Manufacturing method for perovskite tandem solar cell and perovskite tandem solar cell manufactured using same
By forming a metal oxide layer with controlled surface energy using nanoparticles on the hole transport layer, the method addresses the challenge of crystallinity and electrical interference in perovskite silicon tandem solar cells, resulting in improved photoelectric efficiency and reproducibility.
Patent Information
- Application Number
- PCT/KR2026/096521
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional perovskite silicon tandem solar cells face challenges in forming a uniform and highly crystalline perovskite light absorption layer due to the electrical interference from the hole transport layer, leading to reduced crystallinity and photoelectric efficiency.
A method involving the formation of a metal oxide layer using metal oxide nanoparticles on the hole transport layer to control the surface energy, reducing the contact angle and enhancing the crystallinity of the perovskite light absorption layer, thereby preventing electrical interference and improving reproducibility and efficiency.
The method results in a perovskite tandem solar cell with improved crystallinity and uniformity of the light absorption layer, enhancing photoelectric efficiency and reproducibility, while preventing defects and pinholes, thus achieving high power conversion efficiency.
Smart Images

Figure KR2026096521_12112026_PF_FP_ABST
Abstract
Description
Method for manufacturing a perovskite tandem solar cell and a perovskite tandem solar cell manufactured according to the same
[0001] The present invention relates to a method for manufacturing a perovskite tandem solar cell and a perovskite tandem solar cell manufactured according to the method. More specifically, the present invention relates to a perovskite tandem solar cell comprising a perovskite light-absorbing layer with controlled underlying properties and a perovskite tandem solar cell manufactured according to the method.
[0002]
[0003] Generally, a perovskite tandem solar cell, in which a silicon solar cell layer is placed at the bottom and a perovskite solar cell layer is placed at the top, can utilize solar energy over a wide wavelength range more effectively by vertically stacking light-absorbing layers having different band gaps.
[0004] Meanwhile, there is an increasing number of attempts to use perovskite materials, which have a composite structure of organic and inorganic materials, as light-absorbing layers. Organic-inorganic hybrid perovskite materials are presenting a breakthrough in the limitations of existing next-generation solar cells due to unique photoelectric properties not found in conventional light-absorbing materials, the resulting high photoelectric conversion efficiency, and low-cost thin-film manufacturing processes.
[0005] Organic-inorganic hybrid metal and halide-based perovskite materials possess excellent photoelectric properties, such as long exciton diffusion distances, high charge mobility, and high absorption coefficients across a wide wavelength range throughout the visible region of the solar spectrum. Furthermore, perovskite solar cells have the advantage of significantly reducing production costs because thin films based on solution processes are easy to form.
[0006] The technology of coating uniform thin films at the nanoparticle level in multilayer thin-film solar cells is a key technology for increasing the photoelectric conversion efficiency of solar cells. In particular, when thin films are formed on substrate layers with non-uniform surfaces, forming smooth and uniform thin films on these non-uniform substrate layers is presented as a research challenge.
[0007] Conventional two-terminal perovskite silicon tandem solar cells form a recombination layer on a bottom silicon photovoltaic layer, and then sequentially form a hole transport layer, a perovskite layer, an electron transport layer, and a TCO, which are the layers of the top perovskite photovoltaic layer. At this time, in order to form a uniform and highly crystalline perovskite layer, organic materials or metal oxide thin films with various functional groups are used as the hole transport layer, or metal oxide nanoparticles are formed on the surface of the hole transport layer to lower the surface energy; however, it is very difficult to process a highly crystalline perovskite and simultaneously form an electrically advantageous structure.
[0008] Therefore, there is an urgent need to develop perovskite solar cells that improve the crystallinity of the perovskite light absorption layer by simultaneously forming a perovskite light absorption layer and preventing electrical interference caused by the hole transport layer.
[0009] Korean Published Patent Application No. 10-2015-0122598 is disclosed as background technology for the present invention.
[0010]
[0011] The objective of the present invention is to provide a method for manufacturing a perovskite tandem solar cell comprising a perovskite light-absorbing layer with improved crystallinity by controlling the characteristics of the lower hole transport layer.
[0012] Another objective of the present invention is to provide a perovskite solar cell that prevents the crystallinity of the perovskite light absorption layer from decreasing due to the electrical characteristics of the hole transport layer and can exhibit high reproducibility and photoelectric efficiency.
[0013] Another objective of the present invention is to provide a method for manufacturing a perovskite tandem solar cell comprising a perovskite light-absorbing layer with improved crystallinity and controlled underlying properties.
[0014] The above and other objectives of the present invention can all be achieved by the present invention described below.
[0015]
[0016] 1. One aspect of the present invention relates to a method for manufacturing a perovskite tandem solar cell.
[0017] The above method for manufacturing a perovskite tandem solar cell comprises the step of forming a hole transport layer;
[0018] A step of forming a metal oxide layer by coating a solution containing metal oxide nanoparticles onto the hole transport layer; and
[0019] The method includes the step of forming a perovskite light-absorbing layer on the metal oxide layer.
[0020] 2. In the above 1 embodiment, the hole transport layer is hydrophobic, and the contact angle in the droplet state may be about 10° or more.
[0021] 3. In the above 1 or 2 embodiments, in the step of forming the metal oxide layer, the solution may be coated by one of the coating methods including slot die coating, spin coating, blade coating, bar coating, spray coating, gravure coating, and die coating.
[0022] 4. In the above 1 to 3 embodiments, the metal oxide nanoparticles may include one or more of AlOx, SiOx, SnOx, and NiOx.
