Collagen-free additive for copper foil processing and copper foil processing technology
Through a collagen-free additive system, including a combination of sulfonate sodium salts, small molecule thioureas and ether derivatives, the problem of difficult control of collagen molecular weight is solved and the high tensile strength and elongation of lithium battery copper foil are achieved. , circumventing the antagonistic effects of numerous additive components, and preparing uniform and fine grain morphology and bright and uniform copper foil.
Patent Information
- Application Number
- CN202211586909.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-09
AI Technical Summary
In the existing lithium battery copper foil additive system, the molecular weight of collagen is difficult to control, resulting in uneven performance of the copper foil. It is difficult to increase the tensile strength and elongation at the same time, and the large number of additive components causes antagonism and affects the performance of the copper foil.
It adopts a collagen-free additive system, including small molecules such as sulfonate sodium salts, thiourea derivatives containing amide bonds, and ether derivatives containing hydrophilic functional groups. The mass concentration ratio is 1:1-2:0.1-0.2 , by adding additives to the Harlem tank flaking electrolyte, performing air circulation stirring and low-temperature annealing processes to prepare copper foil with high tensile strength and elongation.
It avoids the adverse effects of collagen molecular weight on the performance of copper foil, reduces the number of additive components, and achieves high tensile strength and elongation of copper foil, improved mechanical properties, uniform grain morphology, and uniform foil surface brightness.
Smart Images

Figure CN115838948B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium battery copper foil additives, and in particular, relates to a collagen-free additive for copper foil processing and a copper foil processing technology. Background Art
[0002] With the rapid development of the electric vehicle industry, copper foil, as one of the important basic materials for new energy power lithium batteries, is in increasing demand, and the requirements for its quality and performance are also increasing. Excellent comprehensive mechanical properties can make the battery less likely to break during operation, and improve the battery capacity and safety. At present, the tensile strength of conventional 6μm copper foil is 32-35kgf / mm 2 , and the elongation is 5%-8%. According to current literature reports, when the copper foil properties are regulated by additive technology, the tensile strength and elongation often show opposite trends. Therefore, improving the tensile strength and elongation of copper foil at the same time has become an urgent problem to be solved in the field of copper foil mechanical properties research.
[0003] Collagen is the most commonly used inhibitory additive in the production of lithium battery copper foil. Its molecular weight will affect the surface morphology and grain shape of the copper foil. When the adsorption area on the cathode surface is large, the rough surface of the copper foil is hilly and the grains are uniform and small; when the molecular weight is small, the adsorption area is small, the rough surface of the copper foil is cone-shaped, and the grain morphology is uneven. Since the molecular weight of collagen is difficult to control, it will have an adverse effect on the performance of the copper foil.
[0004] At present, there are many additive components in the research of lithium battery copper foil additive systems. In addition to the common promoters and inhibitors, the system also includes crystal refiners, surface wetting agents, dispersants, etc. According to literature reports, the effects of various additives on the copper ion deposition process are synergistic, but there are also antagonistic effects between some additives. This makes it adversely affected on the performance of copper foil when there are too many types of additives in the system. In addition, it will also make it difficult to control the content of a single additive. Summary of the invention
[0005] The purpose of the present invention is to provide a collagen-free additive for copper foil processing and a copper foil processing process, which solves the problems existing in the prior art.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A collagen-free additive for copper foil processing is composed of small molecules of sodium sulfonate salts, thiourea derivatives containing amide bonds and ether derivatives containing hydrophilic functional groups; the mass concentration ratio of the small molecules of sodium sulfonate salts, the thiourea derivatives containing amide bonds and the ether derivatives containing hydrophilic functional groups is 1:1-2:0.1-0.2.
[0008] Furthermore, the small molecule of the sodium sulfonate salt is one of sodium polydisulfide propane sulfonate, sodium 3-mercaptopropane sulfonate, and sodium 2-mercaptoethyl sulfonate.
[0009] Furthermore, the thiourea derivative containing an amide bond is one of malonylthiourea, 3-methyl-1-(2-phenylacetamido)thiourea, and 1-acetyl-3-phenylthiourea.
[0010] Furthermore, the ether derivative containing a hydrophilic functional group is one of diethylene glycol dimethyl ether, ethylene glycol butyl ether, and triethylene glycol divinyl ether.
