Curable composition, cured film, and display device

A curable composition with semiconductor particles and organic ligands, along with polymerizable compounds, addresses the issue of film appearance in quantum dot-based compositions, resulting in stable and aesthetically pleasing cured films for display devices.

WO2026235123A1PCT designated stage Publication Date: 2026-11-12SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017335
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-01
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing curable compositions containing semiconductor particles, such as quantum dots, do not produce cured films with desirable appearance qualities.

Method used

A curable composition comprising semiconductor particles with organic ligands and specific weight loss characteristics, along with a polymerizable compound and optional additives like polymerization initiators, solvents, and leveling agents, to enhance film appearance and stability.

Benefits of technology

The composition results in a cured film with improved appearance and stability, suitable for use in display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a curable composition having a good appearance; a cured film formed from the curable composition; and a display device including the cured film. The curable composition contains semiconductor particles (A) and a polymerizable compound (D). The semiconductor particles (A) contain an organic ligand (G). The percentage weight loss X at no lower than 300°C obtained according to a prescribed formula (1) is 35% or less when the semiconductor particles (A) containing the organic ligand (G) are heated according to thermogravimetric analysis from 25°C up to 600°C at a temperature increase rate of 10°C / min in a nitrogen atmosphere. The polar surface area of the polymerizable compound (D) is 80 Å2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Curable composition, cured film, and display device

[0001] This disclosure relates to a curable composition containing semiconductor particles, a cured film, and a display device containing the cured film.

[0002] Patent Document 1 describes a composition, a cured film, and a display device comprising quantum dots (A) and resin (B).

[0003] Japanese Patent Publication No. 2021-105108

[0004] In compositions containing semiconductor particles such as quantum dots, it is desirable that the cured film formed from the composition has a good appearance.

[0005] Therefore, the object of this disclosure is to provide a curable composition having a good appearance, a cured film formed from the curable composition, and a display device including the cured film.

[0006] The present disclosure, which has achieved the above objectives, is as follows: [1] A curable composition comprising semiconductor particles (A) and a polymerizable compound (D), wherein the semiconductor particles (A) comprises an organic ligand (G), and the weight loss ratio X above 300°C, calculated by formula (1) when the semiconductor particles (A) comprising the organic ligand (G) are heated from 25°C to 600°C in a nitrogen atmosphere at a heating rate of 10°C / min by thermogravimetric analysis, is 35% or less, and the polar surface area of ​​the polymerizable compound (D) is 80 Å 2 A curable composition that is: Weight reduction ratio X (%) = {T1 / (T0+T1)}×100...(1) [In formula (1), T 0 This is the weight loss rate from 100°C to 300°C, with the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C as the reference weight, and T 1 [1] The weight loss rate at 300°C to 600°C is based on the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C. [2] The curable composition according to [1], further comprising a polymerization initiator (E). [3] The curable composition according to [2], wherein the polymerization initiator (E) comprises an acylphosphine oxide compound or an oxime compound. [4] The weight loss rate X at 300°C or higher is 5 to 25%, and the polar surface area of ​​the polymerizable compound (D) is 70 Å. 2A curable composition according to any one of [1] to [3] below. [5] A curable composition according to any one of [1] to [4] which is an inkjet printer ink. [6] A curable composition according to any one of [1] to [5] in which the content of polymerizable compound (D) is 50% by mass or more and 70% by mass or less based on 100% by mass of the total solid content of the curable composition. [7] A curable composition according to any one of [1] to [6] in which the polymerizable compound (D) comprises at least one selected from the group consisting of dipropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and ethoxylated bisphenol fluorene di(meth)acrylate. [8] Use of the curable composition according to any one of [1] to [7] as an inkjet printer ink. [9] A cured film formed from the curable composition according to any one of [1] to [7].

[10] A display device comprising the cured film according to [9].

[0007] According to this disclosure, it is possible to provide a curable composition with a good appearance, a cured film formed from the curable composition, and a display device including the cured film.

[0008] <<Curable Composition>> The curable composition comprises semiconductor particles (A) and polymerizable compounds (D), wherein the semiconductor particles (A) contain organic ligands (G) and preferably also contain at least one selected from light scattering agents (B), polymerization initiators (E), antioxidants (Fa), leveling agents (H), and solvents (J) as needed.

[0009] In this specification, unless otherwise specified, the compounds exemplified as components may be used individually or in combination of two or more. Furthermore, when using multiple types of components, unless otherwise specified, the content should be adjusted by the total amount of all components used.

[0010] <Semiconductor Particle (A)> Semiconductor particle (A) is preferably a light-emitting inorganic semiconductor particle that absorbs primary light and emits light of a different wavelength than the primary light, and more preferably the light-emitting inorganic semiconductor particle absorbs primary light and emits green or red light, and even more preferably it converts the wavelength of blue light, which is the primary light, to the wavelength of red light or the wavelength of green light.

[0011] In this specification, "blue" refers to all light that is perceived as blue (all light with intensity in the blue wavelength range, for example, 380 nm to 495 nm), and is not limited to light of a single wavelength. "Green" refers to all light that is perceived as green (all light with intensity in the green wavelength range, for example, 495 nm to 585 nm), and is not limited to light of a single wavelength. "Red" refers to all light that is perceived as red (all light with intensity in the red wavelength range, for example, 585 nm to 780 nm), and is not limited to light of a single wavelength.

[0012] Examples of semiconductor particles (A) include quantum dots and particles composed of compounds having a perovskite crystal structure (hereinafter also referred to as "perovskite compounds"), with quantum dots being preferred. Quantum dots are luminescent inorganic semiconductor nanoparticles with a particle diameter of 1 nm to 100 nm (preferably 1 nm to 50 nm, more preferably 1 nm to 30 nm), which utilize the band gap of the semiconductor to absorb ultraviolet light or visible light (e.g., blue light) and emit light.

[0013] Examples of quantum dots include CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, HgS, HgSe, HgTe, CdHgTe, CdSeS, CdSeTe, CdSte, ZnSeS, ZnSeTe, ZnSte, HgSeS, HgSeTe, HgSte, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSte, CdHgSeS, CdHgSte, CdHgSte, HgZnSeS, HgZn Examples include compounds of group 12 elements and group 16 elements such as SeTe and HgZnSte; compounds of group 13 elements and group 15 elements such as GaN, GaP, GaAs, AlN, AlP, AlAs, InN, InP, InAs, GaNP, GaNAs, GaPAs, AlNP, AlNAs, AlPAs, InNP, InNAs, InPAs, GaAlNP, GaAlNAs, GaAlPAs, GaInNP, GaInNAs, GaInPAs, InAlNP, InAlNAs, InAlPAs; and compounds of group 14 elements and group 16 elements such as PdS and PbSe. Among these, quantum dots are preferably compounds of group 12 elements and group 16 elements, or compounds of group 13 elements and group 15 elements.

[0014] If the quantum dots contain sulfur (S) or senium (Se), quantum dots that have been surface-modified with metal oxides or organic materials may be used. By using surface-modified quantum dots, it is possible to prevent the extraction of S or Se by reactive components contained in or that may be contained in the curable composition.

[0015] Furthermore, the quantum dots may form a core-shell structure by combining the above-mentioned compounds. From the viewpoint of luminescence intensity, the core and shell are preferably selected from the group consisting of compounds of group 12 and group 16 elements and compounds of group 13 and group 15 elements. More preferably, the core is selected from the group consisting of compounds of group 12 and group 16 elements and compounds of group 13 and group 15 elements, and the shell is more preferably a compound of group 12 and group 16 elements. It is even more preferably that the core is selected from the group consisting of CdS, CdSe, CdTe, InN, InP, and InAs, and it is even more preferably that the shell is selected from the group consisting of ZnS, ZnSe, ZnTe, ZnSeS, ZnSeTe, and ZnSTe. Among these, examples include fine particles in which the core is CdSe and the shell is ZnS, fine particles in which the core is InP and the shell is ZnSeS, and fine particles in which the core is InP and the shells are ZnSe and ZnS.

[0016] Since the energy state of a quantum dot depends on its size, the emission wavelength can be freely selected by changing the particle size. Furthermore, because the light emitted from quantum dots has a narrow spectral width, it is advantageous for widening the color gamut of display devices. In addition, quantum dots have high responsiveness, which is advantageous in terms of primary light utilization efficiency.

[0017] Examples of perovskite compounds include those described in Japanese Patent Publication No. 2024-61630.

[0018] The curable composition may contain one or more types of semiconductor particles (A). The curable composition may contain only semiconductor particles that emit light of a specific wavelength, or it may contain two or more types of semiconductor particles that emit light of different wavelengths.

[0019] From the viewpoint of luminescence intensity, the content of semiconductor particles (A) in the curable composition is preferably 3% to 60% by mass, more preferably 10% to 55% by mass, even more preferably 20% to 50% by mass, and particularly preferably 20% to 40% by mass, based on 100% by mass of the solid content of the curable composition.

[0020] In the present specification, the total amount of solids in the curable composition means the sum of components included in the curable composition excluding the solvent (J). The content percentage in the solids of the curable composition can be measured by a known analysis means such as liquid chromatography or gas chromatography. The content percentage of each component in the solids of the curable composition may be calculated from the formulation at the time of preparing the curable composition.

[0021] <Organic Ligand (G)> The semiconductor particles (A) preferably contain the organic ligand (G), and the semiconductor particles (A) are present in the curable composition in a state where the organic ligand (G) is coordinated (hereinafter sometimes referred to as coordinated semiconductor particles (AG)). The organic ligand (G) is, for example, an organic compound having a polar group that exhibits coordination ability to the semiconductor particles (A) and an organic group. The organic ligand (G) can be coordinated to the surface of the semiconductor particles (A), for example. The curable composition may contain one or two or more types of organic ligands (G).

[0022] It is preferable that at least some of the molecules of the organic ligand (G) are coordinated to the semiconductor particles (A), and all or almost all of the molecules may be coordinated to the semiconductor particles (A). Including the organic ligand (G) coordinated to the semiconductor particles (A) can be advantageous from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A), as well as the emission intensity when the cured film is used as a wavelength conversion layer.

[0023] The aforementioned polar group of the organic ligand (G) is, for example, a phosphine group (-PR a 2 , R a represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms.), a phosphine oxide group (-PR b 2 O, R b represents a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms), a thiol group (-SH), a carboxy group (-COOH) and an amino group (-NH 2The group consists of at least one group selected from the group consisting of thiol groups and carboxyl groups. A polar group selected from this group may be advantageous in enhancing the coordination to the semiconductor particle (A). High coordination can contribute to improved stability and dispersibility of the semiconductor particle (A) in the curable composition, as well as improved luminescence intensity when the cured film is used as a wavelength conversion layer. In particular, from the viewpoint of increasing luminescence intensity, it is more preferable that the polar group is at least one group selected from the group consisting of thiol groups and carboxyl groups. The organic ligand (G) may have one or more polar groups.

[0024] The organic group of the organic ligand (G) is preferably a hydrocarbon group. The hydrocarbon group may contain heteroatoms (such as N, O, S, halogen atoms, etc.). The hydrocarbon group is preferably an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, or an aromatic hydrocarbon group.

[0025] Examples of aliphatic hydrocarbon groups include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, henicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, hentriacontyl, dotriacontyl, tritriacontyl, tetratriacontyl, pentatriacontyl, hexatriacontyl, heptatriacontyl, octatriacontyl, nonatriacontyl, and tetracontyl; Isopropyl group, isobutyl group, sec-butyl group, tert-butyl group, 2-ethylbutyl group, 3,3-dimethylbutyl group, 1,1,3,3-tetramethylbutyl group, 1-methylbutyl group, 1-ethylpropyl group, 3-methylbutyl group, neopentyl group, 1,1-dimethylpropyl group, 2-methylpentyl group, 3-ethylpentyl group, 1,3-dimethylbutyl group, 2-propylpentyl group, 1-ethyl-1,2-dimethylpropyl group, 1-methylpentyl group, 4-methylpentyl group, 4-methylpentyl group Branched alkyl groups such as hexyl group, 5-methylhexyl group, 2-ethylhexyl group, 1-methylhexyl group, 1-ethylpentyl group, 1-propylbutyl group, 3-ethylheptyl group, 2,2-dimethylheptyl group, 1-methylheptyl group, 1-ethylhexyl group, 1-propylpentyl group, 1-methyloctyl group, 1-ethylheptyl group, 1-propylhexyl group, 1-butylpentyl group, 1-methylnonyl group, 1-ethyloctyl group, 1-propylheptyl group, and 1-butylhexyl group;Ethenyl group (vinyl group), propenyl group (e.g., 1-propenyl group, 2-propenyl group (allyl group)), 1-methylethenyl group, butenyl group (e.g., 1-butenyl group, 2-butenyl group, 3-butenyl group), 3-methyl-1-butenyl group, 1,3-butadienyl group, 1-(2-propenyl)ethenyl group, 1-(1-methylethenyl)ethenyl group, 1,2-dimethyl-1-propenyl group, pentenyl group (e.g., 1-pentenyl group, 2-pentenyl group, 3-pentenyl group, 4-pentenyl group), 1-(1,1-dimethylethyl)ethenyl group, 1,3-dimethyl-1-butenyl group, hexenyl group (e.g., Alkenyl groups such as 1-hexenyl group, 5-hexenyl group, heptenyl group (e.g., 1-heptenyl group, 6-heptenyl group), octenyl group (e.g., 1-octenyl group, 7-octenyl group), nonenyl group (e.g., 1-nonenyl group, 8-nonenyl group), decenyl group (e.g., 1-decenyl group, 9-decenyl group), undecenyl group, dodecenyl group, tridecenyl group, tetradecenyl group, pentadecenyl group, hexadecenyl group, heptadecenyl group, octadecenyl group, nonadecenyl group, icocenyl group, 1,1-dimethyl-2-propenyl group, 1-ethyl-2-propenyl group, and 1-methyl-1-butenyl group; Examples include ethylyl groups, propynyl groups (e.g., 1-propynyl, 2-propynyl), octinyl groups (e.g., 1-octinyl, 7-octinyl), butynyl, pentynyl, hexynyl, heptynyl, noninyl, desinyl, undecynyl, dodecynyl, tridecynyl, tetradecynyl, pentadecynyl, hexadecinyl, heptadecynyl, octadecynyl, nonadecinyl, and icosinyl groups; and other alkynyl groups.

[0026] The number of carbon atoms in the aliphatic hydrocarbon group is preferably 1 to 40, more preferably 2 to 30, and even more preferably 3 to 20.

