A high-stability bath lubricating softener and preparation method thereof

Through a high-stability bath lubricant in a high-stability bath combination of acrylate polymers and silicone oil, the wrinkle printing and crease problems of fabrics in the dyeing and wetting process are solved, and the washing and shear resistance of the fabric is achieved. It also maintains the color and fastness of the fabric, improving the quality of the fabric.

CN116219753BActive Publication Date: 2024-11-29JIANGSU YUDAO BIOLOGICAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310263792.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-01
Publication Date
2024-11-29
Estimated Expiration
2043-03-01

AI Technical Summary

Technical Problem

The existing lubricating softener in the bath causes wrinkles, creases, abrasions, wear and other problems in the dyeing and wetting process, and has poor stability, affecting the quality of the fabric.

Method used

Using a combination of acrylate polymers, silicone oils, surfactants and emulsifiers, a high-stability bath lubricating softener is prepared through homogeneous emulsification technology, which gives the fabrics a wash-resistant, shear-resistant, high-temperature-resistant and salt-alkali-resistant properties. And bathe with the fixing agent to stabilize to avoid affecting the color and fastness of the dyed fabric.

Benefits of technology

Achieve excellent in-bath lubrication and softness, reducing friction between fabric and equipment, the fabric still maintains a good feel after washing, and improves the durability and stability of the fabric, avoiding color and fastness Influence.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004132331380000101
    Figure BDA0004132331380000101
  • Figure BDA0004132331380000111
    Figure BDA0004132331380000111
  • Figure BDA0004132331380000112
    Figure BDA0004132331380000112
Patent Text Reader

Abstract

The invention provides a high-stability bath lubricating softener and a preparation method thereof, and relates to the technical field of textile printing and dyeing auxiliaries. The softener comprises components of an acrylate polymer, silicone oil, a surfactant, an emulsifier, an antibacterial agent, a pH regulator and water; acrylic acid is reacted with an acrylic monomer and maleic anhydride to prepare an acrylate polymer; the acrylate polymer and the silicone oil are fully dispersed under the action of the surfactant and the emulsifier; after reacting at 45-60°C, they are fully homogenized and emulsified to obtain a softener with excellent bath lubrication and softening effects, and imparts washing resistance, shear resistance, high temperature resistance and salt-alkali resistance to fabrics; the softener is stable when bathed with a color fixing agent, and does not affect the fastness and color of dyed fabrics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile printing and dyeing auxiliaries, and particularly relates to a high-stability bath lubricating softener and a preparation method thereof. Background Art

[0002] At present, with the increasing demand for textiles, there are more and more types and structures of fabrics, including single fiber, composite materials, blended interweaving, etc., and the development of fabrics tends to be more advanced and complicated. Although in the wet process of dyeing and finishing, corresponding mechanical equipment will be used according to various fabric types and different fabric structures, the friction between fabrics and fabrics, fabrics and equipment, and the contact between them are increased due to the increasing efficiency, small bath ratio, and large capacity of processing methods, which easily causes wrinkles, creases, scratches and wear on the fabrics. The swelling of fabrics such as rayon will significantly aggravate the above problems. Especially in some heavy and dense fabrics, the above problems are more serious, which seriously affects the quality of the fabrics.

[0003] In order to reduce wrinkles, creases, scratches and wear on fabrics, some studies have used resin treatment, non-ironing and anti-wrinkle treatment, etc. to make the fabrics have good stiffness or resilience. However, some treatments will release formaldehyde during the finishing process, causing harm and pollution to the human body and the environment, and losing the natural friendliness of the fabrics; moreover, some fabrics will become hard after finishing, losing their softness and comfort, and their stability will deteriorate. Therefore, researchers have gradually turned their attention to softeners that can give fabrics a good feel to improve the quality of fabrics.

[0004] Conventional lubricating softeners on the market currently have the following problems: (1) The lubricating effect is not good, and wrinkles, creases, scratches and wear and tear will still occur during the fabric processing and production process; (2) The fabric is hard and rough after washing; (3) The stability is poor, and problems such as demulsification and roller sticking are easily caused during use; (4) It will affect the color and fastness of the fabric, seriously affecting the quality of the final fabric. In order to solve some of the problems caused by the softener itself, the development of a highly stable lubricating softener has a very broad prospect.