[0011] A copper foil processing process comprises the following steps:
[0012] Step S1, preparing 1.5L electrolyte for Haring cell sheeting, adding a collagen-free additive for copper foil processing into the electrolyte, wherein the 1.5L electrolyte contains 10ppm of small molecules of sodium sulfonate salt, and performing aeration circulation stirring;
[0013] Step S2, set the reaction time, reaction current, control the cell pressure, and start preparing the sample copper foil. After completion, turn off the power, take out the titanium cathode, put it in deionized water to wash for 5 seconds, and use a utility knife to manually peel off the copper foil;
[0014] Step S3, placing the prepared copper foil into an annealing furnace for low-temperature annealing process;
[0015] Step S4: Cut the prepared sample into 100mm×50mm samples with a sampling plate, and then cut it into 3 100mm×15mm strips with a cutting knife, and finally test the tensile strength and elongation with a universal testing machine. The tensile strength of the copper foil can reach 37kgf / mm 2 , the elongation can reach 8%.
[0016] Furthermore, in step S1, the sulfuric acid concentration in the electrolyte is 90-120 g / L, the copper ion concentration is 80-100 g / L, the chloride ion concentration is 10-50 mg / L, and the electrolyte temperature is 50-60°C.
[0017] Furthermore, in step S2, the reaction time is 50 s, the reaction current is 26.5 A, and the cell voltage is 4.5-5.5 V.
[0018] Furthermore, the low temperature annealing process in step S3 includes the following steps: placing the copper foil in an annealing furnace and heating it to 60-90° C. within 3-5 hours; keeping warm: keeping the copper foil in the annealing furnace for 1-2 hours; cooling: slowly cooling the copper foil in the furnace for 3-5 hours and then taking it out.
[0019] Beneficial effects of the present invention:
[0020] The present invention attempts to use an additive system that does not contain collagen macromolecules, thereby avoiding the adverse effects on the performance of copper foil caused by the difficulty in controlling and uneven molecular weight of collagen; reducing the number of components in the additive system, avoiding the antagonistic effects between the numerous additive components, and facilitating the regulation of the content of each additive component. The prepared lithium battery copper foil has uniform grain morphology and fine size, and has high tensile strength and high elongation.
[0021] The additive components in the collagen-free additive process of the present invention include small molecules of sodium sulfonate salts, thiourea derivatives containing amide bonds, and ether derivatives containing hydrophilic functional groups, which avoids the difficulty in controlling the molecular weight of collagen and the adverse effects on the performance of copper foil; there are only three components in the additive system, and it is easy to adjust the content of each additive component; the prepared lithium battery copper foil has uniform grain morphology, small size, bright and uniform foil surface, and the tensile strength of the copper foil mechanical properties can reach 37kgf / mm 2 , the elongation can reach 8%. In order to avoid the uncontrolled molecular weight of collagen and the adverse effects on the performance of copper foil, it is easy to adjust the content of each additive component, and at the same time provide a solution to improve the tensile strength and elongation of copper foil. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0023] Figure 1 This is an appearance diagram of the rough surface of the copper foil sample prepared in Example 1 of the present invention.
[0024] Figure 2 This is a 3D microscope image of the rough surface of the copper foil prepared in Example 1 of the present invention.
[0025] Figure 3 This is a SEM image of the rough surface of the copper foil prepared in Example 1 of the present invention.
[0026] Figure 4 This is a SEM image of the tensile cross-section of the copper foil prepared in Example 1 of the present invention.
[0027] Figure 5 This is an appearance diagram of the rough surface of the copper foil sample prepared in Comparative Example 1 of the present invention.
[0028] Figure 6 This is a 3D microscope image of the rough surface of the copper foil prepared in Comparative Example 1 of the present invention.
[0029] Figure 7This is a SEM image of the rough surface of the copper foil prepared in Comparative Example 1 of the present invention.
[0030] Figure 8 This is a SEM image of the tensile cross-section of the copper foil prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] A collagen-free additive for copper foil processing is composed of small molecules of sodium sulfonate salts, thiourea derivatives containing amide bonds and ether derivatives containing hydrophilic functional groups; the mass concentration ratio of the small molecules of sodium sulfonate salts, the thiourea derivatives containing amide bonds and the ether derivatives containing hydrophilic functional groups is 1:(1-2):(0.1-0.2).
