Electroactive particles with conductive coating
By using pre-lithiated electroactive materials and conductive coatings in lithium-ion battery electrode materials, the problem of lithium ion loss after the first cycle of the lithium-ion battery pack is solved, and the cycle stability and energy density of the battery pack are improved.
Patent Information
- Application Number
- CN202110512606.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-30
- Filing Date
- 2021-05-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-05-11
AI Technical Summary
After the first cycle of the lithium-ion battery pack, lithium ions are permanently lost due to the formation of the solid electrolyte interface and interface rupture, resulting in a decrease in the specific energy and power of the battery pack, and a high irreversible capacity loss.
An electrode material containing multiple electroactive material particles is used, where each particle contains a pre-lithiated electroactive material core and a conductive coating. The conductive coating is formed by contact with a fluoride solution such as copper fluoride, titanium tetrafluoride, etc. Enhance the stability and charge rate performance of electroactive materials.
It reduces the loss of lithium ions during the cycle process, improves the cycle stability and energy density of the battery pack, reduces the need for conductive additives, and extends the battery life.
Smart Images

Figure CN114335434B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to electrode materials used in electrochemical cells, such as negative electrode materials, and preparation methods and uses thereof. Background Art
[0002] This section provides background information related to the present disclosure which is not necessarily prior art.
[0003] Advanced energy storage devices and systems are needed to meet the energy and / or power requirements of a variety of products, including automotive products, such as start-stop systems (e.g., 12V start-stop systems), battery auxiliary systems, hybrid electric vehicles ("HEV"), and electric vehicles ("EV"). A typical lithium-ion battery pack includes at least two electrodes and an electrolyte and / or a separator. One of the two electrodes may serve as a positive electrode or cathode, and the other electrode may serve as a negative electrode or anode. The separator and / or electrolyte may be disposed between the negative electrode and the positive electrode. The electrolyte is suitable for conducting lithium ions between the electrodes, and like the two electrodes, may be in solid and / or liquid form and / or a mixture thereof. In the case of a solid-state battery pack (which includes solid electrodes and a solid electrolyte), the solid electrolyte may physically separate the electrodes, thereby eliminating the need for a separate separator.
[0004] Conventional rechargeable lithium-ion batteries operate by reversibly transferring lithium ions back and forth between a negative electrode and a positive electrode. For example, during charging of the battery, lithium ions may move from the positive electrode to the negative electrode, and move in the opposite direction when the battery is discharged. Such lithium-ion batteries may reversibly supply power to an associated load device as required. More specifically, electrical energy may be supplied to the load device by the lithium-ion battery until the lithium content of the negative electrode is effectively depleted. The battery may then be recharged by passing a suitable direct current in the opposite direction between the electrodes.
[0005] During discharge, the negative electrode may contain a relatively high concentration of intercalated lithium, which is oxidized into lithium ions and electrons. The lithium ions may be transported from the negative electrode to the positive electrode, for example, via an ion-conductive electrolyte solution contained in the pores of an interposed porous separator. Simultaneously, electrons are transported from the negative electrode to the positive electrode via an external circuit. These lithium ions may be incorporated into the material of the positive electrode via an electrochemical reduction reaction. After partial or complete discharge of its available capacity, the battery may be recharged or regenerated by an external power source, which reverses the electrochemical reactions occurring during discharge.
[0006] However, in various cases, due to, for example, conversion reactions during the first cycle and / or the formation of a solid electrolyte interface (SEI) layer on the negative electrode, and due to, for example, continuous lithium loss caused by rupture of the solid electrolyte interface, a portion of the intercalated lithium remains with the negative electrode after the first cycle. Such permanent loss of lithium ions may result in reduced specific energy and power in the battery due to, for example, an increase in the mass of the positive electrode that does not participate in the reversible operation of the battery. For example, a lithium-ion battery may experience an irreversible capacity loss of greater than or equal to about 5% and less than or equal to about 30% after the first cycle, and in the case of a silicon-containing negative electrode, the irreversible capacity loss is greater than or equal to about 20% and less than or equal to about 40% after the first cycle. Therefore, it is desirable to develop improved electrodes and electroactive materials that can address these challenges and methods of preparing and using them. Summary of the invention
[0007] This section provides a general summary of the disclosure, and is not a comprehensive disclosure of its full scope or all of its features.
[0008] The present disclosure relates to electrode materials, such as negative electrode materials, for use in electrochemical cells, and preparation methods and uses thereof. The electrode material comprises a plurality of electroactive material particles, wherein each electroactive material particle comprises an electroactive material core and a conductive coating.
[0009] In various aspects, the present disclosure provides a method for preparing an electrode material for use in an electrochemical cell. The method includes contacting an electroactive material precursor comprising a plurality of electroactive material particles with a solution to form a conductive coating on each electroactive material particle, wherein the coated electroactive material particles define the electrode material. The solution comprises one or more of copper fluoride (CuF2), titanium tetrafluoride (TiF3 or TiF4), iron fluoride (FeF3), nickel fluoride (NiF2), manganese fluoride (MnF2, MnF3 or MnF4) and vanadium fluoride (VF3, VF4, VF5) and a solvent. The conductive coating comprises a plurality of first regions and a plurality of second regions. The plurality of first regions comprise lithium fluoride. The plurality of second regions comprise one of copper, titanium, iron, nickel, manganese and vanadium.
[0010] In one aspect, the electroactive material precursor is pre-lithiated.
[0011] In one aspect, the method further comprises pre-lithiating the electroactive material precursor.
[0012] In one aspect, the electroactive material precursor may be pre-lithiated using a thermal evaporation process.
[0013] In one aspect, the electroactive material particles comprise silicon.
[0014] In one aspect, the solvent can be selected from the group consisting of dimethyl ether, hexane, toluene, and combinations thereof.
[0015] In one aspect, the contacting may be performed by using one of a spraying method and a dipping method.
[0016] In one aspect, the method further comprises drying the coated electroactive material particles to remove the solvent.
[0017] In one aspect, the method further comprises applying a vacuum infiltration process to surround the electroactive material precursor with the solution.
[0018] In one aspect, the conductive coating may be the result of a conversion reaction between the solution and the electroactive material particles.
[0019] In one aspect, the electroactive material precursor comprises pre-lithiated silicon and the solution comprises copper fluoride (CuF2). The conversion reaction may be defined as y(CuF2) + Li x Si → 2y(LiF) + Li (x-2y) Si + yCu, where x > 2y.
[0020] In various aspects, the present disclosure provides a method for preparing an electrode material for use in an electrochemical cell. The method may include pre-lithiating a silicon-containing electroactive material precursor to form a pre-lithiated silicon-containing electroactive material, and contacting the pre-lithiated silicon-containing electroactive material with a solution comprising one or more of copper fluoride (CuF2), titanium tetrafluoride (TiF4), iron fluoride (FeF3), nickel fluoride (NiF2), manganese fluoride (MnF2, MnF3 or MnF4) and vanadium fluoride (VF3, VF4, VF5) and a solvent to form a conductive coating on the pre-lithiated silicon-containing electroactive material, wherein the coated pre-lithiated electroactive material defines the electrode material. The conductive coating comprises a plurality of first regions and a plurality of second regions. The plurality of first regions may comprise lithium fluoride, and the plurality of second regions may comprise one of copper, titanium, iron, nickel, manganese, and vanadium.
