16 elements such as PdS and PbSe. Among these, quantum dots are preferably compounds of group 12 elements and group 16 elements, or compounds of group 13 elements and group 15 elements.

[0015] If the quantum dots contain sulfur (S) or senium (Se), quantum dots that have been surface-modified with metal oxides or organic materials may be used. By using surface-modified quantum dots, it is possible to prevent the extraction of S or Se by reactive components contained in or that may be contained in the curable composition.

[0016] Furthermore, the quantum dots may form a core-shell structure by combining the above-mentioned compounds. From the viewpoint of luminescence intensity, the core and shell are preferably selected from the group consisting of compounds of group 12 and group 16 elements and compounds of group 13 and group 15 elements. More preferably, the core is selected from the group consisting of compounds of group 12 and group 16 elements and compounds of group 13 and group 15 elements, and the shell is more preferably a compound of group 12 and group 16 elements. It is even more preferably that the core is selected from the group consisting of CdS, CdSe, CdTe, InN, InP, and InAs, and it is even more preferably that the shell is selected from the group consisting of ZnS, ZnSe, ZnTe, ZnSeS, ZnSeTe, and ZnSTe. Among these, examples include fine particles in which the core is CdSe and the shell is ZnS, fine particles in which the core is InP and the shell is ZnSeS, and fine particles in which the core is InP and the shells are ZnSe and ZnS.

[0017] Since the energy state of a quantum dot depends on its size, the emission wavelength can be freely selected by changing the particle size. Furthermore, because the light emitted from quantum dots has a narrow spectral width, it is advantageous for widening the color gamut of display devices. In addition, quantum dots have high responsiveness, which is advantageous in terms of primary light utilization efficiency.

[0018] Examples of perovskite compounds include those described in Japanese Patent Publication No. 2024-61630.

[0019] The curable composition may contain one or more types of semiconductor particles (A). The curable composition may contain only semiconductor particles that emit light of a specific wavelength, or it may contain two or more types of semiconductor particles that emit light of different wavelengths.

[0020] From the viewpoint of luminescence intensity, the content of semiconductor particles (A) in the curable composition is preferably 3% to 60% by mass, more preferably 10% to 55% by mass, even more preferably 20% to 50% by mass, and particularly preferably 25% to 45% by mass, based on 100% by mass of the solid content of the curable composition.

[0021] In this specification, the total amount of solids in a curable composition means the sum of the components contained in the curable composition, excluding the solvent (J). The content of each component in the solids of a curable composition can be measured by known analytical means such as liquid chromatography or gas chromatography. The content of each component in the solids of a curable composition may be calculated from the formulation at the time of preparation of the curable composition.

[0022] <Organic Ligand (G)> The semiconductor particles (A) contain an organic ligand (G) (hereinafter sometimes referred to as coordination-type semiconductor particles (AG)), and it is preferable that the organic ligand (G) is present in the curable composition in a coordinated state. The organic ligand (G) is, for example, an organic compound having a polar group and an organic group that exhibits coordinating ability to the semiconductor particles (A). The organic ligand (G) can, for example, coordinate to the surface of the semiconductor particles (A). The curable composition may contain one or more organic ligands (G).

[0023] Preferably, at least some of the molecules of the organic ligand (G) are coordinated to the semiconductor particles (A), and all or almost all of the molecules may be coordinated to the semiconductor particles (A). Including organic ligands (G) coordinated to semiconductor particles (A) can be advantageous in terms of the stability and dispersibility of the semiconductor particles (A), as well as improving the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0024] The above polar group of the organic ligand (G) is, for example, a phosphine group (-PR a 2. R a (wherein it represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms (preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms)), a phosphine oxide group (-PR b 2O, R bThe group is at least one group selected from the group consisting of a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms, a thiol group (-SH), a carboxyl group (-COOH), and an amino group (-NH2). A polar group selected from this group may be advantageous in enhancing the coordination to the semiconductor particle (A). High coordination can contribute to improving the stability and dispersibility of the semiconductor particle (A) in the curable composition, as well as improving the luminescence intensity when the cured film is used as a wavelength conversion layer. In particular, from the viewpoint of increasing luminescence intensity, it is more preferable that the polar group is at least one group selected from the group consisting of a thiol group and a carboxyl group. The organic ligand (G) may have one or more polar groups.

[0025] The organic group of the organic ligand (G) is preferably a hydrocarbon group. The hydrocarbon group may contain heteroatoms (such as N, O, S, halogen atoms, etc.). The hydrocarbon group is preferably an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, or an aromatic hydrocarbon group.

[0026] Examples of aliphatic hydrocarbon groups include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, henicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, hentriacontyl, dotriacontyl, tritriacontyl, tetratriacontyl, pentatriacontyl, hexatriacontyl, heptatriacontyl, octatriacontyl, nonatriacontyl, and tetracontyl; Isopropyl group, isobutyl group, sec-butyl group, tert-butyl group, 2-ethylbutyl group, 3,3-dimethylbutyl group, 1,1,3,3-tetramethylbutyl group, 1-methylbutyl group, 1-ethylpropyl group, 3-methylbutyl group, neopentyl group, 1,1-dimethylpropyl group, 2-methylpentyl group, 3-ethylpentyl group, 1,3-dimethylbutyl group, 2-propylpentyl group, 1-ethyl-1,2-dimethylpropyl group, 1-methylpentyl group, 4-methylpentyl group, 4-methylpentyl group Branched alkyl groups such as hexyl group, 5-methylhexyl group, 2-ethylhexyl group, 1-methylhexyl group, 1-ethylpentyl group, 1-propylbutyl group, 3-ethylheptyl group, 2,2-dimethylheptyl group, 1-methylheptyl group, 1-ethylhexyl group, 1-propylpentyl group, 1-methyloctyl group, 1-ethylheptyl group, 1-propylhexyl group, 1-butylpentyl group, 1-methylnonyl group, 1-ethyloctyl group, 1-propylheptyl group, and 1-butylhexyl group;Ethenyl group (vinyl group), propenyl group (e.g., 1-propenyl group, 2-propenyl group (allyl group)), 1-methylethenyl group, butenyl group (e.g., 1-butenyl group, 2-butenyl group, 3-butenyl group), 3-methyl-1-butenyl group, 1,3-butadienyl group, 1-(2-propenyl)ethenyl group, 1-(1-methylethenyl)ethenyl group, 1,2-dimethyl-1-propenyl group, pentenyl group (e.g., 1-pentenyl group, 2-pentenyl group, 3-pentenyl group, 4-pentenyl group), 1-(1,1-dimethylethyl)ethenyl group, 1,3-dimethyl-1-butenyl group, hexenyl group (e.g., Alkenyl groups such as 1-hexenyl group, 5-hexenyl group, heptenyl group (e.g., 1-heptenyl group, 6-heptenyl group), octenyl group (e.g., 1-octenyl group, 7-octenyl group), nonenyl group (e.g., 1-nonenyl group, 8-nonenyl group), decenyl group (e.g., 1-decenyl group, 9-decenyl group), undecenyl group, dodecenyl group, tridecenyl group, tetradecenyl group, pentadecenyl group, hexadecenyl group, heptadecenyl group, octadecenyl group, nonadecenyl group, icocenyl group, 1,1-dimethyl-2-propenyl group, 1-ethyl-2-propenyl group, and 1-methyl-1-butenyl group; Examples include ethylyl groups, propynyl groups (e.g., 1-propynyl, 2-propynyl), octinyl groups (e.g., 1-octinyl, 7-octinyl), butynyl, pentynyl, hexynyl, heptynyl, noninyl, desinyl, undecynyl, dodecynyl, tridecynyl, tetradecynyl, pentadecynyl, hexadecinyl, heptadecynyl, octadecynyl, nonadecinyl, and icosinyl groups; and other alkynyl groups.

[0027] The number of carbon atoms in the aliphatic hydrocarbon group is preferably 1 to 40, more preferably 2 to 30, and even more preferably 3 to 20.

[0028] Examples of alicyclic hydrocarbon groups include cyclopropyl group, 1-methylcyclopropyl group, cyclobutyl group, cyclopentyl group, cyclohexyl group, cycloheptyl group, 1-methylcyclohexyl group, 2-methylcyclohexyl group, 3-methylcyclohexyl group, 4-methylcyclohexyl group, 1,2-dimethylcyclohexyl group, 1,3-dimethylcyclohexyl group, 1,4-dimethylcyclohexyl group, 2,3-dimethylcyclohexyl group, 2,4-dimethylcyclohexyl group, 2,5-dimethylcyclohexyl group, 2,6-dimethylcyclohexyl group, 3,4-dimethylcyclohexyl group, 3,5-dimethylcyclohexyl group, 2,2-dimethylcyclohexyl group, 3,3-dimethylcyclohexyl group, and 4,4 Examples include cycloalkyl groups such as dimethylcyclohexyl group, cyclooctyl group, 2,4,6-trimethylcyclohexyl group, 2,2,6,6-tetramethylcyclohexyl group, 3,3,5,5-tetramethylcyclohexyl group, 4-pentylcyclohexyl group, 4-octylcyclohexyl group, and 4-cyclohexylcyclohexyl group; cycloalkenyl groups such as cyclohexenyl group (e.g., cyclohexa-1-en-1-yl group, cyclohexa-2-en-1-yl group, cyclohexa-3-en-1-yl group), cycloheptenyl group, and cyclooctenyl group; saturated or unsaturated polycyclic hydrocarbon groups such as norbornyl group, norborneyl group, adamantyl group, and bicyclo[2.2.2]octyl group; and so on.

[0029] The number of carbon atoms in the alicyclic hydrocarbon group is preferably 3 to 40, more preferably 3 to 30, and even more preferably 3 to 20.

[0030] Aromatic hydrocarbon groups include phenyl group, o-tolyl group, m-tolyl group, p-tolyl group, 2-ethylphenyl group, 3-ethylphenyl group, 4-ethylphenyl group, 2,3-dimethylphenyl group, 2,4-dimethylphenyl group, 2,5-dimethylphenyl group, 2,6-dimethylphenyl group, 3,4-dimethylphenyl group, 3,5-dimethylphenyl group, 4-vinylphenyl group, o-isopropylphenyl group, m-isopropylphenyl group, p-isopropylphenyl group, o-tert-butylphenyl group, m-tert-butylphenyl group, p-tert-butylphenyl group, 3,5-di(tert-butyl)phenyl group, 3,5-di(tert-butyl)-4-methylphenyl group, and 4-butyl Aromatic hydrocarbon groups such as phenyl group, 4-pentylphenyl group, 2,6-bis(1-methylethyl)phenyl group, 2,4,6-tris(1-methylethyl)phenyl group, 4-cyclohexylphenyl group, 2,4,6-trimethylphenyl group, 4-octylphenyl group, 4-(1,1,3,3-tetramethylbutyl)phenyl group, 1-naphthyl group, 2-naphthyl group, 6-methyl-2-naphthyl group, 5,6,7,8-tetrahydro-1-naphthyl group, 5,6,7,8-tetrahydro-2-naphthyl group, fluorenyl group, phenanthryl group, anthryl group, 2-dodecylphenyl group, 3-dodecylphenyl group, 4-dodecylphenyl group, perilenyl group, chrysenyl group, and pyrenyl group; and the like.

[0031] The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 40, more preferably 6 to 30, and even more preferably 6 to 20.

[0032] The hydrocarbon group may further have hydrophilic functional groups. The hydrophilic functional groups are preferably hydroxyl groups, carboxyl groups, carbonyl groups, thiol groups, amino groups, ether bonds, ester bonds, and siloxane bonds. If the hydrocarbon group has an ether bond, the -CH2- constituting the hydrocarbon group may be replaced with -O-. If the hydrocarbon group has an ester bond, the -CH2-CH2-CH2- constituting the hydrocarbon group may be replaced with -C(=O)-O- or -O-C(=O)-. If the hydrocarbon group has a siloxane bond, the -CH2-CH2- constituting the hydrocarbon group may be replaced with -Si-O-. Furthermore, the methylene group contained in the hydrocarbon group may be replaced with -S-, -C(=O)-, -C(=O)-NH-, -NH-, etc.

[0033] The organic ligand (G) preferably contains at least one selected from the group consisting of a hydrophobic organic ligand (G1) and a hydrophilic organic ligand (G2). The hydrophobic organic ligand (G1) is preferably a compound having the above-mentioned polar group and the above-mentioned hydrocarbon group (preferably a hydrocarbon group without a hydrophilic functional group). The hydrophilic organic ligand (G2) is preferably a compound having the above-mentioned polar group and a hydrocarbon group having a hydrophilic functional group. The presence of a hydrophilic functional group in the organic group enables dispersion in a polar dispersion medium. The organic ligand (G) may contain one or more hydrophobic organic ligands (G1) and hydrophilic organic ligands (G2).

[0034] A hydrophobic organic ligand (G1) is, for example, given by the following formula (x): X A -R X It is preferable that the organic compound is represented by (x). In the formula, X A R is the polar group described above, X It is preferable that the hydrocarbon group is a monovalent hydrocarbon group which may contain heteroatoms (such as N, O, S, halogen atoms, etc.). The hydrocarbon group may have one or more unsaturated bonds, such as carbon-carbon double bonds. The hydrocarbon group may have a linear, branched, or cyclic structure. The number of carbon atoms in the hydrocarbon group is, for example, 1 to 40, and may be 1 to 30.X is more preferably a monovalent aliphatic hydrocarbon group. The monovalent aliphatic hydrocarbon group may be the same as the aforementioned aliphatic hydrocarbon group. Among them, the hydrocarbon group is preferably an alkyl group, alkynyl group, or alkenyl group having 1 to 40 carbon atoms (preferably 1 to 30 carbon atoms. The organic group of the hydrophobic organic ligand (G1) may contain a substituent such as a halogen atom or a hetero atom (N, O, S).

[0035] X A The polar group represented by is preferably at least one group selected from the group consisting of a phosphine group, a phosphine oxide group, a thiol group, a carboxy group, and an amino group. The number of the polar group may be one or two or more.

[0036] Polar group X A Specific examples of the organic ligand having a carboxy group as include saturated or unsaturated fatty acids. Specific examples of the saturated or unsaturated fatty acid include saturated fatty acids such as propionic acid, butyric acid, pentanoic acid, caproic acid, caprylic acid, capric acid, lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid; monounsaturated fatty acids such as myristoleic acid, palmitoleic acid, oleic acid, icosenoic acid, erucic acid, and nervonic acid; and polyunsaturated fatty acids such as linoleic acid, α-linolenic acid, γ-linolenic acid, stearidonic acid, dihomo-γ-linolenic acid, arachidonic acid, eicosatetraenoic acid, docosadienoic acid, and adrenic acid (docosatetraenoic acid).

[0037] Polar group X A Specific examples of the organic ligand having a thiol group or an amino group as include the polar group X exemplified above A and organic ligands in which the carboxy group of the organic ligand having a carboxy group as is replaced with a thiol group or an amino group. Polar group X A Specific examples of the organic ligand having a thiol group as include hexanethiol, octanethiol, decanethiol, 1-dodecanethiol, and the like. Polar group X A Specific examples of the organic ligand having an amino group as include oleylamine and the like. Polar group XA Examples of organic ligands having a phosphine group or a phosphine oxide group include trioctylphosphine and trioctylphosphine oxide.

[0038] From the viewpoint of improving the stability and dispersibility of semiconductor particles, the molecular weight of the hydrophobic organic ligand (G1) is preferably 1500 or less, more preferably 1000 or less, and even more preferably 800 or less. The molecular weight of the hydrophobic organic ligand (G1) is usually 100 or more. The above molecular weight may be the number average molecular weight or the weight average molecular weight. In this case, the number average molecular weight and the weight average molecular weight are the number average molecular weight and the weight average molecular weight on a standard polystyrene basis, measured by gel permeation chromatography (GPC), respectively.