[0027] Examples of alicyclic hydrocarbon groups include cyclopropyl group, 1-methylcyclopropyl group, cyclobutyl group, cyclopentyl group, cyclohexyl group, cycloheptyl group, 1-methylcyclohexyl group, 2-methylcyclohexyl group, 3-methylcyclohexyl group, 4-methylcyclohexyl group, 1,2-dimethylcyclohexyl group, 1,3-dimethylcyclohexyl group, 1,4-dimethylcyclohexyl group, 2,3-dimethylcyclohexyl group, 2,4-dimethylcyclohexyl group, 2,5-dimethylcyclohexyl group, 2,6-dimethylcyclohexyl group, 3,4-dimethylcyclohexyl group, 3,5-dimethylcyclohexyl group, 2,2-dimethylcyclohexyl group, 3,3-dimethylcyclohexyl group, and 4,4 Examples include cycloalkyl groups such as dimethylcyclohexyl group, cyclooctyl group, 2,4,6-trimethylcyclohexyl group, 2,2,6,6-tetramethylcyclohexyl group, 3,3,5,5-tetramethylcyclohexyl group, 4-pentylcyclohexyl group, 4-octylcyclohexyl group, and 4-cyclohexylcyclohexyl group; cycloalkenyl groups such as cyclohexenyl group (e.g., cyclohexa-1-en-1-yl group, cyclohexa-2-en-1-yl group, cyclohexa-3-en-1-yl group), cycloheptenyl group, and cyclooctenyl group; saturated or unsaturated polycyclic hydrocarbon groups such as norbornyl group, norborneyl group, adamantyl group, and bicyclo[2.2.2]octyl group; and so on.

[0028] The number of carbon atoms in the alicyclic hydrocarbon group is preferably 3 to 40, more preferably 3 to 30, and even more preferably 3 to 20.

[0029] Aromatic hydrocarbon groups include phenyl group, o-tolyl group, m-tolyl group, p-tolyl group, 2-ethylphenyl group, 3-ethylphenyl group, 4-ethylphenyl group, 2,3-dimethylphenyl group, 2,4-dimethylphenyl group, 2,5-dimethylphenyl group, 2,6-dimethylphenyl group, 3,4-dimethylphenyl group, 3,5-dimethylphenyl group, 4-vinylphenyl group, o-isopropylphenyl group, m-isopropylphenyl group, p-isopropylphenyl group, o-tert-butylphenyl group, m-tert-butylphenyl group, p-tert-butylphenyl group, 3,5-di(tert-butyl)phenyl group, 3,5-di(tert-butyl)-4-methylphenyl group, and 4-butyl Aromatic hydrocarbon groups such as phenyl group, 4-pentylphenyl group, 2,6-bis(1-methylethyl)phenyl group, 2,4,6-tris(1-methylethyl)phenyl group, 4-cyclohexylphenyl group, 2,4,6-trimethylphenyl group, 4-octylphenyl group, 4-(1,1,3,3-tetramethylbutyl)phenyl group, 1-naphthyl group, 2-naphthyl group, 6-methyl-2-naphthyl group, 5,6,7,8-tetrahydro-1-naphthyl group, 5,6,7,8-tetrahydro-2-naphthyl group, fluorenyl group, phenanthryl group, anthryl group, 2-dodecylphenyl group, 3-dodecylphenyl group, 4-dodecylphenyl group, perilenyl group, chrysenyl group, and pyrenyl group; and the like.

[0030] The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 40, more preferably 6 to 30, and even more preferably 6 to 20.

[0031] The hydrocarbon group may further have hydrophilic functional groups. The hydrophilic functional groups are preferably hydroxyl groups, carboxyl groups, carbonyl groups, thiol groups, amino groups, ether bonds, ester bonds, and siloxane bonds. If the hydrocarbon group has an ether bond, the hydrocarbon group is composed of -CH 2 The - may be replaced by -O-. If the hydrocarbon group has an ester bond, the -CH constituting the hydrocarbon group 2 -CH 2 -CH 2The - may be replaced by -C(=O)-O- or -O-C(=O)-. When the hydrocarbon group has a siloxane bond, the -CH constituting the hydrocarbon group 2 -CH 2 The - may be replaced by -Si-O-. Also, the methylene group contained in the hydrocarbon group may be replaced by -S-, -C(=O)-, -C(=O)-NH-, -NH-, etc.

[0032] The organic ligand (G) preferably contains at least one selected from the group consisting of a hydrophobic organic ligand (G1) and a hydrophilic organic ligand (G2). The hydrophobic organic ligand (G1) is preferably a compound having the above-mentioned polar group and the above-mentioned hydrocarbon group (preferably a hydrocarbon group without a hydrophilic functional group). The hydrophilic organic ligand (G2) is preferably a compound having the above-mentioned polar group and a hydrocarbon group having a hydrophilic functional group. The presence of a hydrophilic functional group in the organic group enables dispersion in a polar dispersion medium. The organic ligand (G) may contain one or more hydrophobic organic ligands (G1) and hydrophilic organic ligands (G2).

[0033] A hydrophobic organic ligand (G1) is, for example, given by the following formula (x): X A -R X It is preferable that the organic compound is represented by (x). In the formula, X A R is the polar group described above, X It is preferable that the hydrocarbon group is a monovalent hydrocarbon group which may contain heteroatoms (such as N, O, S, halogen atoms, etc.). The hydrocarbon group may have one or more unsaturated bonds, such as carbon-carbon double bonds. The hydrocarbon group may have a linear, branched, or cyclic structure. The number of carbon atoms in the hydrocarbon group is, for example, 1 to 40, and may be 1 to 30. XIt is more preferable that the ligand is a monovalent aliphatic hydrocarbon group. The monovalent aliphatic hydrocarbon group may be the same as the aliphatic hydrocarbon group described above. In particular, the hydrocarbon group is preferably an alkyl group, alkynyl group, or alkenyl group having 1 to 40 carbon atoms (preferably 1 to 30 carbon atoms). The organic group of the hydrophobic organic ligand (G1) may also contain substituents such as halogen atoms or heteroatoms (N, O, S).

[0034] X A The polar group represented is preferably at least one group selected from the group consisting of a phosphine group, a phosphine oxide group, a thiol group, a carboxyl group, and an amino group. There may be one or more polar groups.

[0035] polar group A Specific examples of organic ligands having a carboxyl group include saturated or unsaturated fatty acids. Specific examples of saturated or unsaturated fatty acids include saturated fatty acids such as propionic acid, butyric acid, pentanoic acid, caproic acid, caprylic acid, capric acid, lauric acid, myristic acid, pentadecyl acid, palmitic acid, margaric acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid; monounsaturated fatty acids such as myristoleic acid, palmitoleic acid, oleic acid, eicosenoic acid, erucic acid, and nervonic acid; and polyunsaturated fatty acids such as linoleic acid, alpha-linolenic acid, gamma-linolenic acid, stearic acid, dihomo-gamma-linolenic acid, arachidonic acid, eicosatetraenoic acid, docosadienoic acid, and adrenaline (docosatetraenoic acid).

[0036] polar group A Specific examples of organic ligands having a thiol group or an amino group include the polar group X exemplified above. A This includes organic ligands in which the carboxyl group of an organic ligand having a carboxyl group is replaced by a thiol group or an amino group. Polar group X A Specific examples of organic ligands having a thiol group include hexanethiol, octanthiol, decanethiol, and 1-dodecanethiol. Polar group X A Examples of organic ligands having an amino group include oleylamine. Polar group X AExamples of organic ligands having a phosphine group or a phosphine oxide group include trioctylphosphine and trioctylphosphine oxide.

[0037] From the viewpoint of improving the stability and dispersibility of semiconductor particles, the molecular weight of the hydrophobic organic ligand (G1) is preferably 1500 or less, more preferably 1000 or less, and even more preferably 800 or less. The molecular weight of the hydrophobic organic ligand (G1) is usually 100 or more. That is, the molecular weight of the hydrophobic organic ligand (G1) is preferably 100 to 1500, 100 to 1000, or 100 to 800. The above molecular weight may be the number average molecular weight or the weight average molecular weight. In this case, the number average molecular weight and the weight average molecular weight are the number average molecular weight and the weight average molecular weight on a standard polystyrene basis measured by gel permeation chromatography (GPC), respectively.

[0038] Examples of hydrophilic organic ligands (G2) include compound (G2-1) and compound (G2-2).

[0039] [Compound (G2-1)] Compound (G2-1) is preferably a compound having a first functional group, a second functional group, and a divalent organic group. The first functional group is preferably a carboxyl group (-COOH) or a hydroxyl group (-OH), and the second functional group is preferably a carboxyl group or a thiol group (-SH). The first and second functional groups correspond to the hydrophilic functional group and the polar group, respectively. There may be one or more first and second functional groups. Since compound (G2-1) has a carboxyl group, a thiol group, and a hydroxyl group, it can be a ligand that coordinates to semiconductor particles (A). The curable composition may contain only one compound (G2-1) or two or more. The divalent organic group may be any hydrocarbon group that is divalent as described above.

[0040] An example of compound (G2-1) is the compound represented by the following formula (G2-1a). Compound (G2-1) may also be the acid anhydride of the compound represented by formula (G2-1a).

[0041]

[0042] [In the formula, R B R represents a divalent hydrocarbon group. B If present, they may be the same or different. The hydrocarbon group may have one or more substituents. If multiple substituents are present, they may be the same or different, and they may be bonded to each other, forming a ring with the atom to which each substituent is bonded. The hydrocarbon group contains -CH 2 - is -O-, -S-, -SO 2 It may be replaced by at least one of -, -CO-, and -NH-. p represents an integer from 1 to 10.

[0043] R B Examples of divalent hydrocarbon groups represented by this symbol include chain hydrocarbon groups, alicyclic hydrocarbon groups, aromatic hydrocarbon groups, and groups that combine these.

[0044] Examples of linear hydrocarbon groups include linear or branched alkanediyl groups, which typically have 1 to 40 carbon atoms, preferably 1 to 20, and more preferably 1 to 10. Examples of alicyclic hydrocarbon groups include monocyclic or polycyclic cycloalkanediyl groups, which typically have 3 to 40 carbon atoms, preferably 3 to 20, and more preferably 3 to 10. Examples of aromatic hydrocarbon groups include monocyclic or polycyclic arenediyl groups, which typically have 6 to 20 carbon atoms.

[0045] Examples of substituents that the hydrocarbon group may have include C1-C40 alkyl groups, C3-C40 cycloalkyl groups, C6-C20 aryl groups, carboxyl groups, amino groups, and halogen atoms. Preferably, the substituents that the hydrocarbon group may have are carboxyl groups, amino groups, or halogen atoms.

[0046] The above hydrocarbon group contains -CH 2 If - is replaced by at least one of -O-, -CO-, and -NH-, then -CH 2 The hyphen is preferably replaced by at least one of -CO- and -NH-, and more preferably by -NH-. p is preferably 1 or 2.

[0047] Examples of compounds represented by formula (G2-1a) include those represented by the following formulas (1-1) to (1-9).

[0048]

[0049] Specific examples of compounds represented by formula (G2-1a), listed by their chemical names, include, for example, mercaptoacetic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, 3-mercaptobutanoic acid, 4-mercaptobutanoic acid, mercaptohexanoic acid, mercaptooctanoic acid, mercaptoundecanoic acid, mercaptosuccinic acid, mercaptostearic acid, 4-mercaptobenzoic acid, 2,3,5,6-tetrafluoro-4-mercaptobenzoic acid, L-cysteine, N-acetyl-L-cysteine, 3-methoxybutyl 3-mercaptopropionic acid, and 3-mercapto-2-methylpropionic acid. Among these, 3-mercaptopropionic acid and mercaptosuccinic acid are preferred.

[0050] Another example of compound (G2-1) is a polycarboxylic acid compound, preferably a compound (G2-1b) in which the -SH in formula (G2-1a) is replaced with a carboxyl group (-COOH).

[0051] Examples of compounds (G2-1b) include the following:

[0052] Succinic acid, glutaric acid, adipic acid, octafluoroadipic acid, azelaic acid, dodecanediic acid, tetradecanediic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanediic acid, nonadecanedioic acid, dodecafluoroseveric acid, 3-ethyl-3-methylglutaric acid, hexafluoroglutaric acid, trans-3-hexenodioic acid, sebacic acid, hexadecafluorosebacic acid, acetylenedicarboxylic acid, trans-aconitic acid, 1,3-adamantanedicarboxylic acid, bicyclo[2.2.2]octane-1,4-dicarboxylic acid, cis-4-silicon Chlohexene-1,2-dicarboxylic acid, 1,1-cyclopropanedicarboxylic acid, 1,1-cyclobutanedicarboxylic acid, cis- or trans-1,3-cyclohexanedicarboxylic acid, cis- or trans-1,4-cyclohexanedicarboxylic acid, 1,1-cyclopentanediacetic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, decahydro-1,4-naphthalenedicarboxylic acid, 2,3-norbornanedicarboxylic acid, 5-norbornene-2,3-dicarboxylic acid, phthalic acid, 3-fluorophthalic acid, isophthalic acid, tetrafluoroiso Phthalic acid, terephthalic acid, tetrafluoroterephthalic acid, 2,5-dimethylterephthalic acid, 2,6-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,1'-ferrocenedicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 2,5-franzicarboxylic acid, benzophenone-2,4'-dicarboxylic acid monohydrate, benzophenone-4,4'-dicarboxylic acid, 2,3-pyrazinedicarboxylic acid, 2,3-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 3,5-Pyridinedicarboxylic acid, 2,5-Pyridinedicarboxylic acid, 2,6-Pyridinedicarboxylic acid, 3,4-Pyridinedicarboxylic acid, Pyrazole-3,5-dicarboxylic acid monohydrate, 4,4'-Stilbenidicarboxylic acid, Anthraquinone-2,3-dicarboxylic acid, 4-(carboxymethyl)benzoic acid, Cheridonic acid monohydrate, Azobenzene-4,4'-dicarboxylic acid, Azobenzene-3,3'-dicarboxylic acid, Chlorendic acid, 1H-Imidazole-4,5-dicarboxylic acid, 2,2-Bis(4-carboxyphenyl)hexafluoropropane, 1,10-Bis(4-carboxyphenoxy)decane, dipropylmalonic acid, dithiodiglycolic acid, 3,3'-dithiodipropionic acid, 4,4'-dithiodibutanoic acid, 4,4'-dicarboxydiphenyl ether, 4,4'-dicarboxydiphenyl sulfone, ethylene glycol bis(4-carboxyphenyl) ether, 3,4-ethylenedioxythiophene-2,5-dicarboxylic acid, 4,4'-isopropylidenediphenoxyacetic acid, 1,3-acetonedicarboxylic acid, methylenedisalicylic acid, 5,5'-thiodisalicylic acid, tris(2-carboxyethyl) isocyanurate, tetrafluorosuccinic acid, α,α,α',α'-tetramethyl-1,3-benzenedipropionic acid, 1,3,5-benzenetricarboxylic acid, etc.

