Joining component

The joint component with a hot-stamped first steel member and soft layer addresses the challenge of joint strength in high-strength steel sheets, allowing their effective use in complex automobile body structures.

WO2026235192A1PCT designated stage Publication Date: 2026-11-12NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017630
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The challenge lies in the difficulty of manufacturing high-strength steel sheets with complex shapes due to decreased ductility and residual stress leading to fracture and dimensional inaccuracies, while the application of high-strength steel sheets in automobile bodies is limited by poor joint strength, especially in impact-absorbing components.

Method used

A joint component design featuring a hot-stamped first steel member with a soft layer and a hardness gradient, joined by a molten solidified portion and heat-affected zone, ensuring a specific hardness distribution to enhance joint strength.

Benefits of technology

The solution provides a joint component with improved joint strength, enabling the application of high-strength steel sheets in complex automobile body structures, particularly in impact-absorbing components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

A joining component of the disclosure includes: a first steel member that is a hot stamp member having a predetermined chemical composition; a second steel member; and a joining part. The joining part includes a melt-solidified part and a heat-affected part. The first steel member has a soft layer on an overlapping surface side of the first steel member and the second steel member. When the Vickers hardness at a 1 / 4-depth position of the first steel member is defined as A, the Vickers hardness of the soft layer is equal to or less than 0.95 x A. When the maximum value and the minimum value of the Vickers hardness in a range from a position of 50 μm in the thickness direction from the surface on the overlapping surface side of the interface between the joining part and the first steel member to a position of 400 μm from the interface between the molten-solidified part and the heat-affected part to the molten-solidified part side are defined as Hvmax and Hvmin, respectively, Hvmax, Hvmin, and d, which is a linear distance between the position at which Hvmax is indicated and the position at which Hvmin is indicated, satisfy (Hvmax − Hvmin) / d ≤ 350.
Need to check novelty before this filing date? Find Prior Art

Description

Joined component

[0001] The present disclosure relates to a joined component. This application claims priority based on Japanese Patent Application No. 2025-078558 filed in Japan on May 9, 2025, the content of which is incorporated herein by reference.

[0002] In recent years, countries around the world have set higher CO 2 reduction targets, and each automobile manufacturer is advancing fuel efficiency reduction while taking collision safety into consideration. Not only for gasoline vehicles but also for rapidly developing electric vehicles, further high-strength materials are required as vehicle body materials to protect not only passengers but also batteries from collisions and offset the increase in their weight. In the field of automotive steel sheets, against the backdrop of recent stricter environmental regulations and collision safety standards, the application of steel sheets with high tensile strength (high-strength steel sheets) is expanding to improve both fuel efficiency and collision safety. However, since the press formability of steel sheets decreases with increasing strength, it has become difficult to manufacture products with complex shapes.

[0003] Specifically, the ductility of steel sheets decreases with increasing strength, which causes a problem of fracture at highly processed portions when processed into complex shapes. In addition, along with the increase in strength of steel sheets, residual stress after processing causes springback and wall warpage, leading to another problem of degraded dimensional accuracy. Therefore, it is not easy to press-form a steel sheet with high strength, particularly a tensile strength of 780 MPa or more, into a product having a complex shape. Roll forming, instead of press forming, facilitates processing of high-strength steel sheets, but the application destinations of roll-formed high-strength steel sheets are limited to components having a uniform cross section in the longitudinal direction.

[0004] Accordingly, in recent years, as disclosed in Patent Documents 1 to 3 for example, hot stamping has been adopted as a technique for manufacturing extremely high-strength automotive components with good dimensional accuracy. Hot stamping is a hot forming technique in which a material to be formed is heated before being formed.

[0005] In hot stamping, the material is heated before shaping. Therefore, the steel is soft during shaping and has good formability. This allows for the precise shaping of steel into complex shapes without the occurrence of shaping defects such as cracks. In addition, since quenching is performed simultaneously with shaping using a press die in hot stamping, the resulting steel material (steel component) has sufficient strength.

[0006] For example, according to Patent Documents 1 to 3, it is disclosed that it is possible to impart a tensile strength of 980 MPa or more to a steel member obtained by forming a steel plate by hot stamping.

[0007] Japanese Patent Publication No. 2000-38640, International Publication No. 2002 / 103073, Japanese Patent Publication No. 2020-73723

[0008] As described in Patent Documents 1 to 3, hot-stamped members have been proposed in recent years to meet the need for higher strength. However, as strength increases, various properties may deteriorate, making it difficult to apply high-strength members to automobile bodies. For example, when a member is applied to an automobile body, it is joined to other members by resistance spot welding or the like to form a component (jointed component). One of the properties that deteriorates as mentioned above is the joint strength of the joint. Therefore, improvement of the joint strength of the joint is required for application to automobile bodies. Currently, hot-stamped members are mainly applied to structural components that protect the cabin, and their application to impact-absorbing components such as front side members is limited. In impact-absorbing components, the member deforms significantly during a collision, and large forces act on the spot-welded joints. Therefore, improvement of the joint strength of the joint is strongly required to apply hot-stamped members to these components.

[0009] Therefore, the objective of this disclosure is to provide a joint component with excellent joint strength at the connection point.

[0010] The inventors investigated the joint strength of the joints of connecting parts. As a result, they found that the joint strength of the joints can be improved by joining steel members having a soft layer on the surface and by setting the hardness gradient from the molten and solidified part to the heat-affected zone in the joint to a predetermined state.

[0011] This disclosure has been made in view of the above findings. The gist of this disclosure is as follows: [1] A joint component according to one aspect of the present invention includes a first steel member which is a hot-stamped member, a second steel member which is placed on top of the first steel member, and a joint which joins the first steel member and the second steel member, the joint which includes a molten solidified portion and a heat-affected zone formed around the molten solidified portion, the first steel member having a chemical composition in mass%, C: 0.05% or more and less than 0.26%, Si: 0 to 2.00%, Mn: 0.001 to 3.000%, Al: 0.001 to 1.000%, P: 0.100% or less, S: 0.0 100% or less, N: 0.020% or less, O: 0.010% or less, Nb: 0-0.100%, Ti: 0-0.200%, Cu: 0-2.00%, Ni: 0-2.00%, Cr: 0-1.00%, B: 0-0.0200%, Mo: 0-2.00%, V: 0-1.00% , W: 0-1.00%, Ca: 0-0.0200%, Mg: 0-0.0200%, Sn: 0-1.00%, Sb: 0-1.000% , Zr: 0-1.000%, Co: 0-1.000%, Se: 0-1.0000%, Bi: 0-1.000%, As: 0-1.00 The composition is 0%, Ta: 0-1.000%, Re: 0-1.000%, Os: 0-1.000%, Ir: 0-1.000%, REM: 0-0.3000%, and the remainder is Fe and impurities. The first steel member has a soft layer on the overlapping surface side of the first steel member and the second steel member. When the Vickers hardness of the first steel member at a depth of 1 / 4 of the thickness of the first steel member, which is 1 / 4 of the surface of the overlapping surface side of the first steel member, is A, the Vickers hardness of the soft layer is 0.95 × A or less. The joining of the first steel member The Vickers hardness is measured with a measurement range from a position 50 μm in the thickness direction from the surface on the overlapping surface side of the interface between the part and the first steel member, to a position 400 μm on the molten solidification side from the interface between the molten solidification part and the heat-affected zone, in a direction parallel to the surface on the overlapping surface side. When the maximum value of the measured value is Hvmax and the minimum value is Hvmin, Hvmax, Hvmin, and d, which is the straight-line distance in units of mm between the position showing Hvmax and the position showing Hvmin, satisfy the following formula (1).(Hvmax - Hvmin) / d ≤ 350 (1) The joint component of [2] [1] is the first steel member having a chemical composition in mass %, Nb: 0.001 to 0.100%, Ti: 0.001 to 0.200%, Cu: 0.01 to 2.00%, Ni: 0.01 to 2.00%, Cr: 0.01 to 1.00%, B: 0.0001 to 0.0200%, Mo: 0.01 to 2.00%, V: 0.01 to 1.00%, W: 0.01 to 1.00%, Ca: 0.0001 to 0.0200%, Mg: 0.0001 to 0.0200%, Sn: 0.01 to 1.0 It may contain one or more selected from the group consisting of 0%, Sb: 0.001 to 1.000%, Zr: 0.001 to 1.000%, Co: 0.001 to 1.000%, Se: 0.0001 to 1.0000%, Bi: 0.001 to 1.000%, As: 0.001 to 1.000%, Ta: 0.001 to 1.000%, Re: 0.001 to 1.000%, Os: 0.001 to 1.000%, Ir: 0.001 to 1.000%, and REM: 0.0001 to 0.3000%. In the joint component described in [3], [1], or [2], the thickness of the soft layer from the surface of the first steel member may be 50 μm or more. In the joint component described in any one of items [4] [1] to [3], the first steel member may have a coating on its surface. In the joint component described in [5] [4], the coating may be an Fe-Al based coating.

[0012] According to the above embodiments of this disclosure, it is possible to provide a joint component with excellent joint strength at the joint.

[0013] This is a schematic diagram showing an example of a cross-section of a joint component of the present disclosure.

[0014] <Joining Component> A joining component 1 according to one embodiment of the present disclosure (joining component according to this embodiment), as shown in Figure 1, includes a first steel member 11, a second steel member 12 placed on top of the first steel member, and a joining portion 13 that joins the first steel member 11 and the second steel member 12. The joining portion 13 also includes a molten and solidified portion 21 and a heat-affected zone 22 formed around the molten and solidified portion 21. The first steel member 11 and the second steel member 12 include a non-heat-affected zone 23 (sometimes called the base material portion) that is not affected by the heat of welding. The first steel member 11 and the second steel member 12 are superimposed via an overlapping surface 100, which is the surface where one surface of the first steel member and one surface of the second steel member are in contact. Here, in Figure 1, the first steel member 11 and the second steel member 12 are spaced apart, but are judged to be in contact macroscopically. The joint component of this disclosure may be configured such that the first steel member 11 is sandwiched between two second steel members 12, as shown in Figure 2.