[0021] In one aspect, the method further comprises drying the coated pre-lithiated electroactive material to remove the solvent.
[0022] In one aspect, the method further comprises applying a vacuum infiltration process to surround the pre-lithiated silicon-containing electroactive material with the solution.
[0023] In one aspect, the solvent can be selected from the group consisting of dimethyl ether, hexane, toluene, and combinations thereof.
[0024] In one aspect, the conductive coating may be the result of a conversion reaction between the solution and the pre-lithiated silicon-containing electroactive material.
[0025] In one aspect, the solution comprises copper fluoride (CuF2). The conversion reaction can be defined as y(CuF2) + Li x Si → 2y(LiF) + Li (x-2y) Si + yCu, where x > 2y.
[0026] In various aspects, the present disclosure provides an electrode material for use in an electrochemical cell. The electrode material comprises a plurality of electroactive material particles. Each electroactive material particle comprises an electroactive material core and a conductive coating surrounding the electroactive material core. The conductive coating comprises a plurality of first regions and a plurality of second regions. The plurality of first regions may comprise lithium fluoride. The plurality of second regions may comprise one of copper, titanium, iron, nickel, manganese, and vanadium.
[0027] In one aspect, the electroactive material core is a pre-lithiated electroactive material core.
[0028] In one aspect, the conductive coating has a thickness greater than or equal to about 1 nm and less than or equal to about 50 nm.
[0029] Further areas of applicability will become apparent from the description provided herein.The description and specific examples in this summary are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings described herein are for illustrative purposes only of selected embodiments and not all possible implementations, and are not intended to limit the scope of the present disclosure.
[0031] Figure 1 is a schematic diagram of an exemplary electrochemical battery cell;
[0032] Figure 2 is a cross-sectional view of a pre-lithiated negative electrode electroactive material particle with a conductive coating according to various aspects of the present technology;
[0033] Figure 3 is a diagram of a continuous method for forming pre-lithiated negative electrode electroactive material particles with a conductive coating according to various aspects of the present technology; and
[0034] Figure 4 It is a graphical illustration comparing the discharge capacity and capacity retention rate of batteries.
[0035] Corresponding reference numerals indicate corresponding parts throughout the several views of the drawings. DETAILED DESCRIPTION
[0036] Exemplary embodiments are provided so that the present disclosure will be thorough and will fully convey its scope to those skilled in the art. Many specific details, such as examples of specific compositions, components, devices and methods, are set forth to provide a full understanding of the embodiments of the present disclosure. It will be apparent to those skilled in the art that specific details need not be used, that the exemplary embodiments may be embodied in many different forms, and that none of them should be considered to limit the scope of the present disclosure. In some exemplary embodiments, well-known methods, well-known device structures, and well-known technologies are not described in detail.
[0037] The terms used herein are intended only to describe specific exemplary embodiments and are not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms "one", "a kind of" and "the" as used herein may be intended to also include plural forms. The terms "comprise", "include", "contain" and "have" are inclusive, thus illustrating the presence of the described features, elements, compositions, steps, integers, operations and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or their collections. Although the open term "comprise" should be understood as a non-limiting term for describing and claiming the various embodiments described herein, in some aspects, the term may be alternatively understood as a more restrictive and limited term, such as "consisting of" or "consisting essentially of". Thus, for any given embodiment of a narration composition, material, component, element, feature, integer, operation and / or process step, the present disclosure also particularly includes an embodiment consisting of or essentially consisting of such a composition, material, component, element, feature, integer, operation and / or process step. In the case of "consisting of," alternative embodiments exclude any additional compositions, materials, components, elements, features, integers, operations and / or process steps, while in the case of "consisting essentially of," any additional compositions, materials, components, elements, features, integers, operations and / or process steps that materially affect the basic and novel characteristics are excluded from such embodiments, but any compositions, materials, components, elements, features, integers, operations and / or process steps that do not materially affect the basic and novel characteristics may be included in the embodiments.
[0038] Any method steps, processes, and operations described herein are not to be construed as necessarily requiring their performance in the particular order discussed or illustrated, unless specifically identified as a certain order of performance. It is also to be understood that additional or alternative steps may be used unless otherwise stated.
[0039] When a part, element or layer is referred to as being "on," "engaged," "connected," or "coupled" to another element or layer, it may be directly on, engaged, connected, or coupled to another part, element or layer, or there may be intermediate elements or layers. Conversely, when an element is referred to as being directly on, "directly engaged," "directly connected," or "directly coupled" to another element or layer, there may be no intermediate elements or layers. Other words used to describe the relationship between elements should be interpreted in a similar manner (e.g., "between" vs. "directly between," "adjacent" vs. "directly adjacent," etc.). As used herein, the term "and / or" includes any and all combinations of one or more of the associated enumerated items.
[0040] Although the terms first, second, third, etc. can be used to describe various steps, elements, components, regions, layers and / or sections in this article, these steps, elements, components, regions, layers and / or sections should not be limited by these terms unless otherwise specified. These terms can only be used to distinguish a step, element, component, region, layer or section from another step, element, component, region, layer or section. Unless clearly stated in the context, terms such as "first", "second" and other numerical terms do not imply order or sequence when used in this article. Therefore, the first step, element, component, region, layer or section discussed below can be referred to as the second step, element, component, region, layer or section without departing from the teaching of exemplary embodiments.
[0041] For ease of description, spatial or temporal relative terms may be used herein, such as "before", "after", "inside", "outside", "below", "beneath", "lower", "upper", etc. to describe the relationship of one element or feature relative to other elements or features shown in the figures. Spatial or temporal relative terms may be intended to include different orientations of a device or system in use or operation in addition to the orientation shown in the figures.
[0042] Throughout this disclosure, numerical values represent approximate measured values or range limits to include slight deviations from given values and embodiments with roughly listed values and embodiments with exactly listed values.Except in the examples provided at the end of the detailed description part, all numerical values of parameters (such as amounts or conditions) in this specification (including the appended claims) should be understood to be modified by the term "about" in all cases, regardless of whether "about" actually appears before the numerical value. "About" means that the numerical value allows a certain slight imprecision (some close to the exact value; roughly or reasonably close to the value; almost). If the imprecision provided by "about" is not understood in this art with this common meaning, then "about" used herein at least refers to the variation that may be caused by the common method of measuring and using such parameters.For example, "about" can include less than or equal to 5%, optionally less than or equal to 4%, optionally less than or equal to 3%, optionally less than or equal to 2%, optionally less than or equal to 1%, optionally less than or equal to 0.5% and optionally less than or equal to 0.1% variation in some aspects.
[0043] Additionally, disclosure of ranges includes disclosure of all values within the entire range and further subdivided ranges, including endpoints and subranges given within those ranges.
[0044] As used herein, the terms "composition" and "material" are used interchangeably to broadly refer to a substance containing at least a preferred chemical constituent, element or compound, but which may also contain additional elements, compounds or substances, including trace amounts of impurities, unless otherwise specified.
[0045] Example embodiments will now be described more fully with reference to the accompanying drawings.