[0005] Chinese invention patent CN107904954B discloses a stiffening softener for cotton and a preparation method thereof. The softener of the invention is composed of block silicone oil, modified polyurethane emulsion, polyacrylate, surfactant, isopropyl palmitate, polyglycerol fatty acid ester, alkyl polyglycoside, crosslinking agent, preservative and deionized water. The invention adopts block silicone oil and hydroxyl-modified polyurethane emulsion synthesized by end epoxy double-capping method to penetrate into the fiber, reduce the film formation on the fiber surface, so that the fabric has stiffness and a full and fluffy feel, and the water absorption is significantly improved.

[0006] In addition, Chinese invention patent CN108049186A discloses a branched hydrophobic feel finishing agent prepared from acrylate and reactive silicone oil and a preparation method thereof; the feel finishing agent includes acrylate emulsion and silicone oil. After the above components are synthesized, a branched acrylate / silicone oil system is obtained by introducing a mercapto reactive group and grafting with acrylate. The above system is treated with a fabric sample through an immersion / padding process to obtain a fabric covered with an acrylic acid / reactive silicone oil branched structure, so that the fabric has excellent waterproof, washable, and wear-resistant properties, and at the same time has a soft feel.

[0007] This patented product is a highly stable bath lubricating softener obtained by fully dispersing acrylic polymers and silicone oil under the action of surfactants and emulsifiers and homogenizing and emulsifying. The product has excellent bath lubrication effect and washability, and has extremely high stability, self-emulsification, and is easy to use without affecting the color and fastness of dyed fabrics. Summary of the invention

[0008] The invention aims at the problems existing in the prior art and provides a high-stability bath lubricating softener and a preparation method thereof. The softener comprises components of acrylic polymer, silicone oil, surfactant, emulsifier, antibacterial agent, pH regulator and water. The acrylic polymer and silicone oil are fully dispersed under the action of the surfactant and the emulsifier, and homogenized and emulsified to obtain a softener with excellent bath lubrication and softening effects, and imparts washing resistance, shear resistance, high temperature resistance and salt and alkali resistance to fabrics. The softener is stable when bathed with a color fixing agent and does not affect the fastness of dyed fabrics.

[0009] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0010] On the one hand, the present invention provides a high-stability bath lubricating softener, which includes the following components in parts by weight: 3-25 parts of acrylic polymer, 5-15 parts of silicone oil, 1-10 parts of surfactant, 5-20 parts of emulsifier, 0.1-0.5 parts of antibacterial agent, 0.1-0.5 parts of pH regulator and 40-80 parts of water.

[0011] Preferably, the softener comprises the following components in parts by weight: 10-22 parts of acrylic polymer, 8-12 parts of silicone oil, 2-8 parts of surfactant, 10-15 parts of emulsifier, 0.2-0.4 parts of antibacterial agent, 0.2-0.4 parts of pH regulator and 50-60 parts of water.

[0012] More preferably, the softener comprises the following components in parts by weight: 16 parts of acrylic polymer, 12 parts of silicone oil, 5 parts of surfactant, 12 parts of emulsifier, 0.3 parts of antibacterial agent, 0.2 parts of pH adjuster and 54.5 parts of water.

[0013] Preferably, the acrylic polymer comprises the following components in parts by weight: 50-80 parts of acrylic acid, 15-30 parts of acrylic monomers, 1-5 parts of maleic anhydride, 1-5 parts of dispersant, 1-5 parts of hydrogen peroxide and 80-120 parts of water.

[0014] Further preferably, the acrylic acid ester monomer is selected from at least one of long-chain methyl acrylate, long-chain ethyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-octyl acrylate and decyl acrylate.

[0015] Further preferably, the dispersant is selected from at least two of fatty alcohol polyoxyethylene ether, polyoxyethylene stearate, triethanolamine borate, methylcellulose, and polyethylene glycol.