[0033] Furthermore, the small molecule of the sodium sulfonate salt is one of sodium polydisulfide propane sulfonate, sodium 3-mercaptopropane sulfonate, and sodium 2-mercaptoethyl sulfonate.
[0034] Furthermore, the thiourea derivative containing an amide bond is one of malonylthiourea, 3-methyl-1-(2-phenylacetamido)thiourea, and 1-acetyl-3-phenylthiourea.
[0035] Furthermore, the ether derivative containing a hydrophilic functional group is one of diethylene glycol dimethyl ether, ethylene glycol butyl ether, and triethylene glycol divinyl ether.
[0036] A copper foil processing process comprises the following steps:
[0037] Step S1, preparing electrolyte for Haring slot filming, adding collagen-free additive for copper foil processing into the electrolyte, aerating and circulating with stirring, and controlling the temperature at 50-60°C;
[0038] Step S2, set the reaction time, reaction current, control the cell pressure, and start preparing the sample copper foil. After completion, turn off the power, take out the titanium cathode, put it in deionized water to wash for 5 seconds, and use a utility knife to manually peel off the copper foil;
[0039] Step S3, placing the prepared copper foil into an annealing furnace for a low-temperature annealing process;
[0040] Step S4, cutting the prepared sample into 100 mm × 50 mm samples with a sampling plate, and then cutting it into 3 100 mm × 15 mm strips with a cutting knife, and finally testing the tensile strength and elongation with a universal testing machine.
[0041] Furthermore, in step S1, the sulfuric acid concentration in the electrolyte is 90-120 g / L, the copper ion concentration is 80-100 g / L, the chloride ion concentration is 10-50 mg / L, and the electrolyte temperature is 50-60°C.
[0042] Furthermore, in step S2, the reaction time is 50 s, the reaction current is 26.5 A, and the cell voltage is 4.5-5.5 V.
[0043] Furthermore, the low temperature annealing process in step S3 includes the following steps: placing the copper foil in an annealing furnace and heating it to 60-90° C. within 3-5 hours; keeping warm: keeping the copper foil in the annealing furnace for 1-2 hours; cooling: slowly cooling the copper foil in the furnace for 3-5 hours and then taking it out.
[0044] Example 1
[0045] A copper foil processing process comprises the following steps:
[0046] 1.5L electrolyte was prepared for Haring cell filming. The sulfuric acid concentration in the electrolyte was 100g / L, the copper ion concentration was 80g / L, and the chloride ion concentration was 40mg / L. The corresponding additives, sodium polydisulfide propane sulfonate, malonylacetyl thiourea, and diethylene glycol dimethyl ether were added to the electrolyte at a certain mass concentration ratio of 1:2:0.2, and the aeration circulation was stirred. The temperature was controlled at 55°C. The reaction time was set to 50s, the reaction current was 26.5A, and the cell pressure was controlled to 4.5-5.5v to start preparing the sample copper foil. After completion, the power was turned off, the titanium cathode was taken out, and it was washed in deionized water for 5s. The copper foil was manually peeled off using a utility knife. The prepared copper foil was placed in an annealing furnace for a low-temperature annealing process. The low-temperature annealing process includes heating: the copper foil was placed in the annealing furnace and heated to 70°C within 3h; heat preservation: the copper foil was kept in the annealing furnace for 2h; cooling: the copper foil was slowly cooled with the furnace for 4h and then taken out. The prepared samples were cut into 100 mm × 50 mm samples with a sampling plate, and then cut into three 100 mm × 15 mm strips with a cutting knife. Finally, the tensile strength and elongation were tested with a universal testing machine.