[0046] The technology of the present application relates to electrode materials, such as negative electrode materials, used in electrochemical cells, and preparation methods and uses related thereto. The electrode material comprises a plurality of electroactive material particles, wherein each electroactive material particle comprises an electroactive material core and a conductive coating. The electroactive material core may be pre-lithiated. The pre-lithiation of the electroactive material may produce a lithium reserve in the electrochemical cell, which may compensate for lithium loss during cycling, particularly during the first cycle, to reduce capacity loss over time. The conductive coating may improve the stability of the electroactive material and the rate performance of rapid charging. The conductive coating may also reduce mechanical degradation and minimize any increase in surface roughness during initial and subsequent lithiation / delithiation cycles. The conductivity of the coating may reduce the amount of conductive additives required in the electrochemical cell, thereby improving energy density and reducing battery costs.
[0047] A typical lithium-ion battery includes a first electrode (e.g., a positive electrode or cathode), an opposing second electrode (e.g., a negative electrode or anode), and a separator and / or electrolyte disposed therebetween. Typically, in a lithium-ion battery pack, the cells or batteries may be electrically connected in a stacked or wound configuration to increase overall output. Lithium-ion batteries operate by reversibly transferring lithium ions between first and second electrodes. For example, during charging of the battery, lithium ions may move from the positive electrode to the negative electrode, and in the opposite direction when the battery is discharged. The electrolyte is suitable for conducting lithium ions (or sodium ions in the case of a sodium-ion battery, etc.) and may be in liquid, gel, or solid form. For example, in Figure 1 An exemplary and schematic illustration of an electrochemical cell (also referred to as a battery) 20 is shown in FIG.
[0048] Such batteries can be used in vehicles or automotive transportation applications (e.g., motorcycles, boats, tractors, buses, mobile homes, campers, and tanks). However, the technology of the present application can be used in a variety of other industries and applications, including, as non-limiting examples, aerospace parts, consumer products, equipment, buildings (e.g., houses, offices, sheds, and warehouses), office equipment and furniture, and industrial equipment machinery, agricultural or farm equipment, or heavy machinery.
[0049] Although the examples shown include a single cathode and a single anode, those skilled in the art will recognize that the teachings of the present application extend to various other configurations, including those having one or more cathodes and one or more anodes, and various current collectors having an electroactive layer disposed on or adjacent to one or more surfaces thereof. Likewise, although the following discussion relates to an electrochemical cell that circulates lithium ions, those skilled in the art will understand that the technology of the present application is similarly applicable to electrochemical cells that circulate any of sodium (Na), potassium (K), and / or tin (Sn) ions.
[0050] The battery pack 20 includes a negative electrode 22 (e.g., an anode), a positive electrode 24 (e.g., a cathode), and a separator 26 disposed between the two electrodes 22, 24. The separator 26 provides electrical isolation between the electrodes 22, 24 - preventing physical contact. The separator 26 also provides a path of least resistance for the internal passage of lithium ions and, in some cases, related anions during lithium ion cycling. In various aspects, the separator 26 includes an electrolyte 30, which may also be present in the negative electrode 22 and the positive electrode 24 in certain aspects. In some variations, the separator 26 may be formed of a solid electrolyte 30. For example, the separator 26 may be defined by a plurality of solid electrolyte particles (not shown).
[0051] The negative electrode current collector 32 may be located at or near the negative electrode 22, and the positive electrode current collector 34 may be located at or near the positive electrode 24. The negative electrode current collector 32 may be a metal foil, a metal grid or mesh, or an expanded metal, comprising copper or any other suitable conductive material known to those skilled in the art. The positive electrode current collector 34 may be a metal foil, a metal grid or mesh, or an expanded metal, comprising aluminum or any other suitable conductive material known to those skilled in the art. The negative electrode current collector 32 and the positive electrode current collector 34 collect free electrons and move the free electrons to and from the external circuit 40, respectively. For example, an interruptible external circuit 40 and a load device 42 may connect the negative electrode 22 (through the negative electrode current collector 32) and the positive electrode 24 (through the positive electrode current collector 34).
[0052] The battery 20 can generate current during discharge through a reversible electrochemical reaction that occurs when the external circuit 40 is closed (to connect the negative electrode 22 and the positive electrode 24) and the negative electrode 22 is at a lower potential than the positive electrode 24. The chemical potential difference between the positive electrode 24 and the negative electrode 22 drives the electrons generated by the reaction at the negative electrode 22, such as oxidation of the intercalated lithium, to move toward the positive electrode 24 through the external circuit 40. The lithium ions also generated at the negative electrode 22 are simultaneously transferred to the positive electrode 24 through the electrolyte 30 contained in the separator 26. The electrons flow through the external circuit 40 and the lithium ions migrate through the separator 26 containing the electrolyte solution 30 to form intercalated lithium at the positive electrode 24. As described above, the electrolyte 30 is also typically present in the negative electrode 22 and the positive electrode 24. The current through the external circuit 40 can be controlled and directed through the load device 42 until the lithium in the negative electrode 22 is depleted and the capacity of the battery 20 is reduced.
[0053] The battery pack 20 can be charged or recharged at any time by connecting an external power source to the lithium-ion battery pack 20 to reverse the electrochemical reactions that occur during the battery pack discharge process. Connecting an external electrical energy source to the battery pack 20 promotes the reaction at the positive electrode 24 (e.g., non-spontaneous oxidation of embedded lithium), thereby producing electrons and lithium ions. The lithium ions flow back to the negative electrode 22 through the separator 26 through the electrolyte 30 to replenish the negative electrode 22 with lithium (e.g., embedded lithium) for use during the next battery pack discharge event. Thus, a complete discharge event followed by a complete charging event is considered to be a cycle, in which lithium ions circulate between the positive electrode 24 and the negative electrode 22. The external power source that can be used to charge the battery pack 20 can vary depending on the size, structure, and specific end use of the battery pack 20. Some notable and exemplary external power sources include, but are not limited to, AC-DC converters and motor vehicle alternators connected to the AC power grid through a wall outlet.
[0054] In many lithium-ion battery configurations, each of the negative electrode current collector 32, the negative electrode 22, the separator 26, the positive electrode 24, and the positive electrode current collector 34 is prepared as a relatively thin layer (e.g., a few microns to a fraction of a millimeter or less in thickness) and assembled in layers connected in an electrically parallel arrangement to provide suitable power and power packaging. In various aspects, the battery 20 may also include various other components that are not depicted herein but are known to those skilled in the art. For example, the battery 20 may include a housing, a gasket, an end cap, a tab, a battery terminal, and any other conventional components or materials that may be located within the battery 20 (including between or around the negative electrode 22, the positive electrode 24, and / or the separator 26). Figure 1 The battery 20 shown in FIG. 1 contains a liquid electrolyte 30 and shows a representative concept of battery operation. However, the technology of the present application is also applicable to solid-state batteries containing solid electrolytes (and solid electroactive particles) that can have different designs, as known to those skilled in the art.