[0023] 5. In the above 1 to 4 embodiments, the metal oxide nanoparticles are AlO x It includes, and the solution may contain AlOx at a concentration of about 1.5 mg / ml or more and less than about 3.0 mg / ml.
[0024] 6. In the above embodiments 1 to 5, the metal oxide nanoparticles are SiO x It includes, and the solution may contain about 2.0 mg / ml or more.
[0025] 7. In the above 1 to 6 embodiments, prior to the step of forming the hole transport layer,
[0026] Step of forming a first electrode layer;
[0027] A step of forming a silicon solar cell layer on the first electrode layer; and
[0028] The method further includes the step of forming a recombination layer on the silicon solar cell layer;
[0029] The hole transport layer may be formed on the recombination layer.
[0030] 8. In the above embodiments 1 to 7, after the step of forming the perovskite light-absorbing layer,
[0031] A step of forming an electron transport layer on the perovskite light-absorbing layer; and
[0032] The method may further include the step of forming a second electrode layer on the electron transport layer.
[0033] 9. Another aspect of the present invention relates to a perovskite tandem solar cell with controlled underlying characteristics manufactured according to the method for manufacturing a perovskite tandem solar cell.
[0034] The above perovskite tandem solar cell comprises a first electrode layer;
[0035] A silicon solar cell layer formed on the first electrode layer above;
[0036] A recombination layer formed on the above silicon solar cell layer;
[0037] A hole transport layer formed on the above recombination layer;
[0038] A metal oxide layer formed on the hole transport layer above; and
[0039] A perovskite light-absorbing layer formed on the metal oxide layer; comprising
[0040] The above metal oxide layer includes metal oxide nanoparticles, and
[0041] The above metal oxide layer is formed by controlling the contact angle of a droplet containing metal oxide nanoparticles.
[0042] 10. In the above 9 embodiments, the electron transport layer formed on the perovskite light absorption layer and the second electrode layer formed on the electron transport layer may be further included.
[0043] 11. In the above 9 or 10 embodiments, the metal oxide layer and the hole transport layer may contain Al in an amount of 12 wt% to 17 wt%.
[0044] 12. In the above 9 to 11 embodiments, the contact angle of the metal oxide layer may be less than about 10°.
[0045] 13. In the above 9 to 12 embodiments, oxide film coating marks may not be formed on the surface of the perovskite light absorption layer.
[0046] 14. In the above 9 to 13 embodiments, the surface of the perovskite light-absorbing layer of the perovskite tandem solar cell may not have pinholes formed at the grain boundary.
[0047] 15. In the above 9 to 14 embodiments, the perovskite light-absorbing layer may contain about 5 at% or less of oxygen, about 1.0 at% or less of chlorine, about 20 at% or less of carbon, and about 35 at% or more of iodine.
[0048] 16. In the above 9 to 15 embodiments, the perovskite tandem solar cell has an open-circuit voltage (V OC The voltage is approximately 1.85 to 1.90 V, and the current density is approximately 18.5 to 19.0 mA / cm² 2 And, the FF is about 70 to 75%, the photoelectric conversion efficiency (PCE) is about 24 to 26%, and the series resistance (Rs) is about 5 to 6.5 ohm / cm 2 And, the parallel resistance (Rsh) is approximately 2000 to 3000 ohm / cm 2 It could be.
[0049]
[0050] The method for manufacturing a perovskite tandem solar cell according to the present invention can significantly reduce the contact angle of droplets formed on the metal oxide layer by increasing the surface energy of the metal oxide layer through a solution process by coating a hole transport layer with metal oxide nanoparticles at a controlled concentration. As the contact angle of droplets on the metal oxide layer decreases, the underlying characteristics of the perovskite light absorption layer formed on the metal oxide layer are significantly improved, thereby increasing the crystallinity of the perovskite thin film and preventing the formation of pinholes at grain boundaries, as well as enabling the manufacture of a perovskite tandem solar cell having high reproducibility and photoelectric efficiency.
[0051]
[0052] FIG. 1 is a process flowchart of a method for manufacturing a perovskite solar cell according to one embodiment of the present invention.
[0053] FIG. 2 is a schematic diagram of a perovskite solar cell according to one embodiment of the present invention.
[0054] FIG. 3 shows the contact angle of a droplet according to the concentration of a metal oxide nanoparticle solution in a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0055] Figure 4 shows PL images of the surface of a perovskite light-absorbing layer according to the concentration of a metal oxide nanoparticle solution in a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0056] FIG. 5 is an SEM image according to the contact angle of the surface of a perovskite light-absorbing layer in a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0057] FIGS. 6(a) to 6(f) show the efficiency of a perovskite tandem solar cell manufactured according to a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0058] FIG. 7 is a current-voltage graph of a perovskite tandem solar cell manufactured according to a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0059] FIG. 8 shows the contact angle according to the concentration of the SiOx metal oxide nanoparticle solution in a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0060]
[0061] The present invention will be described in more detail below with reference to the attached drawings. However, the following drawings are provided merely to aid in understanding the present invention, and the present invention is not limited by the drawings. Furthermore, the shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings are exemplary, and the present invention is not limited to the depicted details.
[0062] Throughout the specification, the same reference numerals refer to the same components. Additionally, in describing the present invention, detailed descriptions of related prior art are omitted if it is determined that such detailed descriptions would unnecessarily obscure the essence of the invention.
[0063] Where terms such as 'includes,' 'have,' and 'consists of' are used in this specification, other parts may be added unless 'only' is used. Where a component is expressed in the singular, it includes cases where it is in the plural unless specifically stated otherwise.