[0053] From the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer, the molecular weight of compound (G2-1) is preferably 3,000 or less, more preferably 2,500 or less, even more preferably 2,000 or less, still more preferably 1,000 or less, particularly preferably 800 or less, and most preferably 500 or less. The molecular weight of compound (G2-1) is usually 100 or more. That is, the molecular weight of compound (G2-1) is preferably 100 to 3,000, 100 to 2,500, 100 to 2,000, 100 to 1,000, 100 to 800, or 100 to 500.

[0054] The above molecular weight may be either the number-average molecular weight Mn or the weight-average molecular weight Mw. In this case, Mn and Mw are standard polystyrene equivalent values ​​measured by gel permeation chromatography (GPC).

[0055] The content ratio of compound (G2-1) to semiconductor particles (A) in the curable composition is preferably 0.001 to 1 by mass, more preferably 0.01 to 0.5, and even more preferably 0.02 to 0.45. Having this content ratio within this range is advantageous in terms of the stability and dispersibility of the semiconductor particles (A), as well as improving the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0056] The content of compound (G2-1) in the curable composition is preferably 0.1% to 20% by mass, more preferably 0.2% to 20% by mass, even more preferably 0.2% to 10% by mass, even more preferably 0.5% to 10% by mass, and particularly preferably 0.5% to 8% by mass, relative to the total amount of solids in the curable composition, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0057] [Compound (G2-2)] Compound (G2-2) is a compound different from compound (G2-1), containing a polyalkylene glycol structure and having polar groups at its molecular ends. Preferably, the molecular end is the end of the longest carbon chain in compound (G2-2) (the carbon atoms in the carbon chain may be replaced by other atoms such as oxygen atoms).

[0058] The semiconductor particle (A) may contain only one compound (G2-2) or two or more compounds. The semiconductor particle (A) may contain compound (G2-1) or compound (G2-2), or may contain compound (G2-1) and compound (G2-2).

[0059] Compounds containing a polyalkylene glycol structure and having the above-mentioned first functional group, second functional group, and divalent organic group shall be classified as compound (G2-1).

[0060] The structure of polyalkylene glycol is as follows:

[0061]

[0062] This refers to a structure represented by (n is an integer greater than or equal to 2). In the formula, R C This is an alkylene group, such as an ethylene group or a propylene group.

[0063] A specific example of compound (G2-2) is a polyalkylene glycol compound represented by the following formula (G2-2a).

[0064]

[0065] In formula (G2-2a), X is a polar group, Y is a monovalent group, and Z C R is a divalent or trivalent base. n is an integer greater than or equal to 2. m is 1 or 2. C This is an alkylene group.

[0066] Polar group X is a phosphine group (-PR a 2 , R a ) represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms (preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms). ), phosphine oxide group (-PR b 2 O, R b (wherein represents a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms), a thiol group (-SH), a carboxyl group (-COOH), and an amino group (-NH 2 It is preferable that the polar group X is at least one group selected from the group consisting of thiol groups and carboxyl groups. A polar group selected from this group may be advantageous in improving coordination to semiconductor particles (A). In particular, from the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer, it is more preferable that the polar group X is at least one group selected from the group consisting of thiol groups and carboxyl groups, and even more preferable that it is a thiol group.

[0067] Group Y is a monovalent organic group. Group Y is not particularly limited and may include monovalent hydrocarbon groups that have substituents (such as N, O, S, halogen atoms, etc.). The hydrocarbon group contains -CH 2 The hyphen may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. The number of carbon atoms in the hydrocarbon group is, for example, 1 to 12. The hydrocarbon group may have an unsaturated bond.

[0068] Examples of group Y include alkyl groups having 1 to 12 carbon atoms and having a linear, branched, or cyclic structure; and alkoxy groups having 1 to 12 carbon atoms and having a linear, branched, or cyclic structure. The number of carbon atoms in the alkyl and alkoxy groups is preferably 1 to 8, more preferably 1 to 6, and even more preferably 1 to 4. The alkyl and alkoxy groups contain -CH 2 The - may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. In particular, group Y is preferably a linear or branched alkoxy group having 1 to 4 carbon atoms, and more preferably a linear alkoxy group having 1 to 4 carbon atoms.

[0069] Group Y may contain a polar group. The polar group may be a phosphine group (-PR a 2 , R a ) represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms (preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms). ), phosphine oxide group (-PR b 2 O, R b (wherein represents a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms), a thiol group (-SH), a carboxyl group (-COOH), and an amino group (-NH 2 A maximum of one group selected from the group consisting of ) is mentioned. However, as described above, compounds containing a polyalkylene glycol structure and having the first and second functional groups are considered to belong to compound (G2-2). The polar group is preferably located at the terminal end of group Y.

[0070] Base Z C It is a divalent or trivalent group. Group Z C Examples include divalent or trivalent hydrocarbon groups, which are not particularly limited and may contain heteroatoms (such as N, O, S, halogen atoms, etc.). The number of carbon atoms in the hydrocarbon group is, for example, 1 to 24. The hydrocarbon group may have unsaturated bonds.

[0071] The divalent group Z CExamples include alkylene groups having a linear, branched, or cyclic structure with 1 to 24 carbon atoms; and alkenylene groups having a linear, branched, or cyclic structure with 1 to 24 carbon atoms. The number of carbon atoms in the alkyl and alkenylene groups is preferably 1 to 12, more preferably 1 to 8, and even more preferably 1 to 4. The alkyl and alkenylene groups contain -CH 2 The hyphen may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. The trivalent group Z C An example of this is the divalent group Z mentioned above. C We can give an example of a group obtained by removing one hydrogen atom from the same group.

[0072] Base Z C The group Z may have a branched structure. C In a branch chain separate from the branch chain containing the polyalkylene glycol structure shown in formula (G2-2a) above, the branch chain may have a polyalkylene glycol structure separate from the polyalkylene glycol structure shown in formula (G2-2a) above.

[0073] In particular, Base Z C It is preferably a linear or branched alkylene group having 1 to 6 carbon atoms, and more preferably a linear alkylene group having 1 to 4 carbon atoms.

[0074] R C The group is an alkylene group, preferably a linear or branched alkylene group having 1 to 6 carbon atoms, and more preferably a linear alkylene group having 1 to 4 carbon atoms.

[0075] In formula (G2-2a), n is an integer of 2 or more, preferably 2 to 540, more preferably 2 to 120, even more preferably 2 to 60, even more preferably 2 to 30, even more preferably 2 to 15, and particularly preferably 2 to 10.

[0076] Specific examples of compound (G2-2) include, but are not limited to, HS-PEG-COOH, PEG-SH, polyethylene glycol monomethyl ether thiol, polypropylene glycol monomethyl ether thiol, 3-mercaptopropionic acid-PEG ester, and preferably polyethylene glycol monomethyl ether thiol and polypropylene glycol monomethyl ether thiol, and more preferably HS-(CH2CH2O) k It is a compound represented as -CH3 (where k is an integer between 2 and 10).

[0077] The molecular weight of compound (G2-2) may be, for example, 150 to 10,000, but from the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer, it is preferably 150 to 5,000, more preferably 150 to 4,000, even more preferably 150 to 1,500, even more preferably 150 to 1,000, and particularly preferably 150 to 800. The molecular weight may be a number-average molecular weight or a weight-average molecular weight. In this case, the number-average molecular weight and the weight-average molecular weight are standard polystyrene equivalent values ​​measured by GPC.

[0078] The content ratio of compound (G2-2) to semiconductor particles (A) in the curable composition is preferably 0.001 to 2 by mass, more preferably 0.01 to 1.5, and even more preferably 0.1 to 1. Having this content ratio within this range is advantageous in terms of the stability and dispersibility of the semiconductor particles (A), as well as improving the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0079] The content of compound (G2-2) in the curable composition is preferably 0.1% to 40% by mass, more preferably 0.1% to 20% by mass, even more preferably 1% to 15% by mass, and still more preferably 2% to 12% by mass, relative to the total amount of solids in the curable composition, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0080] To improve the dispersion of semiconductor particles (A), and from the viewpoint of improving luminescence intensity, the composition ratio of hydrophilic organic ligands (G2) is preferably 60% or more, more preferably 62% or more, even more preferably 65% ​​or more, even more preferably 75% or more, 80% or more, and 85% or more, relative to all organic ligands (G) that coordinate to the semiconductor particles. Furthermore, from the viewpoint of appearance, the composition ratio is preferably 95% or less, more preferably 90% or less, and even more preferably 87% or less. That is, the composition ratio of hydrophilic organic ligands (G2) is preferably 60-95%, 62-95%, 65-90%, 75-90%, 80-87%, or 85-87%. Furthermore, from the viewpoint of improving the viscosity of the curable composition, the composition ratio is preferably 60% to 86%, more preferably 70% to 86%, and even more preferably 75% to 86%. The ratio of hydrophilic organic ligands (G2) to all organic ligands (G) coordinating to semiconductor particles (A) can be calculated from {T0 / (T0+T1)} × 100 (where T0 and T1 are the same as above). Specifically, this can be determined by the method described in the examples.

[0081] The semiconductor particle (A) preferably contains a hydrophobic organic ligand (G1) and a hydrophilic organic ligand (G2) as an organic ligand (G), more preferably contains a compound represented by formula (x) and a polyalkylene glycol compound represented by formula (G2-2a), and even more preferably contains oleic acid, 1-dodecanethiol, trioctylphosphine and triethylene glycol monomethyl etherthiol.

[0082] The ratio of the content of organic ligands (G) to semiconductor particles (A) in the curable composition is preferably 0.001 or more and 1 or less by mass, more preferably 0.01 or more and 0.8 or less, and even more preferably 0.02 or more and 0.5 or less. Having this content ratio within this range can be advantageous in terms of the stability and dispersibility of the semiconductor particles (A), and in improving the luminescence intensity when the cured film is used as a wavelength conversion layer. The content of organic ligands (G) as used herein refers to the total content of all organic ligands contained in the curable composition.

[0083] Semiconductor particles (A) or coordination-type semiconductor particles (AG) containing an organic ligand (G) are heated from 25°C to 600°C in a nitrogen atmosphere at a heating rate of 10°C / min by thermogravimetric analysis, and the weight loss ratio X above 300°C, calculated by equation (1), is 35% or less. Such semiconductor particles (A) and a polar surface area of ​​80 Å, as described later, are also included. 2By using the following polymerizable compound (D), the appearance of the cured film can be improved, and preferably the process resistance and / or viscosity of the curable composition can be improved as described below. The weight loss ratio X at 300°C or higher of semiconductor particles (A) or coordination semiconductor particles (AG) containing an organic ligand (G) is preferably greater than 0%, more preferably 3% or higher, even more preferably 5% or higher, even more preferably 10% or higher, and even more preferably 12% or higher. Also, the weight loss ratio X at 300°C or higher is preferably 35% or less, more preferably 30% or less, even more preferably 25% or less, even more preferably 20% or less, and even more preferably 15% or less. The weight loss ratio X at 300°C or higher may be greater than 0% and 35% or less, 1% or more and 35% or less, 1% or more and 30% or less, 3% or more and 25% or less, 3% or more and 20% or less, 5% or more and 15% or less, 5% or more and 14% or less, or 12% or more and 14% or less. The reason why the curable composition of this disclosure provides the above-mentioned effects is not entirely clear, but the inventors speculate as follows: When the weight loss ratio X above 300°C is within the aforementioned range, the balance between hydrophobicity and hydrophilicity is appropriately controlled. This allows for good dispersion of semiconductor particles (A) even during exposure. Furthermore, when the polar surface area of ​​the polymerizable compound (D) is within the aforementioned range, the distance between semiconductor particles (A) becomes uniform, improving the compatibility between the polymerizable compound (D) and semiconductor particles (A) or coordination-type semiconductor particles (AG) containing the organic ligand (G), resulting in good dispersibility of each component. As a result, aggregation of semiconductor particles (A) is suppressed in the cured film after exposure, reducing the generation of foreign matter, thus improving the appearance of the cured film and further improving the process resistance described later. Weight loss ratio X above 300°C (%) = {T1 / (T 0+ T1)}×100...(1) [In formula (1), T 0 This is the weight loss rate from 100°C to 300°C, with the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C as the reference weight, and T 1This is the weight loss rate between 300°C and 600°C, relative to the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C. In other words, the weight loss ratio above 300°C represents the proportion of the hydrophobic organic ligand (G1) to all the organic ligands (G) coordinating to the semiconductor particle (A).

[0084] The weight loss ratio of semiconductor particles (A) or coordination-type semiconductor particles (AG) containing an organic ligand (G) at temperatures above 300°C can be adjusted, for example, in a semiconductor particle preparation method in which semiconductor particles are mixed with an organic ligand described later, and then the semiconductor particles are washed one or more times, by adjusting the type, number, and amount of organic ligand (G), or by adjusting the type and amount of solvent, washing temperature, and washing time in the washing process.

[0085] The content of semiconductor particles (A) containing an organic ligand (G) in the curable composition is preferably 10% to 75% by mass, more preferably 12% to 70% by mass, and even more preferably 25% to 60% by mass, relative to the total amount of solids in the curable composition, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer.

[0086] <Polymerizable Compound (D)> Polymerizable compound (D) is a compound that can be polymerized by active radicals generated from polymerization initiator (E), acids, etc., as described later. The polar surface area of ​​polymerizable compound (D) is 80 Å. 2 The following applies: When the polar surface area is within the above range, compatibility with semiconductor particles (A) is good, and the appearance of the cured film formed from the curable composition is good. Furthermore, when the polar surface area is within the above range, when the curable composition is exposed to light and heat-cured to obtain a cured film, the decrease in the ratio of the luminescence intensity of the cured film after heat curing to the luminescence intensity of the cured film after exposure (hereinafter referred to as process tolerance) can be suppressed. In other words, the polar surface area of ​​the polymerizable compound (D) is 80 Å. 2 The following conditions can improve the appearance of the cured film and, preferably, also improve process resistance. Polar surface area is the area value of the polar portion of the molecular surface, and can be calculated using Chem3D version 22.2, etc.

[0087] Furthermore, when using two or more polymerizable compounds (D), the polar surface area of ​​the polymerizable compounds (D) shall be calculated using a weighted average value based on the mass-based content ratio.