[0055] As described above, the size and shape of the battery pack 20 can vary depending on the specific application for which it is designed. Battery-powered vehicles and handheld consumer electronic devices are two examples in which the battery pack 20 will most likely be designed to different sizes, capacities, and power output specifications. The battery pack 20 can also be connected in series or in parallel with other similar lithium-ion cells or battery packs to produce greater voltage output, energy, and power (if the load device 42 requires it). Therefore, the battery pack 20 can generate current to the load device 42, which is part of the external circuit 40. The load device 42 can be powered by the current passing through the external circuit 40 when the battery pack 20 is discharged. Although the electric load device 42 can be any number of known electric drive devices, some specific examples include electric motors for electric vehicles, laptops, tablet computers, mobile phones, and cordless power tools or appliances. The load device 42 can also be a power generation device that charges the battery pack 20 for the purpose of storing electrical energy.
[0056] Refer again Figure 1 , the positive electrode 24, the negative electrode 22, and the separator 26 can each contain an electrolyte solution or system 30 within their pores, capable of conducting lithium ions between the negative electrode 22 and the positive electrode 24. Any suitable electrolyte 30 capable of conducting lithium ions between the negative electrode 22 and the positive electrode 24, whether in solid, liquid or gel form, can be used in the lithium ion battery 20. In certain aspects, the electrolyte 30 can be a non-aqueous liquid electrolyte solution comprising a lithium salt dissolved in an organic solvent or a mixture of organic solvents. A wide variety of conventional non-aqueous liquid electrolyte 30 solutions can be used in the lithium ion battery 20.
[0057] In certain aspects, electrolyte 30 can be a non-aqueous liquid electrolyte solution comprising one or more lithium salts dissolved in an organic solvent or mixture of organic solvents. For example, a non-limiting list of lithium salts that can be dissolved in an organic solvent to form a non-aqueous liquid electrolyte solution includes lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrachloroaluminate (LiAlCl4), lithium iodide (LiI), lithium bromide (LiBr), lithium thiocyanate (LiSCN), lithium tetrafluoroborate (LiBF4), lithium tetraphenylborate (LiB(C6H5)4), lithium bis(oxalato)borate (LiB(C2O4)2) (LiBOB), lithium difluorooxalatoborate (LiBF2(C2O4)), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethane)sulfonyl imide (LiN(CF3SO2)2), lithium bis(fluorosulfonyl)imide (LiN(FSO2)2) (LiSFI), and combinations thereof.
[0058] These and other similar lithium salts are soluble in various non-aqueous aprotic organic solvents, including but not limited to various alkyl carbonates such as cyclic carbonates (e.g., ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), fluoroethylene carbonate (FEC)), linear carbonates (e.g., dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC)), aliphatic carboxylates (e.g., methyl formate, methyl acetate, methyl propionate), γ-lactones (e.g., γ-butyrolactone, γ-valerolactone), chain structure ethers (e.g., 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane), cyclic ethers (e.g., tetrahydrofuran, 2-methyltetrahydrofuran), 1,3-dioxolane), sulfur compounds (e.g., sulfolane), and combinations thereof.
[0059] In some cases, the porous separator 26 may include a microporous polymer separator containing a polyolefin. The polyolefin can be a homopolymer (derived from a single monomer component) or a heteropolymer (derived from more than one monomer component), which can be linear or branched. If the heteropolymer is derived from two monomer components, the polyolefin can present any copolymer chain arrangement, including those of block copolymers or random copolymers. Similarly, if the polyolefin is a heteropolymer derived from more than two monomer components, it can also be a block copolymer or a random copolymer. In some aspects, the polyolefin can be polyethylene (PE), polypropylene (PP), or a blend of PE and PP, or a multilayer structured porous membrane of PE and / or PP. Commercially available polyolefin porous separator membranes include CELGARD available from Celgard LLC. ® 2500 (a single-layer polypropylene separator) and CELGARD® 2320 (a three-layer polypropylene / polyethylene / polypropylene separator).
[0060] In some aspects, the spacer 26 may further include one or more of a ceramic coating and a heat-resistant material coating. The ceramic coating and / or the heat-resistant material coating may be disposed on one or more sides of the spacer 26. The material forming the ceramic layer may be selected from: aluminum oxide (Al2O3), silicon dioxide (SiO2) and combinations thereof. The heat-resistant material may be selected from: Nomex, Aramid and combinations thereof.
[0061] When the separator 26 is a microporous polymer separator, it can be a single layer or a multilayer laminate, which can be manufactured by a dry method or a wet method. For example, in some cases, a single layer of the polyolefin can form the entire separator 26. In other aspects, the separator 26 can be a fiber membrane, which has a large number of pores extending between the relative surfaces and can have an average thickness of, for example, less than 1 mm. However, as another example, multiple discrete layers of the same or different polyolefins can be assembled to form the microporous polymer separator 26. The separator 26 can also include other polymers other than the polyolefin, such as but not limited to polyethylene terephthalate (PET), polyvinylidene fluoride (PVdF), polyamide, polyimide, poly (amide-imide) copolymer, polyetherimide and / or cellulose, or any other material suitable for producing a desired porous structure. The polyolefin layer and any other optional polymer layer can be further included in the separator 26 as a fiber layer to help provide a separator 26 with suitable structure and porosity characteristics. In certain aspects, the separator 26 may also be mixed with a ceramic material, or its surface may be coated with a ceramic material. For example, the ceramic coating may include aluminum oxide (Al2O3), silicon dioxide (SiO2), titanium dioxide (TiO2), or a combination thereof. A variety of conventionally available polymers and commercial products are contemplated for forming the separator 26, as well as many manufacturing methods that can be used to produce such microporous polymer separators 26.
[0062] In all aspects, Figure 1 The porous separator 26 and electrolyte 30 in the embodiment of the present invention can be replaced with a solid electrolyte ("SSE") (not shown) that acts as both an electrolyte and a separator. The solid electrolyte can be disposed between the positive electrode 24 and the negative electrode 22. The solid electrolyte promotes the migration of lithium ions while mechanically separating the negative electrode and the positive electrode 22, 24 and providing electrical insulation between the negative electrode and the positive electrode 22, 24. As non-limiting examples, the solid electrolyte may include LiTi2(PO4)3, LiGe2(PO4)3, Li7La3Zr2O 12 、Li3xLa 2 / 3-xTiO3, Li3PO4, Li3N, Li4GeS4, Li 10 GeP2S 12 , Li2S-P2S5, Li6PS5Cl, Li6PS5Br, Li6PS5I, Li3OCl, Li 2.99 Ba 0.005 C10 or a combination thereof.
[0063] The positive electrode 24 may be formed of a lithium-based active material (or a sodium-based active material in the case of a sodium-ion battery) capable of lithium insertion and extraction, alloying and alloy degradation, or plating and stripping while serving as the positive terminal of the battery 20. The positive electrode 24 may be defined by a plurality of electroactive material particles (not shown) arranged in one or more layers to define a three-dimensional structure of the positive electrode 24. The electrolyte 30 may be introduced, for example, after the battery is assembled, and contained within the pores (not shown) of the positive electrode 24. For example, the positive electrode 24 may include a plurality of electrolyte particles (not shown).