[0016] More preferably, the dispersant is a mixture of fatty alcohol polyoxyethylene ether and polyoxyethylene stearate, with a weight ratio of 1:0.5-2.

[0017] Preferably, the method for preparing the acrylic polymer comprises the steps of:

[0018] (1) preparing acrylic acid into a solution with a concentration of 50-80%, and uniformly mixing the solution with an acrylic acid monomer to obtain a mixture 1;

[0019] (2) the dispersant and the remaining weight portion of water are fully stirred and dispersed, and fully mixed with maleic anhydride to obtain a dispersion solution;

[0020] (3) After the mixture 1 and the dispersion solution are heated to 60-80° C., hydrogen peroxide is added dropwise. After the addition is completed, the mixture is kept warm for reaction for 2-3 hours to obtain an acrylic ester polymer.

[0021] Further preferably, in step (3), the heating rate is 2-3°C / min, and the temperature is raised to 65-75°C.

[0022] Further preferably, in step (3), the dripping speed is 0.5-3 mL / s, and the dripping is completed within 3 hours.

[0023] Preferably, the silicone oil is selected from at least two of octamethylcyclotetrasiloxane, N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane, mercaptomethyldimethoxysilane, and aminomethyldimethoxysilane.

[0024] More preferably, the silicone oil is selected from at least two of octamethylcyclotetrasiloxane, N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane, and mercaptomethyldimethoxysilane.

[0025] More preferably, the silicone oil is a mixture of octamethylcyclotetrasiloxane and N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane in a mass ratio of 1:0.5-1.5; or the silicone oil is a mixture of octamethylcyclotetrasiloxane and aminomethyldimethoxysilane in a mass ratio of 1:0.5-2.

[0026] Preferably, the surfactant is selected from at least one of anionic surfactants and nonionic surfactants.

[0027] More preferably, the surfactant is an anionic surfactant.

[0028] More preferably, the anionic surfactant is selected from at least one of sodium dodecylbenzene sulfonate, distearyl succinic acid sulfonate, monoethanolamine salt of fatty alcohol sulfate, and sodium lauryl sulfate.

[0029] More preferably, the anionic surfactant is selected from at least one of distearyl succinic acid sulfonate, monoethanolamine salt of fatty alcohol sulfate, and sodium lauryl sulfate.

[0030] Preferably, the emulsifier is selected from at least one of fatty alcohol polyoxyethylene ether (AEO), isomeric alcohol polyoxyethylene ether, polyoxyethylene stearate, triethanolamine borate, methylcellulose and polyethylene glycol.

[0031] Further preferably, the emulsifier is a mixture of fatty alcohol polyoxyethylene ether and polyoxyethylene stearate, and the mass ratio thereof is 1:0.1-1.

[0032] More preferably, the emulsifier is a mixture of fatty alcohol polyoxyethylene ether and polyoxyethylene stearate, with a mass ratio of 1:0.3-0.5.

[0033] Preferably, the antibacterial agent refers to a substance having antibacterial and / or bacterial growth inhibitory effects, including but not limited to chitin antibacterial agents, silver ion antibacterial agents, quaternary ammonium salts, and chlorobenzimidazole antibacterial agents.

[0034] Preferably, the pH regulator is an alkaline solution with a concentration of 10-30%. The function of the pH regulator is to control the pH of the softener to be maintained at a neutral or weakly alkaline condition and adjust the pH to 7-8. The amount of the pH regulator added is subject to actual pH detection.

[0035] In another aspect, the present invention provides a method for preparing the above-mentioned softener, comprising the steps of:

[0036] S1. Evenly mix silicone oil, pH regulator and water, stir and react at 70-80°C for 1-5h to obtain a silicone oil mixture, and keep warm;

[0037] S2, mixing the silicone oil mixture and the emulsifier evenly with heat preservation to obtain a silicone oil-emulsion mixture;

[0038] S3, cooling the silicone oil-emulsion mixture to 45-60° C., stirring and reacting with the acrylic polymer for 1-5 hours to obtain a mixture 1, and keeping the mixture warm;

[0039] S4. The mixture 1 is stirred evenly with the surfactant, homogenized and emulsified, then naturally cooled to room temperature, and mixed with the antibacterial agent to obtain a softener.