[0064] In interpreting the components, they are interpreted to include a margin of error even in the absence of a separate explicit statement.
[0065] In this specification, "a to b" indicating a numerical range is defined as "≥a and ≤b".
[0066] In this specification, all numerical ranges include a 95% standard error range.
[0067]
[0068] One aspect of the present invention relates to a perovskite solar cell for tandem solar cells.
[0069] FIG. 1 is a process flowchart of a method for manufacturing a perovskite solar cell according to one embodiment of the present invention.
[0070] One aspect of the present invention relates to a method for manufacturing a perovskite tandem solar cell.
[0071] The above method for manufacturing a perovskite tandem solar cell comprises the step of forming a hole transport layer;
[0072] A step of forming a metal oxide layer by coating a solution containing metal oxide nanoparticles onto the hole transport layer; and
[0073] The method includes the step of forming a perovskite light-absorbing layer on the metal oxide layer.
[0074] First, a hole transport layer is formed (S100).
[0075] The method may further include the steps of forming a first electrode layer before forming the hole transport layer, forming a silicon solar cell layer on the first electrode layer, and forming a recombination layer on the silicon solar cell layer.
[0076] The hole transport layer can be formed on the recombination layer.
[0077] A perovskite tandem solar cell according to one embodiment of the present invention may be composed of a two-terminal perovskite silicon tandem solar cell, and as long as it is possible to form a two-terminal perovskite silicon tandem solar cell, the method of forming the first electrode layer, the silicon solar cell layer, and the recombination layer is not particularly limited.
[0078] The hole transport layer mentioned above may be a component of a perovskite solar cell, and in this case, it is also possible to form a single-junction solar cell.
[0079] The hole transport layer above provides a pathway for the movement of holes generated in the perovskite light absorption layer.
[0080] The hole transport layer and the silicon solar cell layer change the perovskite light absorption layer according to their physical and chemical properties, and can determine the underlying properties of the perovskite light absorption layer.
[0081] When the surface energy of the hole transport layer is controlled, the perovskite light absorption layer can be formed uniformly, and crystallinity can also be significantly improved.
[0082] In one embodiment, the hole transport layer is hydrophobic, and the contact angle in the droplet state may be about 10° or more (e.g., about 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20°).
[0083] The contact angle of the above droplet state refers to the angle formed at the boundary between the hole transport layer and the liquid when a droplet is applied to the surface of the hole transport layer via a solution process.
[0084] When using a solution process to form the above perovskite light-absorbing layer, it is easy to apply the perovskite solution over a wider area and is advantageous for manufacturing large-area devices, but when the hole transport layer is hydrophobic, the contact angle in the droplet state may be about 10° or more, and when the contact angle is 10° or more, a uniform perovskite light-absorbing layer cannot be formed, and there is a problem that the crystallinity of the perovskite light-absorbing layer is also reduced.
[0085] The hole transport layer may be, for example, one or more of Me-4PACz, MeO-2PACz, Br-2PACz, MeO-4PACz and 6-PACz, or may be a hydrophobic material such as PTAA, spiro-OmeTAD, etc.
[0086] When a hole transport layer is formed using the above type of organic material, the contact angle in the droplet state increases to about 10° or more due to hydrophobicity, which may cause problems such as reduced crystallinity and increased defects in the perovskite light absorption layer formed on the hole transport layer. However, when a metal oxide layer is additionally placed to control the contact angle, the surface contact angle can be controlled to improve crystallinity and effectively prevent defects from occurring in the thin film when the perovskite light absorption layer is formed by a solution process.
[0087] A metal oxide layer is formed by coating a solution containing metal oxide nanoparticles onto the hole transport layer (S200).
[0088] The metal oxide layer is formed on the hole transport layer by a solution process, thereby controlling the surface energy of the hole transport layer.
[0089] When the metal oxide layer is formed to control the surface energy of the hole transport layer, the crystallinity of the perovskite light absorption layer formed on the metal oxide layer is increased, and a composition ratio capable of improving power efficiency can be achieved.
[0090] The above metal oxide layer is formed by coating a solution containing metal oxide nanoparticles.
[0091] In the step of forming the metal oxide layer, the metal oxide layer can be formed by coating the solution using one of the following coating methods: slot die coating, spin coating, blade coating, bar coating, spray coating, gravure coating, and die coating.
[0092] However, the method is not particularly limited as long as it allows for forming a coating layer on the hole transport layer by controlling the content of metal oxide nanoparticles included in the metal oxide layer.
[0093] In one embodiment, the metal oxide nanoparticles may include one or more of AlOx, SiOx, SnOx, and NiOx.
[0094] A metal oxide layer can be formed using the above type of metal oxide nanoparticles, and since the content of the metal oxide nanoparticles can be easily controlled, a metal oxide layer can be effectively formed on the hole transport layer through a simple solution process, and the surface energy of the metal oxide layer can be controlled according to the concentration of the metal oxide nanoparticles to reduce the contact angle of the droplet state.
[0095] In one embodiment, the metal oxide nanoparticles are AlO x It includes, and the solution is AlO x It can be formed by coating with a solution containing about 1.5 mg / ml or more and less than 3.0 mg / ml (e.g., about 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, or 2.9 mg / ml).
[0096] When the above AlOx is included within the above range, the contact angle of the surface of the metal oxide layer formed on the hole transport layer is less than about 10° (about 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, Can be formed as 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9.0, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, or 9.9°) there is.