[0064] An exemplary common class of known materials that can be used to form the positive electrode 24 is layered lithium transition metal oxides. For example, in certain aspects, the positive electrode 24 can include one or more materials having a spinel structure, such as lithium manganese oxide (Li (1+x) Mn2O4, where 0.1≤x≤1), lithium manganese nickel oxide (LiMn (2-x) Ni x O4, where 0≤x≤0.5) (e.g. LiMn 1.5 Ni 0.5 O4); one or more materials having a layered structure, such as lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt oxide (Li(Ni x Mn y Co z )O2, where 0≤x≤1, 0≤y≤1, 0≤z≤1, and x + y + z = 1) (e.g. LiMn 0.33 Ni 0.33 Co 0.33 O2) or lithium nickel cobalt metal oxide (LiNi (1-x-y) Co x M y O2, where 0<x<0.2, y<0.2, and M can be Al, Mg, Ti, etc.); or lithium iron polyanion oxides with olivine structure, such as lithium iron phosphate (LiFePO4), lithium manganese iron phosphate (LiMn 2-x Fe x PO4, wherein 0<x<0.3) or lithium iron phosphate (Li2FePO4F).
[0065] In some variations, the positive electrode electroactive material may be optionally mixed with a conductive material providing an electronic conduction path and / or at least one polymer binder material that improves the structural integrity of the electrode. For example, the positive electrode electroactive material and electronic conduction or conductive material can be slurry cast (slurry cast) with such a binder, such as polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), ethylene propylene diene monomer (EPDM) rubber or carboxymethyl cellulose (CMC), nitrile rubber (NBR), styrene butadiene rubber (SBR), lithium polyacrylate (LiPAA), sodium polyacrylate (NaPAA), sodium alginate or lithium alginate. Conductive materials may include carbon-based materials, powdered nickel or other metal particles, or conductive polymers. Carbon-based materials may include, for example, graphite particles, acetylene black (e.g., KETCHEN TM Black or DENKA TM Black), carbon fiber and nanotubes, graphene, etc. Examples of conductive polymers include polyaniline, polythiophene, polyacetylene, polypyrrole, etc. In some aspects, a mixture of conductive materials can be used.
[0066] The negative electrode 22 comprises a lithium main body material capable of serving as a negative terminal of a lithium-ion battery. For example, the negative electrode 22 may comprise a lithium main body material (e.g., a negative electrode electroactive material) capable of serving as a negative terminal of the battery 20. In various aspects, the negative electrode 22 may be defined by a plurality of negative electrode electroactive material particles (not shown). Such negative electrode electroactive material particles may be arranged in one or more layers to define the three-dimensional structure of the negative electrode 22. The electrolyte 30 may be introduced, for example, after the battery is assembled, and contained within the pores (not shown) of the negative electrode 22. For example, the negative electrode 22 may comprise a plurality of electrolyte particles (not shown).
[0067] Negative electrode 22 may include silicon-based negative electroactive materials including silicon, such as lithium-silicon and silicon-containing binary and ternary alloys and / or tin-containing alloys, such as Si-Sn, SiSnFe, SiSnAl, SiFeCo, SnO2, and the like.
[0068] In some variations, the negative electrode electroactive material in the negative electrode 22 may be optionally mixed with one or more conductive materials that provide an electron conduction path and / or at least one polymer binder material that improves the structural integrity of the negative electrode 22. For example, the negative electrode electroactive material in the negative electrode 22 may be optionally mixed with a binder, such as poly(tetrafluoroethylene) (PTFE), sodium carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), poly(vinylidene fluoride) (PVDF), nitrile rubber (NBR), styrene ethylene butylene styrene copolymer (SEBS), styrene butadiene styrene copolymer (SBS), lithium polyacrylate (LiPAA), sodium polyacrylate (NaPAA), sodium alginate, lithium alginate, ethylene propylene diene monomer (EPDM) and combinations thereof. The conductive material may include a carbon-based material, powdered nickel or other metal particles, or a conductive polymer. The carbon-based material may include, for example, carbon black particles, graphite, acetylene black (e.g., KETCHEN TM Black or DENKA TM Black), carbon fiber and nanotubes, graphene, etc. Examples of conductive polymers include polyaniline, polythiophene, polyacetylene, polypyrrole, etc.
[0069] As described above, during discharge, the negative electrode 22 may contain a relatively high concentration of intercalated lithium, which is oxidized to lithium ions and electrons. The lithium ions may be transported from the negative electrode 22 to the positive electrode 24, for example, through the ion-conducting electrolyte 30 contained in the pores of the intercalated porous separator 26. At the same time, electrons are transported from the negative electrode 22 to the positive electrode 24 via the external circuit 40. These lithium ions may be incorporated into the material of the positive electrode 22 through an electrochemical reduction reaction. After its available capacity is partially or completely discharged, the battery 20 may be recharged or regenerated by an external power source, which reverses the electrochemical reactions that occurred during discharge. However, in various cases, particularly in the case of silicon-containing electroactive materials, a portion of the intercalated lithium remains with the negative electrode 22, such as conversion reactions during the first cycle and / or formation of a solid electrolyte interface (SEI) layer (not shown) on the negative electrode 22, as well as continued lithium loss due to, for example, continuous solid electrolyte interface rupture. This permanent loss of lithium ions may result in reduced specific energy and power in the battery 20. The technology of the present application provides improved electroactive and electrode materials and methods of making them that address these challenges.
[0070] For example, in various aspects, the battery 20 can be lithiated to generate a lithium reserve. The electroactive material (or electrode incorporating the electroactive material) can be lithiated before forming the electrode. In particular, the negative electrode electroactive material (e.g., silicon) can be lithiated before forming the negative electrode 22. For example, a certain amount of lithium pre-lithiation together with an appropriate negative electrode capacity and / or positive electrode capacity ratio (N / P ratio) can be used to control the electrochemical potential within an appropriate window to improve the cycling stability of the battery 20. Pre-lithiation can reduce the potential of the silicon-containing electrode. As a non-limiting example, the lithiation of silicon by direct reaction can be from 3.75 x Li + Si → Li 3.75x Si, where 0 ≤ x ≤ 1 represents (at room temperature), and for the electrochemical lithiation of silicon, it can be expressed as 3.75 x Li + +3.75 x e – + Si → Li 3.75x Si. In each case, the reserved lithium can compensate for lithium loss during cycling, including during the first cycle, to reduce capacity loss over time.
[0071] In further cases, the electroactive material, including the pre-lithiated electroactive material, may include a conductive (protective) coating. For example, Figure 2 A negative electrode electroactive particle 100 is shown, which includes a pre-lithiated electroactive material core 110 and has a conductive coating 120. The negative electrode 22 can be defined by a plurality of such electroactive material particles 100. In particular, such electroactive material particles 100 can be arranged in one or more layers to define the three-dimensional structure of the negative electrode 22.