[0040] Preferably, in step S1, the reaction temperature is 75-78°C and the reaction time is 2-4h.

[0041] Preferably, in step S3, the cooling temperature is 45-50° C., and the reaction time is 3-5 hours.

[0042] Preferably, the stirring speeds in step S1 and step S3 are consistent, both are low-speed stirring, and the stirring rate is 100-200 rpm / min.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] 1. The softener of the present invention has a reasonable formula, and the components cooperate with each other. The specific surfactant and emulsifier are compounded, and the combination thereof with silicone oil gives the fabric an excellent lubricating effect in the bath, effectively reducing the mutual friction between fabrics and fabrics, and between fabrics and equipment; and the softening effect in the bath is excellent, which can effectively prevent the generation of creases, scratches, stacking marks, etc. during wet processing.

[0045] 2. The present invention polymerizes acrylic acid to modify the prepared acrylic ester polymer, which has good dispersibility and stability, and imparts salt and alkali resistance to the softener and stability to the co-bath of additives such as the color fixer.

[0046] 3. The softener of the present invention, the acrylic polymer, under the interaction of silicone oil, surfactant and emulsifier, has excellent wash resistance and can still maintain a good hand feel after washing; and will not affect the color and fastness of dyed fabrics; the softener also has excellent shear resistance and high temperature resistance for fabrics. DETAILED DESCRIPTION

[0047] The following non-limiting examples can enable those skilled in the art to more fully understand the present invention, but do not limit the present invention in any way. The following content is merely an exemplary description of the scope of protection claimed in this application, and those skilled in the art can make various changes and modifications to the invention of this application based on the disclosed content, which should also fall within the scope of protection claimed in this application.

[0048] The present invention is further described below by way of specific examples. Unless otherwise specified, the various chemical reagents used in the examples of the present invention are obtained through conventional commercial channels.

[0049] In the technical effect test, the conventional bath lubricant softener 1 used was purchased from Meigao with the product number of bath softener M-287; the conventional bath lubricant softener 2 was purchased from Tuona with the product number of bath lubricant TMC.

[0050] Example 1

[0051] The softener comprises the following components in parts by weight (based on 100 parts): 16 parts of acrylic polymer, 12 parts of silicone oil (8 parts of octamethylcyclotetrasiloxane + 4 parts of N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane), 5 parts of anionic surfactant (disteadecyl succinic acid sulfonate), 12 parts of emulsifier (9 parts of fatty alcohol polyoxyethylene ether + 3 parts of polyoxyethylene stearate), 0.3 parts of quaternary ammonium salt antibacterial agent, 0.2-0.4 parts of 20% NaOH solution and the balance of water.

[0052] Among them, the components of the acrylic polymer in parts by weight are: 60 parts of acrylic acid, 20 parts of acrylic ester monomer (n-butyl acrylate), 2 parts of maleic anhydride, 3 parts of dispersant (a mixture of fatty alcohol polyoxyethylene ether and polyoxyethylene stearate, with a weight ratio of 1:2), 3 parts of hydrogen peroxide and 100 parts of water.

[0053] The preparation method of acrylic acid ester polymer comprises the steps of:

[0054] (1) preparing a solution of acrylic acid with a concentration of 60%, and uniformly mixing the solution with an acrylic acid monomer to obtain a mixture 1;

[0055] (2) the dispersant and the remaining weight portion of water are fully stirred and dispersed, and fully mixed with maleic anhydride to obtain a dispersion solution;

[0056] (3) The mixture 1 and the dispersion solution were heated to 70° C. at a rate of 3° C. / min, and hydrogen peroxide was added dropwise. After the addition was completed within 3 hours, the mixture was kept warm for 2.5 hours to obtain an acrylic polymer.