[0047] Example 2
[0048] A copper foil processing process comprises the following steps:
[0049] 1.5L electrolyte was prepared for Haring cell filming. The sulfuric acid concentration in the electrolyte was 100g / L, the copper ion concentration was 80g / L, and the chloride ion concentration was 40mg / L. The corresponding additives sodium 3-mercaptopropane sulfonate, 3-methyl-1-(2-phenylacetamido)thiourea, and ethylene glycol butyl ether were added to the electrolyte at a certain mass concentration ratio of 1:2:0.2, and the aeration circulation was stirred. The temperature was controlled at 55℃; the reaction time was set to 50s, the reaction current was 26.5A, and the cell pressure was controlled to 4.5-5.5v to start preparing the sample copper foil. After completion, the power was turned off, the titanium cathode was taken out, and it was washed in deionized water for 5s. The copper foil was manually peeled off using a utility knife. The prepared copper foil was placed in an annealing furnace for a low-temperature annealing process. The low-temperature annealing process includes heating: the copper foil was placed in the annealing furnace and heated to 70℃ within 3h; heat preservation: the copper foil was kept in the annealing furnace for 2h; cooling: the copper foil was slowly cooled with the furnace for 4h and then taken out. The prepared samples were cut into 100 mm × 50 mm samples with a sampling plate, and then cut into three 100 mm × 15 mm strips with a cutting knife. Finally, the tensile strength and elongation were tested with a universal testing machine.
[0050] See also Figure 1-Figure 4 As shown:
[0051] Figure 1 This is the appearance of the rough surface of the copper foil sample prepared in Example 1 without collagen additives. The surface of the sample is bright and uniform. Its tensile strength is 37kgf / mm 2 , elongation 7%, glossiness reaches 250.
[0052] Figure 2 The 3D microscope images of the rough surface of the copper foil sample prepared by the process without collagen additive in Example 1 are (a) 500 times and (b) 1000 times. The rough surface is uniformly hilly and has no abnormally grown copper nodules, reflecting that the process method without collagen additive in Example 1 makes the copper ion deposition behavior uniform.
[0053] Figure 3 This is a SEM image of the rough surface of the copper foil sample prepared by processing without collagen additive in Example 1. The grain morphology of the rough surface is uniform and fine, without agglomeration. This reflects that the process method without collagen additive in Example 1 avoids the influence of different molecular weights of collagen on the performance of copper foil.
[0054] Figure 4 This is a SEM image of the tensile section of the copper foil sample prepared without collagen additive in Example 1. There is a sharp split tip in the middle of the tensile section, and the slip patterns on both sides are clearly visible, which belongs to the slip separation fracture, and the entire fracture form is mainly ductile fracture.
[0055] Comparative Example 1
[0056] A copper foil processing process comprises the following steps:
[0057] 1.5L electrolyte was prepared for Haring trough filming. The sulfuric acid concentration in the electrolyte was 100g / L, the copper ion concentration was 80g / L, and the chloride ion concentration was 40mg / L. The corresponding additive components of sodium polydisulfide propane sulfonate, collagen, and polyethylene glycol were added to the electrolyte at a certain mass concentration ratio of 1:2:0.2, and the aeration circulation was stirred. The temperature was controlled at 55℃; the reaction time was set to 50s, the reaction current was 26.5A, and the trough pressure was controlled to 4.5-5.5v to start preparing the sample copper foil. After completion, the power was turned off, the titanium cathode was taken out, and it was washed in deionized water for 5s. The copper foil was peeled off manually using a utility knife. The prepared copper foil was placed in an annealing furnace for a low-temperature annealing process. The low-temperature annealing process was heating: the copper foil was placed in the annealing furnace and heated to 70℃ within 3h; heat preservation: the copper foil was kept in the annealing furnace for 2h; cooling: the copper foil was slowly cooled with the furnace for 4h and then taken out. The prepared samples were cut into 100 mm × 50 mm samples with a sampling plate, and then cut into three 100 mm × 15 mm strips with a cutting knife. Finally, the tensile strength and elongation were tested with a universal testing machine.
[0058] Comparative Example 2
[0059] A copper foil processing process comprises the following steps:
[0060] 1.5L electrolyte was prepared for Haring cell filming. The sulfuric acid concentration in the electrolyte was 100g / L, the copper ion concentration was 80g / L, and the chloride ion concentration was 40mg / L. The corresponding additive components N,N-dimethyl-dithiocarbonyl propane sulfonate sodium, collagen, and polyoxyethylene alkyl ether were added to the electrolyte at a certain mass concentration ratio of 1:2:0.2, and the aeration circulation was stirred. The temperature was controlled at 55°C; the reaction time was set to 50s, the reaction current was 26.5A, and the cell pressure was controlled to 4.5-5.5v to start preparing the sample copper foil. After completion, the power was turned off, the titanium cathode was taken out, and it was washed in deionized water for 5s. The copper foil was peeled off manually using a utility knife. The prepared copper foil was placed in an annealing furnace for a low-temperature annealing process. The low-temperature annealing process was heating: the copper foil was placed in the annealing furnace and heated to 70°C within 3h; heat preservation: the copper foil was kept in the annealing furnace for 2h; cooling: the copper foil was slowly cooled with the furnace for 4h and then taken out. The prepared samples were cut into 100 mm × 50 mm samples with a sampling plate, and then cut into three 100 mm × 15 mm strips with a cutting knife. Finally, the tensile strength and elongation were tested with a universal testing machine.