[0072] like Figure 2 As shown in , the negative electrode electroactive particle 100 comprises a pre-lithiated electroactive material core 110 and a conductive coating 120 disposed on (i.e., surrounding) an exposed surface 112 of the electroactive material core 110. In various aspects, the conductive coating 120 is a continuous layer applied to the surface 112 of the pre-lithiated electroactive material core 110. For example, the conductive coating 120 can cover greater than or equal to about 90% to less than or equal to about 100%, optionally greater than or equal to about 95% to less than or equal to about 100%, and in certain aspects, optionally greater than or equal to about 99% to less than or equal to about 100% of the exposed surface area of the electroactive material core 110. In some cases, the conductive coating 120 can have a thickness of greater than or equal to about 1 nm and less than or equal to about 1000 nm, optionally greater than or equal to about 2 nm and less than or equal to about 20 nm, and in certain variations, optionally greater than or equal to about 3 nm and less than or equal to about 10 nm, for example, about 5 nm.
[0073] The electroactive material core 110 comprises a pre-lithiated electroactive material. The electroactive material may include lithium-silicon and silicon-containing binary and ternary alloys and / or tin-containing alloys, such as Si-Sn, SiSnFe, SiSnAl, SiFeCo, SnO2, etc. Such electroactive materials may undergo significant volume expansion during lithium cycling, such as during lithium ion insertion or lithium alloying. In an initial state before any lithium ion insertion or reaction (e.g., before lithiation), such electroactive material particles may exist in a first or contracted state. After lithium ion insertion (e.g., after lithiation), the lithiated electroactive material particles may exist in a second or expanded state. In the first (contracted) state, the electroactive material particles may include silicon. In the second (expanded) state, the lithiated electroactive material particles (Li) defining the electroactive material core 110 may be present in a second or expanded state. x Si, where 0≤x≤3.75) may have a volume that is up to three times (300%) greater than the volume of the electroactive material particle in the first (contracted) state.
[0074] In certain variations, in the first (contracted) state, the electroactive material particles may have an average particle size (D50) greater than or equal to about 10 nm and less than or equal to about 50 μm, optionally greater than or equal to about 50 nm and less than or equal to about 10 μm, and in certain variations, optionally greater than or equal to about 150 nm and less than or equal to about 5 μm. In the second (expanded) state, the electroactive material particles may have an average particle size (D50) greater than or equal to about 500 nm and less than or equal to about 4 μm, optionally greater than or equal to about 750 nm and less than or equal to about 3 μm, and in certain variations, optionally greater than or equal to about 1 μm and less than or equal to about 3 μm. The electroactive material core 110 may have an average particle size (D50) greater than or equal to about 100 nm and less than or equal to about 20 μm, optionally greater than or equal to about 500 nm and less than or equal to about 5 μm, and in certain variations, optionally greater than or equal to about 1 μm and less than or equal to about 5 μm.
[0075] The conductive coating 120 may be a speckled coating comprising a plurality of first regions 122 and a plurality of second regions 124. Each first region of the plurality of first regions 122 comprises lithium fluoride (LiF). In other cases, the first regions of the plurality of first regions 122 comprise certain oxides and / or nitrides. Each second region of the plurality of second regions 124 comprises one or more conductive metals selected from the group consisting of copper (Cu), aluminum (Al), titanium (Ti), tin (Sn), zirconium (Zr), vanadium (V), hafnium (Hf), zinc (Zn), silicon (Si), lithium (Li), nickel (Ni), manganese (Mn), magnesium (Mg) and combinations thereof. The introduction of the one or more conductive metals reduces the need for conductive additives (conductive materials) within the electrode 22. For example, a battery 20 comprising a negative electrode 22 comprising a plurality of negative electroactive particles 100 may comprise less than or equal to about 1 wt.% of one or more conductive additives. In addition, the presence of the one or more conductive metals may increase the conductivity of the battery 20 and may improve the rate performance of fast charging. The conductivity of the battery 20 should be less than about 1 S / m. The conductive coating 120 generally facilitates charge transfer. In addition, the presence of the protective coating can better passivate the electrode after pre-lithiation occurs, thereby inhibiting electrolyte decomposition and extending battery life.
[0076] Although not shown, it will be appreciated by those skilled in the art that in certain variations, the negative electrode electroactive particles 100 may further include one or more additional coatings, for example disposed on the exposed surface of the conductive coating 120, and in other cases, disposed on the surface of the negative electrode electroactive particles 100 before forming the conductive coating 120. Such additional coatings may provide further stabilization of the lithiated material during transportation and handling. The one or more additional coatings may include, for example, carbon and / or alumina. In the present case, these additional coatings may have improved performance when the underlying conductive coating 120 undergoes volume expansion and contraction. Such additional coatings may be applied to the negative electrode electroactive particles 100 using known methods.
[0077] In various aspects, the present disclosure provides a method for making a negative electrode material, such as Figure 2. The method is a continuous process, generally comprising a first step and a second step, the first step comprising lithiation of the electroactive material, the second step comprising applying a conductive conversion coating ("ECCC"). More specifically, the method may include immersing an electrode comprising a plurality of pre-lithiated electroactive material particles (e.g., pre-lithiated silicon-containing electroactive material particles) in a solution, wherein the solution comprises one or more of copper fluoride (CuF2), titanium tetrafluoride (TiF3 or TiF4), iron fluoride (FeF3), nickel fluoride (NiF2), manganese fluoride (MnF2, MnF3 or MnF4) and vanadium fluoride (VF3, VF4, VF5) in a solvent, such as a low polarity aprotic solvent, such as dimethyl ether (DME), hexane, toluene, etc. The immersion may include, by way of example only, a spraying method and / or a dipping method.
[0078] The method may further include pulling or aspirating the solution into the pores of the electrode (e.g., using vacuum infiltration) and / or drying the electrode (e.g., using vacuum for about 5 minutes) to remove the solvent, during which a conversion reaction occurs to form a surface coating on the exposed surfaces of the pre-lithiated electroactive material particles. The conversion reaction occurs when the pre-lithiated electroactive material particles contact the solution.
[0079] For example, when the solution comprises copper fluoride (CuF2) and the pre-lithiated electroactive material particles are pre-lithiated silicon-containing electroactive material particles, the conversion reaction may be defined by the following formula:
[0080] y(CuF2) + Li x Si → 2y(LiF) + Li (x-2y) Si + yCu
[0081] Where x>2y (eg, 0≤y≤1.875 and 0≤x≤3.75), all copper fluoride (CuF2) and the like are utilized.
[0082] In other cases, for example, when the solution comprises titanium tetrafluoride (TiF4) and the pre-lithiated electroactive material particles are pre-lithiated silicon-containing electroactive material particles, the conversion reaction may be defined by the following formula:
[0083] y(TiF4) + Li x Si → 4y(LiF) + Li (x-4y) Si + 4Ti
[0084] Here, x>4y (eg, 0≤y≤0.9375 and 0≤x≤3.75), so that all titanium tetrafluoride (TiF4) and the like are utilized.
[0085] In further cases, for example, when the solution comprises iron fluoride (FeF3) and the pre-lithiated electroactive material particles are pre-lithiated silicon-containing electroactive material particles, the conversion reaction may be defined by the following formula:
[0086] y(FeF3) + Li x Si → 3y(LiF) + Li (x-3y) Si + 3Fe
[0087] Here, x>4y (eg, 0≤y≤1.25 and 0≤x≤3.75), so that all iron fluoride (FeF3) and the like are utilized.