[0039] Examples of hydrophilic organic ligands (G2) include compound (G2-1) and compound (G2-2).

[0040] [Compound (G2-1)] Compound (G2-1) is preferably a compound having a first functional group, a second functional group, and a divalent organic group. The first functional group is preferably a carboxyl group (-COOH) or a hydroxyl group (-OH), and the second functional group is preferably a carboxyl group or a thiol group (-SH). The first and second functional groups correspond to the hydrophilic functional group and the polar group, respectively. There may be one or more first and second functional groups. Since compound (G2-1) has a carboxyl group, a thiol group, and a hydroxyl group, it can be a ligand that coordinates to semiconductor particles (A). The curable composition may contain only one compound (G2-1) or two or more. The divalent organic group may be any hydrocarbon group that is divalent as described above.

[0041] An example of compound (G2-1) is the compound represented by the following formula (G2-1a). Compound (G2-1) may also be the acid anhydride of the compound represented by formula (G2-1a).

[0042]

[0043] [In the formula, R B R represents a divalent hydrocarbon group.B If present, they may be the same or different. The hydrocarbon group may have one or more substituents. If there are multiple substituents, they may be the same or different, and they may be bonded to each other, forming a ring with the atom to which each substituent is bonded. The -CH2- contained in the hydrocarbon group may be replaced with at least one of -O-, -S-, -SO2-, -CO-, and -NH-. p represents an integer from 1 to 10.

[0044] R B Examples of divalent hydrocarbon groups represented by this symbol include chain hydrocarbon groups, alicyclic hydrocarbon groups, aromatic hydrocarbon groups, and groups that combine these.

[0045] Examples of linear hydrocarbon groups include linear or branched alkanediyl groups, which typically have 1 to 40 carbon atoms, preferably 1 to 20, and more preferably 1 to 10. Examples of alicyclic hydrocarbon groups include monocyclic or polycyclic cycloalkanediyl groups, which typically have 3 to 40 carbon atoms, preferably 3 to 20, and more preferably 3 to 10. Examples of aromatic hydrocarbon groups include monocyclic or polycyclic arenediyl groups, which typically have 6 to 20 carbon atoms.

[0046] Examples of substituents that the hydrocarbon group may have include C1-C40 alkyl groups, C3-C40 cycloalkyl groups, C6-C20 aryl groups, carboxyl groups, amino groups, and halogen atoms. Preferably, the substituents that the hydrocarbon group may have are carboxyl groups, amino groups, or halogen atoms.

[0047] When the -CH2- contained in the above hydrocarbon group is replaced by at least one of -O-, -CO-, and -NH-, the -CH2- is preferably replaced by at least one of -CO- and -NH-, and more preferably by -NH-. p is preferably 1 or 2.

[0048] Examples of compounds represented by formula (G2-1a) include those represented by the following formulas (1-1) to (1-9).

[0049]

[0050] Specific examples of compounds represented by formula (G2-1a), listed by their chemical names, include, for example, mercaptoacetic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, 3-mercaptobutanoic acid, 4-mercaptobutanoic acid, mercaptohexanoic acid, mercaptooctanoic acid, mercaptoundecanoic acid, mercaptosuccinic acid, mercaptostearic acid, 4-mercaptobenzoic acid, 2,3,5,6-tetrafluoro-4-mercaptobenzoic acid, L-cysteine, N-acetyl-L-cysteine, 3-methoxybutyl 3-mercaptopropionic acid, and 3-mercapto-2-methylpropionic acid. Among these, 3-mercaptopropionic acid and mercaptosuccinic acid are preferred.

[0051] Another example of compound (G2-1) is a polycarboxylic acid compound, preferably a compound (G2-1b) in which the -SH in formula (G2-1a) is replaced with a carboxyl group (-COOH).

[0052] Examples of compounds (G2-1b) include the following:

[0053] Succinic acid, glutaric acid, adipic acid, octafluoroadipic acid, azelaic acid, dodecanediic acid, tetradecanediic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanediic acid, nonadecanedioic acid, dodecafluoroseveric acid, 3-ethyl-3-methylglutaric acid, hexafluoroglutaric acid, trans-3-hexenodioic acid, sebacic acid, hexadecafluorosebacic acid, acetylenedicarboxylic acid, trans-aconitic acid, 1,3-adamantanedicarboxylic acid, bicyclo[2.2.2]octane-1,4-dicarboxylic acid, cis-4-silicon Chlohexene-1,2-dicarboxylic acid, 1,1-cyclopropanedicarboxylic acid, 1,1-cyclobutanedicarboxylic acid, cis- or trans-1,3-cyclohexanedicarboxylic acid, cis- or trans-1,4-cyclohexanedicarboxylic acid, 1,1-cyclopentanediacetic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, decahydro-1,4-naphthalenedicarboxylic acid, 2,3-norbornanedicarboxylic acid, 5-norbornene-2,3-dicarboxylic acid, phthalic acid, 3-fluorophthalic acid, isophthalic acid, tetrafluoroiso Phthalic acid, terephthalic acid, tetrafluoroterephthalic acid, 2,5-dimethylterephthalic acid, 2,6-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,1'-ferrocenedicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 2,5-franzicarboxylic acid, benzophenone-2,4'-dicarboxylic acid monohydrate, benzophenone-4,4'-dicarboxylic acid, 2,3-pyrazinedicarboxylic acid, 2,3-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 3,5-Pyridinedicarboxylic acid, 2,5-Pyridinedicarboxylic acid, 2,6-Pyridinedicarboxylic acid, 3,4-Pyridinedicarboxylic acid, Pyrazole-3,5-dicarboxylic acid monohydrate, 4,4'-Stilbenidicarboxylic acid, Anthraquinone-2,3-dicarboxylic acid, 4-(carboxymethyl)benzoic acid, Cheridonic acid monohydrate, Azobenzene-4,4'-dicarboxylic acid, Azobenzene-3,3'-dicarboxylic acid, Chlorendic acid, 1H-Imidazole-4,5-dicarboxylic acid, 2,2-Bis(4-carboxyphenyl)hexafluoropropane, 1,10-Bis(4-carboxyphenoxy)decane, dipropylmalonic acid, dithiodiglycolic acid, 3,3'-dithiodipropionic acid, 4,4'-dithiodibutanoic acid, 4,4'-dicarboxydiphenyl ether, 4,4'-dicarboxydiphenyl sulfone, ethylene glycol bis(4-carboxyphenyl) ether, 3,4-ethylenedioxythiophene-2,5-dicarboxylic acid, 4,4'-isopropylidenediphenoxyacetic acid, 1,3-acetonedicarboxylic acid, methylenedisalicylic acid, 5,5'-thiodisalicylic acid, tris(2-carboxyethyl) isocyanurate, tetrafluorosuccinic acid, α,α,α',α'-tetramethyl-1,3-benzenedipropionic acid, 1,3,5-benzenetricarboxylic acid, etc.

[0054] From the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer, the molecular weight of compound (G2-1) is preferably 3,000 or less, more preferably 2,500 or less, even more preferably 2,000 or less, still more preferably 1,000 or less, particularly preferably 800 or less, and most preferably 500 or less. The molecular weight of compound (G2-1) is usually 100 or more.

[0055] The above molecular weight may be either the number-average molecular weight Mn or the weight-average molecular weight Mw. In this case, Mn and Mw are standard polystyrene equivalent values ​​measured by gel permeation chromatography (GPC).

[0056] The content ratio of compound (G2-1) to semiconductor particles (A) in the curable composition is preferably 0.001 to 1 by mass, more preferably 0.01 to 0.5, and even more preferably 0.02 to 0.45. Having this content ratio within this range is advantageous in terms of the stability and dispersibility of the semiconductor particles (A), as well as improving the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0057] The content of compound (G2-1) in the curable composition is preferably 0.1% to 20% by mass, more preferably 0.2% to 20% by mass, even more preferably 0.2% to 10% by mass, even more preferably 0.5% to 10% by mass, and particularly preferably 0.5% to 8% by mass, relative to the total amount of solids in the curable composition, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0058] [Compound (G2-2)] Compound (G2-2) is a compound different from compound (G2-1), containing a polyalkylene glycol structure and having polar groups at its molecular ends. Preferably, the molecular end is the end of the longest carbon chain in compound (G2-2) (the carbon atoms in the carbon chain may be replaced by other atoms such as oxygen atoms).

[0059] The semiconductor particle (A) may contain only one compound (G2-2) or two or more compounds. The semiconductor particle (A) may contain compound (G2-1) or compound (G2-2), or may contain compound (G2-1) and compound (G2-2).

[0060] Compounds containing a polyalkylene glycol structure and having the above-mentioned first functional group, second functional group, and divalent organic group shall be classified as compound (G2-1).

[0061] The polyalkylene glycol structure is defined by the following formula:

[0062]

[0063] This refers to a structure represented by (where n is an integer greater than or equal to 2). In the formula, R C This is an alkylene group, such as an ethylene group or a propylene group.

[0064] A specific example of compound (G2-2) is a polyalkylene glycol compound represented by the following formula (G2-2a).

[0065]

[0066] In formula (G2-2a), X is a polar group, Y is a monovalent group, and Z C R is a divalent or trivalent base. n is an integer greater than or equal to 2. m is 1 or 2. C This is an alkylene group.

[0067] Polar group X is a phosphine group (-PR a 2. R a )), phosphine oxide group (-PR b 2O, R b It is preferable that the polar group X is at least one group selected from the group consisting of a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms, a thiol group (-SH), a carboxyl group (-COOH), and an amino group (-NH2). A polar group selected from this group may be advantageous in improving coordination to the semiconductor particle (A). In particular, from the viewpoint of improving the stability and dispersibility of the semiconductor particle (A), and the luminescence intensity when the cured film is used as a wavelength conversion layer, it is more preferable that the polar group X is at least one group selected from the group consisting of a thiol group and a carboxyl group, and even more preferable that it is a thiol group.

[0068] Group Y is a monovalent organic group. Group Y is not particularly limited and may include monovalent hydrocarbon groups that have substituents (N, O, S, halogen atoms, etc.). The -CH2- contained in the hydrocarbon group may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. The number of carbon atoms in the hydrocarbon group is, for example, 1 to 12. The hydrocarbon group may have unsaturated bonds.

[0069] Examples of group Y include alkyl groups having 1 to 12 carbon atoms and having a linear, branched, or cyclic structure; and alkoxy groups having 1 to 12 carbon atoms and having a linear, branched, or cyclic structure. The number of carbon atoms in the alkyl and alkoxy groups is preferably 1 to 8, more preferably 1 to 6, and even more preferably 1 to 4. The -CH2- contained in the alkyl and alkoxy groups may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. In particular, group Y is preferably a linear or branched alkoxy group having 1 to 4 carbon atoms, and more preferably a linear alkoxy group having 1 to 4 carbon atoms.

[0070] Group Y may contain a polar group. The polar group may be a phosphine group (-PR a 2. R a ) represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms (preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms). ), phosphine oxide group (-PR b 2O, R b The group includes at least one selected from the group consisting of a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms, a thiol group (-SH), a carboxyl group (-COOH), and an amino group (-NH2). However, as described above, compounds containing a polyalkylene glycol structure and having the above-mentioned first and second functional groups belong to compound (G2-2). The polar group is preferably located at the terminal end of group Y.

[0071] Base Z C It is a divalent or trivalent group. Group Z C Examples include divalent or trivalent hydrocarbon groups, which are not particularly limited and may contain heteroatoms (such as N, O, S, halogen atoms, etc.). The number of carbon atoms in the hydrocarbon group is, for example, 1 to 24. The hydrocarbon group may have unsaturated bonds.

[0072] The divalent group Z CExamples include alkylene groups having 1 to 24 carbon atoms and having a linear, branched, or cyclic structure; and alkenylene groups having 1 to 24 carbon atoms and having a linear, branched, or cyclic structure. The number of carbon atoms in the alkyl and alkenylene groups is preferably 1 to 12, more preferably 1 to 8, and even more preferably 1 to 4. The -CH2- contained in the alkyl and alkenylene groups may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. The group Z is a trivalent group. C An example of this is the divalent group Z mentioned above. C We can give an example of a group obtained by removing one hydrogen atom from the same group.

[0073] Base Z C The group Z may have a branched structure. C In a branch chain separate from the branch chain containing the polyalkylene glycol structure shown in formula (G2-2a) above, the branch chain may have a polyalkylene glycol structure separate from the polyalkylene glycol structure shown in formula (G2-2a) above.

[0074] In particular, Base Z C It is preferably a linear or branched alkylene group having 1 to 6 carbon atoms, and more preferably a linear alkylene group having 1 to 4 carbon atoms.

[0075] R C The group is an alkylene group, preferably a linear or branched alkylene group having 1 to 6 carbon atoms, and more preferably a linear alkylene group having 1 to 4 carbon atoms.

[0076] In formula (G2-2a), n is an integer of 2 or more, preferably 2 to 540, more preferably 2 to 120, even more preferably 2 to 60, even more preferably 2 to 30, even more preferably 2 to 15, and particularly preferably 2 to 10.

[0077] Specific examples of compound (G2-2) include, but are not limited to, HS-PEG-COOH, PEG-SH, polyethylene glycol monomethyl ether thiol, polypropylene glycol monomethyl ether thiol, 3-mercaptopropionic acid-PEG ester, etc. Preferably polyethylene glycol monomethyl ether thiol and polypropylene glycol monomethyl ether thiol, and more preferably HS-(CH2CH2O) k It is a compound represented as -CH3 (where k is an integer between 2 and 10).

[0078] The molecular weight of compound (G2-2) may be, for example, 150 to 10,000, but from the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer, it is preferably 150 to 5,000, more preferably 150 to 4,000, even more preferably 150 to 1,500, even more preferably 150 to 1,000, and particularly preferably 150 to 800. The molecular weight may be a number-average molecular weight or a weight-average molecular weight. In this case, the number-average molecular weight and weight-average molecular weight are the number-average molecular weight and weight-average molecular weight on a standard polystyrene basis measured by GPC, respectively.

[0079] The content ratio of compound (G2-2) to semiconductor particles (A) in the curable composition is preferably 0.001 to 2 by mass, more preferably 0.01 to 1.5, and even more preferably 0.1 to 1. Having this content ratio within this range is advantageous in terms of the stability and dispersibility of the semiconductor particles (A), as well as improving the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0080] The content of compound (G2-2) in the curable composition is preferably 0.1% to 40% by mass, more preferably 0.1% to 20% by mass, even more preferably 1% to 15% by mass, and still more preferably 2% to 12% by mass, relative to the total amount of solids in the curable composition, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0081] To improve the dispersion of semiconductor particles (A) and thus enhance luminescence intensity, the composition ratio of hydrophilic organic ligands (G2) is preferably 60% or more, more preferably 62% or more, even more preferably 65% ​​or more, even more preferably 80% or more, and 85% or more, relative to all organic ligands (G) that coordinate to semiconductor particles (A). Furthermore, the composition ratio is preferably 95% or less, and more preferably 90% or less. The composition ratio of hydrophilic organic ligands (G2) relative to all organic ligands (G) that coordinate to semiconductor particles (A) can be determined from {T0 / (T0+T1)} × 100 (where T0 and T1 are the same as above). Specifically, it can be determined by the method described in the examples.

[0082] The semiconductor particle (A) preferably contains a hydrophobic organic ligand (G1) and a hydrophilic organic ligand (G2) as an organic ligand (G), more preferably contains a compound represented by formula (x) and a polyalkylene glycol compound represented by formula (G2-2a), and even more preferably contains oleic acid, 1-dodecanethiol, trioctylphosphine and triethylene glycol monomethyl etherthiol.