[0061] See also Figure 5-Figure 8 As shown:
[0062] Figure 5 This is the appearance picture of the rough surface of the copper foil sample in Comparative Example 1. The surface of the sample is bright but uneven.
[0063] Figure 6 These are 3D microscope images of the rough surface of the copper foil sample in Comparative Example 1 (a) 500 times and (b) 1000 times; the rough surface is unevenly hilly and has abnormally large copper nodules.
[0064] Figure 7 This is a SEM image of the rough surface of the copper foil sample in comparative example 1. The grains on the rough surface are fine, but the foil surface is uneven compared with the copper foil sample in example 1. This reflects that the additive system containing collagen will be affected by the molecular weight of collagen, resulting in uneven deposition of copper ions.
[0065] Figure 8 This is a SEM image of the tensile fracture of the copper foil sample in Example 1. The copper foil mainly undergoes slip deformation, and the amount of deformation produced is smaller than that in Example 1, so the elongation is also low.
[0066] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0067] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A collagen-free additive for copper foil processing, characterized in that: It is composed of small molecules of sodium sulfonate salt, thiourea derivatives containing amide bonds and ether derivatives containing hydrophilic functional groups; the mass concentration ratio of small molecules of sodium sulfonate salt, thiourea derivatives containing amide bonds and ether derivatives containing hydrophilic functional groups is 1:1-2:0.1-0.2; The small molecule of the sodium sulfonate salt is one of sodium polydisulfide propane sulfonate, sodium 3-mercaptopropane sulfonate, and sodium 2-mercaptoethyl sulfonate; The thiourea derivative containing an amide bond is one of malonylthiourea, 3-methyl-1-(2-phenylacetamido)thiourea, and 1-acetyl-3-phenylthiourea; The ether derivative containing a hydrophilic functional group is one of diethylene glycol dimethyl ether, ethylene glycol butyl ether and triethylene glycol divinyl ether.
2. A copper foil processing process using the additive according to claim 1, characterized in that: The steps include: Step S1, preparing electrolyte for Haring slot filming, adding collagen-free additive for copper foil processing into the electrolyte, and aerating and circulating the electrolyte with stirring; Step S2, setting the reaction time, reaction current, controlling the cell pressure, and preparing the sample copper foil; after completion, turning off the power supply, taking out the titanium cathode, washing it in deionized water for 5 seconds, and manually peeling off the copper foil using a utility knife; Step S3: placing the prepared copper foil into an annealing furnace for low-temperature annealing treatment.
3. The copper foil processing process according to claim 2, characterized in that: In step S1, the sulfuric acid concentration in the electrolyte is 90-120 g / L, the copper ion concentration is 80-100 g / L, the chloride ion concentration is 10-50 mg / L, and the electrolyte temperature is 50-60°C.
4. The copper foil processing process according to claim 2, characterized in that: In step S2, the reaction time is 50 s, the reaction current is 26.5 A, and the cell voltage is 4.5-5.5 V.
5. The copper foil processing process according to claim 2, characterized in that: Step S3: Low temperature The annealing process includes the following steps: placing the copper foil in an annealing furnace and heating it to 60-90°C within 3-5 hours; Insulation: Keep the copper foil in the annealing furnace for 1-2 hours; Cooling: Slowly cool the copper foil in the furnace for 3-5 hours and then take it out.
Citation Information
Patent Citations
Additive used for reducing voids generated after annealing of through-silicon-via copper plating
CN103397354A
Anti-creasing copper foil, electrode comprising same, secondary battery comprising same, and manufacturing method therefor
CN110997983A
Electrolytic copper foil, electric component and battery including the same
EP3067442A1
Electrolytic copper foil, electric component and battery comprising the foil and preparation method thereof
KR1020150062230A
KR20190009048A