[0097] In one embodiment, the metal oxide nanoparticles are SiO x It includes, and the solution is SiO x The metal oxide layer can be formed by coating a solution containing about 2.0 mg / ml or more, for example, about 2.0 to 3.0 mg / ml (for example, about 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, or 3.0 mg / ml).
[0098] In one embodiment, the SiO x When containing about 2.0 mg / ml or more, the contact angle of the surface in the hole transport layer containing the metal oxide layer can be formed to about 17° or less (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, or 17°).
[0099] A solution containing the above metal oxide nanoparticles is coated onto a hole transport layer to form a metal oxide layer, and by increasing the content of the metal oxide nanoparticles in the solution, the surface energy of the metal oxide layer is increased, thereby reducing the contact angle of the metal oxide layer, and consequently, the contact angle of the hole transport layer can be reduced.
[0100] When the above contact angle is reduced, the lower characteristics of the perovskite light absorption layer can be improved, the crystallinity of the perovskite light absorption layer is enhanced, and the effects of the present invention can be realized.
[0101] A perovskite light-absorbing layer is formed on the metal oxide layer (S300).
[0102] A perovskite light-absorbing layer can be formed on the metal oxide layer.
[0103] The above perovskite light-absorbing layer may be an organic or inorganic compound represented by the following chemical formula 1.
[0104] [Chemical Formula 1]
[0105] ABX3
[0106] Here, A is any one of the monovalent organic ammonium ion, Cs ion, methylammonium (MA) and formamidinium (FA), B is Pb, and X is a halogen ion.
[0107] For example, CH3NH3PbI3, CH3NH3PbI x Cl3 -x , MAPbI3, CH3NH3PbI x Br3 -x , CH3NH3PbCl x Br 3-x , HC(NH2)2PbI3, HC(NH2)2PbI x Cl3 -x , HC(NH2)2PbI x Br3 -x , HC(NH2)2PbCl x Br3 -x, (CH3NH3)(HC(NH2)2) 1-y PbI3, (CH3NH3)(HC(NH2)2) 1-y PbI x Cl3 -x , (CH3NH3)(HC(NH2)2) 1-y PbI x Br 3-x , (CH3NH3)(HC(NH2)2) 1-y PbCl x Br3 -x The following may be used, but are not particularly limited as long as they can form a photoactive layer with a perovskite structure.
[0108] The above type of compound can form a perovskite light-absorbing layer through a solution process, which can reduce the manufacturing cost of perovskite tandem solar cells.
[0109] In one embodiment, after the step of forming the perovskite light absorption layer, the method may further include the step of forming an electron transport layer on the perovskite light absorption layer and the step of forming a second electrode layer on the electron transport layer.
[0110] A perovskite tan-dot solar cell can be manufactured by forming an electron transport layer on the perovskite light absorption layer and forming a second electrode on the electron transport layer.
[0111] Accordingly, a method for manufacturing a perovskite tandem solar cell according to one aspect of the present invention forms a metal oxide layer containing metal oxide nanoparticles by coating it on a hole transport layer using a simple solution process, and can precisely control the surface energy of the metal oxide layer by varying the concentration of the metal oxide nanoparticles according to the type of metal oxide, thereby reducing the contact angle on the surface of the metal oxide layer.
[0112] Accordingly, the lower characteristics of the perovskite light absorption layer formed on the metal oxide layer can be improved, crystallinity can be enhanced by forming the perovskite light absorption layer very uniformly, and the photoelectric efficiency of the perovskite solar cell can be significantly improved by forming a perovskite light absorption layer having a composition ratio with increased power conversion efficiency.
[0113] In addition, large-area perovskite solar cells can be manufactured using a simple manufacturing process, and the reproducibility of the manufacturing process can also be improved.
[0114]
[0115] Another aspect of the present invention relates to a perovskite tandem solar cell with controlled underlying characteristics manufactured according to the method for manufacturing a perovskite tandem solar cell.
[0116] FIG. 2 is a schematic diagram of a perovskite solar cell according to one embodiment of the present invention.
[0117] Referring to FIG. 2, the perovskite solar cell comprises a first electrode layer (100), a silicon solar cell layer (200), a recombination layer (300), a hole transport layer (400), a metal oxide layer (500), and a perovskite light absorption layer (600).
[0118] The first electrode layer (100) can transport charges generated in the silicon solar cell layer (200), and the first electrode layer (100) can be selected from an electrically conductive metal such as Al, Ag, or Cu.
[0119] The silicon solar cell layer (200) is formed on the first electrode layer (100), and light can be introduced to generate charge.
[0120] The silicon solar cell layer (200) may be a crystalline silicon solar cell or an amorphous silicon solar cell, and may further include a p-type or n-type substrate (not shown) and an n-type doping layer (not shown).
[0121] The above recombination layer (300) can physically combine and electrically connect the silicon solar cell layer (200) and the hole transport layer (400), and can limit the recombination of charges generated in the silicon solar cell layer (200) and the perovskite light absorption layer (600).
[0122] The above recombination layer (300) is not particularly limited as long as it can combine the silicon solar cell layer (200) and the hole transport layer (400), and may be one or more of a transparent conductive oxide, a carbonaceous conductive material, a metallic material, and a conductive polymer, and may be selected as, for example, one of TCO, FTO, ITO, AZO, and IZO.
[0123] The above hole transport layer (400) is formed on the above recombination layer (300).
[0124] The hole transport layer (400) can transport holes generated in the perovskite light absorption layer (600).
[0125] The hole transport layer (400) may include one or more of Me-4PACz, MeO-2PACz, Br-2PACz, MeO-4PACz and 6-PACz, or may include PTAA or spiro-OmeTAD.