[0088] The polar surface area of ​​polymerizable compound (D) is 20–80 Å. 2 Preferably, 30 to 70 Å 2 More preferably, 30 to 65 Å 2 More preferably, 45-65 Å 2 More preferably, 55-65 Å 2 This is particularly preferable. When the polar surface area of ​​compound (D) is within the above range, the appearance of the cured film and / or process resistance and / or viscosity of the curable composition can be improved.

[0089] Furthermore, the polar surface area is 80 Å. 2 The molecular weight or weight-average molecular weight Mw of the polymerizable compound (D) is preferably, for example, 100 to 850, more preferably 150 to 700, even more preferably 150 to 500, and still more preferably 150 to 400. The polymerizable average molecular weight Mw should be used only when the polymerizable compound (D) is a mixed component and it is difficult to calculate the molecular weight.

[0090] Polar surface area is 80 Å 2 The polymerizable compound (D) below includes polymerizable compounds having one or more groups having an ethylenically unsaturated bond in the molecule (hereinafter sometimes referred to as ethylenically unsaturated groups), where the number of ethylenically unsaturated groups is preferably 2 to 4, and more preferably 2.

[0091] The ethylenically unsaturated group may be, for example, a vinyl group, a (meth)acryloyl group, or other groups that constitute an α-olefin, or a hydrocarbon group in which carbon atoms are bonded to both carbon atoms of a double bond. However, groups that constitute an α-olefin are preferred, (meth)acryloyl groups are more preferred, and acryloyl groups are even more preferred.

[0092] When the molecule contains two or more ethylenically unsaturated groups, it is preferable that the compound is one in which two or more ethylenically unsaturated groups are bonded to a single linking group. For example, when the ethylenically unsaturated group is a (meth)acryloyl group, a compound can be given in which two or more (meth)acrylic acid groups are bonded to a polyhydric alcohol by an ester bond, or a compound in which two or more (meth)acrylic acid groups are bonded to a polyhydric alcohol via a polyoxyalkylene glycol. The (meth)acryloyl group is preferably an acryloyl group.

[0093] The polyhydric alcohol may be an aliphatic polyhydric alcohol or an aromatic polyhydric alcohol. Dihydric alcohols are preferred as aliphatic polyhydric alcohols, including ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, triethylene glycol, dipropylene glycol, and tripropylene glycol. Aromatic polyhydric alcohols include polyhydric alcohols having an aromatic ring, such as compounds having a cardi structure, like 4,4'-(9H-fluorene-9,9-diyl)diphenol. Dihydric to tetrahydric aromatic polyhydric alcohols are preferred, with dihydric being more preferred.

[0094] The number of repeating oxyalkylene groups in polyoxyalkylene glycol is, for example, 1 to 6, preferably 1 to 4, and more preferably 1 to 2. Examples of polyoxyalkylene glycols include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, and tripropylene glycol. Polyoxyalkylene glycol forms ester bonds with (meth)acrylic acid and ether bonds with polyhydric alcohols. When two or more (meth)acrylic acid molecules are bonded to a polyhydric alcohol via polyoxyalkylene glycol, the polyoxyalkylene glycol may be different depending on the (meth)acrylic acid, or it may be the same, but it is preferable that it be the same.

[0095] The number of ethylenically unsaturated groups may be the same as the number of hydroxyl groups in the polyhydric alcohol, or it may be one or two fewer than the number of hydroxyl groups.

[0096] Polar surface area is 80 Å 2 Examples of polymerizable compounds (D) include diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, ethoxylated bisphenol fluorene di(meth)acrylate, and propoxylated bisphenol fluorene di(meth)acrylate. Among these, dipropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and ethoxylated bisphenol fluorene di(meth)acrylate are preferred, and dipropylene glycol di(meth)acrylate and 1,6-hexanediol di(meth)acrylate are more preferred.

[0097] The content of polymerizable compound (D) in the curable composition (total amount if multiple types are included) is preferably 20% to 80% by mass, more preferably 30% to 70% by mass, even more preferably 40% to 70% by mass, and even more preferably 50% to 70% by mass, based on 100% by mass of the total solid content of the curable composition. When the content of polymerizable compound (D) is within the above range, the appearance of the cured film can be made good.

[0098] In particular, the weight loss ratio X of the semiconductor particle (A) containing the organic ligand (G) at 300°C or higher is 5 to 25%, and the polar surface area of ​​the polymerizable compound (D) is 70 Å. 2 Preferably, the following conditions are met: the weight loss ratio X of the semiconductor particle (A) containing the organic ligand (G) at 300°C or higher is 8 to 25%, and the polar surface area of ​​the polymerizable compound (D) is 65 Å. 2 It is more preferable that the following conditions are met: the weight loss ratio X of the semiconductor particle (A) containing the organic ligand (G) at 300°C or higher is 8 to 20%, and the polar surface area of ​​the polymerizable compound (D) is 65 Å. 2It is even more preferable that the weight loss ratio X of the semiconductor particle (A) containing the organic ligand (G) at 300°C or higher is 12 to 15%, and the polar surface area of ​​the polymerizable compound (D) is 65 Å. 2 More preferably, the following conditions are met, and in any of these preferred embodiments, the polar surface area of ​​the polymerizable compound (D) is preferably 20 Å or more. This range allows for a good appearance of the cured film, as well as good process resistance and / or viscosity of the curable composition.

[0099] <Light scattering agent (B)> Examples of light scattering agent (B) include metal or metal oxide particles, and inorganic particles such as glass particles. Examples of metal oxides include TiO 2 SiO 2 , BaTiO 3 Examples include ZnO, and TiO is preferred because it efficiently scatters light and increases the luminescence intensity. 2 These are particles. The particle size of the light scattering agent (B) is, for example, about 0.03 μm to 20 μm, preferably 0.05 μm to 1 μm, and more preferably 0.05 μm to 0.5 μm.

[0100] As the light scattering agent (B), a solution may be used in which the light scattering agent is pre-dispersed in part or all of the solvent (J) using a dispersant (I). Examples of the dispersant (I) include the compounds described in Japanese Patent Application Publication No. 2024-61630.

[0101] The content of the light scattering agent (B) in the curable composition is, for example, 0.001% by mass or more and 50% by mass or less, relative to the total amount of solids in the curable composition. From the viewpoint of improving the light scattering ability and luminescence intensity when the cured film is used as a wavelength conversion layer, it is preferably 1% by mass or more and 40% by mass or less, more preferably 2% by mass or more and 30% by mass or less, even more preferably 3% by mass or more and 25% by mass or less, and still more preferably 4% by mass or more and 20% by mass or less.

[0102] <Polymerization Initiator (E)> A polymerization initiator (E) is a compound that generates active radicals, acids, etc., upon the action of light or heat, and can initiate the polymerization of a polymerizable compound (D). The curable composition may contain one or more polymerization initiators (E).

[0103] Examples of polymerization initiators (E) include photopolymerization initiators such as oxime compounds, alkylphenone compounds, biimidazole compounds, triazine compounds, acylphosphine oxide compounds, benzoin compounds, benzophenone compounds, quinone compounds, 10-butyl-2-chloroacridone, benzyl, methyl phenylglyoxylate, and titanocene compounds; and thermal polymerization initiators such as azo compounds and organic peroxides. Specifically, as the oxime compounds, alkylphenone compounds, biimidazole compounds, triazine compounds, benzoin compounds, benzophenone compounds, and quinone compounds, compounds exemplified in Japanese Patent Application Publication No. 2024-61630 can be used.

[0104] The polymerization initiator (E) preferably contains an acylphosphine oxide compound or an oxime compound, and more preferably contains an acylphosphine oxide compound.

[0105] Including an acylphosphine oxide compound as a polymerization initiator (E) can be advantageous in terms of improving appearance and / or viscosity. One reason for this effect is presumed to be that the acylphosphine oxide compound possesses a bisacyl structure, which allows it to exhibit high radical generation ability upon cleavage by light irradiation, and to absorb ultraviolet light across a wide wavelength range, enabling efficient polymerization initiation even in opaque systems and improving curability under UV irradiation.

[0106] Acylphosphine oxide compounds are compounds having a substructure represented by the following formula (1) (where * indicates a bond).

[0107]

[0108] The acylphosphine oxide compound may be a monoacylphosphine oxide compound, a bisacylphosphine oxide compound, or a triacylphosphine oxide compound, with monoacylphosphine oxide compounds or bisacylphosphine oxide compounds being preferred, and bisacylphosphine oxide compounds being more preferred.

[0109] Examples of the acylphosphine oxide-based compound include a compound represented by the following formula (1A).

[0110] [In formula (1A), a represents an integer of 1 to 3. R 1 and R 2 each independently represent a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent, and -CH contained in the hydrocarbon group 2 - may be replaced with -O-, -CO- or -OCO-. When a plurality of R 1 are present, they may be the same or different, and when a plurality of R 2 are present, they may be the same or different.]

[0111] R 1 and R 2 Examples of the hydrocarbon group having 1 to 25 carbon atoms represented by include a saturated hydrocarbon group having 1 to 25 carbon atoms, an unsaturated hydrocarbon group having 2 to 25 carbon atoms, an aromatic hydrocarbon group having 6 to 25 carbon atoms, and the like.

[0112] Examples of the saturated hydrocarbon group having 1 to 25 carbon atoms include linear alkyl groups such as methyl group, ethyl group, propyl group, butyl group, pentyl group, hexyl group, heptyl group, octyl group, nonyl group, decyl group, dodecyl group, hexadecyl group and icosyl group; branched alkyl groups such as isopropyl group, isobutyl group, isopentyl group, neopentyl group and 2-ethylhexyl group; alicyclic saturated hydrocarbon groups having 3 to 20 carbon atoms such as cyclopropyl group, cyclopentyl group, cyclohexyl group, cycloheptyl group, cyclooctyl group and tricyclodecyl group; and the like. The number of carbon atoms in the saturated hydrocarbon group is preferably 1 to 20, more preferably 1 to 15, and still more preferably 1 to 10.

[0113] Examples of the unsaturated hydrocarbon group having 2 to 25 carbon atoms include alkenyl groups such as vinyl group, allyl group, butenyl group, pentenyl group, hexenyl group, heptenyl group, octenyl group, nonenyl group, decenyl group, undecenyl group, dodecenyl group, hexadecenyl group, octadecenyl group and icosenyl group; alkynyl groups such as ethynyl group, propynyl group, hexynyl group, decynyl group and icosynyl group; cycloalkenyl groups such as cyclopentenyl group, cyclohexenyl group and cycloheptenyl group; and the like. The number of carbon atoms of the unsaturated hydrocarbon group is preferably 2 to 20, more preferably 2 to 15, and still more preferably 2 to 10.

[0114] Examples of the aromatic hydrocarbon group having 6 to 25 carbon atoms include phenyl group, xylyl group, dimethylphenyl group, trimethylphenyl group, dipropylphenyl group, di(2,2-dimethylpropyl)phenyl group, naphthyl group, benzyl group, phenylethyl group, phenylbutyl group and the like. The number of carbon atoms of the aromatic hydrocarbon group is preferably 6 to 20, more preferably 6 to 18, still more preferably 6 to 15, and even more preferably 6 to 12.

[0115] R 1 and R 2 Examples of the substituent that the hydrocarbon group represented by may have include a halogen atom, a cyano group, and a nitro group. The halogen atom is preferably a fluorine atom, a bromine atom, a chlorine atom, or an iodine atom.

[0116] -CH contained in the hydrocarbon group 2 - may be replaced with -O-, -CO- or -OCO-, and adjacent -CH 2 - are not simultaneously substituted with the same type of group, and the terminal -CH 2 - is not substituted.

[0117] a represents any integer of 1 to 3, preferably 1 or 2, and more preferably 2.

[0118] R 1 and R 2The hydrocarbon group having 1 to 25 carbon atoms represented by is preferably an aromatic hydrocarbon group having 6 to 25 carbon atoms, more preferably an aromatic hydrocarbon group having 6 to 20 carbon atoms, even more preferably an aromatic hydrocarbon group having 6 to 12 carbon atoms, even more preferably a phenyl group, a xylyl group, a dimethylphenyl group, or a trimethylphenyl group, even more preferably a phenyl group, a dimethylphenyl group, or a trimethylphenyl group, and even more preferably a phenyl group or a trimethylphenyl group.

[0119] The polymerization initiator (E) preferably contains at least one compound represented by formula (1A) from the viewpoint of improving the appearance and / or viscosity of the curable composition.

[0120] Examples of acylphosphine compounds include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-(2,4-dipentyloxyphenyl), and (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, with bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and (2,4,6-trimethylbenzoyl)diphenylphosphine oxide being preferred. Commercial acylphosphine compounds such as OMNIRAD® 819 (manufactured by IGM Resins) may also be used.

[0121] Examples of oxime compounds include those having a substructure represented by the following formula (da1) or formula (da2). * and ** represent bonding sites.

[0122]

[0123] The oxime compound preferably has at least one substructure selected from those represented by the following formulas (d-1) to (d-4). If the oxime compound has these substructures, a curable composition that can form a cured film with good surface properties can be easily provided. The oxime compound more preferably has the substructure represented by formula (d-1) or the substructure represented by formula (d-3), and even more preferably has the substructure represented by formula (d-1). In particular, if the oxime compound has the substructure represented by formula (d-1) (carbazole skeleton), a curable composition with excellent patternability is obtained. In formulas (d-1) to (d-4), * and ** represent bonding. In the following substructures represented by formulas (d-1) to (d-3), * bonds with a structure other than the substructure represented by formula (da1) or formula (da2). The substructures represented by the following formulas (d-1) to (d-4) are combined with the substructures represented by the aforementioned formula (da1) or formula (da2).

[0124]

[0125] The polymerization initiator (E) preferably contains a compound represented by formula (EA).

[0126] [In the formula, R ea1 R represents a branched hydrocarbon group having 3 to 20 carbon atoms, which may have substituents. ea2 ~R ea5 Each of these independently represents a hydrocarbon group having 1 to 20 carbon atoms, which may have substituents. n represents an integer from 0 to 4. The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-.

[0127] R ea1 Examples of branched hydrocarbon groups having 3 to 20 carbon atoms, represented by , include branched saturated hydrocarbon groups having 3 to 20 carbon atoms and branched unsaturated hydrocarbon groups having 3 to 20 carbon atoms.