[0083] The ratio of the content of organic ligands (G) to semiconductor particles (A) in the curable composition is preferably 0.001 or more and 1 or less by mass, more preferably 0.01 or more and 0.8 or less, and even more preferably 0.02 or more and 0.5 or less. Having this content ratio within this range can be advantageous in terms of the stability and dispersibility of the semiconductor particles (A), and in improving the luminescence intensity when the cured film is used as a wavelength conversion layer. The content of organic ligands (G) as used herein refers to the total content of all organic ligands contained in the curable composition.

[0084] The weight loss ratio X above 300°C of semiconductor particles (A) or coordination semiconductor particles (AG) containing an organic ligand (G) is preferably greater than 0% and 40% or less, more preferably 1% to 35%, even more preferably 1% to 30%, even more preferably 3% to 20%, and even more preferably 5% to 14%. When the weight loss ratio above 300°C of semiconductor particles (A) containing an organic ligand (G) is within the above range, the balance between hydrophobicity and hydrophilicity of the semiconductor particles (A) is appropriately controlled, thereby improving developability and / or luminescence intensity. In other words, the weight loss ratio above 300°C means the composition ratio of hydrophobic organic ligands (G1) to all organic ligands (G) that coordinate to the semiconductor particles (A). The weight loss ratio above 300°C is calculated from {T1 / (T0+T1)} × 100 (T0 and T1 are the same as above). Specifically, it is calculated by the method described in the examples.

[0085] The weight loss ratio of semiconductor particles (A) or coordination-type semiconductor particles (AG) containing an organic ligand (G) at temperatures above 300°C can be adjusted, for example, in a semiconductor particle preparation method in which semiconductor particles are mixed with an organic ligand described later, and then the semiconductor particles are washed one or more times, by adjusting the type, number, and amount of organic ligand (G), or by adjusting the type and amount of solvent, washing temperature, and washing time in the washing process.

[0086] The content of semiconductor particles (A) containing an organic ligand (G) in the curable composition is preferably 10% to 75% by mass, more preferably 12% to 70% by mass, and even more preferably 25% to 60% by mass, relative to the total amount of solids in the curable composition, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0087] <Resin (C)> Resin (C) is preferably an alkali-soluble resin. From the viewpoint of developability, Resin (C) is preferably having at least one structural unit selected from the group consisting of at least one selected from the group consisting of unsaturated carboxylic acids and unsaturated carboxylic acid anhydrides (hereinafter also referred to as "(a)"), a structural unit selected from the group consisting of a monomer (b) having a cyclic ether structure with 2 to 4 carbon atoms and an ethylenically unsaturated bond (hereinafter also referred to as "(b)"), and a structural unit selected from the group consisting of a monomer (c) copolymerizable with (a) (however different from (a) and (b)) (hereinafter also referred to as "(c)"). Resin (C) may further have an ethylenically unsaturated bond and may further have a carboxyl group. Examples of Resin (C) include the following resin [K6]. Examples of other resins include the compounds described in Japanese Patent Application Publication No. 2024-61630.

[0088] Resin [K6]: A copolymer having a structural unit obtained by adding (a) to a structural unit derived from (b) and further ester-bonding a carboxylic acid anhydride, and a structural unit derived from (c).

[0089] (a) includes, for example, unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, o-, m-, p-vinylbenzoic acid; and unsaturated dicarboxylic acids such as maleic acid, fumaric acid, citraconic acid, mesaconic acid, itaconic acid, 3-vinylphthalic acid, 4-vinylphthalic acid, 3,4,5,6-tetrahydrophthalic acid, 1,2,3,6-tetrahydrophthalic acid, dimethyltetrahydrophthalic acid, and 1,4-cyclohexenedicarboxylic acid; Bicyclounsaturated compounds containing carboxyl groups, such as methyl-5-norbornene-2,3-dicarboxylic acid, 5-carboxybicyclo[2.2.1]hept-2-ene, 5,6-dicarboxybicyclo[2.2.1]hept-2-ene, 5-carboxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-carboxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-carboxy-6-methylbicyclo[2.2.1]hept-2-ene, and 5-carboxy-6-ethylbicyclo[2.2.1]hept-2-ene; Examples include unsaturated dicarboxylic acid anhydrides such as maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, and 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride; unsaturated mono[(meth)acryloyloxyalkyl] esters of divalent or higher polycarboxylic acids such as succinate mono[2-(meth)acryloyloxyethyl] and phthalate mono[2-(meth)acryloyloxyethyl]; and unsaturated (meth)acrylates containing both a hydroxyl group and a carboxyl group in the same molecule, such as α-(hydroxymethyl)(meth)acrylic acid.

[0090] Of these, (meth)acrylic acid, mono[2-(meth)acryloyloxyethyl] succinate, maleic anhydride, etc. are preferred from the viewpoint of copolymerization reactivity, etc.

[0091] In this specification, (meth)acrylic acid means acrylic acid and / or methacrylic acid. The same applies to "(meth)acryloyl," "(meth)acrylate," etc.

[0092] (b) is a monomer having, for example, a cyclic ether structure with 2 to 4 carbon atoms (for example, at least one selected from the group consisting of an oxirane ring, an oxetane ring, and a tetrahydrofuran ring) and an ethylenically unsaturated bond. Preferably, (b) is a monomer having a cyclic ether structure with 2 to 4 carbon atoms and a (meth)acryloyloxy group.

[0093] Examples of (b) include monomers having an oxyranyl group and an ethylenically unsaturated bond (b1) (hereinafter sometimes referred to as "(b1)"), monomers having an oxetanyl group and an ethylenically unsaturated bond (b2) (hereinafter sometimes referred to as "(b2)"), monomers having a tetrahydrofuryl group and an ethylenically unsaturated bond (b3) (hereinafter sometimes referred to as "(b3)"), and so on.

[0094] Examples of (b1) include monomers having a linear or branched aliphatic unsaturated hydrocarbon structure that has been epoxidized (b1-1) (hereinafter sometimes referred to as "(b1-1)") and monomers having a cyclic unsaturated hydrocarbon structure that has been epoxidized (b1-2) (hereinafter sometimes referred to as "(b1-2)").

[0095] (b1-1) includes, for example, glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, β-ethylglycidyl (meth)acrylate, glycidyl vinyl ether, o-vinylbenzylglycidyl ether, m-vinylbenzylglycidyl ether, p-vinylbenzylglycidyl ether, α-methyl-o-vinylbenzylglycidyl ether, α-methyl-m-vinylbenzylglycidyl ether, α-methyl-p-vinylbenzylglycidyl ether, 2,3-bis(glycidyl Examples include (zyloxymethyl)styrene, 2,4-bis(glycidyloxymethyl)styrene, 2,5-bis(glycidyloxymethyl)styrene, 2,6-bis(glycidyloxymethyl)styrene, 2,3,4-tris(glycidyloxymethyl)styrene, 2,3,5-tris(glycidyloxymethyl)styrene, 2,3,6-tris(glycidyloxymethyl)styrene, 3,4,5-tris(glycidyloxymethyl)styrene, and 2,4,6-tris(glycidyloxymethyl)styrene.

[0096] Examples of (b1-2) include vinylcyclohexene monooxide, 1,2-epoxy-4-vinylcyclohexane (e.g., Celoxide 2000; manufactured by Daicel Corporation), 3,4-epoxycyclohexylmethyl (meth)acrylate (e.g., Cyclomer A400; manufactured by Daicel Corporation), 3,4-epoxycyclohexylmethyl (meth)acrylate (e.g., Cyclomer M100; manufactured by Daicel Corporation), compounds represented by formula (BI), and compounds represented by formula (BII).

[0097]

[0098] [In formulas (BI) and (BII), R e and R f X represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and the hydrogen atom contained in the alkyl group may be substituted with a hydroxyl group. e and X f This is a single bond, *-R g -, *-R g -O-, *-R g -S- or *-R g Represents -NH-. g * represents an alkanediyl group with 1 to 6 carbon atoms. * represents a bond with oxygen.

[0099] Examples of alkyl groups having 1 to 4 carbon atoms include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, sec-butyl group, and tert-butyl group. Examples of alkyl groups in which hydrogen atoms are substituted with hydroxyl include hydroxymethyl group, 1-hydroxyethyl group, 2-hydroxyethyl group, 1-hydroxypropyl group, 2-hydroxypropyl group, 3-hydroxypropyl group, 1-hydroxy-1-methylethyl group, 2-hydroxy-1-methylethyl group, 1-hydroxybutyl group, 2-hydroxybutyl group, 3-hydroxybutyl group, and 4-hydroxybutyl group. e and R fPreferably, the group is a hydrogen atom, a methyl group, a hydroxymethyl group, a 1-hydroxyethyl group, or a 2-hydroxyethyl group, and more preferably, a hydrogen atom or a methyl group.

[0100] Examples of alkanediyl groups include methylene, ethylene, propane-1,2-diyl, propane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, and hexane-1,6-diyl groups. e and X f Preferably, the bonds include single bonds, methylene groups, ethylene groups, *-CH2-O- and *-CH2CH2-O-, and more preferably single bonds and *-CH2CH2-O- (where * represents a bond with O).

[0101] Compounds represented by formula (BI) include compounds represented by any of formulas (BI-1) to (BI-15). Among these, compounds represented by formulas (BI-1), (BI-3), (BII-5), (BI-7), (BI-9), or (BI-11) to (BI-15) are preferred, and compounds represented by formulas (BI-1), (BI-7), (BI-9), or (BI-15) are more preferred.

[0102]

[0103] Compounds represented by formula (BII) include compounds represented by any of formulas (BII-1) to (BII-15). Among these, compounds represented by formulas (BII-1), (BII-3), (BII-5), (BII-7), (BII-9), or (BII-11) to (BII-15) are preferred, and compounds represented by formulas (BII-1), (BII-7), (BII-9), or (BII-15) are more preferred.

[0104]

[0105] The compound represented by formula (BI) and the compound represented by formula (BII) may be used individually or in combination of two or more. When the compound represented by formula (BI) and the compound represented by formula (BII) are used in combination, their content ratio [compound represented by formula (BI):compound represented by formula (BII)] is preferably 5:95 to 95:5, more preferably 20:80 to 80:20, on a molar basis.

[0106] For (b2), monomers having an oxetanyl group and a (meth)acryloyloxy group are more preferred. Examples of (b2) include 3-methyl-3-methacryloyloxymethyl oxetane, 3-methyl-3-acryloyloxymethyl oxetane, 3-ethyl-3-methacryloyloxymethyl oxetane, 3-methyl-3-methacryloyloxyethyl oxetane, 3-methyl-3-acryloyloxyethyl oxetane, 3-ethyl-3-methacryloyloxyethyl oxetane, and 3-ethyl-3-acryloyloxyethyl oxetane.

[0107] For (b3), monomers having a tetrahydrofurfuryl group and a (meth)acryloyloxy group are more preferred. Specifically for (b3), examples include tetrahydrofurfuryl acrylate (e.g., Viscoat V#150, manufactured by Osaka Organic Chemical Industry Co., Ltd.) and tetrahydrofurfuryl methacrylate.

[0108] (b) is preferable because it allows for higher reliability in terms of chemical resistance, etc.

[0109] Because the resin [K6] has high reactivity during production and unreacted (b) is less likely to remain, a monomer having an oxirane ring and an ethylenically unsaturated bond is preferred for (b).

[0110] (c) For example, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, tricyclo[5.2.1.0 2,6 ] Decane-8-yl (meth)acrylate (in the relevant technical field, it is commonly called "dicyclopentanyl (meth)acrylate". It is also sometimes called "tricyclodecyl (meth)acrylate"), tricyclo[5.2.1.0 2,6(Meth)acrylic acid esters such as decen-8-yl (meth)acrylate (commonly known as "dicyclopentenyl (meth)acrylate" in the relevant technical field), dicyclopentanyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, allyl (meth)acrylate, propargyl (meth)acrylate, phenyl (meth)acrylate, naphthyl (meth)acrylate, and benzyl (meth)acrylate; hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; dicarboxylic acid diesters such as diethyl maleate, diethyl fumarate, and diethyl itaconate;Bicyclo[2.2.1]hept-2-ene, 5-methylbicyclo[2.2.1]hept-2-ene, 5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxybicyclo[2.2.1]hept-2-ene, 5-hydroxymethylbicyclo[2.2.1]hept-2-ene, 5-(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5-methoxybi Cyclo[2.2.1]hept-2-ene, 5-ethoxybicyclo[2.2.1]hept-2-ene, 5,6-dihydroxybicyclo[2.2.1]hept-2-ene, 5,6-di(hydroxymethyl)bicyclo[2.2.1]hept-2-ene, 5,6-di(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5,6-dimethoxybicyclo[2.2.1]hept-2-ene To-2-ene, 5,6-diethoxybicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxymethyl-5-methylbicyclo[2.2.1]hept-2-ene, 5-tert-butoxycarbonylbicyclo[2.2.1]hept-2 Bicyclounsaturated compounds such as -ene, 5-cyclohexyloxycarbonylbicyclo[2.2.1]hept-2-ene, 5-phenoxycarbonylbicyclo[2.2.1]hept-2-ene, 5,6-bis(tert-butoxycarbonyl)bicyclo[2.2.1]hept-2-ene, 5,6-bis(cyclohexyloxycarbonyl)bicyclo[2.2.1]hept-2-ene; dicarbonylimide derivatives such as N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, N-succinimidyl-3-maleimide benzoate, N-succinimidyl-4-maleimide butyrate, N-succinimidyl-6-maleimide caproate, N-succinimidyl-3-maleimide propionate, and N-(9-acridinyl)maleimide;Examples include styrene, α-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, p-methoxystyrene, acrylonitrile, methacrylonitrile, vinyl chloride, vinylidene chloride, acrylamide, methacrylamide, vinyl acetate, 1,3-butadiene isoprene, 2,3-dimethyl-1,3-butadiene, etc.

[0111] Of the above, methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, styrene, vinyltoluene, N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, bicyclo[2.2.1]hept-2-ene, etc. are preferred from the viewpoint of copolymerization reactivity.

[0112] Resin [K6] is a resin obtained by reacting a cyclic ether derived from (b) in a copolymer of (b) and (c) with a carboxylic acid or carboxylic acid anhydride from (a), and then reacting it with a carboxylic acid anhydride. The hydroxyl group generated by the reaction of the cyclic ether with the carboxylic acid or carboxylic acid anhydride is reacted with the carboxylic acid anhydride.

[0113] The ratio of structural units derived from (b) and (c) is preferably such that, with respect to the total number of moles of all structural units constituting the copolymer, the ratio of structural units derived from (b) is 5 mol% to 95 mol%, and the ratio of structural units derived from (c) is 5 mol% to 95 mol%, and it is more preferably such that the ratio of structural units derived from (b) is 10 mol% to 90 mol%, and the ratio of structural units derived from (c) is 10 mol% to 90 mol%.

[0114] The amount of (a) used to react with the copolymer is preferably 5 moles to 120 moles, and more preferably 20 moles to 110 moles, per 100 moles of (b).

[0115] Examples of carboxylic acid anhydrides include succinic anhydride, maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, and 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride.

[0116] The amount of carboxylic acid anhydride used is preferably 0.1 to 1 mole, more preferably 0.2 to 1 mole, and even more preferably 0.3 to 1 mole, per 1 mole of the amount of (a) used.

[0117] Examples of resins [K6] include resins obtained by adding (meth)acrylic acid to a tricyclodecyl (meth)acrylate / glycidyl (meth)acrylate copolymer and then esterifying it with tetrahydrophthalic anhydride or succinic anhydride, and resins obtained by adding (meth)acrylic acid to a dicyclopentanyl (meth)acrylate / 2-ethylhexyl (meth)acrylate / glycidyl (meth)acrylate copolymer and then esterifying it with tetrahydrophthalic anhydride or succinic anhydride. Other resins may be used, for example, the resins described in Japanese Patent Application Publication No. 2024-61630 and Japanese Patent Application Publication No. 2018-123274.