[0057] The preparation method of the softener comprises the steps of:

[0058] S1. Mix silicone oil, pH regulator and water evenly, stir and react at 75-78°C for 3 hours at a stirring rate of 120 rpm / min to obtain a silicone oil mixture, and keep warm;

[0059] S2, mixing the silicone oil mixture and the emulsifier evenly at 75-78° C. to obtain a silicone oil-emulsion mixture;

[0060] S3, cooling the silicone oil-emulsion mixture to 45-50°C, stirring and reacting with the acrylic polymer for 4 hours to obtain a mixture 1, and keeping the mixture warm;

[0061] S4. The mixture 1 kept at 45-50°C is stirred evenly with the surfactant, homogenized and emulsified, then naturally cooled to room temperature, and mixed with the antibacterial agent to obtain a softener.

[0062] Example 2

[0063] The difference from Example 1 is that the weight parts of the softener components are different:

[0064] The softener comprises the following components in parts by weight (based on 100 parts): 22 parts of acrylic polymer, 15 parts of silicone oil (10 parts of octamethylcyclotetrasiloxane + 5 parts of N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane), 8 parts of anionic surfactant (disteadecyl succinic acid sulfonate), 15 parts of emulsifier (10 parts of fatty alcohol polyoxyethylene ether + 5 parts of polyoxyethylene stearate), 0.3 parts of quaternary ammonium salt antibacterial agent, 0.2-0.4 parts of 20% NaOH solution and the balance of water.

[0065] The components and preparation method of the acrylic polymer and the preparation method of the softener are consistent with those in Example 1.

[0066] Example 3

[0067] The difference from Example 1 is that the components of the softener are different:

[0068] The components of the softener in parts by weight are (based on 100 parts): 16 parts of acrylic polymer, 12 parts of silicone oil (8 parts of octamethylcyclotetrasiloxane + 4 parts of aminomethyldimethoxysilane), 5 parts of anionic surfactant (monoethanolamine salt of fatty alcohol sulfate), 12 parts of emulsifier (9 parts of fatty alcohol polyoxyethylene ether + 3 parts of polyoxyethylene stearate), 0.3 parts of quaternary ammonium salt antibacterial agent, 0.2-0.4 parts of 20% NaOH solution and the balance of water.

[0069] The components and preparation method of the acrylic polymer and the preparation method of the softener are consistent with those in Example 1.

[0070] Example 4

[0071] The difference from Example 1 is that the components of the acrylic polymer in the softener are different:

[0072] The components of the acrylic polymer in parts by weight are: 60 parts of acrylic acid, 20 parts of acrylic ester monomers (10 parts of n-octyl acrylate + 10 parts of decyl acrylate), 2 parts of maleic anhydride, 3 parts of dispersant (a mixture of polyethylene glycol and polyoxyethylene stearate, with a weight ratio of 1:2), 3 parts of hydrogen peroxide and 100 parts of water.

[0073] The components and preparation method of the softener and the preparation method of the acrylic polymer are consistent with those in Example 1.

[0074] Example 5

[0075] The difference from Example 1 is that the weight ratio of the acrylic polymer component in the softener is different:

[0076] The components of the acrylic polymer in parts by weight are: 50 parts of acrylic acid, 16 parts of acrylic ester monomer (a mixture of fatty alcohol polyoxyethylene ether and polyoxyethylene stearate, the weight ratio of which is 1:1), 2 parts of maleic anhydride, 3 parts of dispersant (a mixture of fatty alcohol polyoxyethylene ether and polyoxyethylene stearate, the weight ratio of which is 1:2), 1 part of hydrogen peroxide and 100 parts of water. The components and preparation method of the softener and the preparation method of the acrylic polymer are the same as those in Example 1.

[0077] Comparative Example 1

[0078] The difference from Example 1 is that the weight parts of the softener components are different:

[0079] The softener comprises the following components in parts by weight (based on 100 parts): 16 parts of acrylic polymer, 1.2 parts of silicone oil (0.8 parts of octamethylcyclotetrasiloxane+0.4 parts of N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane), 1 part of anionic surfactant (disteadecyl succinic acid sulfonate), 16 parts of emulsifier (12 parts of fatty alcohol polyoxyethylene ether+4 parts of polyoxyethylene stearate), 0.3 parts of quaternary ammonium salt antibacterial agent, 0.1-0.3 parts of 20% NaOH solution and the balance of water.