[0015] The interface between the molten and solidified area and the heat-affected zone, and the interface between the heat-affected zone and the area not affected by heat (non-heat-affected zone) (which can also be called the interface between the joint and the first or second steel member) can be determined by observation with an optical microscope. Specifically, a test piece is cut from the jointed part so that the cross-section in the thickness direction of the jointed part becomes the observation surface, the cross-section is mechanically ground, and then mirror-finished to create a sample for observation. Next, the observation surface of the sample is etched with a metal flow etching solution to reveal the interface between the molten and solidified area and the heat-affected zone, and the interface between the heat-affected zone and the area not affected by heat (non-heat-affected zone), and the location of the interface is identified with an optical microscope. A digital microscope may be used instead of an optical microscope.

[0016] Furthermore, in the following, the position at 1 / 4 of the thickness of the first steel member, moving from the surface of the first steel member toward the center in the thickness direction of the first steel member, may be described as the "1 / 4 depth position," and the position at X μm, moving from the surface of the first steel member toward the center in the thickness direction of the first steel member, may be described as the "X μm depth position."

[0017] The first steel member, the second steel member, and the joint will be described below.

[0018] <First Steel Member> The first steel member is a hot-stamped member (also called a hot-stamped molded body) formed by hot stamping.

[0019] (Chemical Composition) The first steel member included in the joint component according to this embodiment (the first steel member according to this embodiment) has a chemical composition in mass percent of: C: 0.05% or more and less than 0.26%, Si: 0 to 2.00%, Mn: 0.001 to 3.000%, Al: 0.001 to 1.000%, P: 0.100% or less, S: 0.0100% or less, N: 0.020% or less, O: 0.010% or less, Nb: 0 to 0.100%, Ti: 0 to 0.200%, Cu: 0 to 2.00%, Ni: 0 to 2.00%, Cr: 0 to 1.00%, B: 0 to 0.020% The composition is as follows: 0%, Mo: 0-2.00%, V: 0-1.00%, W: 0-1.00%, Ca: 0-0.0200%, Mg: 0-0.0200%, Sn: 0-1.00%, Sb: 0-1.000%, Zr: 0-1.000%, Co: 0-1.000%, Se: 0-1.0000%, Bi: 0-1.000%, As: 0-1.000%, Ta: 0-1.000%, Re: 0-1.000%, Os: 0-1.000%, Ir: 0-1.000%, REM: 0-0.3000%, and the remainder is Fe and impurities. The reasons for limiting the content of each element are as follows. Numerical ranges indicated by a tilde ("~") include both a lower and upper limit. Numbers indicated as "less than" or "greater than" do not include that value in the numerical range. Unless otherwise specified, percentages for elemental content are given in mass percentages.

[0020] (C: 0.05% or more, less than 0.26%) Carbon (C) is an element that enhances the hardenability of steel and improves the strength of steel members obtained after heat treatment (quenching) such as hot stamping of steel plates. If the C content is less than 0.05%, it becomes difficult to secure the target strength (tensile strength of 980 MPa or more) in the steel member after quenching (obtained after quenching). Therefore, the C content should be 0.05% or more. To obtain higher strength, the C content should preferably be 0.08% or more, and more preferably 0.10% or more or 0.12% or more. On the other hand, if the C content is 0.26% or more, the joint strength of the joint will decrease significantly. Also, the bendability of the steel member will deteriorate. Therefore, the C content should be less than 0.26%. The C content should preferably be 0.24% or less, and more preferably 0.22% or less, 0.21% or less, or 0.18% or less.

[0021] (Si: 0-2.00%) Si is not required to be included (it can be 0%), but it is an effective element for improving the hardenability of steel and ensuring stable strength of steel members. Therefore, it may be included. To obtain the above effects, the Si content is preferably 0.10% or more, and more preferably 0.35% or more. On the other hand, if the Si content in the steel exceeds 2.00%, the heating temperature required for austenite transformation during hot stamping (quenching) becomes significantly higher. This can increase the cost required for hot stamping, or cause ferrite to remain during heating, reducing the strength of the steel member. Therefore, the Si content should be 2.00% or less. The Si content is preferably 1.50% or less, and more preferably 0.90% or less.

[0022] (Mn: 0.001 to 3.000%) Mn is a very effective element for improving the hardenability of steel and ensuring stable strength after quenching. Furthermore, Mn lowers the Ac3 point and promotes lowering the maximum heating temperature (quenching temperature) during hot stamping. To obtain these effects, the Mn content should be 0.001% or more. Preferably, the Mn content should be 0.050% or more, and more preferably 0.100% or more, 0.500% or more, or 1.000% or more. On the other hand, if the Mn content exceeds 3.000%, the hydrogen embrittlement resistance of the steel member deteriorates. For this reason, the Mn content should be 3.000% or less. Preferably, the Mn content should be 2.500% or less, 1.900% or less, or 1.500% or less.

[0023] (Al: 0.001 to 1.000%) Al is an element commonly used as a deoxidizing agent for steel. To obtain this effect, the Al content should be 0.001% or more. Preferably, the Al content should be 0.010% or more, and more preferably 0.030% or more. On the other hand, if the Al content exceeds 1.000%, the heating temperature required for austenite transformation during hot stamping (quenching) becomes significantly higher. Therefore, the Al content should be 1.000% or less. Preferably, the Al content should be 0.500% or less, and more preferably 0.100% or less or 0.080% or less.

[0024] (P: 0.100% or less) P is an element that reduces the hydrogen embrittlement resistance of steel members. In particular, when the P content exceeds 0.100%, the decrease in hydrogen embrittlement resistance becomes significant. Therefore, the P content should be 0.100% or less. Preferably, the P content should be 0.070% or less or 0.020% or less. A lower P content is preferable, so it may be 0%, but a certain amount of P is usually present, and setting the P content to 0% would lead to an increase in steelmaking costs and is not economically desirable. Therefore, the P content may be 0.001% or more.

[0025] (S: 0.0100% or less) S is an element that reduces the toughness of steel members. In particular, if the S content exceeds 0.0100%, the reduction in toughness becomes significant. Therefore, the S content should be 0.0100% or less. Preferably, the S content should be 0.0050% or less. A lower S content is preferable, so 0% is acceptable, but a certain amount of S is usually present, and setting the S content to 0% would increase steelmaking costs and is not economically desirable. Therefore, the S content may be 0.0001% or more, or 0.0002% or more.

[0026] (N: 0.020% or less) N is an element that reduces the toughness of steel members. In particular, if the N content exceeds 0.020%, coarse nitrides are formed in the steel, and the toughness is significantly reduced. Therefore, the N content should be 0.020% or less. Preferably, the N content should be 0.005% or less. There is no particular need to limit the lower limit of the N content, and it may be 0%, but a certain amount of N is usually present, and setting the N content to less than 0.001% leads to an increase in steelmaking costs and is not economically desirable. Therefore, the N content may be 0.001% or more, or 0.002% or more, or 0.003% or more.

[0027] (O: 0.010% or less) O ​​is an element that reduces the toughness of steel members. In particular, if the O content exceeds 0.010%, coarse oxides are formed in the steel, and the toughness is significantly reduced. Therefore, the O content should be 0.010% or less. Preferably, the O content should be 0.005% or less. There is no particular need to limit the lower limit of the O content, and it may be 0%, but a certain amount of O is usually present, and setting the O content to less than 0.001% leads to an increase in steelmaking costs and is not economically desirable. Therefore, the O content may be 0.001% or more, or 0.002% or more, or 0.003% or more.

[0028] The steel member according to this embodiment may have a chemical composition containing the above-mentioned elements (basic elements), with the remainder consisting of Fe and impurities. On the other hand, for the purpose of improving various properties, it may further contain one or more of the following elements (arbitrary elements). Since it is not necessary to include the arbitrary elements, the lower limit of the content is 0%.

[0029] (Nb: 0-0.100%) Nb is an element that forms fine carbides and enhances the toughness of steel members through its grain refining effect. Therefore, Nb may be included. To obtain the above effect, it is preferable that the Nb content be 0.001% or more. It is more preferable that the Nb content be 0.010% or more, and even more preferable that it be 0.030% or more. On the other hand, if the Nb content exceeds 0.100%, the above effect saturates and economic efficiency decreases. Therefore, the Nb content should be 0.100% or less. It is preferable that the Nb content be 0.080% or less, more preferably 0.070% or less, and even more preferable that it be 0.060% or less or 0.050% or less.

[0030] (Ti: 0-0.200%) Ti is an element that forms fine carbides, carbonitrides, etc., and through the resulting fine-graining effect, improves the hydrogen embrittlement resistance of steel members. Furthermore, Ti preferentially bonds with N in steel to form nitrides, suppressing the consumption of solid-solution B due to the precipitation of BN, and promoting the effect of improving hardenability by B, which will be described later. For this reason, Ti may be included. To obtain the above effects, it is preferable that the Ti content be 0.001% or more. It is more preferable that the Ti content be 0.010% or more, and even more preferable that be 0.015% or more. On the other hand, if the Ti content exceeds 0.200%, the amount of TiC precipitation increases and C is consumed, so the strength of the steel member decreases. For this reason, the Ti content should be 0.200% or less. It is preferable that the Ti content be 0.080% or less.