[0126] The hole transport layer (400) is provided with the above type of organic material and has the advantage of being easy to form and having an easy manufacturing process compared to a metal oxide thin film, as additional functional groups are not bonded to it. However, the hole transport layer (400) is hydrophobic, so when a perovskite light absorption layer (600) is directly formed on the hole transport layer (400), crystallinity is reduced, defects may occur, and power conversion efficiency may be lowered.
[0127] The metal oxide layer (500) is formed on the hole transport layer (400).
[0128] The metal oxide layer (500) is formed by including metal oxide nanoparticles in a certain amount, thereby controlling the contact angle of the droplet containing the metal oxide nanoparticles.
[0129] The metal oxide layer (500) can effectively prevent the physical and chemical properties of the hole transport layer (400) from being directly transferred to the perovskite light absorption layer (600), and the metal oxide layer (500) does not change the electrical properties of the hole transport layer (400).
[0130] In one embodiment, the metal oxide layer (500) and the hole transport layer (400) contain about 12 wt% to 17 wt% of Al (e.g., about 12.0, 12.1, 12.2, 12.3, 12.4, 12.5, 12.6, 12.7, 12.8, 12.9, 13.0, 13.1, 13.2, 13.3, 13.4, 13.5, 13.6, 13.7, 13.8, 13.9, 14.0, 14.1, 14.2, 14.3, 14.4, 14.5, 14.6, 14.7, 14.8, 14.9, 15.0, 15.1, It may include 15.2, 15.3, 15.4, 15.5, 15.6, 15.7, 15.8, 15.9, 16.0, 16.1, 16.2, 16.3, 16.4, 16.5, 16.6, 16.7, 16.8, 16.9, or 17.0 wt%).
[0131] The metal oxide layer (500) is formed by coating on the hole transport layer (400), and the composition ratio of Al in the metal oxide layer (500) containing AlOx nanoparticles and the hole transport layer (400) can be adjusted to within the above range.
[0132] Within the above range, the surface energy of the metal oxide layer (500) can be increased, and specifically, the contact angle of a droplet containing metal oxide nanoparticles can be controlled to less than 10° within the target range.
[0133] The contact angle of the droplet on the surface of the metal oxide layer (500) is less than about 10° (e.g., about 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, It may be 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9.0, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, or 9.9°).
[0134] When the metal oxide layer (500) contains AlOx within the above range, the surface energy increases, and the contact angle of the droplet on the surface of the metal oxide layer (500) can be reduced to less than about 10°.
[0135] When the contact angle of the metal oxide layer (500) is reduced within the above range, the perovskite light absorption layer (600) in the solution process can be formed as a very uniform thin film, and because it has an optimal composition ratio that increases crystallinity and improves photoelectric conversion efficiency, the overall efficiency of the perovskite tandem solar cell is also improved, thereby achieving the effects of the present invention.
[0136] When the metal oxide layer (500) is formed, changes in the perovskite light absorption layer (600) due to changes in the electrical characteristics of the hole transport layer (400) can also be prevented.
[0137] The above perovskite light-absorbing layer (600) is formed on the metal oxide layer (500).
[0138] The above perovskite light absorption layer (600) can generate charge by introducing light, and is a component identical to the composition of the perovskite light absorption layer (600) manufactured according to the above-described perovskite tandem solar cell manufacturing method.
[0139] The above perovskite light absorption layer (600) can have its surface energy of the hole transport layer (400) including the metal oxide layer (500) increased, thereby reducing the contact angle and increasing the bonding with the hole transport layer (400), and can be formed very uniformly, so that its crystallinity can be greatly improved.
[0140] Oxide film coating marks may not be formed on the surface of the above perovskite light absorption layer (600).
[0141] The surface of the above perovskite light-absorbing layer (600) may not have oxide film coating marks formed according to the formation of the above metal oxide layer (500). The oxide film coating marks are formed by the uneven coating of the perovskite light-absorbing layer (600) and the aggregation of nanoparticles.
[0142] Specifically, when the contact angle of the metal oxide layer (500) is adjusted to within the above range, the perovskite light absorption layer (600) is formed very uniformly, so that oxide film coating marks are not formed or are formed very faintly.
[0143] If the content of the above metal oxide nanoparticles is not limited, oxide film coating marks may become more distinct, and in this case, a problem may arise in which battery efficiency is reduced due to insulating properties.
[0144] The surface of the perovskite light-absorbing layer (600) of the above perovskite tandem solar cell may not have pinholes formed at the grain boundary.
[0145] The surface of the perovskite light absorption layer (600) has greatly improved crystallinity, so that pinholes may not be formed compared to the case where the perovskite light absorption layer (600) is directly formed on a hole transport layer (400) with a surface contact angle of about 10° or more, and it is possible to form a higher quality perovskite light absorption layer (600).
[0146] The perovskite light-absorbing layer (600) contains oxygen of about 5 at% or less (e.g., about 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9 or 5.0 at%), chlorine of about 1.0 at% Less than (e.g., about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1.0 at%), about 20 at% or less of carbon (e.g., about 18.0, 18.1, 18.2, 18.3, 18.4, 18.5, 18.6, 18.7, 18.8, 18.9, 19.0, 19.1, 19.2, 19.3, 19.4, 19.5, 19.6, 19.7, 19.8, 19.9, or 20.0 at%), and about 35 at% or more of iodine (e.g., about 35.0, 35.1, 35.2, 35.3, It may include 35.4, 35.5, 35.6, 35.7, 35.8, 35.9, 36.0, 36.1, 36.2, 36.3, 36.4, 36.5, 36.6, 36.7, 36.8, 36.9, or 37.0 at%).