[0118] The resin (C) has a standard polystyrene equivalent Mw measured by GPC, for example, 1,000 to 100,000, preferably 2,000 to 50,000, more preferably 3,000 to 20,000, and even more preferably 5,000 to 8,000, from the viewpoint of developability and luminescence intensity of the curable composition. The Mw of resin (C) can be adjusted by appropriately combining reaction conditions such as the selection of raw materials used, the preparation method, the reaction temperature and time. The Mw of resin (C) can be measured according to the measurement method described in the Examples section below. Alternatively, the Mw of resin (C) contained in the curable composition may be measured using GPC.

[0119] From the viewpoint of the developability and solvent resistance of the curable composition, the acid value of resin (C) is preferably 1 mg KOH / g or more and 150 mg KOH / g or less, more preferably 20 mg KOH / g or more and 110 mg KOH / g or less, even more preferably 30 mg KOH / g or more and 80 mg KOH / g or less, and even more preferably 30 mg KOH / g or more and 50 mg KOH / g or less. In the method for producing the cured film described later, the acid value of resin (C) can be adjusted by the content of monomer components having acid groups and the content of carboxylic acid anhydrides.

[0120] The acid value of resin (C) is measured as the amount of potassium hydroxide (mg) required to neutralize 1 g of resin (C), and can be determined, for example, by titration using an aqueous potassium hydroxide solution. Specifically, it can be measured according to the measurement method described in the Examples section below. Alternatively, the acid value of resin (C) contained in the composition may be determined, for example, by performing a structural analysis of it.

[0121] The resin (C) content in the curable composition is, for example, 5% by mass or more and 80% by mass or less, preferably 10% by mass or more and 70% by mass or less, more preferably 13% by mass or more and 60% by mass or less, and even more preferably 17% by mass or more and 55% by mass or less, based on the total amount of solids in the curable composition.

[0122] The mass ratio (C / (A+G)) of the resin (C) to the semiconductor particles (A) containing the organic ligand (G) is preferably 0.1 or more and less than 3, more preferably 0.3 or more and 2 or less, and even more preferably 0.3 or more and 1 or less, from the viewpoint of developability.

[0123] <Light Scattering Agent (B)> Examples of light scattering agent (B) include metal or metal oxide particles, and inorganic particles such as glass particles. Examples of metal oxides include TiO2, SiO2, BaTiO3, and ZnO, and TiO2 particles are preferred because they efficiently scatter light and increase the emission intensity. The particle size of the light scattering agent (B) is, for example, about 0.03 μm to 20 μm, preferably 0.05 μm to 1 μm, and more preferably 0.05 μm to 0.5 μm.

[0124] As the light scattering agent (B), a solution may be used in which the light scattering agent is pre-dispersed in part or all of the solvent (J) using a dispersant (I). Examples of the dispersant (I) include the compounds described in Japanese Patent Application Publication No. 2024-61630.

[0125] The content of the light scattering agent (B) in the curable composition is, for example, 0.001% by mass or more and 50% by mass or less, relative to the total amount of solids in the curable composition. From the viewpoint of improving the light scattering ability and luminescence intensity when the cured film is used as a wavelength conversion layer, it is preferably 1% by mass or more and 40% by mass or less, more preferably 2% by mass or more and 30% by mass or less, even more preferably 5% by mass or more and 30% by mass or less, and still more preferably 5% by mass or more and 15% by mass or less.

[0126] <Polymerizable Compound (D)> Polymerizable compound (D) is a compound that can be polymerized by active radicals, acids, etc., generated from the polymerization initiator (E) described later. Examples of polymerizable compound (D) include photopolymerizable compounds such as compounds having ethylenically unsaturated bonds, such as (meth)acrylic acid ester compounds. Another example of polymerizable compound (D) is a thermopolymerizable compound. The curable composition may contain two or more polymerizable compounds (D).

[0127] Examples of polymerizable compounds (D) include photopolymerizable compounds (Dα) having two ethylenically unsaturated bonds in the molecule, and photopolymerizable compounds (Dβ) having three or more ethylenically unsaturated bonds in the molecule, where the number of ethylenically unsaturated bonds in the molecule of photopolymerizable compound (Dβ) is preferably six or less. The ethylenically unsaturated bonds are preferably (meth)acryloyloxy groups. The molecular weight or weight-average molecular weight of polymerizable compound (D) is preferably 150 to 2900, more preferably 250 to 1500. Polymerizable compound (D) preferably contains one or more selected from photopolymerizable compounds (Dα) and photopolymerizable compounds (Dβ), and more preferably contains both photopolymerizable compound (Dα) and photopolymerizable compound (Dβ). Photopolymerizable compound (D) may contain one or more photopolymerizable compounds (Dα) and one or more photopolymerizable compounds (Dβ).

[0128] Examples of photopolymerizable compounds (Dα) having two ethylenically unsaturated bonds in the molecule include difunctional (meth)acrylic compounds, such as alkylene glycol di(meth)acrylate, polyoxyalkylene glycol di(meth)acrylate, halogen-substituted alkylene glycol di(meth)acrylate, aliphatic polyol di(meth)acrylate, hydrogenated dicyclopentadiene or tricyclodecanedialkanol di(meth)acrylate, dioxane glycol or dioxanedialkanol di(meth)acrylate, alkylene oxide adduct of bisphenol A or bisphenol F di(meth)acrylate, and bisphenol fluorene alkylene oxide adduct di(meth)acrylate.

[0129] More specific examples of the above-mentioned bifunctional (meth)acrylic compounds include ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol di(meth)acrylate, and ditrimethylolpropane di(meth)acrylate. Diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, hydroxypivalate neopentyl glycol ester di(meth)acrylate, 2,2-bis[4-(meth)acryloyloxyethoxyethyl [Xyphenyl]propane, 2,2-bis[4-(meth)acryloyloxyethoxyethoxycyclohexyl]propane, hydrogenated dicyclopentadienyl di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, 1,3-dioxane-2,5-diyldi(meth)acrylate [also known as: dioxane glycol di(meth)acrylate], acetal compound of hydroxypivalaldehyde and trimethylolpropane [chemical name: 2-(2-hydroxy-1,1-dimethylethyl)-5-ethyl-5-H These include di(meth)acrylate of droxymethyl-1,3-dioxane, tris(hydroxyethyl) isocyanurate di(meth)acrylate, di(meth)acrylate of ethoxylated bisphenol A, di(meth)acrylate of propoxylated bisphenol A, di(meth)acrylate of ethoxylated bisphenol F, di(meth)acrylate of propoxylated bisphenol F, di(meth)acrylate of ethoxylated bisphenol fluorene, and di(meth)acrylate of propoxylated bisphenol fluorene.

[0130] The photopolymerizable compound (Dα) having two ethylenically unsaturated bonds in its molecule is preferably a photopolymerizable compound (Dα1) having one or more cyclic hydrocarbon groups and two ethylenically unsaturated bonds in one molecule, and it is preferable that the polymerizable compound (D) contains one or more types of photopolymerizable compounds (Dα1). In the photopolymerizable compound (Dα1), the cyclic hydrocarbon group is preferably a group containing an aromatic hydrocarbon ring, and examples of aromatic hydrocarbon rings include monocyclic rings such as benzene rings, fused rings such as naphthalene rings and fluorene rings. Two or more of these aromatic hydrocarbon rings may be combined, for example, a structure having two benzene rings such as a biphenyl structure or a bisphenol structure, or a structure combining a benzene ring and a fluorene ring such as a diphenylfluorene structure. Furthermore, in the photopolymerizable compound (Dα1), the number of aromatic hydrocarbon rings in one molecule is preferably two to four, and more preferably two to three. Specific examples of photopolymerizable compounds (Dα1) include di(meth)acrylate of ethoxylated bisphenol A, di(meth)acrylate of propoxylated bisphenol A, di(meth)acrylate of ethoxylated bisphenol F, di(meth)acrylate of propoxylated bisphenol F, di(meth)acrylate of ethoxylated bisphenol fluorene, and di(meth)acrylate of propoxylated bisphenol fluorene.

[0131] Polymerizable compounds (Dβ) having three or more ethylenically unsaturated bonds in their molecule include compounds (Dβ1) having three or more (meth)acryloyloxy groups in their molecule and having an acidic functional group, and compounds (Dβ2) having three or more (meth)acryloyloxy groups in their molecule but not having an acidic functional group. Polymerizable compound (D) preferably contains at least one of compounds (Dβ1) and (Dβ2), and more preferably contains at least one of compounds (Dβ1). Examples of the above-mentioned acidic functional group include carboxyl groups, sulfonic acid groups, and phosphate groups. Among these, the acidic functional group is preferably a carboxyl group.

[0132] The number of (meth)acryloyloxy groups in one molecule of compound (Dβ1) is, for example, 3 to 6, preferably 3 to 5. The number of acidic functional groups in one molecule of compound (Dβ1) is, for example, 1 or more, preferably 1. If there are two or more acidic functional groups, each acidic functional group may be different or the same, but it is preferable that there is at least one carboxyl group.

[0133] Examples of compound (Dβ1) include compounds obtained by esterifying a compound having three or more (meth)acryloyloxy groups and hydroxyl groups, such as pentaerythritol tri(meth)acrylate or dipentaerythritol penta(meth)acrylate, with a dicarboxylic acid or dicarboxylic acid anhydride. Examples of such compounds include compounds obtained by monoesterifying pentaerythritol tri(meth)acrylate with succinic acid, compounds obtained by monoesterifying dipentaerythritol penta(meth)acrylate with succinic acid, compounds obtained by monoesterifying pentaerythritol tri(meth)acrylate with maleic acid, and compounds obtained by monoesterifying dipentaerythritol penta(meth)acrylate with maleic acid. Among these, compounds obtained by monoesterifying pentaerythritol tri(meth)acrylate with succinic acid are preferred.

[0134] Examples of commercially available compounds containing compound (Dβ1) include "Aronics M-510" manufactured by Toagosei Co., Ltd., which mainly consists of a dibasic acid anhydride adduct of pentaerythritol tri(meth)acrylate, and "Aronics M-520D" manufactured by Toagosei Co., Ltd., which mainly consists of a dibasic acid anhydride adduct of dipentaerythritol penta(meth)acrylate. These commercially available products have a carboxyl group as an acidic functional group.

[0135] The number of (meth)acryloyloxy groups in compound (Dβ2) is preferably 3 to 6, and more preferably 4 to 6.

[0136] Examples of compounds (Dβ2) include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol octa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, tetrapentaerythritol nona(meth)acrylate, tris( Examples include 2-(meth)acryloyloxyethyl) isocyanurate, ethylene glycol-modified pentaerythritol tetra(meth)acrylate, ethylene glycol-modified dipentaerythritol hexa(meth)acrylate, propylene glycol-modified pentaerythritol tetra(meth)acrylate, propylene glycol-modified dipentaerythritol hexa(meth)acrylate, caprolactone-modified pentaerythritol tetra(meth)acrylate, and caprolactone-modified dipentaerythritol hexa(meth)acrylate. Among these, dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate are preferred.

[0137] The polymerizable compound (D) in the curable composition is preferable because it includes compound (Dα) (particularly compound (Dα1)) and compound (Dβ), which improves curability during exposure and patternability during development, further improves the dispersibility of semiconductor particles (A), and can improve the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0138] In the curable composition, the content of compound (Dα) (particularly compound (Dα1)) in 100% by mass of polymerizable compound (D) is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and may be 60% by mass or less. In the curable composition, the content of compound (Dβ) in 100% by mass of polymerizable compound (D) is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and may be 100% by mass or 70% by mass or less.

[0139] When the polymerizable compound (D) in the curable composition contains both compound (Dα) and compound (Dβ), it is preferable that it contains compound (Dα1) and (Dβ1). The total content of compound (Dα1) and compound (Dβ1) relative to 100% by mass of polymerizable compound (D) is preferably 70% by mass or more, more preferably 85% by mass or more, and may be 100% by mass. The content of compound (Dα1) relative to 100% by mass of the total amount of compound (Dα1) and compound (Dβ1) is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and may be 70% by mass or less.

[0140] When the polymerizable compound (D) in the curable composition contains both compound (Dβ1) and compound (Dβ2), the total content of compound (Dβ1) and compound (Dβ2) relative to 100% by mass of polymerizable compound (D) is preferably 70% by mass or more, more preferably 85% by mass or more, and may be 100% by mass. The content of compound (Dβ2) relative to 100% by mass of the total amount of compound (Dβ1) and compound (Dβ2) is preferably more than 50% by mass, more preferably 53% by mass or more, even more preferably 55% by mass or more, and may be 70% by mass or less.

[0141] The content of polymerizable compound (D) in the curable composition (total amount if multiple types are included) is preferably 3% to 30% by mass, more preferably 4% to 25% by mass, and even more preferably 5% to 20% by mass, based on 100% by mass of the total solid content of the curable composition.

[0142] <Polymerization Initiator (E)> A polymerization initiator (E) is a compound that generates active radicals, acids, etc., upon the action of light or heat, and can initiate the polymerization of a polymerizable compound (D). The curable composition may contain one or more polymerization initiators (E).

[0143] The clogP of the polymerization initiator (E) is preferably 1 to 25, more preferably 2 to 20, even more preferably 3 to 15, even more preferably 4 to 14, particularly preferably 5 to 13, and most preferably 7 to 13. If the clogP of the polymerization initiator (E) is within the above range, the hydrophobicity of the polymerization initiator can be appropriately controlled, thereby improving both developability and luminescence intensity.

[0144] clogP is obtained by dividing the chemical structure into substructures (fragments) and summing the logP contributions assigned to each fragment to estimate the logP value of the compound. clogP can be calculated using programs such as "CLOGP" available from Daylight Chemical Information System, Inc., MOLINSPIRATION CHEMINFORMATICS (http: / / www.molinspiration.com), or ChemDraw 22.0 (Cambridge Soft). If two or more polymerization initiators (E) are included, the clogP of the polymerization initiator (E) may be a weighted average based on the clogP of each initiator and its mass ratio.

[0145] The polymerization initiator (E) preferably contains an oxime compound.

[0146] Including an oxime compound as a polymerization initiator (E) can be advantageous from the viewpoint of improving luminescence intensity. One reason for this effect is presumed to be that, due to the unique molecular structure of the oxime compound, the absorption wavelength of the oxime compound changes significantly before and after cleavage (decomposition) of the oxime compound, which is necessary for the oxime compound to initiate photopolymerization. Therefore, oxime compounds have a high photoradical polymerization initiation ability.

[0147] Examples of oxime compounds include those having a substructure represented by the following formula (da1) or formula (da2). * and ** represent bonding sites.

[0148]

[0149] The oxime compound preferably has at least one substructure selected from those represented by the following formulas (d-1) to (d-4). If the oxime compound has these substructures, a curable composition that can form a cured film with good surface properties can be easily provided. The oxime compound more preferably has the substructure represented by formula (d-1) or the substructure represented by formula (d-2), and even more preferably has the substructure represented by formula (d-1). In particular, if the oxime compound has the substructure represented by formula (d-1) (carbazole skeleton), a curable composition with excellent patternability is obtained. In formulas (d-1) to (d-4), * and ** represent bonding. In the following substructures represented by formulas (d-1) to (d-3), * bonds with structures other than the substructure represented by formula (da1) or formula (da2). The substructures represented by the following formulas (d-1) to (d-4) are combined with the substructures represented by the aforementioned formula (da1) or formula (da2).

[0150]

[0151] The polymerization initiator (E) preferably contains a compound represented by formula (EA).