[0031] (Cu: 0-2.00%) Cu is an effective element for improving the hardenability of steel and ensuring stable strength of steel components. Cu is also an element that improves corrosion resistance in corrosive environments. Therefore, Cu may be included. To obtain the above effects, it is preferable that the Cu content be 0.01% or more. It is more preferable that the Cu content be 0.10% or more, and even more preferable that it be 0.20% or more. On the other hand, if the Cu content exceeds 2.00%, the above effects saturate, and the cost increases. Therefore, the Cu content should be 2.00% or less. It is preferable that the Cu content be 1.50% or less, and more preferable that it be 1.00% or less or 0.60% or less.

[0032] (Ni: 0-2.00%) Ni is an effective element for improving the hardenability of steel and ensuring stable strength of steel members. Therefore, Ni may be included. To obtain the above effects, it is preferable that the Ni content be 0.01% or more. It is more preferable that the Ni content be 0.05% or more or 0.10% or more, and even more preferable that it be 0.15% or more. On the other hand, if the Ni content exceeds 2.00%, the above effects saturate and the cost increases. Therefore, the Ni content should be 2.00% or less. It is preferable that the Ni content be 1.00% or less, more preferably 0.50% or less, and even more preferable that it be 0.25% or less.

[0033] (Cr: 0-1.00%) Cr is an effective element for improving the hardenability of steel and ensuring stable strength of steel members. Therefore, Cr may be included. To obtain the above effects, it is preferable that the Cr content be 0.01% or more. It is more preferable that the Cr content be 0.03% or more, and even more preferable that it be 0.05% or more. On the other hand, if the Cr content exceeds 1.00%, the above effects become saturated and the cost increases. Cr is also an element that has the effect of stabilizing iron carbides. If the Cr content exceeds 1.00%, coarse iron carbides may remain undissolved during hot stamping, which may reduce the toughness of the steel member. Therefore, the Cr content should be 1.00% or less. It is preferable that the Cr content be 0.80% or less or 0.50% or less, more preferably 0.20% or less, and even more preferably 0.15% or less.

[0034] (B: 0 to 0.0200%) B is an element that enhances the hardenability of steel even in trace amounts. Furthermore, B strengthens grain boundaries by segregating at them, thereby improving hydrogen embrittlement resistance, and it is an element that suppresses austenite grain growth when steel plates are heated. For this reason, B may be included. To obtain the above effects, the B content is preferably 0.0001% or more, more preferably 0.0005% or more, and even more preferably 0.0010% or more or 0.0015% or more. On the other hand, if the B content exceeds 0.0200%, many coarse compounds precipitate, and the hydrogen embrittlement resistance of the steel member decreases. Therefore, if B is included, the B content should be 0.0200% or less. The B content is preferably 0.0080% or less or 0.0040% or less.

[0035] (Mo: 0-2.00%) Mo is a very effective element for improving the hardenability of steel and ensuring stable strength of steel members. In particular, a synergistic effect of improving hardenability can be obtained by combining it with B above. For this reason, Mo may be included. To obtain the above effect, the Mo content is preferably 0.01% or more, more preferably 0.05% or more, even more preferably 0.10% or more, and even more preferably 0.20% or more. On the other hand, Mo is an element that has the effect of stabilizing iron carbides. If the Mo content exceeds 2.00%, coarse iron carbides may remain undissolved during hot stamping, which may reduce the toughness of the steel member. In addition, the cost increases significantly. Therefore, if included, the Mo content should be 2.00% or less. The Mo content is preferably 1.00% or less, 0.80% or less, or 0.40% or less.

[0036] (V: 0-1.00%) V is an element that forms fine carbides and enhances the toughness of steel members through its grain refining effect. Therefore, V may be included. To obtain the above effect, it is preferable that the V content be 0.01% or more. More preferably, the V content is 0.10% or more or 0.15% or more. On the other hand, if the V content exceeds 1.00%, the above effect saturates and economic efficiency decreases. Therefore, if V is included, the V content should be 1.00% or less. It is preferable that the V content be 0.60% or less, and more preferably 0.40% or less.

[0037] (W: 0-1.00%) W is a very effective element for improving the hardenability of steel and ensuring stable strength of steel members. Therefore, W may be included. To obtain the above effects, the W content is preferably 0.01% or more, more preferably 0.10% or more, and even more preferably 0.20% or more or 0.30% or more. On the other hand, W is an element that has the effect of stabilizing iron carbides. If the W content exceeds 1.00%, coarse iron carbides may remain undissolved during hot stamping, which may reduce the toughness of the steel member. In addition, the cost increases significantly. Therefore, if W is included, the W content should be 1.00% or less. The W content is preferably 0.80% or less or 0.60% or less.

[0038] (Ca: 0 to 0.0200%) Ca is an element that refines inclusions in steel and enhances the toughness of steel members. Therefore, Ca may be included. To obtain the above effect, it is preferable that the Ca content be 0.0001% or more. It is more preferable that the Ca content be 0.0010% or more, and even more preferable that it be 0.0020% or more, 0.0030% or more, or 0.0040% or more. On the other hand, if the Ca content exceeds 0.0200%, the effect saturates and the cost increases. Therefore, if Ca is included, the Ca content should be 0.0200% or less. It is preferable that the Ca content be 0.0100% or less or 0.0080% or less, and more preferable that it be 0.0060% or less.

[0039] (Mg: 0-0.0200%) Mg is an element that refines inclusions in steel and enhances the toughness of steel members. Therefore, Mg may be included. To obtain the above effect, it is preferable that the Mg content be 0.0001% or more. The Mg content is more preferably 0.0010% or more, and even more preferably 0.0020% or more or 0.0040% or more. On the other hand, if the Mg content exceeds 0.0200%, the effect saturates and the cost increases. Therefore, if Mg is included, the Mg content should be 0.0200% or less. The Mg content is preferably 0.0150% or less or 0.0100% or less.

[0040] (Sn: 0 to 1.00%) Sn is an element that improves corrosion resistance in corrosive environments. Therefore, Sn may be contained. To obtain the above effect, the Sn content is preferably 0.01% or more. The Sn content is more preferably 0.03% or more, and even more preferably 0.05% or more. On the other hand, if the Sn content exceeds 1.00%, the grain boundary strength decreases, and the hydrogen embrittlement resistance of the steel member decreases. Therefore, when contained, the Sn content is 1.00% or less. The Sn content may be 0.50% or less or 0.10% or less.

[0041] (Sb: 0 to 1.000%) Sb is an element that improves corrosion resistance in corrosive environments. Therefore, Sb may be contained. To obtain the above effect, the Sb content is preferably 0.001% or more, more preferably 0.010% or more, and even more preferably 0.040% or more. On the other hand, if the Sb content exceeds 1.000%, the grain boundary strength decreases, and the hydrogen embrittlement resistance of the steel member decreases. Therefore, when contained, the Sb content is 1.000% or less. The Sb content may be 0.500% or less, 0.150% or less, or 0.100% or less.

[0042] (Zr: 0 to 1.000%) Zr is an element that improves corrosion resistance in corrosive environments. Therefore, Zr may be contained. To obtain the above effect, the Zr content is preferably 0.001% or more, more preferably 0.010% or more, and even more preferably 0.100% or more or 0.150% or more. On the other hand, if the Zr content exceeds 1.000%, the grain boundary strength decreases, and the hydrogen embrittlement resistance of the steel member decreases. Therefore, when contained, the Zr content is 1.000% or less. The Zr content may be 0.500% or less, 0.400% or less, or 0.300% or less.

[0043] (Co: 0 to 1.000%) Co is an element that improves corrosion resistance in corrosive environments. Therefore, Co may be contained. To obtain the above effect, the Co content is preferably 0.001% or more, more preferably 0.010% or more, and further preferably 0.100% or more or 0.200% or more. On the other hand, if the Co content exceeds 1.000%, the above effect is saturated and economic efficiency decreases. Therefore, when contained, the Co content is set to 1.000% or less. The Co content may be 0.500% or less or 0.400% or less.

[0044] (Se: 0 to 1.0000%) Se is an element that improves hydrogen embrittlement resistance. Therefore, Se may be contained. To obtain the above effect, the Se content is preferably 0.0001% or more. The Se content is more preferably 0.0010% or more, and further preferably 0.0100% or more, 0.1000% or more, or 0.1500% or more. On the other hand, if the Se content exceeds 1.0000%, the effect is saturated and the cost increases. Therefore, when contained, the Se content is set to 1.0000% or less. The Se content may be 0.5000% or less, 0.4000% or less, or 0.3000% or less.

[0045] (Bi: 0 to 1.000%) Bi is an element that improves hydrogen embrittlement resistance. Therefore, Bi may be contained. To obtain the above effect, the Bi content is preferably 0.001% or more, more preferably 0.010% or more, and further preferably 0.100% or more. On the other hand, if the Bi content exceeds 1.000%, the effect is saturated and the cost increases. Therefore, when contained, the Bi content is set to 1.000% or less. The Bi content may be 0.500% or less or 0.200% or less.

[0046] (As: 0-1.000%) As is an element that improves resistance to hydrogen embrittlement. Therefore, it is possible to include As. To obtain the above effect, it is preferable to have an As content of 0.001% or more, more preferably 0.010% or more, and even more preferably 0.060% or more. On the other hand, if the As content exceeds 1.000%, the effect saturates and the cost increases. Therefore, if As is included, the As content should be 1.000% or less. The As content may also be 0.500% or less or 0.200% or less.

[0047] (Ta: 0-1.000%) Ta is an element that improves resistance to hydrogen embrittlement. Therefore, Ta may be included. To obtain the above effect, it is preferable that the Ta content be 0.001% or more, more preferably 0.010% or more, and even more preferably 0.100% or more or 0.150% or more. On the other hand, if the Ta content exceeds 1.000%, the effect saturates and the cost increases. Therefore, if Ta is included, the Ta content should be 1.000% or less. The Ta content may also be 0.500% or less, 0.400% or less, or 0.300% or less.