[0128] R ea1Examples of branched saturated hydrocarbon groups having 3 to 20 carbon atoms, represented by , include 1-methylethyl group (isopropyl group), 1-methylpropyl group (sec-butyl group), 2-methylpropyl group (isobutyl group), 1,1-dimethylethyl group (tert-butyl group), 1,1-dimethylpropyl group, 2,2-dimethylpropyl group, 1,2-dimethylpropyl group, 1-ethylpropyl group, 1-methylbutyl group, 2-methylbutyl group, 3-methylbutyl group, 1,1-dimethylbutyl group, and 2,2-dimethylbutyl group. ,3,3-dimethylbutyl group, 1,2-dimethylbutyl group, 1,3-dimethylbutyl group, 2,3-dimethylbutyl group, 1-ethylbutyl group, 2-ethylbutyl group, 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 4-methylpentyl group, 1,1-dimethylpentyl group, 2,2-dimethylpentyl group, 3,3-dimethylpentyl group, 1,2-dimethylpentyl group, 1,3-dimethylpentyl group, 2,3-dimethylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3 - Ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 4-methylhexyl group, 1,1-dimethylhexyl group, 2,2-dimethylhexyl group, 3,3-dimethylhexyl group, 1,2-dimethylhexyl group, 1,3-dimethylhexyl group, 2,3-dimethylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 4-methylheptyl group, 1,1-dimethylheptyl Butyl group, 2,2-dimethylheptyl group, 3,3-dimethylheptyl group, 1,2-dimethylheptyl group, 1,3-dimethylheptyl group, 2,3-dimethylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, 3-ethylheptyl group, 1-methyloctyl group, 2-methyloctyl group, 3-methyloctyl group, 4-methyloctyl group, 1,1-dimethyloctyl group, 2,2-dimethyloctyl group, 3,3-dimethyloctyl group, 1,2-dimethyloctyl group, 1,3-dimethyloctyl group, 2,Examples include branched alkyl groups such as 3-dimethyloctyl group, 1-ethyloctyl group, 2-ethyloctyl group, 3-ethyloctyl group, 1-methylnonyl group, 2-methylnonyl group, 3-methylnonyl group, 4-methylnonyl group, dimethylnonyl group, ethylnonyl group, methyldecyl group, dimethyldecyl group, ethyldecyl group, methylundecyl group, dimethylundecyl group, ethylundecyl group, and methyldodecyl group. ea1 The branched alkyl group represented by may be a primary branched alkyl group, a secondary branched alkyl group, or a tertiary branched alkyl group. ea1 The number of carbon atoms in the branched saturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, preferably 16 or less, more preferably 12 or less, and even more preferably 10 or less (i.e., 4 to 16, 4 to 12, or 5 to 10 are preferred).

[0129] R ea1 The branched unsaturated hydrocarbon group represented by the above-mentioned R is ea1 Examples include groups in which at least one carbon-carbon single bond in a branched saturated hydrocarbon group represented by is replaced by a carbon-carbon double bond or a carbon-carbon triple bond. ea1 Examples of branched unsaturated hydrocarbon groups represented by include alkenyl groups such as isopropenyl, isobutenyl, isopentenyl, isohexenyl, isoheptenyl, isooctenyl, isononyl, and isodecenyl groups; alkynyl groups such as isopropynyl, isobutynyl, isopentinyl, isohexynyl, isoheptynyl, isooctynyl, isononinyl, and isodesynyl groups; and so on. ea1 The number of carbon atoms in the branched unsaturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, preferably 16 or less, more preferably 12 or less, and even more preferably 10 or less (i.e., 4 to 16, 4 to 12, or 5 to 10 are preferred).

[0130] R ea2 , R ea3 , R ea4 and R ea5Examples of hydrocarbon groups having 1 to 20 carbon atoms represented by include saturated hydrocarbon groups having 1 to 20 carbon atoms, unsaturated hydrocarbon groups having 2 to 20 carbon atoms, and aromatic hydrocarbon groups having 6 to 20 carbon atoms. ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon groups represented by may be the same or different.

[0131] Examples of the saturated hydrocarbon groups having 1 to 20 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, hexadecyl, and eicosyl groups; branched alkyl groups such as isopropyl, isobutyl, isopentyl, neopentyl, and 2-ethylhexyl groups; and alicyclic saturated hydrocarbon groups having 3 to 20 carbon atoms such as cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and tricyclodecyl groups. The number of carbon atoms in the saturated hydrocarbon group is preferably 1 to 18, more preferably 1 to 15, even more preferably 1 to 10, and even more preferably 1 to 8.

[0132] Examples of the carbon-2 to carbon-20 unsaturated hydrocarbon groups include alkenyl groups such as vinyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, dodecenyl, hexadecenyl, octadecenyl, and eicosenyl groups; alkynyl groups such as ethynyl, propynyl, hexynyl, desinyl, and eicosinyl groups; and cycloalkenyl groups such as cyclopentenyl, cyclohexenyl, and cycloheptenyl groups. The carbon number of the unsaturated hydrocarbon group is preferably 2 to 18, more preferably 2 to 15, and even more preferably 2 to 10.

[0133] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include phenyl group, xylyl group, trimethylphenyl group, dipropylphenyl group, di(2,2-dimethylpropyl)phenyl group, naphthyl group, benzyl group, phenylethyl group, and phenylbutyl group. The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 18, more preferably 6 to 15, and even more preferably 6 to 12.

[0134] R ea1 , R ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon group represented by may have substituents such as halogen atoms, cyano groups, and nitro groups. The halogen atom is preferably a fluorine atom, a bromine atom, a chlorine atom, or an iodine atom.

[0135] The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-, and adjacent -CH2- will not be substituted with the same type of group at the same time, nor will terminal -CH2- be substituted.

[0136] n represents an integer from 0 to 4, preferably an integer from 0 to 3, more preferably an integer from 0 to 2, even more preferably an integer of 0 or 1, and even more preferably 0.

[0137] *-OCO-R ea4 The bond position of the group (* represents the bond with the phenyl group) is *-OCO-R ea4 The group may be attached to the 2nd, 3rd, or 4th position of the phenyl group, but is preferably at the 3rd or 4th position, and more preferably at the 4th position.

[0138] R ea1The branched hydrocarbon group having 3 to 20 carbon atoms represented by is preferably a branched saturated hydrocarbon group having 3 to 20 carbon atoms, more preferably a branched alkyl group having 3 to 20 carbon atoms, even more preferably a branched alkyl group having 3 to 10 carbon atoms, and preferably one or more selected from the group consisting of 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, and 3-ethylheptyl group.

[0139] R ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon group having 1 to 20 carbon atoms represented by is preferably a saturated hydrocarbon group having 1 to 20 carbon atoms, an unsaturated hydrocarbon group having 2 to 20 carbon atoms, more preferably a saturated hydrocarbon group having 1 to 20 carbon atoms, even more preferably a chain-like saturated hydrocarbon group having 1 to 10 carbon atoms, and even more preferably a chain-like alkyl group having 1 to 8 carbon atoms. ea2 A chain-like alkyl group having 1 to 8 carbon atoms is preferred, and a chain-like alkyl group having 1 to 6 carbon atoms is more preferred. ea3 A chain-like alkyl group having 1 to 8 carbon atoms is preferred, and a chain-like alkyl group having 1 to 3 carbon atoms is more preferred. ea4 A chain-like alkyl group having 1 to 8 carbon atoms is preferred, and a chain-like alkyl group having 1 to 3 carbon atoms is more preferred. ea5 The alkyl group is preferably a chain-like or branched alkyl group having 1 to 8 carbon atoms, and more preferably a chain-like or branched alkyl group having 1 to 6 carbon atoms.

[0140] Furthermore, the polymerization initiator (E) preferably contains a compound represented by formula (EB).

[0141] [In the formula, R eb1 R represents a branched hydrocarbon group having 3 to 20 carbon atoms, which may have substituents. eb2 ~R eb4Each of these independently represents a hydrocarbon group having 1 to 20 carbon atoms, which may have substituents. m represents an integer from 0 to 4. The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-.

[0142] R eb1 Examples of branched hydrocarbon groups having 3 to 20 carbon atoms, represented by , include branched saturated hydrocarbon groups having 3 to 20 carbon atoms and branched unsaturated hydrocarbon groups having 3 to 20 carbon atoms.

[0143] R eb1 As a branched saturated hydrocarbon group having 3 to 20 carbon atoms, R ea1 Examples of branched saturated hydrocarbon groups having 3 to 20 carbon atoms, as represented by R, are similar to those exemplified above. eb1 The branched alkyl group represented by may be a primary branched alkyl group, a secondary branched alkyl group, or a tertiary branched alkyl group. eb1 The number of carbon atoms in the branched saturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, preferably 16 or less, more preferably 12 or less, and even more preferably 10 or less (i.e., 4 to 16, 4 to 12, or 5 to 10 are preferred).

[0144] R eb1 The branched unsaturated hydrocarbon group represented by the above-mentioned R is eb1 Examples include groups in which at least one carbon-carbon single bond in a branched saturated hydrocarbon group represented by is replaced by a carbon-carbon double bond or a carbon-carbon triple bond. eb1 Examples of branched unsaturated hydrocarbon groups represented by include alkenyl groups such as isopropenyl, isobutenyl, isopentenyl, isohexenyl, isoheptenyl, isooctenyl, isononyl, and isodecenyl groups; alkynyl groups such as isopropynyl, isobutynyl, isopentinyl, isohexynyl, isoheptynyl, isooctynyl, isononinyl, and isodesynyl groups; and so on. eb1The number of carbon atoms in the branched unsaturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, preferably 16 or less, more preferably 12 or less, and even more preferably 10 or less (i.e., 4 to 16, 4 to 12, or 5 to 10 are preferred).

[0145] R eb2 , R eb3 and R eb4 Examples of hydrocarbon groups having 1 to 20 carbon atoms represented by include saturated hydrocarbon groups having 1 to 20 carbon atoms, unsaturated hydrocarbon groups having 2 to 20 carbon atoms, and aromatic hydrocarbon groups having 6 to 20 carbon atoms. eb2 , R eb3 and R eb4 The hydrocarbon groups represented by may be the same or different.

[0146] Examples of the saturated hydrocarbon groups having 1 to 20 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, hexadecyl, and eicosyl groups; branched alkyl groups such as isopropyl, isobutyl, isopentyl, neopentyl, and 2-ethylhexyl groups; and alicyclic saturated hydrocarbon groups having 3 to 20 carbon atoms such as cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and tricyclodecyl groups. The number of carbon atoms in the saturated hydrocarbon group is preferably 1 to 18, more preferably 1 to 15, even more preferably 1 to 10, and even more preferably 1 to 8.

[0147] Examples of the carbon-2 to carbon-20 unsaturated hydrocarbon groups include alkenyl groups such as vinyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, dodecenyl, hexadecenyl, octadecenyl, and eicosenyl groups; alkynyl groups such as ethynyl, propynyl, hexynyl, desinyl, and eicosinyl groups; and cycloalkenyl groups such as cyclopentenyl, cyclohexenyl, and cycloheptenyl groups. The carbon number of the unsaturated hydrocarbon group is preferably 2 to 18, more preferably 2 to 15, and even more preferably 2 to 10.

[0148] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include phenyl group, xylyl group, trimethylphenyl group, dipropylphenyl group, di(2,2-dimethylpropyl)phenyl group, naphthyl group, benzyl group, phenylethyl group, and phenylbutyl group. The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 18, more preferably 6 to 15, and even more preferably 6 to 12.

[0149] R eb1 , R eb2 , R eb3 and R eb4 The hydrocarbon group represented by may have substituents such as halogen atoms, cyano groups, and nitro groups. The halogen atom is preferably a fluorine atom, a bromine atom, a chlorine atom, or an iodine atom, and more preferably a fluorine atom.

[0150] The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-, and in particular may be replaced with -O-, and adjacent -CH2- will not be simultaneously replaced with the same type of group, and terminal -CH2- will not be replaced.

[0151] m represents an integer from 0 to 4, preferably an integer from 1 to 3, more preferably an integer from 2 to 3, and even more preferably 3.

[0152] If m is 1 or greater, *-R eb4 At least one of the 2nd, 4th, and 6th positions of the phenyl group to which it is attached contains *-R eb4 (* represents a bond with a phenyl group) It is preferable that *-R is bonded, eb4 *-R is attached to at least two positions (2, 4, and 6) of the phenyl group to which it is bonded. eb4 It is more preferable that *-R is bonded. eb4 *-R is attached to all of the phenyl groups at positions 2, 4, and 6. eb4 It is even more preferable that they are bonded together.

[0153] R eb1The branched hydrocarbon group having 3 to 20 carbon atoms represented by is preferably a branched saturated hydrocarbon group having 3 to 20 carbon atoms, more preferably a branched alkyl group having 3 to 20 carbon atoms, even more preferably a branched alkyl group having 3 to 10 carbon atoms, and more preferably one or more selected from the group consisting of 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, and 3-ethylheptyl group.

[0154] R eb2 The hydrocarbon group having 1 to 20 carbon atoms represented by is preferably an aromatic hydrocarbon group having 6 to 20 carbon atoms, more preferably an aromatic hydrocarbon group having 6 to 17 carbon atoms, even more preferably an aromatic hydrocarbon group having 7 to 15 carbon atoms, and particularly preferably an aromatic hydrocarbon group having 8 to 13 carbon atoms. In any of these preferred embodiments, it is preferable to have a structure in which 1 to 8 (particularly 1 to 5) fluorine atoms as substituents, and 1 to 2 -CH2- are replaced by -O-.

[0155] R eb2 The preferred embodiment of the aromatic hydrocarbon group having 8 to 13 carbon atoms is preferably one of the following (eb2-1) to (eb2-6).

[0156]

[0157] R eb3 and R eb4 The hydrocarbon groups having 1 to 20 carbon atoms represented by the formula are, independently, preferably saturated hydrocarbon groups having 1 to 20 carbon atoms, unsaturated hydrocarbon groups having 2 to 20 carbon atoms, more preferably saturated hydrocarbon groups having 1 to 20 carbon atoms, even more preferably linear saturated hydrocarbon groups having 1 to 10 carbon atoms, even more preferably linear alkyl groups having 1 to 8 carbon atoms, and particularly preferably linear alkyl groups having 1 to 3 carbon atoms.

[0158] In formula (EB), if the -CH2- contained in the hydrocarbon group is replaced with -O-, -S-, -CO-, or -OCO-, the number of carbon atoms in the replaced portion shall be counted as the number of carbon atoms of the -CH2- before the replacement.

[0159] Furthermore, the polymerization initiator (E) preferably contains a compound represented by formula (EC).