[0152] [In the formula, R ea1 R represents a branched hydrocarbon group having 3 to 20 carbon atoms, which may have substituents. ea2 ~R ea5 Each of these independently represents a hydrocarbon group having 1 to 20 carbon atoms, which may have substituents. n represents an integer from 0 to 4. The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-.

[0153] R ea1Examples of branched hydrocarbon groups having 3 to 20 carbon atoms, represented by , include branched saturated hydrocarbon groups having 3 to 20 carbon atoms and branched unsaturated hydrocarbon groups having 3 to 20 carbon atoms.

[0154] R ea1Examples of branched saturated hydrocarbon groups having 3 to 20 carbon atoms, represented by , include 1-methylethyl group (isopropyl group), 1-methylpropyl group (sec-butyl group), 2-methylpropyl group (isobutyl group), 1,1-dimethylethyl group (tert-butyl group), 1,1-dimethylpropyl group, 2,2-dimethylpropyl group, 1,2-dimethylpropyl group, 1-ethylpropyl group, 1-methylbutyl group, 2-methylbutyl group, 3-methylbutyl group, 1,1-dimethylbutyl group, and 2,2-dimethylbutyl group. ,3,3-dimethylbutyl group, 1,2-dimethylbutyl group, 1,3-dimethylbutyl group, 2,3-dimethylbutyl group, 1-ethylbutyl group, 2-ethylbutyl group, 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 4-methylpentyl group, 1,1-dimethylpentyl group, 2,2-dimethylpentyl group, 3,3-dimethylpentyl group, 1,2-dimethylpentyl group, 1,3-dimethylpentyl group, 2,3-dimethylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3 - Ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 4-methylhexyl group, 1,1-dimethylhexyl group, 2,2-dimethylhexyl group, 3,3-dimethylhexyl group, 1,2-dimethylhexyl group, 1,3-dimethylhexyl group, 2,3-dimethylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 4-methylheptyl group, 1,1-dimethylheptyl Butyl group, 2,2-dimethylheptyl group, 3,3-dimethylheptyl group, 1,2-dimethylheptyl group, 1,3-dimethylheptyl group, 2,3-dimethylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, 3-ethylheptyl group, 1-methyloctyl group, 2-methyloctyl group, 3-methyloctyl group, 4-methyloctyl group, 1,1-dimethyloctyl group, 2,2-dimethyloctyl group, 3,3-dimethyloctyl group, 1,2-dimethyloctyl group, 1,3-dimethyloctyl group, 2,Examples include branched alkyl groups such as 3-dimethyloctyl group, 1-ethyloctyl group, 2-ethyloctyl group, 3-ethyloctyl group, 1-methylnonyl group, 2-methylnonyl group, 3-methylnonyl group, 4-methylnonyl group, dimethylnonyl group, ethylnonyl group, methyldecyl group, dimethyldecyl group, ethyldecyl group, methylundecyl group, dimethylundecyl group, ethylundecyl group, and methyldodecyl group. ea1 The branched alkyl group represented by may be a primary branched alkyl group, a secondary branched alkyl group, or a tertiary branched alkyl group. ea1 The number of carbon atoms in the branched saturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, preferably 16 or less, more preferably 12 or less, and even more preferably 10 or less.

[0155] R ea1 The branched unsaturated hydrocarbon group represented by the above-mentioned R is ea1 Examples include groups in which at least one carbon-carbon single bond in a branched saturated hydrocarbon group represented by is replaced by a carbon-carbon double bond or a carbon-carbon triple bond. ea1 Examples of branched unsaturated hydrocarbon groups represented by include alkenyl groups such as isopropenyl, isobutenyl, isopentenyl, isohexenyl, isoheptenyl, isooctenyl, isononyl, and isodecenyl groups; alkynyl groups such as isopropynyl, isobutynyl, isopentinyl, isohexynyl, isoheptynyl, isooctynyl, isononinyl, and isodesynyl groups; and so on. ea1 The number of carbon atoms in the branched unsaturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, preferably 16 or less, more preferably 12 or less, and even more preferably 10 or less.

[0156] R ea2 , R ea3 , R ea4 and R ea5Examples of hydrocarbon groups having 1 to 20 carbon atoms represented by include saturated hydrocarbon groups having 1 to 20 carbon atoms, unsaturated hydrocarbon groups having 2 to 20 carbon atoms, and aromatic hydrocarbon groups having 6 to 20 carbon atoms. ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon groups represented by may be the same or different.

[0157] Examples of the saturated hydrocarbon groups having 1 to 20 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, hexadecyl, and eicosyl groups; branched alkyl groups such as isopropyl, isobutyl, isopentyl, neopentyl, and 2-ethylhexyl groups; and alicyclic saturated hydrocarbon groups having 3 to 20 carbon atoms such as cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and tricyclodecyl groups. The number of carbon atoms in the saturated hydrocarbon group is preferably 1 to 18, more preferably 1 to 15, even more preferably 1 to 10, and even more preferably 1 to 8.

[0158] Examples of the carbon-2 to carbon-20 unsaturated hydrocarbon groups include alkenyl groups such as vinyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, dodecenyl, hexadecenyl, octadecenyl, and eicosenyl groups; alkynyl groups such as ethynyl, propynyl, hexynyl, desinyl, and eicosinyl groups; and cycloalkenyl groups such as cyclopentenyl, cyclohexenyl, and cycloheptenyl groups. The carbon number of the unsaturated hydrocarbon group is preferably 2 to 18, more preferably 2 to 15, and even more preferably 2 to 10.

[0159] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include phenyl group, xylyl group, trimethylphenyl group, dipropylphenyl group, di(2,2-dimethylpropyl)phenyl group, naphthyl group, benzyl group, phenylethyl group, and phenylbutyl group. The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 18, more preferably 6 to 15, and even more preferably 6 to 12.

[0160] R ea1 , R ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon group represented by may have substituents such as halogen atoms, cyano groups, and nitro groups. The halogen atom is preferably a fluorine atom, a bromine atom, a chlorine atom, or an iodine atom.

[0161] The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-, and adjacent -CH2- will not be substituted with the same type of group at the same time, nor will terminal -CH2- be substituted.

[0162] n represents an integer from 0 to 4, preferably an integer from 0 to 3, more preferably an integer from 0 to 2, even more preferably an integer of 0 or 1, and even more preferably 0.

[0163] *-OCO-R ea4 The bond position of the group (* represents the bond with the phenyl group) is *-OCO-R ea4 The group may be attached to the 2nd, 3rd, or 4th position of the phenyl group, but is preferably at the 3rd or 4th position, and more preferably at the 4th position.

[0164] R ea1The branched hydrocarbon group having 3 to 20 carbon atoms represented by is preferably a branched saturated hydrocarbon group having 3 to 20 carbon atoms, more preferably a branched alkyl group having 3 to 20 carbon atoms, even more preferably a branched alkyl group having 3 to 10 carbon atoms, and is preferably one or more selected from the group consisting of 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group and 3-ethylheptyl group.

[0165] R ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon group having 1 to 20 carbon atoms represented by is preferably a saturated hydrocarbon group having 1 to 20 carbon atoms or an unsaturated hydrocarbon group having 2 to 20 carbon atoms, more preferably a saturated hydrocarbon group having 1 to 20 carbon atoms, even more preferably a linear saturated hydrocarbon group having 1 to 10 carbon atoms, and still even more preferably a linear alkyl group having 1 to 8 carbon atoms. R ea2 is preferably a linear alkyl group having 1 to 8 carbon atoms, more preferably a linear alkyl group having 1 to 6 carbon atoms. R ea3 is preferably a linear alkyl group having 1 to 8 carbon atoms, more preferably a linear alkyl group having 1 to 3 carbon atoms. R ea4 is preferably a linear alkyl group having 1 to 8 carbon atoms, more preferably a linear alkyl group having 1 to 3 carbon atoms. R ea5 is preferably a linear or branched alkyl group having 1 to 8 carbon atoms, more preferably a linear or branched alkyl group having 1 to 6 carbon atoms.

[0166] Further, the polymerization initiator (E) preferably contains a compound represented by the formula (EB).

[0167] [In the formula, R eb1 represents an optionally substituted branched hydrocarbon group having 3 to 20 carbon atoms. R eb2 to R eb4each independently represents a C1-C20 hydrocarbon group which may have a substituent. m represents any integer of 0 to 4. -CH₂- contained in the aforementioned hydrocarbon group may be replaced by -O-, -S-, -CO- or -OCO-.]

[0168] R eb1 Examples of the C3-C20 branched hydrocarbon group represented by include a C3-C20 branched saturated hydrocarbon group, a C3-C20 branched unsaturated hydrocarbon group, and the like.

[0169] R eb1 Examples of the C3-C20 branched saturated hydrocarbon group represented by include those similar to the groups exemplified above as the C3-C20 branched saturated hydrocarbon group represented by R ea1 . The branched alkyl group represented by R eb1 may be any of a primary branched alkyl group, a secondary branched alkyl group, or a tertiary branched alkyl group. The number of carbon atoms of the branched saturated hydrocarbon group represented by R eb1 is preferably 4 or more, more preferably 5 or more, and is preferably 16 or less, more preferably 12 or less, still more preferably 10 or less.

[0170] R eb1 Examples of the branched unsaturated hydrocarbon group represented by include groups in which at least one or more carbon-carbon single bonds contained in the aforementioned branched saturated hydrocarbon group represented by R eb1 are replaced with carbon-carbon double bonds or carbon-carbon triple bonds, and the like. Examples of the branched unsaturated hydrocarbon group represented by R eb1 include alkenyl groups such as isopropenyl group, isobutenyl group, isopentenyl group, isohexenyl group, isoheptenyl group, isooctenyl group, isononenyl group, isodecenyl group and the like; alkynyl groups such as isopropynyl group, isobutynyl group, isopentynyl group, isohexynyl group, isoheptynyl group, isooctynyl group, isononynyl group, isodecynyl group and the like; and the like. R eb1The number of carbon atoms in the branched unsaturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, preferably 16 or less, more preferably 12 or less, and even more preferably 10 or less.

[0171] R eb2 , R eb3 and R eb4 Examples of hydrocarbon groups having 1 to 20 carbon atoms represented by include saturated hydrocarbon groups having 1 to 20 carbon atoms, unsaturated hydrocarbon groups having 2 to 20 carbon atoms, and aromatic hydrocarbon groups having 6 to 20 carbon atoms. eb2 , R eb3 and R eb4 The hydrocarbon groups represented by may be the same or different.

[0172] Examples of the saturated hydrocarbon groups having 1 to 20 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, hexadecyl, and eicosyl groups; branched alkyl groups such as isopropyl, isobutyl, isopentyl, neopentyl, and 2-ethylhexyl groups; and alicyclic saturated hydrocarbon groups having 3 to 20 carbon atoms such as cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and tricyclodecyl groups. The number of carbon atoms in the saturated hydrocarbon group is preferably 1 to 18, more preferably 1 to 15, even more preferably 1 to 10, and even more preferably 1 to 8.

[0173] Examples of the carbon-2 to carbon-20 unsaturated hydrocarbon groups include alkenyl groups such as vinyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, dodecenyl, hexadecenyl, octadecenyl, and eicosenyl groups; alkynyl groups such as ethynyl, propynyl, hexynyl, desinyl, and eicosinyl groups; and cycloalkenyl groups such as cyclopentenyl, cyclohexenyl, and cycloheptenyl groups. The carbon number of the unsaturated hydrocarbon group is preferably 2 to 18, more preferably 2 to 15, and even more preferably 2 to 10.

[0174] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include phenyl group, xylyl group, trimethylphenyl group, dipropylphenyl group, di(2,2-dimethylpropyl)phenyl group, naphthyl group, benzyl group, phenylethyl group, and phenylbutyl group. The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 18, more preferably 6 to 15, and even more preferably 6 to 12.

[0175] R eb1 , R eb2 , R eb3 and R eb4 The hydrocarbon group represented by may have substituents such as halogen atoms, cyano groups, and nitro groups. The halogen atom is preferably a fluorine atom, a bromine atom, a chlorine atom, or an iodine atom, and more preferably a fluorine atom.

[0176] The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-, and in particular may be replaced with -O-, and adjacent -CH2- will not be simultaneously replaced with the same type of group, and terminal -CH2- will not be replaced.

[0177] m represents an integer from 0 to 4, preferably an integer from 1 to 3, more preferably an integer from 2 to 3, and even more preferably 3.

[0178] If m is 1 or greater, *-R eb4 At least one of the 2nd, 4th, and 6th positions of the phenyl group to which it is attached contains *-R eb4 (* represents a bond with a phenyl group) It is preferable that *-R is bonded, eb4 *-R is attached to at least two positions (2, 4, and 6) of the phenyl group to which it is bonded. eb4 It is more preferable that *-R is bonded. eb4 *-R is attached to all of the phenyl groups at positions 2, 4, and 6. eb4 It is even more preferable that they are bonded together.

[0179] R eb1The branched hydrocarbon group having 3 to 20 carbon atoms represented by is preferably a branched saturated hydrocarbon group having 3 to 20 carbon atoms, more preferably a branched alkyl group having 3 to 20 carbon atoms, even more preferably a branched alkyl group having 3 to 10 carbon atoms, and more preferably one or more selected from the group consisting of 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, and 3-ethylheptyl group.

[0180] R eb2 The hydrocarbon group having 1 to 20 carbon atoms represented by is preferably an aromatic hydrocarbon group having 6 to 20 carbon atoms, more preferably an aromatic hydrocarbon group having 6 to 17 carbon atoms, even more preferably an aromatic hydrocarbon group having 7 to 15 carbon atoms, and particularly preferably an aromatic hydrocarbon group having 8 to 13 carbon atoms. In any of these preferred embodiments, it is preferable to have a structure in which 1 to 8 (particularly 1 to 5) fluorine atoms as substituents, and 1 to 2 -CH2- are replaced by -O-.

[0181] R eb2 The preferred embodiment of the aromatic hydrocarbon group having 8 to 13 carbon atoms is preferably one of the following (eb2-1) to (eb2-6).

[0182]

[0183] R eb3 and R eb4 The hydrocarbon groups having 1 to 20 carbon atoms represented by the formula are, independently, preferably saturated hydrocarbon groups having 1 to 20 carbon atoms, unsaturated hydrocarbon groups having 2 to 20 carbon atoms, more preferably saturated hydrocarbon groups having 1 to 20 carbon atoms, even more preferably linear saturated hydrocarbon groups having 1 to 10 carbon atoms, even more preferably linear alkyl groups having 1 to 8 carbon atoms, and particularly preferably linear alkyl groups having 1 to 3 carbon atoms.

[0184] In formula (EB), if the -CH2- contained in the hydrocarbon group is replaced with -O-, -S-, -CO-, or -OCO-, the number of carbon atoms in the replaced portion shall be counted as the number of carbon atoms of the -CH2- before the replacement.