[0048] (Re: 0 to 1.000%) Re is an element that improves resistance to hydrogen embrittlement. Therefore, Re may be included. To obtain the above effect, it is preferable that the Re content be 0.001% or more, more preferably 0.010% or more, and even more preferably 0.060% or more. On the other hand, if the Re content exceeds 1.000%, the effect saturates and the cost increases. Therefore, if Re is included, the Re content should be 1.000% or less. The Re content may also be 0.500% or less, 0.300% or less, or 0.200% or less.

[0049] (Os: 0 to 1.000%) Os is an element that improves resistance to hydrogen embrittlement. Therefore, Os may be included. To obtain the above effect, it is preferable that the Os content be 0.001% or more, more preferably 0.010% or more, and even more preferably 0.100% or more. On the other hand, if the Os content exceeds 1.000%, the effect saturates and the cost increases. Therefore, if Os is included, the Os content should be 1.000% or less. The Os content may also be 0.500% or less, 0.350% or less, or 0.200% or less.

[0050] (Ir: 0 to 1.000%) Ir is an element that improves resistance to hydrogen embrittlement. Therefore, Ir may be included. To obtain the above effect, it is preferable that the Ir content be 0.001% or more, more preferably 0.010% or more, and even more preferably 0.060% or more. On the other hand, if the Ir content exceeds 1.000%, the effect saturates and the cost increases. Therefore, if Ir is included, the Ir content should be 1.000% or less. The Ir content may also be 0.500% or less, 0.300% or less, or 0.200% or less.

[0051] (REM: 0-0.3000%) REM (rare earth elements) are elements that, like Ca, refine inclusions in steel and improve the toughness of steel members. Therefore, REM may be included. To obtain the above effect, it is preferable that the REM content be 0.0001% or more. It is more preferable that the REM content be 0.0100% or more, and even more preferable that it be 0.0200% or more. On the other hand, if the REM content exceeds 0.3000%, the effect saturates and the cost increases. Therefore, if REM is included, the REM content should be 0.3000% or less. It is preferable that the REM content be 0.2000% or less, 0.1000% or less, or 0.0500% or less. Here, REM refers to a total of 17 elements including Sc, Y, and lanthanides such as La, Ce, and Nd, and the REM content means the total content of these elements. REM is added to molten steel using, for example, an Fe-Si-REM alloy, which contains, for example, Sc, Y, La, Ce, Pr, and Nd.

[0052] (Remainder: Fe and impurities) In the chemical composition of the steel member according to this embodiment, the elements other than those described above, i.e., the remainder, are Fe and impurities. Here, "impurities" means components that are mixed in during the industrial production of steel plates due to raw materials such as ore and scrap, and various factors in the manufacturing process, and are acceptable within a range that does not adversely affect the properties of the steel member according to this embodiment. The industrial production method is the blast furnace steelmaking method or the electric furnace steelmaking method, and also includes the level of mixing (impurity level) that occurs when manufactured by either method. Impurities may also include Pb, Sr, and Zn. The content of impurities is generally 0.10% or less each, but it is preferable that each be 0.01% or less. If the first steel member is a steel member comprising a portion having a tensile strength of 980 MPa or more, such as a tailored property material, and a portion having a tensile strength of less than 980 MPa, it is sufficient that at least the portion with a tensile strength of 980 MPa or more has the above-described chemical composition.

[0053] The chemical composition of steel members can be determined by the following method: A test specimen is taken from the surface of the steel member in the thickness direction from 1 / 4 to 3 / 4 of the way through (1 / 4 depth to 3 / 4 depth), and elemental analysis is performed on this specimen using a common method such as ICP-AES. For C and S, which are difficult to measure with ICP-AES, the combustion-infrared absorption method can be used, for N, the inert gas fusion-thermal conductivity method can be used, and for O, the inert gas fusion-nondispersive infrared absorption method can be used.

[0054] Here, the surface used as the reference for depth position is the surface of the steel member. That is, the chemical composition of the steel member is the chemical composition of the steel member excluding the coating, if the steel member has a coating on its surface. Similarly, the surface used as the reference for measurement positions of Vickers hardness and metal structure, which will be discussed later, also refers to the surface of the steel member excluding the coating.

[0055] (Soft layer) As shown in Figure 1, the first steel member 11 according to this embodiment has a soft layer 31 on the overlapping surface 100 side of the non-heat-affected zone 23 between the first steel member 11 and the second steel member 12. When the Vickers hardness at a 1 / 4 depth position in the non-heat-affected zone is A, the Vickers hardness of this soft layer is 0.95 × A or less. By joining a steel member having a soft layer in a certain range from the surface (surface layer) by welding under specific welding conditions, a hardness distribution as described later can be obtained at the joint. Since the hardness outside the joint does not change due to welding, the hardness of the non-heat-affected zone of the steel member does not change from before welding even after it has become a joined part. In addition, the presence of a soft layer in the surface layer improves the bending characteristics of the first steel member. The thickness of the soft layer from the surface of the first steel member is preferably 50 μm or more, and more preferably 150 μm or more. There is no upper limit to the thickness of the soft layer, but since excessive thickness of the soft layer tends to reduce strength, the thickness of the soft layer may be set to less than 1 / 4 of the thickness of the first steel member and 300 μm or less. If the first steel member comprises a portion having a tensile strength of 980 MPa or more and a portion having a tensile strength of less than 980 MPa, it is sufficient that at least the portion with a tensile strength of 980 MPa or more has the soft layer described above.

[0056] The presence or absence of a soft layer and its thickness are measured by the following method. A test piece is cut from the jointed part so that the cross-section in the thickness direction of the first steel member becomes the measurement surface, and this is used as a sample for Vickers hardness measurement. Next, the non-heat-affected zone is identified by the observation described above. Vickers hardness measurements are taken at intervals of 0.01 mm from a depth of 20 μm on the overlapping surface side of the non-heat-affected zone toward the center in the thickness direction, up to a position beyond the 1 / 4 depth position. In the Vickers hardness test, the applied load is 0.098 N and the load holding time is 10 seconds. Five measurements are taken at each depth, shifting the measurement position perpendicular to the thickness direction, and the average value is taken as the Vickers hardness (unit: HV) at each depth. The Vickers hardness at the depth position closest to the 1 / 4 depth position is taken as the Vickers hardness at the 1 / 4 depth position (A), and the distance from the surface to the maximum depth where the Vickers hardness is 0.95 × A or less is taken as the thickness of the soft layer. If the Vickers hardness at a depth of 20 μm exceeds 0.95 × A, the thickness of the soft layer is set to 0 μm.

[0057] (Metal structure) The metal structure of the first steel member according to this embodiment is not limited, but in order to obtain a target tensile strength of 980 MPa or more, it is preferable that the metal structure at a 1 / 4 depth position in the non-heat-affected zone contains 75% or more by volume of martensite. The volume fraction of martensite is more preferably 90% or more, 92% or more, or 95% or more. The volume fraction of martensite may be 100%. Martensite includes not only so-called fresh martensite, but also tempered martensite and auto-tempered martensite. Auto-tempered martensite is tempered martensite that is generated during cooling during quenching without heat treatment for tempering, and is generated when the martensite generated is tempered on the spot by self-heating associated with martensitic transformation. In addition to martensite, the metal structure at a 1 / 4 depth position in the non-heat-affected zone of the first steel member may also contain retained austenite, bainite, ferrite, and / or pearlite. The volume fraction of retained austenite is preferably less than 6% in order to obtain the target tensile strength.

[0058] The volume fraction of each microstructure in the metallographic structure of a steel member can be measured by the following method. The volume fraction of martensite (including fresh martensite, tempered martensite, and auto-tempered martensite) is measured using bright-field images and electron diffraction patterns acquired with a transmission electron microscope (TEM). Specifically, a test piece is cut from a position at least 30 mm away from the end of the steel member, including a 1 / 4 depth position in the non-heat-affected zone of the steel member, to be used as a thin film sample for TEM observation. The 400 μm portion of this thin film sample is measured at a 1 / 4 depth position of the steel member (acceptable if it is within the range of 1 / 4 to 3 / 8 and 5 / 8 to 3 / 4 of the thickness from the surface in the thickness direction). 2 The above range is observed using TEM. The electron diffraction pattern of the thin film sample is used to distinguish between body-centered cubic lattices such as martensite and bainite and face-centered cubic lattices such as retained austenite. Then, iron carbides (Fe) in martensite and bainite are examined. 3C) is identified by electron diffraction patterns, and the microstructure fractions of martensite and bainite are measured by observing its precipitation morphology. Specifically, if the precipitation morphology is in three directions, it is determined to be martensite (tempered martensite or auto-tempered martensite), and if it is limited to one direction, it is determined to be bainite. If no iron carbide precipitation is observed, it is also determined to be martensite (fresh martensite). The microstructure fractions of martensite and bainite measured by TEM are measured as area percentages, but since the steel member according to this embodiment has an isotropic metal structure, the area fraction value can be directly replaced with a volume fraction. Iron carbides are observed to distinguish between martensite and bainite, but in this embodiment, these iron carbides are included in the volume fraction of either martensite or bainite. The volume fraction of retained austenite is measured using X-ray diffraction. Specifically, a test piece is cut from a position 30 mm or more away from the end of the steel member to be used as a sample for X-ray diffraction. The cut specimen is chemically polished using hydrofluoric acid and hydrogen peroxide to a depth of 1 / 4 of the way from the surface (acceptable if the depth is between 1 / 4 and 3 / 8 and 5 / 8 and 3 / 4 of the way from the surface in the thickness direction). If chemical polishing takes a long time, for example, the specimen may be polished with waterproof sandpaper to about 1 / 8 of the way from the surface, and then chemically polished to a depth of 1 / 4. The measurement conditions are a Co tube with a 2θ range of 45 to 105°. The integrated intensity of the diffracted X-rays of the face-centered cubic lattice (retained austenite) and body-centered cubic lattice contained in the sample is measured, and the volume fraction of retained austenite is calculated from the value obtained by dividing the integrated intensity by the theoretical intensity (scale factor). If ferrite or pearlite is present as the remaining structure, it can be easily confirmed with an optical microscope or scanning electron microscope. Specifically, a specimen is cut from a position at least 30 mm away from the edge to be used as an observation sample. The cross-section in the thickness direction of the cut specimen is mechanically polished, and then mirror-finished. Next, the test specimen is etched with Nital etching solution to reveal ferrite and pearlite. Using an optical microscope or scanning electron microscope, an area of ​​40,000 μm is measured at a depth of 1 / 4 of the steel member (acceptable if it is within the range of 1 / 4 to 3 / 8 and 5 / 8 to 3 / 4 of the thickness from the surface in the thickness direction). 2By observing the above range, the presence of ferrite or pearlite can be confirmed. A structure in which ferrite and cementite are arranged in alternating layers is identified as pearlite, and it can be distinguished from bainite, in which cementite precipitates in granular form.