[0088] In yet other cases, for example, when the solution comprises nickel fluoride (NiF2) and the pre-lithiated electroactive material particles are pre-lithiated silicon-containing electroactive material particles, the conversion reaction may be defined by the following formula:
[0089] y(NiF2) + Li x Si → 2y(LiF) + Li (x-2y) Si + yNi
[0090] Here, x>2y (eg, 0≤y≤1.875 and 0≤x≤3.75), so that all nickel fluoride (NiF2) and the like are utilized.
[0091] In each case, the amount of lithium pre-lithiated into the electroactive material particles (e.g., silicon-containing electroactive material particles) can be controlled so that copper fluoride (CuF2) or the like can react completely while retaining enough lithium for the electroactive material particles to achieve the desired energy density (e.g., >250 wh / kg, >530 wh / l). The lithium fluoride and copper (or the like) together form a protective (conductive) coating, and the lithiated silicon defines the electroactive material core. The lithium fluoride can improve the cycle life performance of an electrochemical cell containing the negative electrode material, while the copper can improve the rate performance of the electrochemical cell. In addition, the lithium fluoride can passivate the lithiated silicon, thereby making the electroactive material particles stable to dry air and inhibiting electrolyte decomposition in the battery.
[0092] like Figure 3 As shown in , in certain variations, the negative electrode material, e.g. Figure 2The negative electrode electroactive particles 100 shown in FIG. 1 can be prepared using a roll-to-roll continuous process in which an electrode precursor material 150 is unwound from a first spool or roll 152, introduced into a reactor 140, and conveyed through a series of reaction chambers 142, 144, 146 before being wound again to form a second roll 154. Those skilled in the art will appreciate that in various cases, the electrode precursor material 150 can be an elongated sheet of prefabricated electrode material that can be wound and unwound as shown, or can be a discrete sheet conveyed on a conveyor or a plurality of electroactive material particles conveyed on a conveyor belt that can be dispensed onto a conveyor and collected after processing in the reactor 140.
[0093] The electrode precursor material 150 may be lithiated in the first reaction chamber 142. In some variations, the lithiation is performed by a thermal evaporation process. During the thermal evaporation process, a vacuum pump (not shown) may be used to maintain a pressure (e.g., <10 -3 Torr). The process uses increased vapor pressure and applied heat to evaporate source material 166 (e.g., lithium metal). The evaporate is deposited on an exposed surface of a substrate (here, an electrode precursor material comprising, for example, silicon) that is typically significantly cooler than the evaporate. For example, a heater 164 may be disposed below source material 166. As the temperature of lithium metal 166 increases (e.g., >50°C higher than its melting point), lithium metal evaporates or volatilizes and lithium molecules 168 are directed and deposited on the exposed surface of electrode precursor material 150. In the case of using a thermal evaporation process, the thickness of the applied layer 162 may be greater than or equal to about 1 μm and less than or equal to about 50 μm, optionally greater than or equal to about 2 μm and less than or equal to about 20 μm, and in certain variations, optionally greater than or equal to about 3 nm and less than or equal to about 10 μm of lithium metal.
[0094] The pre-lithiated electrode material 170 moves from the first reaction chamber 142 to the second reaction chamber 144. In the second reaction chamber 144, as Figure 3 As shown in , the coating precursor 180 is disposed on the exposed surface of the pre-lithiated electrode material 170. The coating precursor 180 may be disposed on the surface of the pre-lithiated electrode material 170 using any known method, such as, by way of example only, a spray coating method or a dipping method. The coating precursor 180 comprises one or more of copper fluoride (CuF2), titanium tetrafluoride (TiF3 or TiF4), iron fluoride (FeF3), nickel fluoride (NiF2), manganese fluoride (MnF2, MnF3 or MnF4) and vanadium fluoride (VF3, VF4, VF5) dissolved in a solvent, such as a low polar aprotic solvent, such as dimethyl ether (DME), hexane, toluene, and the like.
[0095] The pre-lithiated electrode material 170 with the coating precursor 180 is moved from the second chamber 144 to the third reaction chamber 146. In the third reaction chamber 146, a vacuum is generated, and Figure 3 As shown in FIG. 1 , the pre-lithiated electrode material 170 having the coating precursor 180 is heated so that a conversion reaction occurs to form a conductive coating 190 .
[0096] For example, when the solution comprises copper fluoride (CuF2) and the pre-lithiated electroactive material particles are pre-lithiated silicon-containing electroactive material particles, the conversion reaction may be defined by the following formula:
[0097] y(CuF2) + Li x Si → 2y(LiF) + Li (x-2y) Si + yCu
[0098] Where x>2y (eg, 0≤y≤1.875 and 0≤x≤3.75), all copper fluoride (CuF2) and the like are utilized.
[0099] In other cases, for example, when the solution comprises titanium tetrafluoride (TiF4) and the pre-lithiated electroactive material particles are pre-lithiated silicon-containing electroactive material particles, the conversion reaction may be defined by the following formula:
[0100] y(TiF4) + Li x Si → 4y(LiF) + Li (x-4y) Si + 4Ti
[0101] Here, x>4y (eg, 0≤y≤0.9375 and 0≤x≤3.75), so that all titanium tetrafluoride (TiF4) and the like are utilized.
[0102] In further cases, for example, when the solution comprises iron fluoride (FeF3) and the pre-lithiated electroactive material particles are pre-lithiated silicon-containing electroactive material particles, the conversion reaction may be defined by the following formula:
[0103] y(FeF3) + Li x Si → 3y(LiF) + Li (x-3y) Si + 3Fe
[0104] Here, x>4y (eg, 0≤y≤1.25 and 0≤x≤3.75), so that all iron fluoride (FeF3) and the like are utilized.
[0105] In yet other cases, for example, when the solution comprises nickel fluoride (NiF2) and the pre-lithiated electroactive material particles are pre-lithiated silicon-containing electroactive material particles, the conversion reaction may be defined by the following formula:
[0106] y(NiF2) + Li x Si → 2y(LiF) + Li (x-2y) Si + yNi
[0107] Here, x>2y (eg, 0≤y≤1.875 and 0≤x≤3.75), so that all nickel fluoride (NiF2) and the like are utilized.
[0108] In each case, the amount of lithium pre-lithiated into the electroactive material particles (e.g., silicon-containing electroactive material particles) can be controlled so that copper fluoride (CuF2) or the like can react completely while retaining enough lithium for the electroactive material particles to achieve a desired energy density.
[0109] Certain features of the present application's technology are further illustrated in the following non-limiting examples. Example
[0110] An embodiment battery can be prepared according to various aspects of the present disclosure. The embodiment battery can include a pre-lithiated electroactive material with a conductive coating according to various aspects of the present disclosure. For example, the embodiment battery includes a pre-lithiated silicon-containing electroactive material (N / P ratio of about 2) with a conductive coating disposed on a surface thereof, wherein the conductive coating includes a patterned configuration including a plurality of first regions including lithium fluoride and a plurality of second regions including copper.
[0111] A comparative cell can also be prepared. The comparative cell can include a silicon-containing electroactive material that is neither pre-lithiated nor includes a conductive coating.