[0147] For example, it may contain about 3.5 to 5 at% oxygen, about 0.9 to 1.0 at% chlorine, about 19.8 to 20 at% carbon, and about 35 to 36.6 at% iodine.
[0148] The above perovskite light absorption layer (600) may contain elements within the above range and may have a low oxygen, carbon, and chlorine ratio and a high iodine ratio compared to when formed on a hole transport layer (400) with a contact angle of about 10° or more, which can reduce pinhole generation and significantly reduce non-radiative recombination of charges and can exhibit optimal power conversion efficiency because it is close to a composition ratio that can exhibit ideal photoelectric conversion efficiency.
[0149] The above perovskite light absorption layer (600) may further include an electron transport layer (700) and a second electrode (not shown).
[0150] A two-terminal perovskite tandem solar cell can be configured by further including the electron transport layer (700) and a second electrode (not shown).
[0151] The above perovskite tandem solar cell has an open-circuit voltage (V OC ) is about 1.85 to 1.90 V (e.g., about 1.85, 1.86, 1.87, 1.88, 1.89, or 1.90 V), and the current density is about 18.5 to 19.0 mA / cm² 2 (e.g., approximately 18.5, 18.6, 18.7, 18.8, 18.9, or 19.0 mA / cm²) 2) and FF is approximately 70 to 75% (e.g., 70.0, 70.1, 70.2, 70.3, 70.4, 70.5, 70.6, 70.7, 70.8, 70.9, 71.0, 71.1, 71.2, 71.3, 71.4, 71.5, 71.6, 71.7, 71.8, 71.9, 72.0, 72.1, 72.2, 72.3, 72.4, 72.5, 72.6, 72.7, 72.8, 72.9, 73.0, 73.1, 73.2, 73.3, 73.4, 73.5, 73.6, 73.7, 73.8, 73.9, 74.0, 74.1, 74.2, 74.3, 74.4, 74.5, 74.6, 74.7, 74.8, 74.9, or 75.0%), and the photoelectric conversion efficiency (PCE) is about 24 to 26% (e.g., about 24.0, 24.1, 24.2, 24.3, 24.4, 24.5, 24.6, 24.7, 24.8, 24.9, 25.0, 25.1, 25.2, 25.3, 25.4, 25.5, 25.6, 25.7, 25.8, 25.9, or 26.0%), and the series resistance (Rs) is Approximately 5 to 6.5 ohm / cm 2 (e.g., approximately 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, or 6.5 ohm / cm) 2 ) and the parallel resistance (Rsh) is approximately 2000 to 3000 ohm / cm 2 (For example, approximately 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, or 3000 ohm / cm) 2 It can be.
[0152] The above perovskite tandem solar cell has the perovskite light absorption layer (600) formed uniformly to increase crystallinity and control surface defects, so that it can exhibit open circuit voltage, current density, FF, photoelectric conversion efficiency, series resistance, and parallel resistance within the above range, so that not only the photoelectric conversion efficiency but also the electrical characteristics can be greatly improved.
[0153] Accordingly, in a perovskite tandem solar cell according to another aspect of the present invention, a metal oxide layer (500) containing metal oxide nanoparticles is formed in the hole transport layer (400), and the contact angle of a droplet on the surface of the hole transport layer (400) changes depending on the content of the metal oxide nanoparticles, and in particular, when AlOx is included as the metal oxide, the contact angle of the droplet is controlled to be less than about 10°, thereby significantly reducing the surface energy of the hole transport layer (400) and forming a very uniform thin film.
[0154] The perovskite light absorption layer (600) on the hole transport layer (400) is formed more uniformly, so that crystallinity is also increased and coverage is reduced, which can dramatically improve the efficiency of the perovskite tandem solar cell.
[0155]
[0156] Hereinafter, preferred embodiments are presented to aid in understanding the present invention; however, the following embodiments are merely illustrative of the invention and the scope of the invention is not limited to the following embodiments.
[0157]
[0158] Example 1
[0159] A recombination layer was formed on a silicon solar cell substrate, and a hole transport layer was formed using Me-4PACz spin coating. After heat treatment, a solution containing AlOx nanoparticles (Aluminum oxide powder from Evonik Industries) with the content adjusted according to Table 1 below was also coated under the same conditions to form a metal oxide layer on the hole transport layer.
[0160] Table 1 shows the composition ratio of the metal on the surface of the hole transport layer and the metal on the metal oxide layer according to the concentration of the metal oxide nanoparticle solution in a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0161] AlOx Nanoparticle Content (mg / mL) ON iPC NA lw / o NPs 39.5 24.6 1.3 32.5 2.1 -w / 0.5 40.7 24.0 1.1 28.2 1.5 4.5 w / 1.0 41.5 20.8 1.0 26.2 1.5 9.0 w / 1.5 43.4 17.1 0.8 25.3 1.2 12.2 w / 2.0 45.2 14.5 0.7 22.9 1.2 15.5 w / 3.0 46.5 12.7 0.6 21.9 1.2 17.1
[0162]
[0163] Experimental Example 1
[0164] According to Example 1, a metal oxide layer was formed by controlling the content of metal oxide nanoparticles (AlOx NPs), and the composition ratio of the hole transport layer and the metal oxide layer was confirmed.
[0165] Referring to Table 1 above, when metal oxide nanoparticles were coated on Me-4PACz, nanoparticles were formed at different ratios depending on the concentration of the nanoparticle solution. As the concentration of the metal oxide nanoparticle solution increased, the proportion of metal oxide (Al) on the surface increased, and it was confirmed that a metal oxide layer was formed on Me-4PACz.