[0059] (Coating) The first steel member according to this embodiment may have a coating on part or all of its surface. The coating may be a coating mainly composed of an Fe-Al alloy (Fe-Al coating) or a coating mainly composed of an Fe-Zn alloy (Fe-Zn coating). The coating is also called a film, alloyed plating layer, or intermetallic compound layer. It is not necessary to exclude coatings other than those mainly composed of an Fe-Al alloy and those mainly composed of an Fe-Zn alloy, and other coatings, such as Sn coatings or non-metallic resin coatings, may also be used. These coatings may be formed in multiple layers. A coating mainly composed of an Fe-Al alloy is a coating containing a total of 70% by mass or more of Fe and Al, and a coating mainly composed of an Fe-Zn alloy is a coating containing a total of 70% by mass or more of Fe and Zn. A coating mainly composed of Fe-Al alloy may contain, in addition to Fe and Al, one or more of the following: Si, Mg, Ca, Sr, Ni, Cu, Mo, Mn, Cr, C, Nb, Ti, B, V, Sn, W, Sb, Zn, Co, In, Bi, Zr, Se, As, and REM, with the remainder being impurities. A coating mainly composed of Fe-Zn alloy may contain, in addition to Fe and Zn, one or more of the following: Si, Mg, Ca, Sr, Ni, Cu, Mo, Mn, Cr, C, Nb, Ti, B, V, Sn, W, Sb, Al, Co, In, Bi, Zr, Se, As, and REM, with the remainder being impurities. The total content of impurities may be 1% by mass or less. The presence of the coating provides corrosion resistance, resulting in improved hydrogen embrittlement resistance in automotive applications. The coating is preferably an Fe-Al based coating in terms of hydrogen embrittlement resistance. Furthermore, the coating is also preferably an Fe-Al based coating in terms of heat resistance. The thickness of the coating is preferably 10 to 100 μm.

[0060] The thickness of the coating can be determined by scanning electron microscopy observation of the cross-section in the thickness direction. Specifically, a test piece is cut from a position at least 30 mm away from the end of the steel member and observed. The observation range with the scanning electron microscope is, for example, 400x magnification, covering an area of ​​40,000 μm. 2 The above range shall be used. The cut test piece shall be mechanically polished, and then mirror-finished. Next, the thickness of the coating shall be measured as follows. When observed using a BSE image (or COMPO image), a clear difference in contrast between the coating and the base metal (steel plate substrate) shall be observed. Therefore, the thickness of the coating can be measured by measuring the thickness from the outermost surface to the point where the contrast changes. Measurements shall be taken at 20 equally spaced points within the observation photograph, with a distance of 6.5 μm between measurement points. In addition, five fields of view shall be observed in the manner described above, and the average value shall be used as the thickness of the coating. Furthermore, the chemical composition of the coating can be determined by performing elemental analysis of spots (beam diameter: 1.0 μm) using an electron probe microanalyzer (EPMA) on the same observation range as described above to determine the Fe, Al, and Zn content contained in the coating. Ten points shall be analyzed in a total of 10 arbitrary fields of view of the coating, and the average value of all measured values ​​shall be taken as the Fe, Al, and Zn content contained in the coating. Even if elements other than Fe, Al, and Zn are present, the same method shall be used to determine them.

[0061] (Thickness) In the first steel member according to this embodiment, the thickness of the flat portion (for example, the thickness of the steel plate if it is made of a steel plate) is preferably 0.8 to 4.0 mm, taking into consideration the improvement of collision safety and fuel efficiency when applied to the body of an automobile.

[0062] (Tensile Strength) In order to achieve both fuel efficiency and collision safety when applied to automobile components, the first steel member according to this embodiment preferably has a tensile strength of 980 MPa or more in the base material portion (non-heat-affected zone). More preferably, the tensile strength is 1100 MPa or more, and even more preferably 1300 MPa or more. On the other hand, in order to ensure flexibility, the tensile strength is preferably 1650 MPa or less, and more preferably less than 1600 MPa or less than 1500 MPa.

[0063] The tensile strength is determined by taking a No. 5 or No. 13B test specimen as described in JIS Z2241:2023 from the base material of the first steel member, and performing a tensile test on this specimen at room temperature according to the test method described in JIS Z2241:2023. The tensile speed is controlled so that the strain rate is 2.5% / min. If it is difficult to take the above-mentioned tensile test specimen due to the small size of the steel member, the test specimen shape may be a half-size plate-shaped test specimen as specified in ASTM standard E8 (parallel section length: 32 mm, parallel section plate width: 6.25 mm). Even when this test specimen is used, the shape of the test specimen does not affect the tensile strength. Furthermore, if it is not possible to take a tensile test specimen of the predetermined shape from the first steel member due to the shape of the jointed part, the tensile strength may be determined by calculating from the Vickers hardness (loaded load 0.098 N) at a depth of 1 / 4 of the base material of the first steel member. Specifically, the tensile strength (in MPa) is determined by multiplying the Vickers hardness (in HV) value at a depth of 1 / 4 by 3.10.

[0064] The shape of the first steel member according to this embodiment is not particularly limited. That is, the first steel member may be a molded body in which a steel plate is formed into a predetermined shape. The first steel member may be a tailored property material in which the strength and thickness differ depending on the location. In this case, it is preferable that at least a part of the first steel member has a tensile strength of 980 MPa or more. For example, 10 volume percent or more of the first steel member may have a tensile strength of 980 MPa or more, or 30 volume percent or more may have a tensile strength of 980 MPa or more. The jointed part according to this embodiment is preferably joined to the second steel member at the portion of the first steel member having a tensile strength of 980 MPa or more. The tailored property material may be obtained by joining steel plates according to this embodiment, as described later, and then hot-forming, or by joining a steel plate according to this embodiment with any steel plate and then hot-forming. Alternatively, a part of the steel member may be heat-treated to adjust the strength of that part. When steel plates are joined and then hot-formed, the joint portion that existed before hot-forming does not need to have the hardness gradient described later. In the joints that existed before hot forming, the interface between the heat-affected zone and the non-heat-affected zone is not observed.

[0065] <Second Steel Member> The second steel member joined to the first steel member is not limited. There may be one second steel member or two or more. As described above, for example, as shown in Figure 1, one second steel member 12 may be used for one first steel member 11, or as shown in Figure 2, two second steel members 12 may be used for one first steel member 11. The second steel member may be, for example, a known steel material with a tensile strength of less than 980 MPa in the base material, or a known steel material with a tensile strength of less than 780 MPa in the base material. Depending on the performance required for the joined part, a steel member with a different tensile strength from the first steel member may be used as the second steel member. When multiple second steel members are used, each of the multiple second steel members may be a different steel member having different performance characteristics. The second steel member may be a hot-stamped molded body. On the other hand, if the overall component (joint component) is to be high-strength, the second steel member may be a steel member with a base material tensile strength of 980 MPa or more, 1100 MPa or more, or 1300 MPa or more. If the second steel member has a tensile strength of 980 MPa or more, it is preferable that it has the same chemical composition and soft layer as the first steel member described above. The same steel member as the first steel member may be used as the second steel member. If the same steel member as the first steel member is used as the second steel member, it is preferable that the second steel member has the same chemical composition, tensile strength, and soft layer as the first steel member.

[0066] <Joint> As shown in Figures 1 and 2, the joint (joint according to this embodiment) 13 included in the joint component according to this embodiment joins a first steel member 11 and a second steel member 12 which is placed on top of the first steel member, and has a molten and solidified portion 21 and a heat-affected zone (HAZ) 22 formed around the molten and solidified portion 21. The molten and solidified portion 21 is a part formed when the first steel member and the second steel member before joining are melted by the heat of welding and then solidified again, and the heat-affected zone 22 is a part that did not melt by the heat of welding but underwent a change in its structure. If the welding is resistance spot welding, the molten and solidified portion 21 is a nugget.

[0067] In the joint according to this embodiment, the Vickers hardness (unit: HV) is measured from a position 50 μm in the thickness direction from the surface on the overlapping side of the first steel member at the interface between the joint and the first steel member (interface between the heat-affected zone and the non-heat-affected zone) (50 μm depth position) to a position 400 μm on the molten and solidified side from the interface between the molten and solidified zone to the heat-affected zone in a direction parallel to the surface on the overlapping side of the first steel member (for example, the range of the straight arrow R in Figure 1). When the maximum value of the measured value is taken as Hvmax and the minimum value as Hvmin, Hvmax, Hvmin, and d, which is the straight-line distance in units of mm between the position showing Hvmax and the position showing Hvmin, satisfy the following equation (1). (Hvmax - Hvmin) / d ≤ 350 (1) (Hvmax - Hvmin) / d is an index that shows the change in Vickers hardness per 1 mm, and a small (Hvmax - Hvmin) / d indicates a small gradient in hardness. By satisfying (Hvmax - Hvmin) / d ≤ 350, deterioration of joint strength can be suppressed. (Hvmax - Hvmin) / d is preferably 330 or less, more preferably 300 or less. (Hvmax - Hvmin) / d may be 80 or more. As described above, the surface used when determining the 50 μm depth position, which is the measurement position for Vickers hardness, is the surface of the steel member if the steel member does not have a coating on its surface, and the surface of the steel member with the coating removed if the steel member has a coating.