[0160] [In the formula, R ec1 and R ec2 Each of them is independent of R ec11 , OR ec11 COR ec11 , SR ec11 CONR ec12 R ec13 Or it represents CN. R ec11 , R ec12 and R ec13 Each of these independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ec11 , R ec12 or R ec13 The hydrogen atom of the group represented by OR ec21 COR ec21 , SR ec21 , NR ec22 R ec23 CONR ec22 R ec23 , -NR ec22 -OR ec23 , -N(COR ec22 )-OCOR ec23 , -C(=N-OR ec21 )-R ec22 , -C(=N-OCOR ec21 )-R ec22 , CN, halogen atom, or COOR ec21 It may be replaced with R. ec21 , R ec22 and R ec23 Each of these independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ec21 , R ec22or R ec23 The hydrogen atoms of the group represented by may be substituted with CN, halogen atoms, hydroxyl groups, or carboxyl groups. ec11 , R ec12 , R ec13 , R ec21 , R ec22 or R ec23 When the group represented has an alkylene portion, the alkylene portion is -O-, -S-, -COO-, -OCO-, -NR ec24 -, -NR ec24 CO-, -NR ec24 COO-,-OCONR ec24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS-, or -CSO-. ec24 R represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ec11 , R ec12 , R ec13 , R ec21 , R ec22 or R ec23 When the group represented by has an alkyl moiety, the alkyl moiety may be branched, cyclic, or R ec12 and R ec13 and R ec22 and R ec23 They may each form a ring together. ec4 is a hydroxyl group, a carboxyl group, or the following formula (2-2)

[0161]

[0162] (In formula (2-2), L ec11 * represents *-O- or *-OCO-, where * is L ec12 This represents a bonding with L ec12 R represents an alkylene group having 1 to 20 carbon atoms, and the alkylene group may be interrupted by 1 to 3 -O- atoms. ec44a is OR ec55 or COOR ec55 Represents R ec55 ) represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0163] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and R ec24 Examples of alkyl groups having 1 to 20 carbon atoms represented by include methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, sec-butyl group, tert-butyl group, pentyl group, isopentyl group, tert-pentyl group, hexyl group, heptyl group, octyl group, isooctyl group, 2-ethylhexyl group, tert-octyl group, nonyl group, isononyl group, decyl group, isodecyl group, undecyl group, dodecyl group, tetradecyl group, hexadecyl group, octadecyl group, eicosyl group, cyclopentyl group, cyclohexyl group, cyclohexylmethyl group, cyclohexylethyl group, and the like.

[0164] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and R ec24 Examples of aryl groups having 6 to 30 carbon atoms represented by the formula include phenyl, tolyl, xylyl, ethylphenyl, naphthyl, anthryl, phenanthryl, phenyl, biphenylyl, naphthyl, and anthryl groups substituted with one or more of the above alkyl groups.

[0165] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and R ec24 Examples of aralkyl groups having 7 to 30 carbon atoms, represented by the formula, include benzyl group, α-methylbenzyl group, α,α-dimethylbenzyl group, and phenylethyl group.

[0166] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23and R ec24 Examples of heterocyclic groups having 2 to 20 carbon atoms represented by include pyridyl group, pyrimidyl group, furyl group, thienyl group, tetrahydrofuryl group, dioxolanyl group, benzoxazole-2-yl group, tetrahydropyranyl group, pyrrolidyl group, imidazolidyl group, pyrazolidyl group, thiazolidyl group, isothiazolidyl group, oxazolidyl group, isoxazolidyl group, piperidyl group, piperadyl group, morpholinyl group, and the like, and are preferably 5 to 7 membered heterocyclic groups.

[0167] R in equation (EC) ec12 and R ec13 and R ec22 and R ec23 The statement that they may each form a ring together means that R ec12 and R ec13 and R ec22 and R ec23 This means that each atom may form a ring with the nitrogen, carbon, or oxygen atoms it connects to.

[0168] R in equation (EC) ec12 and R ec13 and R ec22 and R ec23 Examples of rings that can be formed by these rings together include cyclopentane rings, cyclohexane rings, cyclopentene rings, benzene rings, piperidine rings, morpholine rings, lactone rings, lactam rings, and the like, and are preferably 5 to 7 membered rings.

[0169] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 and R ec23 Examples of halogen atoms that may be present as substituents include fluorine, chlorine, bromine, and iodine atoms.

[0170] R in equation (EC) ec1 Preferably R ec11 The alkyl group is more preferably a C1 to C20 alkyl group, even more preferably a C1 to C10 alkyl group, and still more preferably a C1 to C6 alkyl group.

[0171] R ec4 Preferably, the group is represented by formula (2-2). In this case, it is advantageous in terms of the solubility of the oxime compound in solvent (J) and the developability of the curable composition.

[0172] L ec12 The number of carbon atoms in the alkylene group represented by is preferably 1 to 10, and more preferably 1 to 4.

[0173] R ec44a This is preferably a hydroxyl group or a carboxyl group, and more preferably a hydroxyl group.

[0174] Furthermore, the polymerization initiator (E) preferably contains a compound represented by formula (ED). [In the formula, R ed1 This represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or CN, and the hydrogen atoms of the alkyl group, aryl group, and arylalkyl group are further OR ed21 COR ed21 , SR ed21 , NR ed22 R ed23 ,-NCOR ed22 -OCOR ed23 CN, halogen atom, -CR ed21 =CR ed22 R ed23 or -CO-CR ed21 =CR ed22 R ed23 It may be replaced with R ed21 , R ed22 and R ed23 Each of these independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ed2 R ed11 OR ed11 Represents R ed11 R represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms, and the hydrogen atoms of the alkyl group, aryl group, and arylalkyl group may be further substituted with halogen atoms.ed3 R represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms. ed1 , R ed3 , R ed21 , R ed22 and R ed23 The methylene group in the alkyl group represented by may be interrupted 1 to 5 times by unsaturated bonds, ether bonds, thioether bonds, ester bonds, thioester bonds, amide bonds, or urethane bonds. ed3 It may form a ring together with an adjacent benzene ring. ed4 and R ed5 Each of them independently, R ed11 , OR ed11 [This represents a CN or halogen atom. a and b are each independently between 0 and 3.]

[0175] In the above formula (ED), R ed1 , R ed11 , R ed21 , R ed22 , R ed23 , R ed3 Examples of alkyl groups represented by include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, s-butyl, t-butyl, pentyl, 1-methylbutyl, hexyl, heptyl, octyl, isooctyl, 2-ethylhexyl, t-octyl, nonyl, isononyl, decyl, isodecyl, undecyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, cyclopentyl, cyclohexyl, cyclohexylmethyl, vinyl, allyl, butenyl, ethinyl, propynyl, methoxyethyl, ethoxyethyl, propoxyethyl, pentyloxyethyl, octyloxyethyl, methoxyethoxyethyl, ethoxyethoxyethyl, propoxyethoxyethyl, methoxypropyl, 2-methoxy-1-methylethyl, and the like. The number of carbon atoms in the alkyl group is preferably 1 to 15, more preferably 1 to 10, even more preferably 1 to 8, and even more preferably 1 to 6. In particular, the alkyl group is preferably methyl, ethyl, propyl, or 1-methylbutyl.

[0176] Red1 , R ed11 , R ed21 , R ed22 , R ed23 , R ed3 Examples of aryl groups represented by include phenyl, tolyl, xylyl, ethylphenyl, chlorophenyl, naphthyl, anthuryl, phenanthrenyl, and phenyl, biphenylyl, naphthyl, and anthuryl groups substituted with one or more of the above alkyl groups. The number of carbon atoms in the aryl group is preferably 6 to 20, more preferably 6 to 15, even more preferably 6 to 12, and even more preferably 6 to 10. Among these, tolyl is preferred, o-tolyl and m-tolyl are more preferred, and o-tolyl is even more preferred.

[0177] R ed1 , R ed11 , R ed21 , R ed22 , R ed23 , R ed3 Examples of arylalkyl groups represented by include benzyl, chlorobenzyl, α-methylbenzyl, α,α-dimethylbenzyl, phenylethyl, and phenylethenyl. The number of carbon atoms in the arylalkyl group is preferably 7 to 20, more preferably 7 to 15, and even more preferably 7 to 12.

[0178] R ed21 , R ed22 and R ed23 Examples of heterocyclic groups represented by include, for example, 5- to 7-membered heterocycles such as pyridyl, pyrimidyl, furyl, thienyl, tetrahydrofuryl, dioxolanil, benzoxazole-2-yl, tetrahydropyranil, pyrrolidyl, imidazolidyl, pyrazolidyl, thiazolidyl, isothiazolidyl, oxazolidyl, isoxazolidyl, piperidyl, piperadyl, and morpholinil. The number of carbon atoms in the heterocyclic group is preferably 2 to 15, more preferably 3 to 12, and even more preferably 3 to 9.

[0179] Together with the adjacent benzene ring, R ed3Examples of rings formed by the nitrogen atom to which it is bonded include 5- to 7-membered rings such as cyclopentane rings, cyclohexane rings, cyclopentene rings, benzene rings, piperidine rings, morpholine rings, lactone rings, and lactam rings.

[0180] R ed1 , R ed11 , R ed21 , R ed22 and R ed23 Halogen atoms and R that may be substituted ed4 , R ed5 Examples of halogen atoms represented by this formula include fluorine, chlorine, bromine, and iodine.

[0181] The methylene group contained in the alkyl group described above may be interrupted one to five times by unsaturated bonds, ether bonds, thioether bonds, ester bonds, thioester bonds, amide bonds, or urethane bonds. In this case, the interrupting group may be one or two or more types of groups, and if the group can be interrupted consecutively, it may be interrupted two or more times consecutively. Furthermore, the alkyl group may have branched side chains, may be a cyclic alkyl group, and the alkyl group terminus may be an unsaturated bond. Among these, it is preferable that the methylene group is interrupted by an ether bond.

[0182] Examples of alkyl groups interrupted by ether bonds include the following:

[0183]

[0184] In particular, in the above formula (ED), R ed1 This represents an aryl group with 6 to 20 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 Replaced with R ed21 R represents an alkyl group having 1 to 15 carbon atoms. ed21 The methylene group in the alkyl group is interrupted 1 to 5 times by ether bonds, R ed2 However, R ed11 Represents R ed11 However, R represents an alkyl group with 1 to 15 carbon atoms. ed3 However, it is preferable that it represents an alkyl group having 1 to 15 carbon atoms, and that a and b are 0.

[0185] Red1 This represents an aryl group with 6 to 15 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 Replaced with R ed21 R represents an alkyl group having 1 to 10 carbon atoms. ed21 The methylene group in the alkyl group is interrupted 1 to 3 times by ether bonds, R ed2 However, R ed11 Represents R ed11 However, R represents an alkyl group with 1 to 10 carbon atoms. ed3 However, it is more preferable that the alkyl group has 1 to 10 carbon atoms, and that a and b are 0.

[0186] R ed1 This represents an aryl group with 6 to 12 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 Replaced with R ed21 R represents an alkyl group having 1 to 8 carbon atoms. ed21 The methylene group in the alkyl group is interrupted once or twice by an ether bond, R ed2 However, R ed11 Represents R ed11 However, R represents an alkyl group with 1 to 8 carbon atoms. ed3 However, it is more preferable that it represents an alkyl group having 1 to 8 carbon atoms, and that a and b are 0.

[0187] R ed1 This represents an aryl group with 6 to 10 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 Replaced with R ed21 R represents an alkyl group having 1 to 6 carbon atoms. ed21 The methylene group in the alkyl group is interrupted once by an ether bond, R ed2 However, R ed11 Represents R ed11 However, it represents an alkyl group with 1 to 3 carbon atoms, R ed3 However, it is even more preferable that it represents an alkyl group having 1 to 3 carbon atoms, and that a and b are 0.

[0188] The polymerization initiator (E) preferably contains at least one compound represented by formulas (EA) to (ED), more preferably contains a compound represented by formula (EA) or formula (ED) from the viewpoint of the appearance of the cured film, and even more preferably contains a compound represented by formula (EA).

[0189] Examples of oxime compounds include acetophenone O-benzoyl oxime, N-benzoyloxy-1-(4-phenylsulfanylphenyl)butan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)-3-cyclopentylpropane-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethane-1-imine, and N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2,4-dioxacyclopentanylmethyl Examples include compounds described in Japanese Patent Publication No. 2011-132215, International Publication Nos. 2008 / 78678, 2008 / 78686, 2012 / 132558, 2017 / 051680, and 2020 / 004601. Commercially available products such as Irgacure OXE01 (N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine), OXE02 (N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethane-1-imine), OXE03, OXE05 (all manufactured by BASF), N-1919, NCI-930, NCI-831 (all manufactured by ADEKA) may also be used.

[0190] Other polymerization initiators (E) include photopolymerization initiators such as alkylphenone compounds, biimidazole compounds, and triazine compounds, and thermal polymerization initiators such as azo compounds and organic peroxides.

[0191] The content of the polymerization initiator (E) in the curable composition is preferably 0.1 parts by mass or more and 80 parts by mass or less, more preferably 0.1 parts by mass or more and 30 parts by mass or less, per 100 parts by mass of the polymerizable compound (D).

[0192] From the viewpoint of increasing the luminescence intensity of the curable composition and the cured film, the content of the polymerization initiator (E) in the curable composition is, for example, 0.01% by mass or more and 20% by mass or less, preferably 0.1% by mass or more and 15% by mass or less, more preferably 0.2% by mass or more and 10% by mass or less, even more preferably 0.3% by mass or more and 8% by mass or less, even more preferably 0.5% by mass or more and 5% by mass or less, and particularly preferably 3% by mass or less.

[0193] <Antioxidant (Fa)> The curable composition may contain an antioxidant (Fa). The antioxidant (Fa) is not particularly limited as long as it is an antioxidant commonly used in industry, and phenolic antioxidants, phosphorus-based antioxidants, phosphorus / phenol complex antioxidants, and sulfur-based antioxidants can be used, but from the viewpoint of luminescence intensity, phenolic antioxidants and phosphorus / phenol complex antioxidants are preferred, and phosphorus / phenol complex antioxidants are more preferred. The curable composition may contain two or more antioxidants.

[0194] Examples of phosphorus / phenol complex antioxidants include Sumirizer® GP (6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenz[d,f][1.3.2]dioxaphosfepine) (manufactured by Sumitomo Chemical Co., Ltd.). Other antioxidants include, for example, the compounds described in Japanese Patent Application Publication No. 2024-61630.

[0195] The content of the antioxidant (Fa) is, for example, 0.01% by mass or more and 60% by mass or less with respect to the total amount of solids in the curable composition. From the viewpoint of increasing the luminescence intensity and heat resistance of the curable composition and cured film, it is preferably 0.1% by mass or more and 50% by mass or less, more preferably 0.2% by mass or more and 40% by mass or less, and even more preferably 0.5% by mass or more and 30% by mass or less, and may also be 20% by mass or less, 10% by mass or less, 5% by mass or less, or 2% by mass or less.