[0166]
[0167] Experimental Example 2
[0168] FIG. 3 shows the contact angle of a droplet according to the concentration of a metal oxide nanoparticle solution in a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0169] Referring to Figure 3, it was confirmed that as the concentration of the metal oxide nanoparticle solution increases, the proportion of metal oxide (AlOx) increases, the surface energy decreases, and as a result, the surface contact angle becomes smaller.
[0170] When the concentration of metal oxide nanoparticles contained in the metal oxide nanoparticle solution is about 1.0 mg / mL, the contact angle is about 14.9°, which exceeds about 10°, but when it is about 1.5 mg / mL or higher, the contact angle is about 7.6°, confirming that the target contact angle of about 10° can be achieved.
[0171]
[0172] Example 2
[0173] A perovskite light absorption layer was formed by coating it on a hole transport layer containing a metal oxide layer according to Example 1.
[0174]
[0175] Experimental Example 3
[0176] The characteristics of the perovskite light absorption layer formed according to Example 2 were confirmed.
[0177] Figure 4 shows PL images of the surface of a perovskite light-absorbing layer according to the concentration of a metal oxide nanoparticle solution in a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0178] Referring to Figure 4, it was confirmed that it is difficult to form a uniform coating film on a surface with a contact angle of approximately 30° or more under w / o AlOx conditions. As the AlOx concentration increases, the contact angle decreases, allowing for the formation of a uniform coating; however, as the AlOx concentration increases, oxide film coating marks occur. Furthermore, if the AlOx concentration increases beyond the surface modification level and becomes excessively high, there is a concern that the battery efficiency may decrease due to insulation properties; therefore, it was necessary to set an appropriate AlOx concentration. It was confirmed that a very uniform coating is formed at approximately 1.5 mg / mL, and that a uniform coating can be formed up to approximately 2.0 mg / mL.
[0179] FIG. 5 is an SEM image according to the contact angle of the surface of a perovskite light-absorbing layer in a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0180] Referring to Figure 5, in the case of a perovskite light-absorbing layer coated on a metal oxide layer with a contact angle of about 10° or more, where a low concentration metal oxide nanoparticle solution is applied, it was confirmed that the surface crystallinity is low and small pinholes are formed at the grain boundaries. In contrast, when the contact angle is less than about 10°, no pinholes are formed, confirming that the crystallinity of the perovskite light-absorbing layer is improved.
[0181] Contact Angle Condition OCCsNPbIBrCl Contact Angle < 10° 3.5 19.8 3.0 9.8 20.7 36.6 5.8 0.9 Contact Angle ≥ 10° 9.3 36.2 1.4 8.1 19.0 18.4 6.1 1.5
[0182] Table 2 above shows the composition ratio of the perovskite light-absorbing layer according to XPS analysis of the contact angle of the metal oxide layer. Referring to Table 2, it was confirmed that the surface of the thin film with a contact angle of about 10° or more has a high oxygen (about 5 at% or more) and chlorine (about 1 at% or more) ratio, as well as a high carbon and low iodine ratio. On the other hand, the surface composition ratio of the perovskite light-absorbing layer coated on a metal oxide layer formed with a high concentration of metal oxide nanoparticle solution and having a contact angle of about 10° has a lower oxygen and chlorine ratio than this, and in particular has a low carbon and high iodine ratio, and it was confirmed that it approaches the composition of an ideal perovskite light-absorbing layer with optimal photoelectric conversion efficiency.
[0183] In conclusion, it was confirmed that when a perovskite light-absorbing layer is coated on a metal oxide layer having a contact angle of less than about 10°, a perovskite light-absorbing layer having high crystallinity and an ideal composition ratio is formed.
[0184] FIGS. 6(a) to 6(f) show the efficiency of a perovskite tandem solar cell manufactured according to a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0185] Referring to Figures 6(a) to 6(f), it was confirmed that when a metal oxide nanoparticle solution with a concentration of 1.5 mg / mL is applied and the contact angle is less than 10°, the higher shunt resistance is achieved due to fewer pinholes and better crystallinity compared to when a metal oxide nanoparticle solution with a low concentration of about 0.5 mg / mL is applied and the contact angle is less than 10°, and the results show improved performance in all performance factors, leading to higher photoelectric conversion efficiency.
[0186] In addition, when a metal oxide nanoparticle solution with a higher concentration of about 3.0 mg / mL was applied, the insulating metal oxide formed excessively on the hole transport layer, which hindered hole transport, resulting in an increase in Rs and inferior performance in all device performance factors.
[0187] FIG. 7 is a current-voltage graph of a perovskite tandem solar cell manufactured according to a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0188] Referring to Fig. 7, it was confirmed that a perovskite tandem solar cell containing a metal oxide layer with a contact angle of less than about 10° according to Example 1 was close to an ideal diode type, and a perovskite thin film with high crystallinity and a good composition ratio was formed, and consequently, it was possible to fabricate a solar cell having high photoelectric efficiency.
[0189] In contrast, it can be confirmed that the device efficiency under high AlOx concentration conditions (3.0 mg / mL) exhibits a non-ideal diode type despite having a lower contact angle.
[0190] Therefore, when excessive metal oxide coating is applied during the fabrication of perovskite tandem solar cells, the photoelectric efficiency actually decreases, so it is necessary to control the concentration of metal oxide nanoparticles, and it was confirmed that when selecting aluminum oxide (AlOx) nanoparticles, a concentration of less than about 3.0 mg / mL should be applied.