[0068] In the joint of the joint component according to this embodiment, the reason why the joint strength is higher when (Hvmax - Hvmin) / d ≤ 350 (small hardness gradient) is satisfied is considered to be as follows: In the deformation of a joint component using a high-strength member, the deformation may concentrate at the softest point of the heat-affected zone, i.e., at the position indicating Hvmin, which can lead to fracture. Therefore, by reducing the hardness gradient in the joint (heat-affected zone and the molten and solidified zone near the heat-affected zone), the deformation is dispersed and fracture is suppressed, thereby increasing the joint strength. Furthermore, if the Vickers hardness of the molten and solidified zone is lower than that of the heat-affected zone, there is a risk of the joint fracturing in the molten and solidified zone. Therefore, it is preferable that the Vickers hardness of the molten and solidified zone is higher than that of the heat-affected zone.

[0069] Hvmax, Hvmin, and d are measured by the following method. A test piece is cut from the jointed part so that the cross-section in the thickness direction of the joint becomes the measurement surface, and this is used as a sample for hardness measurement. Next, the interface between the heat-affected zone and the non-heat-affected zone, and the interface between the heat-affected zone and the molten solidified zone are identified by observation as described above. From a position 50 μm from the surface on the overlapping side of the first steel member at the interface between the joint and the first steel member (interface between the heat-affected zone and the non-heat-affected zone) (a range of 40 to 60 μm in the thickness direction from the surface is acceptable), the measurement range is set to 400 μm from the interface between the heat-affected zone and the molten solidified zone toward the molten solidified zone, in a direction parallel to the surface on the overlapping side of the first steel member, and the Vickers hardness is measured at 50 μm intervals. The applied load is 0.98 N, and the load holding time is 10 seconds. For the obtained Vickers hardness, the largest measured value is denoted as Hvmax and the smallest measured value as Hvmin, and the straight-line distance between the measurement point showing Hvmax and the measurement point showing Hvmin is denoted as d. In Figure 1, the measurement range R is shown on the left side of the paper, but since it is thought that the trend will be similar on both the left and right sides, the measurement range should be set from the interface between the joint and the first steel member (the interface between the heat-affected zone and the non-heat-affected zone) on either the left or the right side, in a direction parallel to the surface on the overlapping side of the first steel member, to a position 400 μm from the interface between the heat-affected zone and the molten solidified zone toward the molten solidified zone.

[0070] When the same material as the first steel member is used as the second steel member, or when the tensile strength of the second steel member is 980 MPa or more, Hvmax, Hvmin, and d are measured on both the first steel member side and the second steel member side (within the Vickers hardness measurement range on both sides of the overlapping surface). In this case, it is sufficient that Hvmax, Hvmin, and d satisfy the above formula (1) at least on the first steel member side, but it is preferable that Hvmax, Hvmin, and d similarly satisfy the above formula (1) on the second steel member side as well. When the first steel member is sandwiched between two second steel members as shown in Figure 2, Hvmax, Hvmin, and d are measured on the overlapping surfaces on both sides of the first steel member (within the Vickers hardness measurement range on both sides). It is sufficient for Hvmax, Hvmin, and d to satisfy equation (1) in either one of the measurement ranges, but it is preferable that Hvmax, Hvmin, and d satisfy equation (1) in the measurement range R of the overlapping surfaces on both sides (R1 and R2 in Figure 2).

[0071] <Manufacturing Method> The manufacturing method of the jointed parts according to this embodiment is not limited, but can be manufactured by using a manufacturing method that includes the following steps, for example: (I) A joining step of joining a steel member having a predetermined chemical composition and a soft layer on its surface (first steel member) and another steel member (second steel member) by resistance spot welding.

[0072] Furthermore, this first steel member can be manufactured by using a manufacturing method that includes, for example, the following steps: (i) a billet manufacturing step of manufacturing a steel billet such as a slab having a predetermined chemical composition; (ii) a hot rolling step of heating the obtained steel billet and then hot rolling it to make a hot-rolled steel sheet; (iii) a winding step of winding the hot-rolled steel sheet; (iv) a hot-rolled sheet annealing step of annealing the hot-rolled steel sheet after the winding step if necessary; (v) a cold rolling step of descaling the hot-rolled steel sheet after the winding step or the hot-rolled sheet annealing step and then cold rolling it to make a cold-rolled steel sheet; (vi) an annealing step of annealing the hot-rolled steel sheet or cold-rolled steel sheet to make an annealed steel sheet; (vii) a coating step of coating the annealed steel sheet to make a coated steel sheet if necessary. (viiii) A hot stamping process in which annealed steel sheets or coated steel sheets are hot stamped to form steel members (hot stamped members).

[0073] The second steel member may be manufactured by a known method, or by the same method as the first steel member.

[0074] The preferred conditions for each process will be explained.

[0075] (Steel billet manufacturing process) In the steel billet manufacturing process, steel billets such as slabs having a predetermined chemical composition are manufactured. Under known conditions, molten steel adjusted to the predetermined chemical composition can be formed into steel billets by continuous casting or the like. Regarding the chemical composition, since it hardly changes in subsequent processes except for the surface layer, the chemical composition of the steel billet should be the same as that of the first steel member to be obtained.

[0076] (Hot Rolling Process) In the hot rolling process, the obtained steel billet is heated and hot-rolled to produce a hot-rolled steel sheet. During the hot rolling process, scale (hot-rolled scale) is formed on the surface of the steel sheet. The hot rolling conditions are not particularly limited and can be set appropriately within a known range of conditions according to the required characteristics of the steel sheet.

[0077] (Winding Process) In the winding process, the hot-rolled steel sheet obtained in the hot-rolling process is wound into a coil to form a hot-rolled coil. The winding temperature and other conditions are not particularly limited.

[0078] (Hot-rolled sheet annealing process) Hot-rolled sheet annealing can be performed because it softens the hot-rolled steel sheet and reduces the load in the subsequent cold-rolling process. The conditions are not limited and can be those known.

[0079] (Cold Rolling Process) In the cold rolling process, the steel sheet is descaled after the winding process or after the hot-rolled sheet annealing process, and then cold-rolled to obtain a cold-rolled steel sheet of a predetermined thickness. The reduction ratio (thickness reduction rate), etc., are not limited. Before descaling, the steel sheet after the winding process or after the hot-rolled sheet annealing process may be subjected to skin pass rolling according to conventional methods. Also, after cold rolling, treatments such as degreasing may be performed according to conventional methods. The cold rolling process may be omitted.

[0080] (Annealing Process) In the annealing process, the steel sheet (hot-rolled or cold-rolled steel sheet) is annealed under the conditions described below. Specifically, the hot-rolled or cold-rolled steel sheet is annealed in a humid hydrogen atmosphere with a dew point of -20 to +20°C at a temperature range of 700 to 950°C. For example, in a two-stage heating furnace with a direct-flame burner and radiant tubes, the sheet is heated to 560 to 650°C, and then heated to 700 to 950°C in an atmosphere with a hydrogen concentration of 1 to 15 volume percent and a dew point of -20 to +20°C. When heating to 560 to 650°C, the air-fuel ratio of the direct-flame burner may be set to 0.9 to 1.2. A preferred dew point is -10°C or higher, and a more preferred dew point is 0°C or higher. After heating, the sheet is held at a temperature range of 700°C or higher for 30 seconds or more in a high-dew-point atmosphere containing hydrogen. By performing annealing under the above conditions, the CO desorption reaction on the steel sheet surface proceeds due to the reduction of moisture in the atmosphere, and a soft layer can be formed on the surface. If the dew point is below -20°C or the atmosphere is not a humid hydrogen atmosphere, decarburization will not proceed sufficiently. If the dew point is above +20°C, the internal oxidation of easily oxidizable elements such as Si and Mn in the steel sheet will proceed excessively, not only preventing sufficient decarburization but also potentially degrading the quality of the steel sheet surface. Furthermore, the cost will also be excessive. For this reason, a dew point of +20°C or lower is preferable. Also, if the annealing temperature is below 700°C or the holding time at 700°C or higher is less than 30 seconds, decarburization will not proceed sufficiently. On the other hand, if the annealing temperature is above 950°C, it is difficult to control the uniform heat distribution, and the flatness of the steel sheet may deteriorate. When the thickness of the soft layer is 50 μm or more, it is preferable to hold it at a temperature of 700°C or higher for 45 seconds or more. When the thickness is 150 μm or more, it is preferable to hold it at a temperature of 700°C or higher in an atmosphere with a dew point of +5°C or higher for 60 seconds or more. The holding time at 700 to 950°C may be 1000 seconds or less in terms of productivity. Also, the holding time may be less than 90 seconds in order to suppress the decrease in tensile strength.

[0081] (Coating Process) When forming a coating on the surface of the first steel member, the coating may be formed on the surface at the stage of the steel sheet material. The coating method is not particularly limited, and various methods are possible, including hot-dip galvanizing, electroplating, vacuum deposition, cladding, and thermal spraying. Hot-dip galvanizing is the most widely used method industrially.