[0080] The components and preparation method of the acrylic polymer and the preparation method of the softener are consistent with those in Example 1.

[0081] Comparative Example 2

[0082] The difference from Example 1 is that the weight parts of the softener components are different:

[0083] The softener comprises the following components in parts by weight (based on 100 parts): 30 parts of acrylic polymer, 15 parts of silicone oil (10 parts of octamethylcyclotetrasiloxane + 5 parts of N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane), 1 part of anionic surfactant (disteadecyl succinic acid sulfonate), 4 parts of emulsifier (3 parts of fatty alcohol polyoxyethylene ether + 1 part of polyoxyethylene stearate), 0.3 parts of quaternary ammonium salt antibacterial agent, 0.2-0.4 parts of 20% NaOH solution and the balance of water.

[0084] The components and preparation method of the acrylic polymer and the preparation method of the softener are consistent with those in Example 1.

[0085] Comparative Example 3

[0086] The difference from Example 1 is that the components of the softener are different:

[0087] The softener comprises the following components in parts by weight (based on 100 parts): 16 parts of acrylic polymer, 12 parts of silicone oil (8 parts of octamethylcyclotetrasiloxane + 4 parts of N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane), 5 parts of cationic surfactant (amine salt type cationic surfactant), 12 parts of emulsifier (9 parts of fatty alcohol polyoxyethylene ether + 3 parts of polyoxyethylene stearate), 0.3 parts of quaternary ammonium salt antibacterial agent, 0.2-0.4 parts of 20% NaOH solution and the balance of water.

[0088] The components and preparation method of the acrylic polymer and the preparation method of the softener are consistent with those in Example 1.

[0089] Comparative Example 4

[0090] The difference from Example 1 is that the components of the softener are different, no emulsifier is used, and the emulsifier is replaced by an anionic surfactant:

[0091] The softener comprises the following components in parts by weight (based on 100 parts): 16 parts of acrylic polymer, 12 parts of silicone oil (8 parts of octamethylcyclotetrasiloxane + 4 parts of N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane), 17 parts of anionic surfactant (disteadecyl succinic acid sulfonate), 0.3 parts of quaternary ammonium salt antibacterial agent, 0.2-0.4 parts of 20% NaOH solution and the balance of water.

[0092] The components and preparation method of the acrylic polymer and the preparation method of the softener are consistent with those in Example 1.

[0093] Comparative Example 5

[0094] The difference from Example 1 is that the components of the acrylic polymer are different:

[0095] The components of the acrylic polymer in parts by weight are: 60 parts of acrylic acid, 20 parts of acrylic acid ester monomer (n-butyl acrylate), 2 parts of maleic anhydride, 0.6 parts of dispersant (a mixture of sodium isopropylbenzene sulfonate and isomeric decanol polyoxyethylene ether, with a weight ratio of 1:2), 3 parts of hydrogen peroxide and 100 parts of water.

[0096] The components and preparation method of the softener and the preparation method of the acrylic polymer are consistent with those in Example 1.

[0097] Comparative Example 6

[0098] The difference from Example 1 is that the weight parts of the acrylic polymer component are different:

[0099] The components of the acrylic polymer in parts by weight are: 60 parts of acrylic acid, 5 parts of acrylic ester monomer (n-butyl acrylate), 2 parts of maleic anhydride, 3 parts of dispersant (a mixture of fatty alcohol polyoxyethylene ether and polyoxyethylene stearate, with a weight ratio of 1:2), 3 parts of hydrogen peroxide and 100 parts of water.

[0100] The components and preparation method of the softener and the preparation method of the acrylic polymer are consistent with those in Example 1.