[0185] Furthermore, the polymerization initiator (E) may contain a compound represented by formula (EC). [In the formula, R ec1 and R ec2 Each of them is independent of R ec11 , OR ec11 COR ec11 , SR ec11 CONR ec12 R ec13 Or it represents CN. R ec11 , R ec12 and R ec13 Each of these independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ec11 , R ec12 or R ec13 The hydrogen atom of the group represented by OR ec21 COR ec21 , SR ec21 , NR ec22 R ec23 CONR ec22 R ec23 , -NR ec22 -OR ec23 , -N(COR ec22 )-OCOR ec23 , -C(=N-OR ec21 )-R ec22 , -C(=N-OCOR ec21 )-R ec22 , CN, halogen atoms, or COOR ec21 It may be replaced with R. ec21 , R ec22 and R ec23 Each of these independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ec21 , R ec22 or R ec23The hydrogen atoms of the group represented by may be substituted with CN, halogen atoms, hydroxyl groups, or carboxyl groups. ec11 , R ec12 , R ec13 , R ec21 , R ec22 or R ec23 When the group represented by has an alkylene portion, the alkylene portion is -O-, -S-, -COO-, -OCO-, -NR ec24 -, -NR ec24 CO-, -NR ec24 COO-,-OCONR ec24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS-, or -CSO-. ec24 R represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ec11 , R ec12 , R ec13 , R ec21 , R ec22 or R ec23 When the group represented by has an alkyl moiety, the alkyl moiety may be branched, cyclic, or R ec12 and R ec13 and R ec22 and R ec23 They may each form a ring together. ec4 is a hydroxyl group, a carboxyl group, or the following formula (2-2)

[0186]

[0187] (In formula (2-2), L ec11 * represents *-O- or *-OCO-, where * is L ec12 This represents a bonding with L ec12 R represents an alkylene group having 1 to 20 carbon atoms, and the alkylene group may be interrupted by 1 to 3 -O- atoms. ec44a is OR ec55 or COOR ec55 Represents R ec55 ) represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0188] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and R ec24 Examples of alkyl groups having 1 to 20 carbon atoms represented by include methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, sec-butyl group, tert-butyl group, pentyl group, isopentyl group, tert-pentyl group, hexyl group, heptyl group, octyl group, isooctyl group, 2-ethylhexyl group, tert-octyl group, nonyl group, isononyl group, decyl group, isodecyl group, undecyl group, dodecyl group, tetradecyl group, hexadecyl group, octadecyl group, eicosyl group, cyclopentyl group, cyclohexyl group, cyclohexylmethyl group, cyclohexylethyl group, and the like.

[0189] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and R ec24 Examples of aryl groups having 6 to 30 carbon atoms represented by the formula include phenyl, tolyl, xylyl, ethylphenyl, naphthyl, anthryl, phenanthryl, phenyl, biphenylyl, naphthyl, and anthryl groups substituted with one or more of the above alkyl groups.

[0190] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and R ec24 Examples of aralkyl groups having 7 to 30 carbon atoms, represented by the formula, include benzyl group, α-methylbenzyl group, α,α-dimethylbenzyl group, and phenylethyl group.

[0191] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and Rec24 Examples of heterocyclic groups having 2 to 20 carbon atoms represented by include pyridyl group, pyrimidyl group, furyl group, thienyl group, tetrahydrofuryl group, dioxolanyl group, benzoxazole-2-yl group, tetrahydropyranyl group, pyrrolidyl group, imidazolidyl group, pyrazolidyl group, thiazolidyl group, isothiazolidyl group, oxazolidyl group, isoxazolidyl group, piperidyl group, piperadyl group, morpholinyl group, and the like, and are preferably 5 to 7 membered heterocyclic groups.

[0192] R in equation (EC) ec12 and R ec13 and R ec22 and R ec23 The statement that they may each form a ring together means that R ec12 and R ec13 and R ec22 and R ec23 This means that each atom may form a ring with the nitrogen, carbon, or oxygen atoms it connects to.

[0193] R in equation (EC) ec12 and R ec13 and R ec22 and R ec23 Examples of rings that can be formed by these rings together include cyclopentane rings, cyclohexane rings, cyclopentene rings, benzene rings, piperidine rings, morpholine rings, lactone rings, lactam rings, and the like, and are preferably 5 to 7 membered rings.

[0194] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 and R ec23 Examples of halogen atoms that may be present as substituents include fluorine, chlorine, bromine, and iodine atoms.

[0195] R in equation (EC) ec1 Preferably R ec11 The alkyl group is more preferably a C1 to C20 alkyl group, even more preferably a C1 to C10 alkyl group, and still more preferably a C1 to C6 alkyl group.

[0196] Rec4 Preferably, the group is represented by formula (2-2). In this case, it is advantageous in terms of the solubility of the oxime compound in solvent (J) and the developability of the curable composition.

[0197] L ec12 The number of carbon atoms in the alkylene group represented by is preferably 1 to 10, and more preferably 1 to 4.

[0198] R ec44a This is preferably a hydroxyl group or a carboxyl group, and more preferably a hydroxyl group.

[0199] Furthermore, the polymerization initiator (E) preferably contains a compound represented by formula (ED). [In the formula, R ed1 This represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or CN, and the hydrogen atoms of the alkyl group, aryl group, and arylalkyl group are further OR ed21 COR ed21 , SR ed21 , NR ed22 R ed23 ,-NCOR ed22 -OCOR ed23 CN, halogen atom, -CR ed21 =CR ed22 R ed23 or -CO-CR ed21 =CR ed22 R ed23 It may be replaced with R ed21 , R ed22 and R ed23 Each of these independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ed2 R ed11 OR ed11 Represents R ed11 R represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms, and the hydrogen atoms of the alkyl group, aryl group, and arylalkyl group may be further substituted with halogen atoms. ed3R represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms. ed1 , R ed3 , R ed21 , R ed22 and R ed23 The methylene group in the alkyl group represented by may be interrupted 1 to 5 times by unsaturated bonds, ether bonds, thioether bonds, ester bonds, thioester bonds, amide bonds, or urethane bonds. ed3 It may form a ring together with an adjacent benzene ring. ed4 and R ed5 Each of them independently, R ed11 , OR ed11 , represents a CN or halogen atom. a and b are each independently between 0 and 3.

[0200] In the above formula (ED), R ed1 , R ed11 , R ed21 , R ed22 , R ed23 , R ed3 Examples of alkyl groups represented by include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, s-butyl, t-butyl, pentyl, 1-methylbutyl, hexyl, heptyl, octyl, isooctyl, 2-ethylhexyl, t-octyl, nonyl, isononyl, decyl, isodecyl, undecyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, cyclopentyl, cyclohexyl, cyclohexylmethyl, vinyl, allyl, butenyl, ethinyl, propynyl, methoxyethyl, ethoxyethyl, propoxyethyl, pentyloxyethyl, octyloxyethyl, methoxyethoxyethyl, ethoxyethoxyethyl, propoxyethoxyethyl, methoxypropyl, 2-methoxy-1-methylethyl, and the like. The number of carbon atoms in the alkyl group is preferably 1 to 15, more preferably 1 to 10, even more preferably 1 to 8, and even more preferably 1 to 6. In particular, the alkyl group is preferably methyl, ethyl, propyl, or 1-methylbutyl.

[0201] R ed1 , Red11 , R ed21 , R ed22 , R ed23 , R ed3 Examples of aryl groups represented by include phenyl, tolyl, xylyl, ethylphenyl, chlorophenyl, naphthyl, anthuryl, phenanthrenyl, and phenyl, biphenylyl, naphthyl, and anthuryl groups substituted with one or more of the above alkyl groups. The number of carbon atoms in the aryl group is preferably 6 to 20, more preferably 6 to 15, even more preferably 6 to 12, and even more preferably 6 to 10. Among these, tolyl is preferred, o-tolyl and m-tolyl are more preferred, and o-tolyl is even more preferred.

[0202] R ed1 , R ed11 , R ed21 , R ed22 , R ed23 , R ed3 Examples of arylalkyl groups represented by include benzyl, chlorobenzyl, α-methylbenzyl, α,α-dimethylbenzyl, phenylethyl, and phenylethenyl. The number of carbon atoms in the arylalkyl group is preferably 7 to 20, more preferably 7 to 15, and even more preferably 7 to 12.

[0203] R ed21 , R ed22 and R ed23 Examples of heterocyclic groups represented by include, for example, 5- to 7-membered heterocycles such as pyridyl, pyrimidyl, furyl, thienyl, tetrahydrofuryl, dioxolanil, benzoxazole-2-yl, tetrahydropyranil, pyrrolidyl, imidazolidyl, pyrazolidyl, thiazolidyl, isothiazolidyl, oxazolidyl, isoxazolidyl, piperidyl, piperadyl, and morpholinil. The number of carbon atoms in the heterocyclic group is preferably 2 to 15, more preferably 3 to 12, and even more preferably 3 to 9.

[0204] Together with the adjacent benzene ring, R ed3Examples of rings formed by the nitrogen atom to which it is bonded include 5- to 7-membered rings such as cyclopentane rings, cyclohexane rings, cyclopentene rings, benzene rings, piperidine rings, morpholine rings, lactone rings, and lactam rings.

[0205] R ed1 , R ed11 , R ed21 , R ed22 and R ed23 Halogen atoms and R that may be substituted ed4 , R ed5 Examples of halogen atoms represented by this formula include fluorine, chlorine, bromine, and iodine.

[0206] The methylene group contained in the alkyl group described above may be interrupted one to five times by unsaturated bonds, ether bonds, thioether bonds, ester bonds, thioester bonds, amide bonds, or urethane bonds. In this case, the interrupting group may be one or two or more types of groups, and if the group can be interrupted consecutively, it may be interrupted two or more times consecutively. Furthermore, the alkyl group may have branched side chains, may be a cyclic alkyl group, and the alkyl group terminus may be an unsaturated bond. Among these, it is preferable that the methylene group is interrupted by an ether bond.

[0207] Examples of alkyl groups interrupted by ether bonds include the following:

[0208] In particular, in the above formula (ED), R ed1 This represents an aryl group with 6 to 20 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 It is replaced with R ed21 R represents an alkyl group having 1 to 15 carbon atoms. ed21 The methylene group in the alkyl group is interrupted 1 to 5 times by ether bonds, R ed2 However, R ed11 Represents R ed11 However, R represents an alkyl group with 1 to 15 carbon atoms. ed3 However, it is preferable that it represents an alkyl group having 1 to 15 carbon atoms, and that a and b are 0.

[0209] R ed1This represents an aryl group with 6 to 15 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 It is replaced with R ed21 R represents an alkyl group having 1 to 10 carbon atoms. ed21 The methylene group in the alkyl group is interrupted 1 to 3 times by ether bonds, R ed2 However, R ed11 Represents R ed11 However, R represents an alkyl group with 1 to 10 carbon atoms. ed3 However, it is more preferable that the alkyl group has 1 to 10 carbon atoms, and that a and b are 0.

[0210] R ed1 This represents an aryl group with 6 to 12 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 It is replaced with R ed21 R represents an alkyl group having 1 to 8 carbon atoms. ed21 The methylene group in the alkyl group is interrupted once or twice by an ether bond, R ed2 However, R ed11 Represents R ed11 However, R represents an alkyl group with 1 to 8 carbon atoms. ed3 However, it is more preferable that it represents an alkyl group having 1 to 8 carbon atoms, and that a and b are 0.

[0211] R ed1 This represents an aryl group with 6 to 10 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 It is replaced with R ed21 R represents an alkyl group having 1 to 6 carbon atoms. ed21 The methylene group in the alkyl group is interrupted once by an ether bond, R ed2 However, R ed11 Represents R ed11 However, it represents an alkyl group with 1 to 3 carbon atoms, R ed3 However, it is even more preferable that it represents an alkyl group having 1 to 3 carbon atoms, and that a and b are 0.

[0212] The polymerization initiator (E) preferably contains at least one compound represented by formula (EA), formula (EB), or formula (ED), and more preferably contains a compound represented by formula (EA) or formula (ED) from the viewpoint of developability and luminescence intensity, and even more preferably contains a compound represented by formula (EA). The reason why the curable composition of the present invention provides the above effects is not entirely clear, but the inventors speculate as follows: That is, the structures represented by formula (EA), formula (EB), or formula (ED) all have a structure similar to a carbazole ring with many conjugated double bonds in the molecule, and are therefore presumed to have high photoradical polymerization initiation ability. This makes it easier to adjust the polymerization rate of the curable composition and makes it easier to improve solubility in the developer.

[0213] Examples of oxime compounds include acetophenone O-benzoyl oxime, N-benzoyloxy-1-(4-phenylsulfanylphenyl)butan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)-3-cyclopentylpropane-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethane-1-imine, and N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2,4-dioxacyclopentanylmethyl Examples include compounds described in Japanese Patent Publication No. 2011-132215, International Publication Nos. 2008 / 78678, 2008 / 78686, 2012 / 132558, 2017 / 051680, and 2020 / 004601. Commercially available products such as Irgacure OXE01 (N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine), OXE02 (N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethane-1-imine), OXE03 (all manufactured by BASF), N-1919, NCI-930, NCI-831 (all manufactured by ADEKA) may also be used.

[0214] Other polymerization initiators (E) include photopolymerization initiators such as alkylphenone compounds, biimidazole compounds, triazine compounds, and acylphosphine compounds, and thermal polymerization initiators such as azo compounds and organic peroxides.

[0215] From the viewpoint of luminescence intensity, the content of polymerization initiator (E) in the curable composition is preferably 0.1 parts by mass or more and 80 parts by mass or less, more preferably 0.1 parts by mass or more and 30 parts by mass or less, per 100 parts by mass of polymerizable compound (D). Furthermore, the content of polymerization initiator (E) in the curable composition is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 20 parts by mass or less, per 100 parts by mass of the total amount of resin (C) and polymerizable compound (D).

[0216] The content of the polymerization initiator (E) in the curable composition is, from the viewpoint of luminescence intensity, for example, 0.01% by mass or more and 20% by mass or less, preferably 0.1% by mass or more and 15% by mass or less, more preferably 0.2% by mass or more and 10% by mass or less, even more preferably 0.3% by mass or more and 8% by mass or less, even more preferably 0.5% by mass or more and 5% by mass or less, and particularly preferably 3% by mass or less, based on the total amount of solids in the curable composition.

[0217] <Antioxidant (Fa)> The curable composition may contain an antioxidant (Fa). The antioxidant (Fa) is not particularly limited as long as it is an antioxidant commonly used in industry, and phenolic antioxidants, phosphorus-based antioxidants, phosphorus / phenol complex antioxidants, sulfur-based antioxidants, etc., can be used. The curable composition may contain two or more antioxidants.

[0218] Examples of phosphorus / phenol complex antioxidants include Sumirizer® GP (6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenz[d,f][1.3.2]dioxaphosfepine) (manufactured by Sumitomo Chemical Co., Ltd.). Other antioxidants include, for example, the compounds described in Japanese Patent Application Publication No. 2024-61630.

[0219] The content of antioxidants (Fa) in the curable composition (total amount in the case of multiple types) is, for example, 1 part by mass or more and 50 parts by mass or less per 100 parts by mass of resin (C), and from the viewpoint of luminescence intensity, it is preferably 5 parts by mass or more and 40 parts by mass or less, and more preferably 7 parts by mass or more and 30 parts by mass or less.

[0220] <Leveling agent (H)> Examples of leveling agent (H) include silicone-based surfactants, fluorine-based surfactants, and silicone-based surfactants having a fluorine atom. These may have polymerizable groups in their side chains. It is preferable that the leveling agent (H) includes a silicone-based surfactant. The curable composition may contain two or more types of leveling agent (H).

[0221] Examples of silicone-based surfactants include surfactants having siloxane bonds in their molecules. Examples of such surfactants include the compounds described in Japanese Patent Application Publication No. 2024-61630.

[0222] Examples of fluorine-based surfactants include surfactants having fluorocarbon chains in their molecules. Examples of such surfactants include the compounds described in Japanese Patent Application Publication No. 2024-61630.

[0223] When the curable composition contains a leveling agent (H), the content of the leveling agent (H) in the curable composition is, for example, 0.001% by mass or more and 1.0% by mass or less, preferably 0.005% by mass or more and 0.75% by mass or less, and more preferably 0.01% by mass or more and 0.5% by mass or less, relative to the total amount of solids in the curable composition. When the content of the leveling agent (H) is within the above range, the flatness of the cured film when used as a wavelength conversion layer can be improved.

[0224] <Solvent (J)> Solvent (J) dissolves the resin (C) and the polymerizable compound (D) and polymerization initiator (E) used in a preferred embodiment. Examples of solvent (J) include the solvent described in Japanese Patent Application Publication No. 2024-61630.