[0196] <Leveling agent (H)> Examples of leveling agent (H) include silicone-based surfactants, fluorine-based surfactants, and silicone-based surfactants having a fluorine atom. These may have polymerizable groups in their side chains. It is preferable that the leveling agent (H) includes a silicone-based surfactant. The curable composition may contain two or more types of leveling agent (H).

[0197] Examples of silicone-based surfactants include surfactants having siloxane bonds in their molecules. Examples of such surfactants include the compounds described in Japanese Patent Application Publication No. 2024-61630.

[0198] Examples of fluorine-based surfactants include surfactants having fluorocarbon chains in their molecules. Examples of such surfactants include the compounds described in Japanese Patent Application Publication No. 2024-61630.

[0199] When the curable composition contains a leveling agent (H), the content of the leveling agent (H) in the curable composition is, for example, 0.001% by mass or more and 1.0% by mass or less, preferably 0.005% by mass or more and 0.75% by mass or less, and more preferably 0.01% by mass or more and 0.5% by mass or less, relative to the total amount of solids in the curable composition. When the content of the leveling agent (H) is within the above range, the flatness of the cured film when used as a wavelength conversion layer can be improved.

[0200] <Solvent (J)> Solvent (J) is a component other than the solid content, and includes dispersion media for dispersing other components and solvents for dissolving them. The curable composition may contain solvent (J), but a low content is preferable. The content of solvent (J) is preferably 0 to 10% by mass, more preferably 0 to 5% by mass, and even more preferably 0 to 2% by mass, based on 100% by mass of the total amount of the curable composition. Examples of solvents are described in Japanese Patent Application Publication No. 2024-61630.

[0201] <Resin (C)> The curable composition may contain resin (C), but a low content is preferable. The resin (C) content is preferably 0 to 10% by mass, more preferably 0.5 to 5% by mass, even more preferably 0.5 to 3% by mass, even more preferably 0.5 to 2% by mass, and most preferably 0.5 to 1% by mass, based on 100% by mass of the total solid content of the curable composition. By reducing the resin (C) content, the viscosity of the curable composition can be reduced, which in turn can improve the ejectability, particularly the ejectability when ejected from the ejection head of an inkjet printer.

[0202] As resin (C), resins such as those described in Japanese Patent Publication No. 2024-61630 can be used.

[0203] <Other components> The curable composition may further contain additives known in the art, such as polymerization inhibitors, fillers, other polymer compounds, adhesion promoters, and chain transfer agents, as needed.

[0204] <<Cured Film>> This disclosure includes cured films formed from curable compositions. A cured film containing semiconductor particles (A) can emit light of a different wavelength from the irradiated light when irradiated with ultraviolet or visible light. Therefore, a cured film containing semiconductor particles (A) can be used as a wavelength conversion film.

[0205] The thickness of the cured film is, for example, 0.5 μm or more and 40 μm or less, preferably 1 μm or more and 30 μm or less, more preferably 5 μm or more and 25 μm or less, even more preferably 6 μm or more and 20 μm or less, and may also be 7 μm or more and 15 μm or less, or 8 μm or more and 12 μm or less.

[0206] <<Method for Manufacturing Curable Compositions>> Curable compositions can be manufactured by a method that includes mixing predetermined components and other components used as needed. Among the components contained in the curable composition, semiconductor particles (A) and light scattering agents (B) may be mixed with some or all of the solvent (J) beforehand before being mixed with the other components.

[0207] <<Viscosity of the Curable Composition>> The viscosity of the curable composition (especially the curable composition immediately after preparation) at 50°C is preferably 23 cP or less, more preferably 21 cP or less, and even more preferably 19 cP or less. The lower limit is not particularly limited, but may be 1 cP or more, 2 cP or more, or 3 cP or more. By setting the viscosity of the curable composition within the above range, the curable composition can be stably and continuously ejected from the ejection head of an inkjet printer, making it suitable for use as an inkjet printer ink. The viscosity of the curable composition can be measured using a Brookfield rotational viscometer (manufactured by Brookfield).

[0208] <<Method for Manufacturing a Cured Film>> A cured film can be obtained by curing a film (layer) made of a curable composition. Specifically, a curable composition is applied to a substrate to form a coating film, the obtained coating film is exposed to light, and a cured film can be obtained by further thermal curing (post-bake) after exposure. Thermal curing allows for further polymerization of the polymerizable compound (D).

[0209] The curable composition of this disclosure uses semiconductor particles (A) that satisfy a predetermined weight loss ratio of 300°C or higher and a polymerizable compound (D) that satisfies a predetermined polar surface area, thereby enabling a good appearance of the cured film. Furthermore, the decrease in the luminescence intensity of the cured film after exposure and heat curing compared to the luminescence intensity of the cured film after exposure but before heat curing can be suppressed. The process resistance evaluated in the examples described later is, for example, 50 to 95%, preferably 60 to 90%, more preferably 65 to 90%, even more preferably 70 to 90%, and even more preferably 75 to 90%.

[0210] As substrates, glass plates such as quartz glass, borosilicate glass, aluminasilate glass, and soda-lime glass with a silica coating on the surface can be used; resin plates such as polycarbonate, polymethyl methacrylate, and polyethylene terephthalate; silicon; and substrates on which aluminum, silver, or silver / copper / palladium alloy thin films have been formed. Preferred substrates are glass plates and silicon substrates.

[0211] For applying the curable composition, various printing methods such as gravure printing, offset printing, letterpress printing, screen printing, transfer printing, electrostatic printing, and plateless printing, as well as coating methods such as gravure coating, roll coating, knife coating, air knife coating, bar coating, dip coating, kiss coating, spray coating, die coating, comma coating, inkjet, spin coating, and slit coating, or combinations thereof, can be used as appropriate.

[0212] For exposure, a light source that generates light with a wavelength of 250 nm to 450 nm is preferred. Light below 350 nm may be filtered out using a filter that cuts out this wavelength range, or light around 436 nm, 408 nm, 395 nm, and 365 nm may be selectively extracted using a bandpass filter that extracts these wavelength ranges. Examples of light sources include mercury lamps, light-emitting diodes, metal halide lamps, and halogen lamps. Exposure is preferably carried out in an inert gas atmosphere (nitrogen, argon, etc.). The exposure amount in the exposure process is preferably 50 to 1000 mJ / cm². 2 More preferably, 80 to 800 mJ / cm² 2 And more preferably 100 to 700 mJ / cm² 2 And more preferably 150 to 700 mJ / cm² 2 The exposure amount in the exposure process is 1000 mJ / cm². 2The following conditions prevent excessive shrinkage of the cured film, thereby preventing the semiconductor particles (A) from coming into close proximity within the film due to shrinkage and preventing a decrease in emitted light intensity. The exposure amount is the exposure amount based on a wavelength of 365 nm and can be measured using an ultraviolet integrated light meter (UIT-250, manufactured by Ushio Inc.).

[0213] The temperature of the thermosetting process after exposure is preferably 100°C to 250°C, and more preferably 150°C to 200°C. The heating time is preferably 1 minute to 120 minutes, and more preferably 10 minutes to 60 minutes.

[0214] Furthermore, the thermosetting process may be carried out in either an air atmosphere or an inert atmosphere.

[0215] Furthermore, it is preferable to form the patterned cured film from the curable composition by patterning using an inkjet method.

[0216] One method for manufacturing a cured film patterned by an inkjet method is to form banks on a substrate, selectively deposit a curable composition into the areas partitioned by the banks on the substrate using an inkjet method, and then cure the curable composition by exposure and thermal curing. As the substrate, the substrates exemplified in the description of the method for manufacturing the cured film can be used.

[0217] Inkjet methods include the bubble jet (registered trademark) method, which uses an electrothermal converter as an energy generating element, and the piezo jet method, which uses a piezoelectric element.

[0218] As the light source used for exposure, the light source exemplified in the description of the method for manufacturing the cured film described above can be used.

[0219] For the thermal curing conditions after exposure, please refer to the description of the manufacturing method for the cured film above.

[0220] The patterned cured film can be suitably used as a wavelength conversion film (wavelength conversion filter) that emits light of a different wavelength than the light incident from light-emitting parts such as LEDs. In particular, it is preferable that the patterned cured film be positioned above light-emitting elements such as LEDs corresponding to each pattern. By individually converting the wavelength of each light-emitting element, the shape of the emission spectrum of red, green, blue, etc. can be appropriately controlled, and high color reproducibility can be achieved. Display members having a wavelength conversion film can be suitably used in display devices such as liquid crystal displays and organic EL displays.

[0221] A display member formed by an inkjet method according to one embodiment has banks formed on a substrate and light-emitting elements such as LEDs placed between the banks. The curable composition of this disclosure is deposited on the light-emitting elements between the banks by an inkjet method, and then cured to obtain a cured film (wavelength conversion film) (hereinafter, each cured film patterned to the size of the area between the banks is also referred to as a "cured film pixel"). A color filter or a gas barrier layer may be placed on each cured film pixel.

[0222] By forming cured film pixels using an inkjet method, it becomes possible to pattern relatively large sizes, making it suitable for large displays such as digital signage.

[0223] When employing the inkjet method, the vertical dimension (L1) of the cured film pixel formed from the curable composition of this disclosure is preferably 9 to 40 μm, more preferably 12 to 30 μm, and even more preferably 15 to 30 μm or more. The vertical dimension (L1) may be the same length as the horizontal dimension (L3) of the light-emitting element.

[0224] Furthermore, when employing the inkjet method, the horizontal dimension (L2) of the cured film pixels formed from the curable composition of this disclosure is preferably 10 to 900 μm, more preferably 30 to 800 μm, even more preferably 50 to 700 μm, still more preferably 80 to 700 μm, and particularly preferably 100 to 700 μm.

[0225] The vertical dimension (L1) of the cured film pixel refers to the dimension in the substrate thickness direction of a cross-section cut perpendicular to the substrate. This cross-section is cut at the location where the vertical dimension of the cured film pixel is maximum. The horizontal dimension (L2) of the cured film pixel refers to the maximum dimension of the cured film pixel in a direction horizontal to the substrate, and refers to the dimension when the substrate is viewed from the vertical (plan view dimension). The horizontal dimension (L3) of the light-emitting element refers to the maximum dimension of the light-emitting element in a direction horizontal to the substrate, and refers to the dimension when the substrate is viewed from the vertical (plan view dimension).

[0226] <<Display Devices>> Because the cured film has the function of converting the wavelength of irradiated light, it can be used as a color conversion layer (wavelength conversion film) for display devices. Examples of such display devices include those described in Japanese Patent Publication No. 2006-309219, Japanese Patent Publication No. 2006-310303, Japanese Patent Publication No. 2013-15812, Japanese Patent Publication No. 2009-251129, Japanese Patent Publication No. 2014-2363, etc. The cured film according to this disclosure is useful as a color conversion layer (wavelength conversion film) for display devices, particularly for liquid crystal display devices, organic EL display devices, or inorganic EL display devices.

[0227] This application claims the benefit of priority based on Japanese Patent Application No. 2025-078616, filed on 9 May 2025. The entire specification of Japanese Patent Application No. 2025-078616, filed on 9 May 2025, is incorporated herein by reference.

[0228] The present disclosure will be described in more detail below with reference to examples. The present disclosure is not limited by the following examples, and it is certainly possible to implement it with appropriate modifications to the extent that it is in line with the spirit described above and below, and such modifications will all be included within the technical scope of the present disclosure.

[0229] The present disclosure will be further described below with reference to examples. Unless otherwise specified, "%" and "parts" in the examples refer to mass percent and parts by mass.

[0230] (1) Measurement of weight loss ratio above 300°C and composition ratio of organic ligand of semiconductor particles containing organic ligand (G) The weight loss ratio above 300°C of semiconductor particles (A) containing organic ligand (G) was measured under the following conditions. 0.1 g of semiconductor particles (A) containing organic ligand (G) was redispersed in 1 mL of toluene, 9 mL of poor solvent was added to precipitate, and then the mixture was centrifuged at 4000 G for 20 minutes. The precipitated semiconductor particles (A) containing organic ligand (G) was redispersed in 0.5 mL of toluene. The resulting dispersion was dried at 110°C for 10 minutes to prepare a dry powder. Using thermogravimetric analysis (Bruker TG-DTA2000SA), the powder was heated from 25°C to 600°C at a heating rate of 10°C / min under a nitrogen atmosphere. Here, using the TG graph obtained by thermogravimetric analysis, the weight loss rate from 100°C to 300°C and from 300°C to 600°C were calculated, with the 100°C value (weight) as the baseline. The ratio of the weight loss rate from 300°C to 600°C to the sum of these was defined as the weight loss rate above 300°C (%). In other words, the weight loss rate above 300°C (%), calculated using equation (1), was measured when semiconductor particles (A) containing each organic ligand (G) were heated from 25°C to 600°C under a nitrogen atmosphere at a heating rate of 10°C / min using thermogravimetric analysis. Note that the weight loss rate above 300°C (%) refers to a simple ratio. Weight loss rate above 300°C X (%) = {T1 / (T 0+ T1)}×100...(1) [In formula (1), T 0 This is the weight loss rate from 100°C to 300°C, with the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C as the reference weight, and T 1This is the weight loss rate from 300°C to 600°C, with the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C as the baseline. Furthermore, when comparing the TG graph of the thermogravimetric analysis for the purified semiconductor particle (A) containing the organic ligand (G) of Preparation Example 1 with the TG graphs of the purified semiconductor particle (A) containing the organic ligand (G) of Preparation Examples 2 to 4, a mass loss behavior in the temperature range of 100°C to 300°C was observed only in the TG graph of the semiconductor particle (A) containing the organic ligand (G) of Preparation Examples 2 to 4. This mass loss behavior in the 100°C to 300°C range is presumed to be due to the hydrophilic organic ligand coordinated by ligand exchange. Therefore, the composition ratio of each organic ligand was calculated, with the ratio T0 / (T0+T1) being the composition ratio of the hydrophilic organic ligand and the ratio T1 / (T0+T1) being the composition ratio of the hydrophobic organic ligand. Note that the composition ratios of each organic ligand represent simple proportions.

[0231] (2) Polar surface area of ​​polymerizable compound (D) The polar surface area of ​​polymerizable compound (D) was determined using Chem3D (Chem3D version 22.2, manufactured by Cambridge Soft).