[0082] Examples of coatings include Al-based coatings containing Al and Zn-based coatings containing Zn. When forming an Al-based coating by hot-dip plating, the plating bath often contains Fe as an impurity in addition to Al. Furthermore, as long as it contains 70% by mass or more of Al, the plating bath may also contain one or more of the following elements in addition to those mentioned above: Si, Mg, Ca, Sr, Ni, Cu, Mo, Mn, Cr, C, Nb, Ti, B, V, Sn, W, Sb, Zn, Co, In, Bi, Zr, Se, As, and REM. When forming a Zn-based coating by hot-dip plating, the plating bath often contains Fe as an impurity in addition to Zn. Furthermore, as long as the plating bath contains 70% by mass or more of Zn, one or more of the following elements may be added to the plating bath in addition to the elements mentioned above: Si, Mg, Ca, Sr, Ni, Cu, Mo, Mn, Cr, C, Nb, Ti, B, V, Sn, W, Sb, Al, Co, In, Bi, Zr, Se, As, and REM. When performing hot-dip plating, the annealed steel sheet may be cooled to room temperature and then reheated for plating, or the annealed steel sheet may be cooled to a temperature near the plating bath temperature (for example, 650 to 750°C for Al-based coatings, and 420 to 500°C for Zn-based coatings), and hot-dip plating may be performed without first cooling to room temperature. If the steel sheet has an Al-based coating, the steel member that has gone through the next step, the hot stamping step, will have an Fe-Al-based coating. Also, if the steel sheet has a Zn-based coating, the steel member that has gone through the next step, the hot stamping step, will have an Fe-Zn-based coating.

[0083] There are no particular limitations on the pre- and post-treatment of the coating; pre-coating, solvent application, alloying treatment, and temper rolling are possible. As an alloying treatment, the coating can be alloyed by heating the coated steel sheet to, for example, 450 to 800°C. Temper rolling is useful for shape adjustment, and for example, it allows for reduction by a reduction ratio of 0.1 to 0.5%.

[0084] (Hot Stamping Process) In the hot stamping process, a steel sheet (annealed steel sheet or coated steel sheet) that has undergone the above process is hot stamped to form a steel member. Hot stamping is performed, for example, by heating the steel sheet to the maximum heating temperature in the temperature range of Ac3 point to (Ac3 point + 300)°C at an average heating rate of 1 to 1000°C / second, and then cooling it to below the Ms point at an average cooling rate above the upper critical cooling rate. Forming of the steel sheet is not required during hot stamping, but it is preferable to perform hot forming at the same time as the cooling process to the Ms point after heating to the temperature range of Ac3 point to (Ac3 point + 300)°C, that is, while cooling at a rate above the upper critical cooling rate. Examples of hot forming include bending, drawing, stretching, hole widening, and stretch flange forming. A heating rate of less than 1°C / second is undesirable because it reduces the productivity of hot stamping. On the other hand, a heating rate exceeding 1000°C / second is undesirable because it results in a mixed grain structure and a decrease in the critical hydrogen content. Also, if the maximum heating temperature is below the Ac3 point (°C), ferrite will remain after cooling, reducing the volume fraction of martensite in the steel structure and potentially leading to insufficient strength in the steel member, which is undesirable. On the other hand, if the maximum heating temperature exceeds (Ac3 point + 300)°C, the structure becomes coarser and the critical hydrogen content decreases, which is undesirable. The upper critical cooling rate is the minimum cooling rate at which austenite is overcooled to generate martensite without precipitating ferrite or pearlite in the metal structure. Cooling at a rate below the upper critical cooling rate will generate ferrite or pearlite, reducing the volume fraction of martensite in the steel structure and potentially leading to insufficient strength in the steel member. During heating, the temperature may be held in the Ac3 point to (Ac3 point + 300)°C range for 1 to 300 seconds. When the thickness of the soft layer is 150 μm or more, it is preferable that the holding time be 5 seconds or less. Alternatively, after cooling to a temperature below the Ms point, tempering treatment may be performed in a temperature range of approximately 100 to 600°C to adjust the strength of the steel member.

[0085] The Ac3 point, Ms point, and upper critical cooling rate are measured by the following method. A strip-shaped test piece measuring 30 mm in width and 200 mm in length is cut from the steel plate according to this embodiment. This test piece is heated to 1000°C in a nitrogen atmosphere at a heating rate of 10°C / second, held at that temperature for 5 minutes, and then cooled to room temperature at various cooling rates. The cooling rate is set from 1°C / second to 100°C / second in 10°C / second intervals (however, the next setting after 1°C / second is 10°C / second). The Ac3 point and Ms point are measured by measuring the change in thermal expansion of the test piece during heating and cooling. The average value of the Ac3 points obtained from all tests is taken as the Ac3 point of the steel plate. In addition, the metallographic structure of each test piece cooled at the above cooling rates is observed, and the minimum cooling rate at which ferrite and pearlite precipitation does not occur is taken as the upper critical cooling rate. Furthermore, the average value of the Ms points obtained from the change in thermal expansion when cooled at a rate above the upper critical cooling rate is defined as the Ms point of the steel plate.

[0086] When increasing the volume fraction of martensite, it is preferable to set the starting temperature for hot forming to Ar3 or higher, and to cool the material to below Ms point by contact with the mold at an average cooling rate greater than the upper critical cooling rate. Since the hardness gradient of the joint can be reduced by increasing the release temperature (surface temperature of the steel member when removing the steel member from the mold), the release temperature is preferably 100°C or higher, and more preferably 200°C or higher. Ar3 can be determined by measuring the change in thermal expansion when a test piece is heated and held, and then cooled at a cooling rate of 1°C / second, as described above in the measurement method for Ac3 point, Ms point, and upper critical cooling rate. Hot forming may be repeated according to the thermal history described above. Alternatively, the above series of hot stamping may be repeated multiple times.

[0087] This hot stamping process yields a first steel member, which is a hot-stamped component. The hot stamping may also be performed on a portion of the steel sheet that serves as the base material. In this case, a first steel member with regions of varying strengths is obtained.

[0088] The above series of hot stamping steps can be carried out by any method; for example, heating may be performed by high-frequency heating, electric heating, infrared heating, or furnace heating. The atmosphere inside the heating furnace may be air, combustion gas, or nitrogen gas. Furthermore, the dew point inside the heating furnace may be controlled to suppress hydrogen generation during hot stamping.

[0089] (Joining Process) In the joining process, the steel member having a soft layer on its surface (first steel member) that has undergone the above process and the other steel member (second steel member) are joined by resistance spot welding. In resistance spot welding, the first steel member and the second steel member that will be welded are placed overlapping so that at least a portion of them overlap, and an electrode is pressed against the overlapping portion with a predetermined pressure and current is passed to form a nugget. If the first steel member has a portion having a tensile strength of 980 MPa or more and a portion having a tensile strength of less than 980 MPa, the second steel member is joined to the portion of the first steel member where the tensile strength is 980 MPa or more. When obtaining a joined part according to this embodiment, the following conditions are adopted when performing resistance spot welding. Electrode material: Alumina-dispersed copper, cadmium copper, zirconium copper, chromium copper, or beryllium copper The electrode material may be alumina-dispersed copper, cadmium copper, zirconium copper, chromium copper, or beryllium copper. Beryllium copper, which has low thermal conductivity, is suitable for reducing the hardness gradient of the joint. By using beryllium copper, the cooling rate of the weld decreases, and Hvmax decreases, thereby reducing the value of (Hvmax - Hvmin) / d. Upslope: 5 cycles or less Upslope is the number of cycles to reach the current that melts the steel member and forms a nugget. If the upslope exceeds 5 cycles, excessive heat input to form the required nugget may decrease d, and the hardness gradient of the joint may increase, which is undesirable. The upslope is preferably 3 cycles or less, and more preferably 1 cycle or less. Downslope: 2 cycles or more Downslope is the number of cycles to reach the current that becomes zero after energization. The downslope should be 2 cycles or more, and may be 10 cycles or more. By providing a downslope, the cooling rate of the weld decreases, and Hvmax decreases, which has the effect of reducing the value of (Hvmax - Hvmin) / d. • Hold time: 8 cycles or less. Hold time refers to the number of cycles from the start of downsloping until electrode holding is complete. If the hold time exceeds 8 cycles, there is a concern that the Hvmax will increase due to the cooling of the weld to a low temperature, and the hardness gradient of the joint will become larger.The holding time is preferably 5 cycles or less, and more preferably 2 cycles or less. Other conditions, such as welding current, energizing time, welding angle, and pressure, can be known conditions depending on the thickness. For example, the following ranges apply: ・Welding current and energizing time: The welding current and energizing time should be selected to obtain the required weld nugget diameter. ・Welding angle: 15° or less The welding angle of the energizing electrode is the contact angle between the energizing electrode and the steel plate, and is expressed as the deviation from the angle where the axial direction of the energizing electrode and the direction parallel to the surface of the steel plate are perpendicular, which is defined as 0°. If the welding angle exceeds 15°, the shape of the nugget may become irregular, and the hardness gradient of the joint may not be sufficiently reduced, which is undesirable. The welding angle is preferably 5° or less, and more preferably 3° or less. ・Pressure: 200 kgf or more By applying pressure between the welding electrodes, the steel member conforms to the mating material, and a nugget is formed by energizing. To suppress the generation of dust during energizing, the pressure is preferably 200 kgf or more. More preferably 300 kgf or more. (Other): For the power supply, either an AC or DC inverter may be used. The frequency may be either 50 Hz or 60 Hz.

[0090] A joining component is obtained by performing the joining process under the above conditions, which includes a first steel member, a second steel member, and a joint connecting the first steel member and the second steel member.

[0091] The present invention will be described more specifically below with reference to examples, but the present invention is not limited to these examples.

[0092] First, in manufacturing steel members and joint components, steel having the chemical compositions A1 to A11, a1, and a2 shown in Tables 1-1 and 1-2 was melted to obtain slabs for hot rolling.