[0101] Comparative Example 7

[0102] Different from Example 1, the preparation method of the acrylic polymer is different, and the acrylic polymer is not dispersed step by step during the preparation process:

[0103] The preparation method of acrylic acid ester polymer comprises the steps of:

[0104] (1) mixing acrylic acid with water to prepare a solution, and fully stirring and dispersing the mixture with an acrylic monomer, a dispersant, and maleic anhydride to obtain a dispersion solution;

[0105] (3) The dispersion solution was heated to 90°C at a rate of 3°C / min, and hydrogen peroxide was added dropwise. After the addition was completed within 3 hours, the solution was kept warm for 2.5 hours to obtain an acrylic polymer.

[0106] The components and preparation method of the softener and the components of the acrylic polymer are the same as those in Example 1.

[0107] Comparative Example 8

[0108] The difference from Example 1 is that the preparation method of the softener is different:

[0109] S1. Mix silicone oil, pH regulator and water evenly, stir and react at 75-78°C for 3 hours at a stirring rate of 120 rpm / min to obtain a silicone oil mixture, and keep warm;

[0110] S2, mixing the silicone oil mixture and the emulsifier uniformly at 45-50° C. to obtain a silicone oil-emulsion mixture;

[0111] S3, stirring and reacting with an acrylic acid ester polymer at 45-50°C for 5 hours to obtain a mixture 1, and keeping the mixture warm;

[0112] S4. The mixture 1 kept at 45-50°C is stirred evenly with the surfactant, homogenized and emulsified, then naturally cooled to room temperature, and mixed with the antibacterial agent to obtain a softener.

[0113] The components of the softener, the components of the acrylic polymer and the preparation method are the same as those in Example 1.

[0114] Test 1: Stability test of lubricating softener in high stability bath under different conditions

[0115] Formula: 20g / L lubricating softener in the bath. See Table 1 for other conditions and test results:

[0116] The stability test results are divided into two levels: stable and unstable. Leave the prepared working solution for 1-7 days to observe whether the working solution is stable.

[0117] Table 1

[0118]

[0119]

[0120] It can be seen from Table 1 that the high stability bath lubricating softener of the present invention has excellent stability.

[0121] Test 2: Lubricating effect of different lubricating softeners in the bath

[0122] Formula: Lubricating softener in bath Xg / l; Fabric: 45×45 black rayon cloth 10g; Bath ratio: 1:10;

[0123] Process: 60℃×30min immersion treatment → squeeze out the residual liquid after the cloth is taken out, and conduct wet evaluation in the bath to check the lubrication effect.

[0124] The score is based on a 100-point system and is scored by three bath lubrication professionals. The higher the score, the better the bath lubrication effect, and the lower the score, the worse the feel. The scoring results are shown in Table 2.

[0125] Table 2

[0126]

[0127]

[0128] It can be seen from Table 2 that the high stability bath lubricating softener of the present invention has an excellent bath lubricating effect.

[0129] Test 3: Fabrics treated with lubricating softeners in different baths, and the retention of fabric feel after washing

[0130] Formula: Lubricating softener in bath Xg / l; Fabric: 45×45 black rayon cloth 10g; Bath ratio: 1:10;

[0131] Process: 60℃×30min immersion treatment → room temperature water washing for 10min → dehydration → drying (105℃) → evaluation of hand feel.

[0132] The score is based on a 100-point system and is scored by three professionals who evaluate the feel. The higher the score, the better the feel, and the lower the score, the worse the feel. The scoring results are shown in Table 3.

[0133] Table 3

[0134]

[0135] It can be seen from Table 3 that the fabric treated with the high stability bath lubricating softener of the present invention can still retain a good hand feel after washing, and the subsequent softener dosage can be reduced.

[0136] Experiment 4 Effect of adding lubricating softener in bath to treat fabric at different process stages on the final fabric color shade Formula: Lubricating softener in bath Xg / L (see the dosage in the process for details); Fabric: 40×40 / 133×72 pure cotton grey cloth 10g; Bath ratio: 1:10;

[0137] Process: semi-finished product → pre-treatment (add 2g / L lubricating softener in the bath on the basis of normal process) → washing → neutralization → dyeing → washing → 98℃×10min soap washing (add 1g / L lubricating softener in the bath on the basis of normal process) → washing → drying → color difference test. The color light test results are shown in Table 4.