[0232] (3) Appearance evaluation of the cured film A composition layer was formed on a 5 cm square glass substrate (Corning's "Eagle XG") by spin coating, with curable compositions 1 to 8 described below applied so that the thickness of the post-baked layer was 5 μm. The substrate on which this composition layer was formed was then exposed using an exposure machine (Topcon Corporation's "TME-150RSK"), and N 2 Under atmospheric conditions, 200 mJ / cm² 2 A cured film was formed by irradiating with light at an exposure level of 365 nm (based on 365 nm) and performing post-bake at 180°C for 10 minutes. The surface of the cured film was visually observed and evaluated according to the following criteria: A: No haze B: Haze present C: Foreign matter present

[0233] (4) Measurement of process resistance A surface-emitting backlight (OPSM series: manufactured by Optex FA Co., Ltd.) equipped with an LED lamp and diffuser plate with an emission peak wavelength of 450 nm was prepared as the backlight. The backlight was installed with the diffuser plate facing upwards, and a spectroradiometer (SR-UL1R: manufactured by Topcon Techno House Co., Ltd.) was placed at a height of 60 cm from the surface of the diffuser plate. A glass substrate (Eagle 2000: manufactured by Corning Corporation) was placed on the surface of the diffuser plate of the backlight as a reference. With the backlight turned on in this state, the integrated spectral irradiance value in the wavelength range of the backlight from 380 nm to 480 nm was measured through the reference glass substrate at 3.15 W·sr -1 ・m -2 The backlight intensity was adjusted to achieve the following. Next, the reference glass substrate was removed, and the cured film after exposure and the cured film after post-baking, which were formed on a glass substrate prepared using the same procedure as in (3) above, were placed on the surface of the backlight diffuser plate as measurement samples. With the backlight turned on in this state, the light emitted from the cured films after exposure and after heat curing (post-baking) was measured as the integrated spectral irradiance in the wavelength range of 480 nm to 780 nm, and the luminous intensity (unit: mW・sr -1 ・m -2 The following measurements were taken. The process resistance was determined according to the following formula, with EIa being the luminescence intensity of the heat-cured film formed on the glass substrate and EIb being the luminescence intensity of the exposure-cured film formed on the glass substrate: Process resistance (%) = [EIa / EIb] × 100

[0234] (5) Measurement of the viscosity of the curable composition The viscosity of the curable composition immediately after preparation at 50°C was measured at a constant temperature of 50°C using a Brookfield rotational viscometer (Brookfield). Apparatus: Brookfield Viscometer DV2T LV Spindle: Cone spindle CPA-40Z Rotation speed: 20 rpm

[0235] Preparation Example 1: Preparation of semiconductor particles (A) containing organic ligand (G) (hydrophobic organic ligand (G1)) <Production of core particles> Indium acetate (0.3 mmol) and zinc oleate (0.05 mmol) were added to a mixture of oleic acid (0.9 mmol), 1-dodecanethiol (0.1 mmol), and octadecene (10 mL), and the mixture was heated from room temperature to 120°C at a heating rate of 10°C per minute under vacuum (<20 Pa) and reacted for 1 hour. Next, the mixture reacted under vacuum (<20 Pa) was heated to 25°C under a nitrogen atmosphere, and tris(trimethylsilyl)phosphine (0.15 mmol) was added, followed by heating to 300°C at a heating rate of 10°C per minute and reacting for 10 minutes. Furthermore, the reaction mixture was cooled to 25°C, octanoic acid chloride (0.60 mmol) was injected, and the mixture was heated to 250°C at a rate of 10°C per minute. After reacting for 30 minutes, it was cooled to 25°C to obtain a dispersion solution of core particles.

[0236] <Preparation of Precursor Solution for Shell Formation> 40 mmol of zinc oleate and 75 mL of octadecene were mixed and heated under vacuum at 110°C for 1 hour to prepare a Zn precursor solution with [Zn] = 0.4 M. Separately, 22 mmol of selenium powder and 10 mL of trioctylphosphine were mixed in nitrogen and stirred until completely dissolved to obtain selenide trioctylphosphine with [Se] = 2.2 M. Furthermore, 22 mmol of sulfur powder and 10 mL of trioctylphosphine were mixed in nitrogen and stirred until completely dissolved to obtain sulfide trioctylphosphine with [S] = 2.2 M.

[0237] <Shell Formation> The core particle dispersion solution was heated to 250°C. At 250°C, 4.3 mL of Zn precursor solution and 1.5 mL of selenite trioctylphosphine were added and reacted for 30 minutes to form a ZnSe shell on the surface of the InP-based semiconductor nanoparticles. Furthermore, 3.8 mL of Zn precursor solution and 0.5 mL of sulfide trioctylphosphine were added, the temperature was raised to 280°C, and the reaction was allowed to proceed for 1 hour to form a ZnS shell.

[0238] <Purification of Core-Shell Particles> The reaction solution of the obtained core-shell particles was added to acetone, mixed well, and then centrifuged. The centrifugal acceleration was set to 4000 G. The precipitate was collected, and n-hexane was added to the precipitate to prepare a dispersion. This operation was repeated several times to obtain purified core-shell particles (semiconductor particles (A) containing organic ligand (G) (hydrophobic organic ligand (G1))).

[0239] Preparation Example 2: Preparation of semiconductor particles (A1) containing organic ligands (Ga) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2)) In a flask, semiconductor particles (A) containing organic ligand (G) obtained in Preparation Example 1 were dispersed in 1-octadecene at a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in a flask, and 1.0 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.1 g of zinc acetate were added to prepare the mixture. The mixture was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. Centrifugation at 4000 G for 20 minutes separated the mixture into a clear 1-octadecene phase and a phase containing semiconductor particles (A1) containing organic ligands (Ga). The 1-octadecene phase was removed, and the phase containing semiconductor particles (A1) containing organic ligands (Ga) was recovered.

[0240] 5.0 mL of acetone was added to the obtained phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was collected. This procedure was repeated several times to obtain semiconductor particles (A1) containing purified organic ligands (Ga) ((hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2))). The weight loss ratio above 300°C for the semiconductor particles (A1) containing organic ligand (Ga), as determined by the above measurement method, was 32.0%. The composition ratios of hydrophilic organic ligand (G2) and hydrophobic organic ligand (G1) in the semiconductor particles (A1) containing organic ligand (Ga), as determined by the above measurement method, were 68.0% and 32.0%, respectively.

[0241] Preparation Example 3: Preparation of semiconductor particles (A2) containing organic ligand (Gb) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2)) In a flask, semiconductor particles (A) containing organic ligand (G) obtained in Preparation Example 1 were dispersed in 1-octadecene at a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in a flask, and 1.0 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.1 g of zinc acetate were added to prepare mixture 1. Mixture 1 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating into a clear 1-octadecene phase and a phase containing semiconductor particles (A) containing organic ligand (G). The 1-octadecene phase was removed, and the phase containing semiconductor particles (A) containing organic ligand (G) was recovered.

[0242] Propylene glycol monomethyl ether acetate (hereinafter referred to as "PGMEA") (dispersion medium) was added to the semiconductor particle (A) phase containing the remaining organic ligand (G), and a PGMEA dispersion was prepared so that the semiconductor particle (A) containing the organic ligand (G) was 10% by mass. The prepared PGMEA dispersion was placed in a flask, and 1.0 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.1 g of zinc acetate were added to prepare mixture 2. The mixture 2 was stirred at 110°C for 60 minutes under a nitrogen atmosphere and cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, 50 mL of n-hexane was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes to recover the phase containing the semiconductor particle (A2) containing the organic ligand (Gb).

[0243] To the obtained phase, 5.0 mL of acetone was added to prepare a dispersion. 50 mL of n-hexane was added to the resulting dispersion, followed by centrifugation at 4000 G for 20 minutes. After centrifugation, the transparent supernatant was removed, and the precipitate was collected. This operation was repeated several times to obtain purified semiconductor particles (A2) comprising an organic ligand (Gb) (including a hydrophobic organic ligand (G1) and a hydrophilic organic ligand (G2)). The weight reduction ratio at 300°C or higher of the semiconductor particles (A2) containing the organic ligand (Gb) determined by the above measurement method was 18.3%. The compositional ratios of the hydrophilic organic ligand (G2) and the hydrophobic organic ligand (G1) in the semiconductor particles (A2) containing the organic ligand (Gb) determined by the above measurement method were 81.7% and 18.3%, respectively.

[0244] Preparation Example 4: Preparation of semiconductor particles (A3) comprising organic ligand (Gc) (hydrophobic organic ligand and hydrophilic organic ligand) The semiconductor particles (A) comprising the organic ligand (G) obtained in Preparation Example 1 were dispersed in 1-octadecene to a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in a flask, and 1.2 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.12 g of zinc acetate were added to prepare Mixture 3. The Mixture 3 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, then transferred to a centrifuge tube, and centrifuged at 4000 G for 20 minutes, whereby the mixture separated into a transparent 1-octadecene phase and a phase containing the semiconductor particles (A) containing the organic ligand (G). The 1-octadecene phase was removed, and the phase containing the semiconductor particles (A) containing the organic ligand (G) was collected.

[0245] PGMEA (dispersion medium) was added to the remaining semiconductor particle (A) phase containing the organic ligand (G) to prepare a PGMEA dispersion so that the semiconductor particle (A) containing the organic ligand (G) was 10% by mass. The prepared PGMEA dispersion was placed in a flask, and 1.2 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.12 g of zinc acetate were added to prepare mixture 4. The mixture 4 was stirred at 110°C for 60 minutes under a nitrogen atmosphere and cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, 50 mL of n-hexane was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes to recover the phase containing the semiconductor particle (A3) containing the organic ligand (Gc).

[0246] 5.0 mL of acetone was added to the obtained phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was collected. This procedure was repeated several times to obtain semiconductor particles (A3) containing purified organic ligands (Gc) ((hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2))). The weight loss ratio above 300°C for the semiconductor particles (A3) containing organic ligand (Gc), as determined by the above measurement method, was 13.8%. The composition ratios of hydrophilic organic ligand (G2) and hydrophobic organic ligand (G1) in the semiconductor particles (A3) containing organic ligand (Gc), as determined by the above measurement method, were 86.2% and 13.8%, respectively.

[0247] Preparation Example 5: Preparation of semiconductor particles (A4) containing organic ligand (Gd) (hydrophobic organic ligand and hydrophilic organic ligand) In a flask, the semiconductor particles (A) containing the organic ligand (G) obtained in Preparation Example 1 were dispersed in 1-octadecene to a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in a flask, 1.2 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.12 g of zinc acetate were added to prepare Mixture 5. The Mixture 5 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, then transferred to a centrifuge tube, and centrifuged at 4000 G for 20 minutes, whereby the mixture was separated into a transparent 1-octadecene phase and a phase containing the semiconductor particles (A) containing the organic ligand (G). The 1-octadecene phase was removed, and the phase containing the semiconductor particles (A) containing the organic ligand (G) was recovered.

[0248] PGMEA (dispersion medium) was added to the remaining phase of the semiconductor particles (A) containing the organic ligand (G), to prepare a PGMEA dispersion such that the mass ratio of the semiconductor particles (A) containing the organic ligand (G) was 10% by mass. The prepared PGMEA dispersion was placed in a flask, 1.2 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.12 g of zinc acetate were added to prepare Mixture 6. The Mixture 6 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, and then cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, 50 mL of n-hexane was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes to recover the phase containing the semiconductor particles (A4) containing the organic ligand (Gd).

[0249] 25.0 mL of acetone was added to the obtained phase to prepare a dispersion. 250 mL of n-hexane was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed, and the precipitate was collected. This procedure was repeated several times to obtain semiconductor particles (A4) containing purified organic ligands (Gd) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2)). The weight loss ratio above 300°C for the semiconductor particles (A4) containing organic ligand (Gd), as determined by the above measurement method, was 22.0%. The composition ratios of hydrophilic organic ligand (G2) and hydrophobic organic ligand (G1) in the semiconductor particles (A4) containing organic ligand (Gd), as determined by the above measurement method, were 78.0% and 22.0%, respectively.

[0250] Examples 1-8, Comparative Example 1: Preparation of curable compositions 1-9 The semiconductor particles (A) obtained in the above preparation examples were mixed with each component to prepare curable compositions 1-9 having the compositions shown in Table 1.

[0251]

[0252] (A1) + (Ga): Semiconductor particle (A1) containing the hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2) prepared in Preparation Example 2 (A2) + (Gb): Semiconductor particle (A2) containing the hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2) prepared in Preparation Example 3 (A3) + (Gc): Semiconductor particle (A3) containing the hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2) prepared in Preparation Example 4 (A4) + (Gd): Semiconductor particle (A4) containing the hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2) prepared in Preparation Example 5 Polymerizable compound (D1): 1,6-Hexanediol diacrylate (polar surface area is 52.6 Å) 2 ) Polymerizable compound (D2): Dipropylene glycol diacrylate (polar surface area is 61.8 Å) 2 ) Polymerizable compound (D3): Ethylene oxide-modified bisphenol A diacrylate (manufactured by Daicel Ornex, EBECRYL150, polar surface area is 89.5 Å) 2 ) Polymerizable compound (D5): Diacrylate of ethoxylated bisphenol fluorene (polar surface area is 71.1 Å) 2Polymerization initiator (E1): Compound represented by the following formula (EA-1) Polymerization initiator (E2): OMNIRAD® 819 (manufactured by IGM Resins)

[0253]

[0254] Table 2 shows the results of the appearance and process resistance of the cured films measured according to (3) and (4) above for curable compositions 1 to 8.

[0255]

Claims

1. A curable composition comprising semiconductor particles (A) and a polymerizable compound (D), wherein the semiconductor particles (A) contain an organic ligand (G), and the weight loss ratio X above 300°C, calculated by formula (1) when the semiconductor particles (A) containing the organic ligand (G) are heated from 25°C to 600°C in a nitrogen atmosphere at a heating rate of 10°C / min, is 35% or less, and the polar surface area of ​​the polymerizable compound (D) is 80 Å. 2 A curable composition that is: Weight reduction ratio X (%) = {T1 / (T0+T1)}×100...(1) [In formula (1), T 0 This is the weight loss rate from 100°C to 300°C, with the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C as the reference weight, and T 1 This is the weight loss rate from 300°C to 600°C, relative to the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C.

2. The curable composition according to claim 1, further comprising a polymerization initiator (E).

3. The curable composition according to claim 2, wherein the polymerization initiator (E) comprises an acylphosphine oxide compound or an oxime compound.

4. The weight loss ratio X at 300°C or higher is 5 to 25%, and the polar surface area of ​​the polymerizable compound (D) is 70 Å. 2 The curable composition according to claim 1 or 2, which is as follows:

5. The curable composition according to claim 1 or 2, which is an ink for inkjet printers.

6. A cured film formed from the curable composition according to claim 1 or 2.

7. A display device comprising the cured film according to claim 6.