[0112] Figure 4 The discharge capacity and capacity retention rate of the embodiment battery and the comparative battery are shown. For example, line 200A represents the discharge capacity of the embodiment battery, and line 200B represents the capacity retention rate of the embodiment battery. Line 210A represents the discharge capacity of the comparative battery, and line 210B represents the capacity retention rate of the comparative battery. The x-axis 230 represents the number of cycles. The y-axis 240 represents the discharge capacity (mAh / cm 2 ), and the y2 axis 250 represents the capacity retention rate (%). As shown in the figure, the example battery 200 has a 20% improvement in long-term capacity retention.
[0113] The above description of the embodiments has been provided for the purpose of illustration and description. It is not intended to be exhaustive or to limit the present disclosure. Individual elements or features of a particular embodiment are generally not limited to that particular embodiment, but are interchangeable and can be used in selected embodiments when applicable, even if not explicitly shown or described. It can also be changed in many ways. Such changes are not considered to depart from the present disclosure, and all such modifications are intended to be included within the scope of the present disclosure.
[0114] This application may include the following technical solutions.
[0115] 1. A method for preparing an electrode material for use in an electrochemical cell, the method comprising:
[0116] contacting an electroactive material precursor comprising a plurality of electroactive material particles with a solution to form a conductive coating on each electroactive material particle, wherein the coated electroactive material particles define the electrode material,
[0117] The solution comprises one or more of copper fluoride (CuF2), titanium tetrafluoride (TiF3 or TiF4), iron fluoride (FeF3), nickel fluoride (NiF2), manganese fluoride (MnF2, MnF3 or MnF4) and vanadium fluoride (VF3, VF4, VF5) and a solvent, and the conductive coating comprises a plurality of first regions and a plurality of second regions, the plurality of first regions comprise lithium fluoride, and the plurality of second regions comprise one of copper, titanium, iron, nickel, manganese and vanadium.
[0118] 2. A method according to Scheme 1, wherein the electroactive material precursor is pre-lithiated.
[0119] 3. The method according to Scheme 1, wherein the method further comprises pre-lithiation of the electroactive material precursor.
[0120] 4. The method according to Scheme 1, wherein the electroactive material precursor is pre-lithiated using a thermal evaporation process.
[0121] 5. A method according to Option 1, wherein the electroactive material particles contain silicon.
[0122] 6. The method according to Scheme 1, wherein the solvent is selected from: dimethyl ether, hexane, toluene and combinations thereof.
[0123] 7. The method according to Scheme 1, wherein the contacting is carried out using one of a spraying method and a dipping method.
[0124] 8. The method of claim 1, wherein the method further comprises drying the coated electroactive material particles to remove the solvent.
[0125] 9. The method according to Option 1, wherein the method further comprises applying a vacuum infiltration process to surround the electroactive material precursor with the solution.
[0126] 10. The method of claim 1, wherein the conductive coating is the result of a conversion reaction between the solution and the electroactive material particles.
[0127] 11. The method of claim 10, wherein the electroactive material precursor comprises pre-lithiated silicon, and the solution comprises copper fluoride (CuF2), and the conversion reaction is defined as:
[0128] y(CuF2) + Li x Si → 2y(LiF) + Li (x-2y) Si + yCu
[0129] Where x>2y.
[0130] 12. A method for preparing an electrode material for use in an electrochemical cell, the method comprising:
[0131] pre-lithiating a silicon-containing electroactive material precursor to form a pre-lithiated silicon-containing electroactive material, and
[0132] The pre-lithiated silicon-containing electroactive material is contacted with a solution comprising one or more of copper fluoride (CuF2), titanium tetrafluoride (TiF4), iron fluoride (FeF3), nickel fluoride (NiF2), manganese fluoride (MnF2, MnF3 or MnF4) and vanadium fluoride (VF3, VF4, VF5) and a solvent to form a conductive coating on the pre-lithiated silicon-containing electroactive material, thereby forming a coated pre-lithiated electroactive material defining the electrode material, wherein the conductive coating comprises a plurality of first regions and a plurality of second regions, wherein the plurality of first regions comprise lithium fluoride and the plurality of second regions comprise one of copper, titanium, iron, nickel, manganese and vanadium.
[0133] 13. The method of claim 12, wherein the method further comprises drying the coated pre-lithiated electroactive material to remove the solvent.
[0134] 14. The method of claim 12, wherein the method further comprises applying a vacuum infiltration process to surround the pre-lithiated silicon-containing electroactive material with the solution.
[0135] 15. The method according to Scheme 12, wherein the solvent is selected from: dimethyl ether, hexane, toluene and combinations thereof.
[0136] 16. The method of claim 12, wherein the conductive coating is the result of a conversion reaction between the solution and the pre-lithiated silicon-containing electroactive material.
[0137] 17. The method of claim 16, wherein the solution comprises copper fluoride (CuF2), and the conversion reaction is defined as:
[0138] y(CuF2) + Li x Si → 2y(LiF) + Li(x-2y) Si + yCu
[0139] Where x>2y.
[0140] 18. An electrode material for use in an electrochemical cell, the electrode material comprising a plurality of electroactive material particles, each electroactive material particle comprising:
[0141] an electroactive material core, and
[0142] A conductive coating surrounding the electroactive material core, wherein the conductive coating comprises a plurality of first regions and a plurality of second regions, the plurality of first regions comprising lithium fluoride and the plurality of second regions comprising one of copper, titanium, iron, nickel, manganese and vanadium.
[0143] 19. An electrode material according to Scheme 18, wherein the electroactive material core is a pre-lithiated electroactive material core.
[0144] 20. An electrode material according to Option 18, wherein the thickness of the conductive coating is greater than or equal to about 1 nm and less than or equal to about 50 nm.
Claims
1. A method for preparing an electrode material for an electrochemical cell, the method comprising: Pre-lithiating a silicon-containing electroactive material precursor to form a pre-lithiated silicon-containing electroactive material, the pre-lithiated silicon-containing electroactive material being LixSi, where 0 < x ≤ 3.75, and Contacting the pre-lithiated silicon-containing electroactive material with a solution to form a conductive coating on the pre-lithiated silicon-containing electroactive material, thereby forming a coated pre-lithiated electroactive material defining the electrode material, the solution comprising one or more of copper fluoride (CuF2), titanium tetrafluoride (TiF4), iron fluoride (FeF3), nickel fluoride (NiF2), manganese fluoride, and vanadium fluoride and a solvent, wherein the conductive coating comprises a plurality of first regions and a plurality of second regions, wherein the plurality of first regions comprise lithium fluoride and the plurality of second regions comprise one of copper, titanium, iron, nickel, manganese, and vanadium, and wherein the conductive coating is the result of a conversion reaction between the solution and the pre-lithiated silicon-containing electroactive material.
2. The method according to claim 1, wherein the method further comprises drying the coated pre-lithiated electroactive material to remove the solvent.
3. The method according to claim 1, wherein the method further comprises applying a vacuum infiltration process to surround the pre-lithiated silicon-containing electroactive material with the solution.
4. The method according to claim 1, wherein the solvent is selected from: dimethyl ether, hexane, toluene, and combinations thereof.
5. The method according to claim 1, wherein the solution comprises copper fluoride (CuF2), and the conversion reaction is defined as: y(CuF2)+Li x Si→2y(LiF)+Li (x-2y) Si+yCu where x > 2y.