[0225] The solvent (J) preferably contains one or more selected from the group consisting of propylene glycol monomethyl ether acetate, ethyl lactate, propylene glycol monomethyl ether, cyclohexyl acetate, ethyl 3-ethoxypropionate, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, 4-hydroxy-4-methyl-2-pentanone, and aromatic hydrocarbon solvents.

[0226] Solvent (J) is a component other than the solid content, and includes, for example, solvents contained in dispersions of semiconductor particles (A) or solutions of resins (C).

[0227] The solvent (J) content in the curable composition is the ratio of the total mass of all solvents contained in the curable composition to the total amount of the curable composition, and is, for example, 40% by mass or more and 95% by mass or less, preferably 50% by mass or more and 90% by mass or less, relative to the total amount of the curable composition. In other words, the solid content of the curable composition is, for example, 5% by mass or more and 60% by mass or less, preferably 10% by mass or more and 50% by mass or less. When the solvent (J) content is within the above range, the flatness of the curable composition layer during application is improved, and it tends to be easier to form a wavelength conversion layer of appropriate thickness.

[0228] <Other components> The curable composition may further contain additives known in the art, such as polymerization inhibitors, fillers, other polymer compounds, adhesion promoters, and chain transfer agents, as needed.

[0229] <<Cured Film>> The present invention includes a cured film formed from a curable composition. A cured film containing semiconductor particles (A) can emit light of a different wavelength from the irradiated light when irradiated with ultraviolet light or visible light. Therefore, a cured film containing semiconductor particles (A) can be used as a wavelength conversion film.

[0230] The thickness of the cured film is, for example, 0.5 μm or more and 10 μm or less, preferably 1 μm or more and 9 μm or less, more preferably 1.5 μm or more and 7 μm or less, and even more preferably 2 μm or more and 5 μm or less.

[0231] <<Method for Manufacturing a Curable Composition>> A curable composition can be manufactured by a method that includes mixing predetermined components and other components used as needed. The method for manufacturing a curable composition may further include a step of preparing a resin (C). Among the components contained in the curable composition, semiconductor particles (A) and light scattering agents (B) may be mixed with some or all of the solvent (J) beforehand before being mixed with the other components.

[0232] <<Method for Manufacturing a Cured Film>> The cured film according to the present invention can be manufactured by a manufacturing method that includes the steps of applying a curable composition containing semiconductor particles (A), a polymerizable compound (D), and a polymerization initiator (E), and a thermosetting step of thermally curing the coated film of the curable composition (hereinafter also referred to as the "composition layer"). Preferably, after the step of applying the curable composition, an exposure step of irradiating the coated film of the curable composition with light is included, and more preferably, the thermosetting step is performed after the exposure step.

[0233] The method for manufacturing a cured film may include steps other than those described above. Other steps include, for example, a drying step for drying the composition layer formed by the coating step, and a developing step performed on the composition layer after the exposure step. The cured film may be formed over the entire surface of the substrate, or it may be formed as a cured pattern on a part of the substrate surface. In this specification, a cured pattern is one aspect of a cured film, and refers to a cured film formed in a pattern.

[0234] The curable composition used for forming the cured film comprises semiconductor particles (A), a polymerizable compound (D), and a polymerization initiator (E), and an example thereof is the curable composition described above.

[0235] The coating process involves applying a curable composition to a substrate to form a composition layer. Coating methods include spin coating, slit coating, slit and spin coating, and inkjet printing. In the printing method, the curable composition is applied to the substrate via a mask, and after the mask is removed from the substrate, the composition layer formed in the coating process is cured to form a cured film as a cured pattern on a portion of the substrate surface.

[0236] When a curable composition is used as an inkjet ink, the curable composition may contain resin (C), but a low content is preferable. The content of resin (C) is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 3% by mass or less, even more preferably 2% by mass or less, particularly preferably 1% by mass or less, and may also be 0% by mass or 0.5% by mass or more, based on the total amount of solids in the curable composition. By reducing the content of resin (C), the viscosity of the curable composition can be reduced, which in turn can improve the ejection properties, particularly the ejection properties when ejected from the ejection head of an inkjet printer. The curable composition may contain two or more types of resin (C).

[0237] When used as an ink for inkjet printers, the curable composition can be ejected from the inkjet printer's ejection head at a temperature of 40°C or higher. The temperature of the curable composition when ejected from the inkjet printer's ejection head may be 50°C or higher, 60°C or higher, or 80°C or lower.

[0238] Examples of substrates include glass plates such as quartz glass, borosilicate glass, aluminasilate glass, and soda-lime glass with a silica coating on the surface; resin plates such as polycarbonate, polymethyl methacrylate, and polyethylene terephthalate; silicon; and substrates on which aluminum, silver, or silver / copper / palladium alloy thin films are formed. Preferably, the substrate is a glass plate or a silicon substrate.

[0239] The substrate may be pre-treated to adjust the wettability of the substrate surface. Examples of pre-treatment include solvent cleaning with alcohol or acetone, acid treatment, alkali treatment, plasma treatment, and corona treatment. By selecting an appropriate pre-treatment for the substrate on which the cured film is to be laminated, the applicability of the curable composition can be improved compared to an untreated substrate.

[0240] If the curable composition contains a solvent (J), it is preferable to perform a drying step after the coating step to remove volatile components such as the solvent (J) from the composition layer. The drying step may include a heat drying (pre-bake) treatment, a vacuum drying treatment, or both. When heat drying is performed, the temperature is preferably 30°C to 130°C, and more preferably 50°C to 120°C. The heating time is preferably 10 seconds to 60 minutes, and more preferably 30 seconds to 30 minutes. When vacuum drying is performed, it is preferable to perform it under a pressure of 50 Pa to 150 Pa and at a temperature range of 20°C to 25°C.

[0241] The thickness of the composition layer after the coating or drying process is not particularly limited and can be appropriately selected according to the desired thickness of the cured film. For example, it is 0.5 μm or more and 10 μm or less, preferably 1 μm or more and 9 μm or less, more preferably 1.5 μm or more and 7 μm or less, and even more preferably 2 μm or more and 5 μm or less. The thickness of the final cured film may also be the same as described above.

[0242] Next, it is preferable to perform an exposure step on the composition layer after the coating step or drying step. The exposed composition layer hardens due to polymerization of polymerizable compounds (D), etc., contained in the composition layer, including in preferred embodiments. As the light source used for exposure, a light source that generates light with a wavelength of 250 nm to 450 nm is preferred. If the curable composition contains a photopolymerization initiator (E), light around 436 nm, 408 nm, or 365 nm may be selectively extracted from the above wavelengths of light using a bandpass filter, depending on the absorption wavelength of the polymerization initiator (E). Specific examples of light sources include mercury lamps, light-emitting diodes, metal halide lamps, halogen lamps, etc.

[0243] The exposure amount in the exposure process is preferably 50 mJ / cm². 2 More preferably, 80 mJ / cm 2 More preferably 100 mJ / cm 2 More preferably, the concentration is 150 mJ / cm². 2 That's all. The exposure dose is typically 1000 mJ / cm².2 The following, preferably 800 mJ / cm² 2 More preferably, 700 mJ / cm 2 The following applies: The exposure amount in the exposure process is 1000 mJ / cm². 2 The following conditions prevent excessive shrinkage of the cured film, thereby preventing the semiconductor particles (A) from coming into close proximity within the film due to shrinkage and preventing a decrease in emitted light intensity. The exposure amount is the exposure amount based on a wavelength of 365 nm and can be measured using an ultraviolet integrated light meter (UIT-250, manufactured by Ushio Inc.).

[0244] One example of a method for forming a cured pattern, which is a form of a cured film, is photolithography. Photolithography is a method of exposing a composition layer through a photomask for forming the desired cured pattern and then developing it. In this case, it is preferable to use an exposure apparatus such as a mask aligner and a stepper, as this allows for uniform irradiation of the entire exposure surface with parallel light and enables precise alignment between the photomask and the substrate on which the composition layer is formed.

[0245] By subjecting the composition layer after the exposure process to a developing process in which it is brought into contact with a developer, the unexposed parts of the composition layer are dissolved and removed in the developer, thereby imparting a pattern to the composition layer. Examples of the developer include aqueous solutions of alkaline compounds such as potassium hydroxide, sodium bicarbonate, sodium carbonate, and tetramethylammonium hydroxide, or organic solvents. The concentration of the alkaline compound in the aqueous solution is preferably 0.01% by mass or more and 10% by mass or less, more preferably 0.03% by mass or more and 5% by mass or less. Examples of organic solvents include those similar to solvent (J) described above. The developer may also contain a surfactant. The developing method may be any of the following: the paddle method, the dipping method, or the spray method. Furthermore, the substrate may be tilted at any angle during development.

[0246] The composition layer after the exposure or development process is heat-cured (post-baked) in a heat-curing process. The heat-curing process allows for further polymerization of resins (C), polymerizable compounds (D), etc., including preferred embodiments, and improves resistance to solvents compared to before post-baking.

[0247] It is preferable to further heat (post-bake) the cured pattern obtained by development. The heating temperature is preferably 100°C to 250°C, and more preferably 150°C to 200°C. The heating time is preferably 1 minute to 120 minutes, and more preferably 10 minutes to 60 minutes. By heating after development, polymerization of unreacted polymerizable compounds (D) etc. contained in the cured pattern can be promoted, so a cured pattern with better chemical resistance can be obtained. Even if development is not performed, it is preferable to further heat (post-bake) the exposed composition layer.

[0248] The curing time in the curing process is preferably 0.1 hours or more, more preferably 0.2 hours or more, even more preferably 0.4 hours or more, and still more preferably 0.5 hours or more. The curing time is usually 2 hours or less, preferably 1.5 hours or less, and more preferably 1.2 hours or less.

[0249] The thermosetting process can be carried out in an atmospheric environment, or, from the viewpoint of increasing the intensity of the emitted light of the cured film, it can be carried out in a vacuum environment. A vacuum environment refers to a pressure range of 150 Pa or less, preferably 120 Pa or less, more preferably 100 Pa or less, and may be 50 Pa or more.

[0250] The cured film can exhibit good luminescence intensity. Preferably, the luminescence intensity of the cured film, as measured according to the measurement method described in the Examples section below, is 600 mW·sr. -1 ・m -2 The above is more more accurate, and more preferably 630 mW·sr -1 ・m -2 The above is preferable to 645 mW·sr -1 ・m -2 The above, and more preferably 700 mW·sr -1 ・m-2 The above is true, and more preferably 800 mW·sr -1 ・m -2 That's all.

[0251] <<Display Devices>> Because the cured film has the function of converting the wavelength of irradiated light, it can be used as a color conversion layer (wavelength conversion film) for display devices. Examples of such display devices include those described in Japanese Patent Publication No. 2006-309219, Japanese Patent Publication No. 2006-310303, Japanese Patent Publication No. 2013-15812, Japanese Patent Publication No. 2009-251129, Japanese Patent Publication No. 2014-2363, etc. The cured film according to the present invention is useful as a display device, in particular as a color conversion layer (wavelength conversion film) for liquid crystal display devices, organic EL display devices, or inorganic EL display devices.

[0252] This application claims the benefit of priority based on Japanese Patent Application No. 2025-078613, filed on 9 May 2025. The entire specification of Japanese Patent Application No. 2025-078613, filed on 9 May 2025, is incorporated herein by reference.

[0253] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" refer to mass percent and parts by mass, respectively, unless otherwise specified.

[0254] [Measurement of weight loss ratio above 300°C of semiconductor particles (A) containing organic ligand (G) (Measurement of X and measurement of the composition ratio of organic ligand)] The weight loss ratio above 300°C of semiconductor particles (A) containing organic ligand (G) was measured under the following conditions. 0.1 g of semiconductor particles (A) containing organic ligand (G) was redispersed in 1 mL of toluene, 9 mL of poor solvent was added to precipitate, and then the mixture was centrifuged at 4000 G for 20 minutes. The precipitated semiconductor particles (A) containing organic ligand (G) were redispersed in 0.5 mL of toluene. The resulting dispersion was dried at 110°C for 10 minutes to prepare a dry powder. The dry powder was heated from 25°C to 600°C at a heating rate of 10°C / min under a nitrogen atmosphere using thermogravimetric analysis (Bruker TG-DTA2000SA). Here, using the TG graph obtained by thermogravimetric analysis, the weight loss rate from 100°C to 300°C and from 300°C to 600°C were calculated, with the value (weight) at 100°C as the baseline. The ratio of the weight loss rate from 300°C to 600°C to the sum of these was defined as the weight loss rate above 300°C. In other words, the weight loss rate above 300°C (%), calculated by equation (2), was measured when semiconductor particles (A) containing each organic ligand (G) were heated from 25°C to 600°C under a nitrogen atmosphere at a heating rate of 10°C / min using thermogravimetric analysis. Note that the weight loss rate above 300°C (%) represents a simple ratio. Weight loss ratio above 300°C X (%) = {T1 / (T0 + T1)} × 100 … (2) (In equation (2), T0: Weight loss rate from 100°C to 300°C, based on the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C. T1: Weight loss rate from 300°C to 600°C, based on the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C.) Furthermore, when comparing the TG graph of the thermogravimetric analysis for the purified semiconductor particle (A) containing the organic ligand (G) of Preparation Example 1 with the TG graphs of the purified semiconductor particle (A) containing the organic ligand (G) of Preparation Examples 2 to 4, weight loss behavior was observed only in the TG graphs of the semiconductor particle (A) containing the organic ligand (G) of Preparation Examples 2 to 4 in the temperature range of 100°C to 300°C. This weight loss behavior between 100°C and 300°C is presumed to be due to hydrophilic organic ligands coordinated through ligand exchange.Therefore, the composition ratio of each organic ligand was calculated by using the ratio T0 / (T0+T1)×100 as the percentage of hydrophilic organic ligands and the ratio T1 / (T0+T1)×100 as the percentage of hydrophobic organic ligands. Note that the composition ratio of each organic ligand represents a simple proportion.

[0255] [Measurement of clogP of polymerization initiators (measurement of Y)] ClagP of each polymerization initiator was determined using ChemDraw 22.0 (manufactured by Cambridge Soft).

[0256] [Weight-average molecular weight] The weight-average molecular weight (Mw) of resin (C) was measured by the GPC method under the following conditions: Apparatus: K2479 (Shimadzu Corporation) Column: SHIMADZU Shim-pack GPC-80M Column temperature: 40°C Solvent: Tetrahydrofuran Flow rate: 1.0 mL / min Detector: RI Calibration standards: TSK STANDARD POLYSTYRENE F-40, F-4, F-288, A-2500, A-500 (Tosoh Corporation)

[0257] [Acid Value] 3 g of resin (C) solution was accurately weighed and dissolved in a mixed solvent of 90 g of acetone and 10 g of water. Using a 0.1 N KOH aqueous solution as the titrant, the acid value of resin (C) solution was measured using an automatic titrator (manufactured by Hiranuma Sangyo Co., Ltd., product name: COM-555). The acid value per gram of solids was determined from the acid value of the solution and the solids content of the solution.

[0258] [Solid Content] Approximately 1 g of resin (C) solution was weighed into an aluminum cup, dried at 180°C for 1 hour, and then its mass was measured. The solid content (mass %) of resin (C) solution was calculated from the amount of mass loss.