[0093]

[0094]

[0095] The obtained slabs were hot-rolled to produce hot-rolled steel sheets with a thickness of 2.7 mm. The hot-rolled steel sheets were then descaled by pickling and cold-rolled to produce cold-rolled steel sheets with a thickness of 1.2 to 1.6 mm. The resulting cold-rolled steel sheets were annealed under the conditions shown in Table 2 to produce annealed steel sheets. During annealing, the hydrogen concentration in the atmosphere was set to 3 vol%. Some of the steel sheets were immersed in an Al plating bath containing 10 mass% Si, 2 mass% Fe, and the remainder being impurities to produce Al-plated steel sheets with an Al-based coating on the surface (coating in Table 2: example of Al-based coating). The thickness of the coating was adjusted to approximately 30 μm in all cases. (In Table 2, "-" for coating indicates that no coating was formed.)

[0096] From the obtained annealed steel sheet or coated annealed steel sheet, a hot stamping base sheet measuring 300 mm in width and 300 mm in length was taken. Hot stamping was performed on this base sheet under the conditions shown in Table 2 to obtain steel members or coated steel members (collectively referred to as steel members) B1 to B13 and b1 to b5. In Table 2, the cooling rate is the average cooling rate down to the Ms point, and the cooling stop temperature is the surface temperature of the steel member (release temperature) when the steel member was removed from the mold. The molding start temperature was set to Ar3 or higher.

[0097] Test specimens were cut from the obtained steel members, and tensile strength was evaluated by performing tensile tests using the following method. The evaluation results are shown in Table 2. The microstructure of these steel members was also observed using the method described above. The remaining microstructure, excluding martensite, contained one or more of the following: retained austenite, bainite, ferrite, and pearlite, with retained austenite accounting for less than 6% by volume.

[0098] <Tensile Strength> Tensile strength was measured in accordance with the provisions of JIS Z2241:2023. A No. 13B test specimen was taken from the uniformly heated area of ​​the steel member (a part at least 50 mm away from the end) so that the test direction was parallel to the rolling direction. A tensile test was then performed at room temperature at a tensile speed of 2.5% / min, and the tensile strength (maximum strength) was measured. In this example, a tensile strength of 980 MPa or higher was evaluated as having high tensile strength.

[0099] In addition to the steel members B1 to B13 and b1 to b5 obtained above, a cold-rolled steel sheet (CR1) having a chemical composition of mass%, C: 0.14%, Si: 0.45%, Mn: 2.403%, P: 0.010%, S: 0.0021%, Al: 0.033%, N: 0.004%, the remainder being Fe and impurities, with a tensile strength of 965 MPa and a thickness of 2.3 mm, and A cold-rolled steel sheet (CR2) with a chemical composition of C: 0.09%, Si: 0.57%, Mn: 2.121%, P: 0.009%, S: 0.0022%, Al: 0.033%, Ti: 0.017%, Nb: 0.020%, N: 0.004%, the remainder being Fe and impurities, with a tensile strength of 809 MPa and a thickness of 2.3 mm was prepared and used as a steel member.

[0100] Steel members were welded together using the combinations and spot welding conditions (electrode material, upslope, downslope, hold time, welding current) shown in Tables 3-1 and 3-2 to obtain joined parts. The welding angle was 0° and the applied pressure was 400 kgf. The nugget diameter was set to 3.5√t to 4.5√t relative to the thickness t (mm) of the thinner plate. In part No. C18, one first steel member was welded between two second steel members. In part No. C18, the welding angle was 0° and the applied pressure was 500 kgf. The welding machine was a single-phase AC type (60 Hz power supply), and the above current was applied with a current-on time of 20 cycles. A dome radius electrode with a tip diameter of 6 mmφ was used.

[0101] For the obtained joint components C1 to C18 and c1 to c13, the hardness parameters Hvmax, Hvmin, d, (Hvmax - Hvmin) / d, the Vickers hardness (A) at a 1 / 4 depth position, and the thickness of the soft layer were determined for the first steel member using the method described above. In addition, for some of the second steel member, the hardness parameters Hvmax, Hvmin, d, (Hvmax - Hvmin) / d, the Vickers hardness (A) at a 1 / 4 depth position, and the thickness of the soft layer were also determined. The evaluation results are shown in Table 3-2. Furthermore, test pieces were cut from the joint components, and joint tensile tests were performed using the following method to evaluate the tensile shear strength.

[0102] <Tensile Shear Strength> The joint tensile test was conducted in accordance with the provisions of JIS Z 3136:1999 (Test Specimens) and JIS Z 2241:2023 (Tensile Test). A joint tensile test specimen with a length of 125 mm, a width of 40 mm, and an overlap of 40 mm was taken from the center of the welded joint of the jointed component. A tensile test was then performed at room temperature at a speed of 5 mm / min, and the tensile shear strength was measured. Since tensile shear strength has a positive correlation with the tensile strength of steel in the region where the tensile strength of the steel member is low, in this example, a value of tensile shear strength / (tensile strength × plate thickness) exceeding 0.0100 (kN / (MPa・mm)) was evaluated as having high tensile shear strength. In the case of three layers (part No. C18), in accordance with the provisions of JIS Z 3136:1999, the first and second steel members were cut out so that either one could be grasped and pulled, and the tensile shear strength was measured. The value of (tensile strength × plate thickness) was determined for each of the first and second steel members, and the lower value was used to calculate the tensile shear strength / (tensile strength × plate thickness). The tensile strength and plate thickness used were the values ​​shown in Table 2. The results are shown in Table 3-3.

[0103]

[0104]

[0105]

[0106]

[0107] As shown in Tables 1-1 to 3-3, the inventive examples C1 to C18, which satisfy the scope of the present invention, exhibited excellent tensile strength and tensile shear strength. On the other hand, in comparative examples c1 to c13, either the chemical composition, hardness parameter, or presence or absence of a soft layer was outside the scope of the present invention, and they exhibited inferior tensile strength and / or tensile shear strength.

[0108] According to this disclosure, it is possible to provide a joint component with excellent joint strength at the connection point.

[0109] 1 Joining component 11 First steel member 12 Second steel member 13 Joint 21 Molten and solidified area 22 Heat-affected zone 23 Non-heat-affected zone 31 Soft layer 100 Overlap surface R Vickers hardness measurement range

Claims

1. A first steel member which is a hot-stamped member, a second steel member which is placed on top of the first steel member, and a joint which joins the first steel member and the second steel member, wherein the joint includes a molten solidified portion and a heat-affected zone formed around the molten solidified portion, and the first steel member has a chemical composition in mass%, of which C: 0.05% or more and less than 0.26%, Si: 0 to 2.00%, Mn: 0.001 to 3.000%, Al: 0.001 to 1.000%, P: 0.100% or less, S: 0.0100% or less, N: 0.020% or less, O: 0.010% or less, Nb: 0 to 0.100%, Ti: 0 to 0.200%, Cu: 0 to 2.00%. Ni: 0-2.00%, Cr: 0-1.00%, B: 0-0.0200%, Mo: 0-2.00%, V: 0-1.00%, W: 0-1.00%, Ca: 0-0.0200%, Mg: 0-0.0200%, Sn: 0-1.00%, Sb: 0-1.000%, Zr: 0-1.000%, Co: 0-1.000%, Se: 0-1.0000%, Bi: 0-1.000%, As: 0-1.000%, Ta: 0-1.000%, Re: 0-1.000%, Os: 0 to 1.000%, Ir: 0 to 1.000%, REM: 0 to 0.3000%, and the remainder: Fe and impurities, the first steel member has a soft layer on the overlapping surface side of the first steel member and the second steel member, and when the Vickers hardness of the first steel member at a depth position of 1 / 4 of the thickness of the first steel member, which is 1 / 4 of the surface on the overlapping surface side of the first steel member, is A, the Vickers hardness of the soft layer is 0.95 × A or less, and the Vickers hardness of the first steel member is measured with a measurement range from a position 50 μm in the thickness direction from the surface on the overlapping surface side of the interface between the joint and the first steel member, to a position 400 μm on the molten solidification side from the interface between the molten solidification part and the heat-affected zone, in a direction parallel to the surface on the overlapping surface side, and when the maximum value of the measured value is Hvmax and the minimum value is Hvmin,A joint component characterized in that Hvmax, Hvmin, and d, which is the straight-line distance in units of mm between the position indicating Hvmax and the position indicating Hvmin, satisfy the following formula (1): (Hvmax - Hvmin) / d ≤ 350 (1) 2. The chemical composition of the first steel member is, in mass%, Nb: 0.001 to 0.100%, Ti: 0.001 to 0.200%, Cu: 0.01 to 2.00%, Ni: 0.01 to 2.00%, Cr: 0.01 to 1.00%, B: 0.0001 to 0.0200%, Mo: 0.01 to 2.00%, V: 0.01 to 1.00%, W: 0.01 to 1.00%, Ca: 0.0001 to 0.0200%, Mg: 0.0001 to 0.0200%, Sn: 0.01 to 1.00%, Sb: 0.001 to 1.000%, Zr: 0.001 to 1.000%. The joining component according to claim 1, characterized in that it contains one or more selected from the group consisting of Co: 0.001 to 1.000%, Se: 0.0001 to 1.0000%, Bi: 0.001 to 1.000%, As: 0.001 to 1.000%, Ta: 0.001 to 1.000%, Re: 0.001 to 1.000%, Os: 0.001 to 1.000%, Ir: 0.001 to 1.000%, and REM: 0.0001 to 0.3000%.

3. The joining component according to claim 1, characterized in that the thickness of the soft layer from the surface of the first steel member is 50 μm or more.

4. The joining component according to claim 2, characterized in that the thickness of the soft layer from the surface of the first steel member is 50 μm or more.

5. The joint component according to any one of claims 1 to 4, characterized in that the first steel member has a coating on its surface.

6. The joining component according to claim 5, characterized in that the coating is an Fe-Al-based coating.