[0138] Method for testing color difference: Use a colorimeter to test 4 points on the front and back of the test fabric and take the average value.

[0139] Table 4

[0140]

[0141]

[0142] It can be seen from Table 4 that adding the lubricating softener in the bath of the present invention to treat the fabric in different process stages has no effect on the final fabric color.

[0143] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.

Claims

1. A high stability bath lubricating softener, characterized in that: The composition comprises 16 parts by weight of an acrylic acid ester polymer, 12 parts of silicone oil, 5 parts of anionic surfactant, 12 parts of emulsifier, 0.3 parts of quaternary ammonium salt antibacterial agent, 0.2 parts to 0.4 parts of 20% NaOH solution and the balance of water. The acrylic polymer comprises the following components in parts by weight: 60 parts of acrylic acid, 20 parts of n-butyl acrylate, 2 parts of maleic anhydride, 3 parts of dispersant, 3 parts of hydrogen peroxide and 100 parts of water; the dispersant is a mixture of fatty alcohol polyoxyethylene ether and polyoxyethylene stearate in a weight ratio of 1:2; The method for preparing the acrylic acid ester polymer comprises the steps of: (1) preparing a 60% solution of acrylic acid and uniformly mixing it with n-butyl acrylate to obtain a mixture 1; (2) fully stirring and dispersing the dispersant and the remaining weight portion of water, and fully mixing it with maleic anhydride to obtain a dispersion solution; (3) heating the mixture 1 and the dispersion solution to 70° C. at a rate of 3° C. / min, adding hydrogen peroxide dropwise, and after the addition is completed within 3 hours, keeping the temperature for reaction for 2.5 hours to obtain an acrylic ester polymer; The silicone oil is a mixture of octamethylcyclotetrasiloxane and N-(β-aminoethyl-γ-aminopropyl)methyldimethoxysilane in a mass ratio of 2:1; The anionic surfactant is dioctadecyl succinate sulfonate; The emulsifier is a mixture of fatty alcohol polyoxyethylene ether and polyoxyethylene stearate, with a mass ratio of 3:1; The above softener is prepared by the preparation method of the following steps: S1. Evenly mix silicone oil with 20% NaOH solution and water, and stir and react at 75-78°C for 3 hours at a stirring rate of 120 rpm / min to obtain a silicone oil mixture, and keep warm; S2. Evenly mix the silicone oil mixture with an emulsifier at 75-78°C to obtain a silicone oil-emulsion mixture; S3. Cool the silicone oil-emulsion mixture to 45-50°C, stir and react with an acrylic polymer for 4 hours to obtain a mixture 1, and keep warm; S4. Evenly stir the mixture 1 kept at 45-50°C with an anionic surfactant, homogenize and emulsify, naturally cool to room temperature, and mix with a quaternary ammonium salt antibacterial agent to obtain a softener.

2. The method for preparing the softener according to claim 1, characterized in that: The method comprises the following steps: S1, uniformly mixing silicone oil with 20% NaOH solution and water, stirring and reacting at 75-78°C for 3 hours at a stirring rate of 120 rpm / min to obtain a silicone oil mixture, and keeping the mixture warm; S2, uniformly mixing the silicone oil mixture with an emulsifier at 75-78°C to obtain a silicone oil-emulsion mixture; S3, cooling the silicone oil-emulsion mixture to 45-50°C, stirring and reacting the mixture with an acrylic acid ester polymer for 4 hours to obtain a mixture 1, and keeping the mixture warm; S4, uniformly stirring the mixture 1 kept at 45-50°C with an anionic surfactant, homogenizing and emulsifying, naturally cooling the mixture to room temperature, and mixing the mixture with a quaternary ammonium salt antibacterial agent to obtain a softener.

Citation Information

Patent Citations

  • A cotton-grade stiffening softener and its preparation method

    CN107904954B

  • Branched-structured hydrophobic feeling finishing agent prepared from acrylate and reactive silicone oil as well as preparation method and application of branched-structured hydrophobic feeling finishing agent

    CN108049186A

  • Preparation method of super-soft IPN (interpenetrating polymer network) pigment printing binder

    CN104610512A