[0191] FIG. 8 shows the contact angle according to the concentration of the SiOx metal oxide nanoparticle solution in a method for manufacturing a perovskite tandem solar cell according to one embodiment of the present invention.
[0192] Referring to Figure 8, it was confirmed that when the metal oxide nanoparticles were SiOx, the contact angle was about 10° or more, unlike AlOx, even though about 2 wt% SiOx was coated, and it was confirmed that the contact angle could be reduced only by varying the concentration depending on the type of metal oxide nanoparticles.
[0193]
[0194] Therefore, the optimal concentration of metal oxide nanoparticles varies depending on the surface energy of the hole transport layer, and various metal oxides such as SiOx, SnOx, and NiOx, in addition to AlOx, can be used as metal oxide nanoparticles. Since the electrical conductivity varies for each metal oxide, the contact angle can be reduced by adjusting the optimal coating concentration for each metal oxide, thereby improving the underlying properties of the perovskite photoactive layer.
[0195] A perovskite tandem solar cell manufactured according to the method for manufacturing a perovskite tandem solar cell according to the present invention additionally forms a metal oxide layer by controlling the concentration of metal oxide nanoparticles in the hole transport layer, and the high concentration of metal oxide nanoparticles can reduce the surface energy and thus reduce the contact angle at the surface of the metal oxide layer, thereby increasing the bonding strength with the perovskite light absorption layer, uniformly forming the perovskite light absorption layer, and increasing crystallinity to prevent defects in the perovskite light absorption layer, as well as improving the efficiency of the solar cell.
Claims
1. A step of forming a hole transport layer; A step of forming a metal oxide layer by coating a solution containing metal oxide nanoparticles onto the hole transport layer; and A step comprising forming a perovskite light-absorbing layer on the metal oxide layer; Method for manufacturing a perovskite tandem solar cell.
2. A method for manufacturing a perovskite tandem solar cell according to claim 1, wherein the hole transport layer is hydrophobic and has a contact angle of about 10° or more in the droplet state.
3. A method for manufacturing a perovskite tandem solar cell according to claim 1, wherein in the step of forming the metal oxide layer, the solution is coated by one of the following coating methods: slot die coating, spin coating, blade coating, bar coating, spray coating, gravure coating, and die coating.
4. In claim 1, the metal oxide nanoparticles are AlO x , SiO x , SnO x , and NiO x A method for manufacturing a perovskite tandem solar cell comprising one or more of the following.
5. In paragraph 4, the metal oxide nanoparticles are AlO x A method for manufacturing a perovskite tandem solar cell, comprising, wherein the solution contains AlOx at a concentration of about 1.5 mg / ml or more and about 3.0 mg / ml or less.
6. In paragraph 4, the metal oxide nanoparticles are SiO x A method for manufacturing a perovskite tandem solar cell, comprising, wherein the solution contains at least 2.0 mg / ml of SiOx.
7. In claim 1, prior to the step of forming the hole transport layer, Step of forming a first electrode layer; A step of forming a silicon solar cell layer on the first electrode layer; and The method further includes the step of forming a recombination layer on the silicon solar cell layer; A method for manufacturing a perovskite tandem solar cell, wherein the hole transport layer is formed on the recombination layer.
8. In claim 1, after the step of forming the perovskite light-absorbing layer, A step of forming an electron transport layer on the perovskite light-absorbing layer; and A method for manufacturing a perovskite tandem solar cell, further comprising the step of forming a second electrode layer on the electron transport layer.
9. First electrode layer; A silicon solar cell layer formed on the first electrode layer above; A recombination layer formed on the above silicon solar cell layer; A hole transport layer formed on the above recombination layer; A metal oxide layer formed on the hole transport layer above; and A perovskite light-absorbing layer formed on the metal oxide layer; comprising The above metal oxide layer comprises metal oxide nanoparticles, and The above metal oxide layer is formed by controlling the contact angle of a droplet containing metal oxide nanoparticles. Perovskite tandem solar cell.
10. In claim 9, the electron transport layer formed on the perovskite light absorption layer and A perovskite tandem solar cell further comprising a second electrode layer formed on the electron transport layer.
11. A perovskite tandem solar cell according to claim 9, wherein the metal oxide layer and the hole transport layer contain about 12 wt% to 17 wt% of Al.
12. A perovskite tandem solar cell according to claim 9, wherein the contact angle of the metal oxide layer is less than 10°.
13. A perovskite tandem solar cell according to claim 9, wherein oxide film coating marks are not formed on the surface of the perovskite light-absorbing layer.
14. A perovskite tandem solar cell according to claim 9, wherein the surface of the perovskite light-absorbing layer of the perovskite tandem solar cell has no pinholes formed at the grain boundaries.
15. A perovskite tandem solar cell according to claim 9, wherein the perovskite light-absorbing layer comprises about 5 at% or less of oxygen, about 1.0 at% or less of chlorine, about 20 at% or less of carbon, and about 35 at% or more of iodine.
16. In paragraph 9, the perovskite tandem solar cell has an open-circuit voltage (V OC The voltage is approximately 1.85 to 1.90 V, and the current density is approximately 18.5 to 19.0 mA / cm² 2 and, FF is about 70 to 75%, photoelectric conversion efficiency (PCE) is about 24 to 26%, and series resistance (R s ) is about 5 to 6.5 ohm / cm 2 and parallel resistor (R sh ) is approximately 2000 to 3000 ohm / cm 2 A perovskite tandem solar cell.