[0259] [Measurement of Fluorescence Emission Intensity of Cured Film] A surface-emitting backlight (OPSM series: manufactured by Optex FA Co., Ltd.) equipped with an LED lamp and diffuser plate with an emission peak wavelength of 450 nm was prepared as the backlight. The backlight was installed with the diffuser plate facing upwards, and a spectroradiometer (SR-UL1R: manufactured by Topcon Techno House Co., Ltd.) was placed at a height of 60 cm from the surface of the diffuser plate. A glass substrate (Eagle 2000: manufactured by Corning Corporation) was placed on the surface of the diffuser plate of the backlight as a reference. With the backlight turned on in this state, the integrated spectral irradiance value in the wavelength range of the backlight from 380 nm to 480 nm was measured through the reference glass substrate at 3.15 W·sr. -1 ・m -2 The backlight intensity was adjusted to achieve the following. Next, the reference glass substrate was removed, and a 5 cm square substrate having a cured film made from a curable composition was placed on the surface of the backlight diffuser plate. With the backlight turned on in this state, the light emitted from the cured film was measured as the integrated spectral irradiance (unit: mW・sr) in the wavelength range of 380 nm to 780 nm, and the luminous intensity was measured. -1 ・m -2 The following measurements were taken. Since the amount of absorbance of the initiator is affected by light from 380 nm to 480 nm, the luminescence intensity was evaluated including the region derived from the wavelength of the backlight.

[0260] [Evaluation of Developability] After the drying process (pre-bake), the coated film was immersed in a developer solution (0.10% TMAH aqueous solution) for 20 seconds and developed. The cured film after development was evaluated according to the following criteria. Developability was evaluated for coated films prepared under pre-bake temperatures of 90°C or 100°C. Good developability at higher pre-bake temperatures is advantageous in process selection because it allows for a wider range of selectable temperatures in the heating process after the exposure process. A: No undissolved residue B: Undissolved residue present (white haze)

[0261] (Preparation Example 1: Preparation of semiconductor particles (A) containing organic ligand (G) (hydrophobic organic ligand (G1))) <Production of core particles> Indium acetate (0.3 mmol) and zinc oleate (0.05 mmol) were added to a mixture of oleic acid (0.9 mmol), 1-dodecanethiol (0.1 mmol) and octadecene (10 mL), heated from room temperature to 120°C at a heating rate of 10°C per minute under vacuum (<20 Pa), and allowed to react for 1 hour. Subsequently, the mixture reacted under vacuum (<20 Pa) was brought to 25°C under a nitrogen atmosphere, tris(trimethylsilyl)phosphine (0.15 mmol) was added, then the mixture was heated to 300°C at a heating rate of 10°C per minute and allowed to react for 10 minutes. Furthermore, the reaction solution was cooled to 25°C, octanoyl chloride (0.60 mmol) was injected, the mixture was heated to 250°C at a heating rate of 10°C per minute and allowed to react for 30 minutes, then cooled to 25°C to obtain a dispersion solution of core particles.

[0262] <Production of precursor solution for shell formation> 40 mmol of zinc oleate and 75 mL of octadecene were mixed, and heated at 110°C for 1 hour under vacuum to prepare a Zn precursor solution with [Zn] = 0.4 M. Separately, 22 mmol of selenium powder and 10 mL of trioctylphosphine were mixed in nitrogen, and stirred until completely dissolved to obtain trioctylphosphine selenide with [Se] = 2.2 M. Further separately, 22 mmol of sulfur powder and 10 mL of trioctylphosphine were mixed in nitrogen, and stirred until completely dissolved to obtain trioctylphosphine sulfide with [S] = 2.2 M.

[0263] <Shell formation> The dispersion solution of core particles was heated to 250°C. At 250°C, 4.3 mL of the Zn precursor solution and 1.5 mL of trioctylphosphine selenide were added and allowed to react for 30 minutes, forming a ZnSe shell on the surface of the InP-based semiconductor nanoparticles. Furthermore, 3.8 mL of the Zn precursor solution and 0.5 mL of trioctylphosphine sulfide were added, the temperature was raised to 280°C and the mixture was allowed to react for 1 hour to form a ZnS shell.

[0264] <Purification of Core-Shell Particles> The reaction solution of the obtained core-shell particles was added to acetone, mixed well, and then centrifuged. The centrifugal acceleration was set to 4000 G. The precipitate was collected, and n-hexane was added to the precipitate to prepare a dispersion. This operation was repeated several times to obtain purified core-shell particles (semiconductor particles (A) containing organic ligand (G) (hydrophobic organic ligand (G1))).

[0265] (Preparation Example 2: Preparation of semiconductor particles (A1) containing organic ligand (Ga) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2))) In a flask, the semiconductor particles (A) containing organic ligand (G) obtained in Preparation Example 1 were dispersed in 1-octadecene at a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in a flask, and 1.0 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.1 g of zinc acetate were added to prepare the mixture. The mixture was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating it into a transparent 1-octadecene phase and a phase containing semiconductor particles (A1) containing organic ligand (Ga). The 1-octadecene phase was removed, and the phase containing semiconductor particles (A1) containing organic ligand (Ga) was recovered.

[0266] 5.0 mL of acetone was added to the obtained phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was collected. This procedure was repeated several times to obtain semiconductor particles (A1) containing purified organic ligands (Ga) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2)). The weight loss ratio above 300°C for the semiconductor particles (A1) containing organic ligands (Ga), as determined by the above measurement method, was 32.0%. The composition ratios of hydrophilic organic ligand (G2) and hydrophobic organic ligand (G1) in the semiconductor particles (A1) containing organic ligands (Ga), as determined by the above measurement method, were 68.0% and 32.0%, respectively.

[0267] (Preparation Example 3: Preparation of semiconductor particles (A2) containing organic ligand (Gb) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2))) In a flask, the semiconductor particles (A) containing the organic ligand (G) obtained in Preparation Example 1 were dispersed in 1-octadecene to a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in a flask, 1.0 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.1 g of zinc acetate were added to prepare Mixture 1. The Mixture 1 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, then transferred to a centrifuge tube, and centrifuged at 4000 G for 20 minutes, which separated the mixture into a transparent 1-octadecene phase and a phase containing the semiconductor particles (A) containing the organic ligand (G). The 1-octadecene phase was removed, and the phase containing the semiconductor particles (A) containing the organic ligand (G) was recovered.

[0268] Propylene glycol monomethyl ether acetate (hereinafter referred to as "PGMEA") (dispersion medium) was added to the remaining phase of semiconductor particles (A) containing the organic ligand (G), and a PGMEA dispersion was prepared such that the mass ratio of the semiconductor particles (A) containing the organic ligand (G) was 10% by mass. The prepared PGMEA dispersion was placed in a flask, 1.0 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.1 g of zinc acetate were added to prepare Mixture 2. The Mixture 2 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, and cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, 50 mL of n-hexane was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes to recover the phase containing the semiconductor particles (A2) containing the organic ligand (Gb).

[0269] 5.0 mL of acetone was added to the obtained phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was collected. This procedure was repeated several times to obtain semiconductor particles (A2) containing purified organic ligands (Gb) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2)). The weight loss ratio above 300°C for the semiconductor particles (A2) containing organic ligand (Gb), as determined by the above measurement method, was 18.3%. The composition ratios of hydrophilic organic ligand (G2) and hydrophobic organic ligand (G1) in the semiconductor particles (A2) containing organic ligand (Gb), as determined by the above measurement method, were 81.7% and 18.3%, respectively.

[0270] (Preparation Example 4: Preparation of semiconductor particles (A3) containing organic ligand (Gc) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2))) Semiconductor particles (A) containing organic ligand (G) obtained in Preparation Example 1 were dispersed in 1-octadecene in a flask at a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in a flask, and 1.2 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.12 g of zinc acetate were added to prepare mixture 3. The mixture 3 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating it into a transparent 1-octadecene phase and a phase containing semiconductor particles (A) containing organic ligand (G). The 1-octadecene phase was removed, and the phase containing semiconductor particles (A) containing organic ligand (G) was recovered.

[0271] PGMEA (dispersion medium) was added to the remaining semiconductor particle (A) phase containing the organic ligand (G) to prepare a PGMEA dispersion so that the semiconductor particle (A) containing the organic ligand (G) was 10% by mass. The prepared PGMEA dispersion was placed in a flask, and 1.2 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.12 g of zinc acetate were added to prepare mixture 4. The mixture 4 was stirred at 110°C for 60 minutes under a nitrogen atmosphere and cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, 50 mL of n-hexane was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes to recover the phase containing the semiconductor particle (A3) containing the organic ligand (Gc).

[0272] 5.0 mL of acetone was added to the obtained phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was collected. This procedure was repeated several times to obtain semiconductor particles (A3) containing purified organic ligands (Gc) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2)). The weight loss ratio above 300°C for the semiconductor particles (A3) containing organic ligands (Gc), as determined by the above measurement method, was 13.8%. The composition ratios of hydrophilic organic ligand (G2) and hydrophobic organic ligand (G1) in the semiconductor particles (A3) containing organic ligands (Gc), as determined by the above measurement method, were 86.2% and 13.8%, respectively.

[0273] (Preparation Example 5: Synthesis of Resin (C1)) 276.8 parts of propylene glycol monomethyl ether acetate were placed in a flask equipped with a stirrer, dropping funnel, condenser, thermometer, and gas inlet tube, and stirred while purging with nitrogen, and the temperature was raised to 120°C. Next, a monomer mixture consisting of 92.4 parts of 2-ethylhexyl acrylate, 184.9 parts of glycidyl methacrylate, and 12.3 parts of dicyclopentanyl methacrylate was mixed with 35.3 parts of t-butyl peroxy-2-ethylhexanoate (polymerization initiator), and this mixture was added dropwise to the flask from the dropping funnel over a period of 2 hours. After the addition was complete, the mixture was stirred at 120°C for a further 30 minutes to carry out the copolymerization reaction and produce an addition copolymer.

[0274] Subsequently, the flask was purged with air, and 93.7 parts of acrylic acid, 1.5 parts of triphenylphosphine (catalyst), and 0.8 parts of methoquinone (polymerization inhibitor) were added to the above addition copolymer solution. The reaction was continued at 110°C for 10 hours, during which the epoxy groups derived from glycidyl methacrylate reacted with acrylic acid to cleave the epoxy groups and simultaneously introduce polymerizable unsaturated bonds into the side chains of the polymer. Next, 24.2 parts of succinic anhydride were added to the reaction system, and the reaction was continued at 110°C for 1 hour, during which the hydroxyl groups generated by the cleavage of the epoxy groups reacted with succinic anhydride to introduce carboxyl groups into the side chains, thereby obtaining a polymer (resin (C1)).

[0275] Finally, 383.3 g of propylene glycol monomethyl ether acetate was added to the reaction solution to obtain a resin (C1) solution with a polymer solids content of 40%.

[0276] The weight-average molecular weight Mw of the resulting copolymer is 6.2 × 10⁻⁶. 3 The acid value, calculated on a solid content basis, was 35 mg KOH / g.

[0277] (Preparation Example 6: Preparation of dispersion c of light scattering agent (B)) 70 parts of titanium dioxide nanoparticles (B1) were mixed with 3 parts of BYK-LPN21116 (manufactured by Bic Chemie Japan) in solid content and PGMEA in total volume of 100 parts. The mixture was then stirred in a paint shaker until it was thoroughly dispersed to obtain dispersion c of light scattering agent (B1) (solid content 73%).

[0278] (Preparation Examples 7-13: Preparation of Curable Compositions No. 1-7) Semiconductor particles (A) and a dispersion c of a light scattering agent (B) were mixed with each component to prepare curable compositions No. 1-7 having the compositions shown in Table 1. In Table 1, the amounts of components other than the solvent (J) are shown as solid content equivalents.

[0279]

[0280] <Semiconductor Particles (A) and Organic Ligands (G)> (A1) + (Ga): Semiconductor particle (A1) containing hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2) prepared in Preparation Example 2 (A2) + (Gb): Semiconductor particle (A2) containing hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2) prepared in Preparation Example 3 (A3) + (Gc): Semiconductor particle (A3) containing hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2) prepared in Preparation Example 4 <Light Scattering Agent (B)> Light Scattering Agent (B1): Dispersion of light scattering agent (B) prepared in Preparation Example 6 <Resin (C)> Resin (C1): Resin (C1) prepared in Preparation Example 5 <Polymerizable Compound (D)> Polymerizable compound (D1): Carboxylate-containing polyfunctional (meth)acrylate (product name "Aronics® M-510" manufactured by Toagosei Co., Ltd.) Polymerizable compound (D2): Ethylene oxide-modified bisphenol A diacrylate (manufactured by Daicel Ornex, EBECRYL150, molecular weight 512) <Polymerization initiator (E)> Polymerization initiator (E1): Compound represented by the following formula (EA-1) (clogP 10.3)

[0281]

[0282] Polymerization initiator (E2): Compound represented by the following formula (ED-1) (ADEKA Corporation NCI-831, clogP 6.8)

[0283]

[0284] Polymerization initiator (E3): Compound represented by the following formula (EB-1) (OXE03clogP 14.2, manufactured by BASF)

[0285]

[0286] Polymerization initiator (E4): Compound represented by the following formula (EC-1) (ADEKA Corporation NCI-930 clogP 3.5)

[0287]

[0288] <Antioxidant (Fa)> Antioxidant (Fa1): "SumiLizer® GP" manufactured by Sumitomo Chemical Co., Ltd. <Leveling agent (H)> Leveling agent (H1): Polyether-modified silicone oil ("Toray Silicone SH8400" manufactured by Toray Dow Corning Co., Ltd.) <Solvent (J)> Solvent (J1): PGMEA (Propylene glycol monomethyl ether acetate)

[0289] (Example 1) On a 5 cm square glass substrate (Eagle 2000; Corning), curable compositions No. 1 to 7 obtained in Preparation Examples 7 to 13 were applied by spin coating to a post-baking film thickness of 2 μm. Then, a drying process (pre-baking) was performed at 90°C or 100°C for 3 minutes to form coating films 1 to 7 of curable compositions No. 1 to 7. After cooling, exposure was performed using an exposure machine (UPE-1255MA; Ushio Lighting Co., Ltd.) under an atmospheric atmosphere at 200 mJ / cm². 2 An exposure process was performed by irradiating with light at an exposure dose (based on a wavelength of 365 nm), and a heat curing process was performed by carrying out a heat curing treatment (post-bake) at 180°C for 30 minutes to obtain a substrate having cured films 1 to 7.

[0290] The developability (pre-bake temperature 90°C or 100°C) of the coating film obtained after the drying process (pre-bake) was evaluated. The results are shown in Table 2. In addition, the luminescence intensity of the obtained cured film was evaluated. The results are shown in Table 2.

[0291]

Claims

A curable composition comprising semiconductor particles (A), a polymerizable compound (D), and a polymerization initiator (E), The semiconductor particle (A) contains an organic ligand (G), A curable composition in which the value Z obtained from formula (1) satisfies the range of 115 to 600. Z = X × Y …(1) (In equation (1), X represents the weight loss ratio (%) above 300°C, calculated by equation (2), when semiconductor particles (A) containing an organic ligand (G) are heated from 25°C to 600°C under a nitrogen atmosphere at a heating rate of 10°C / min by thermogravimetric analysis. Y represents the clogP of the polymerization initiator (E).) Weight reduction ratio over 300℃ X (%) = {T1 / (T0+T1)}×100...(2) (In equation (2), T0: the weight loss rate from 100°C to 300°C, with the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C as the reference weight.) T1: The weight loss rate from 300°C to 600°C, relative to the weight of semiconductor particles (A) containing organic ligands (G) at 100°C. The curable composition according to claim 1, wherein the weight loss ratio X at 300°C or higher is 30% or less.   The curable composition according to claim 1 or 2, wherein the clogP of the polymerization initiator (E) is 1 to 25.   The curable composition according to claim 1 or 2, wherein the polymerization initiator (E) comprises an oxime compound.   The curable composition according to claim 1 or 2, further comprising a light scattering agent (B).   The curable composition according to claim 1 or 2, further comprising resin (C).   A cured film formed from the curable composition according to claim 1 or 2.   A display device comprising the cured film according to claim 7.