Iron-aluminum covalent coagulant modified activated carbon material for simultaneous oxidation and adsorption for efficient removal of organic arsenic and its preparation and application

Through the preparation of modified activated carbon materials with iron-carrying aluminum covalent bonding agent, the problems of low organic arsenic removal rate and large loss of activated carbon heads in water treatment are solved, and efficient organic arsenic removal and industrial application of materials are achieved.

CN116492982BActive Publication Date: 2024-11-22ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310298635.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-11-22
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

The prior art has a low removal rate of organic arsenic in water treatment, and the water head loss of activated carbon is large, which leads to difficulty in solid-liquid separation and limits its industrial application.

Method used

Using iron-carrying aluminum covalent bonding agent to modify activated carbon materials, the silane coupling agent, aluminum salt and iron salt and activated carbon powder are modified to form an iron-carrying aluminum covalent bonding agent with advanced oxidation capacity. Modified activated carbon to achieve synchronous removal of organic arsenic oxidation and adsorption.

Benefits of technology

It improves the removal rate of organic arsenic, reduces the loss rate of activated carbon, and the materials are easy to settle, solves the problems of poor removal rate of coagulants and activated carbon alone and excessive head loss, and realizes industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116492982B_ABST
    Figure CN116492982B_ABST
Patent Text Reader

Abstract

The present invention provides an activated carbon material modified by an iron-aluminum covalent coagulant that can efficiently remove organic arsenic by integrating oxidation and adsorption, and its preparation and application, and belongs to the field of water treatment technology. The present invention uses an iron-aluminum covalent coagulant to modify activated carbon. The modified activated carbon has adsorption capacity and advanced oxidation capacity at the same time, which greatly improves the removal effect of organic arsenic. It can be reused after recycling and treatment, and the modified activated carbon is very easy to settle, which not only improves the simultaneous and efficient removal of organic arsenic, but also solves the problems that the removal rate of organic arsenic is not good when using coagulants alone and activated carbon alone in practice, and the extremely fine particle size of activated carbon in the adsorption method leads to excessive head loss in actual application, difficulty in solid-liquid separation, easy blockage of structure pipelines or equipment, and limitation of its industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water treatment, and in particular to an activated carbon material modified by an iron-aluminum covalent bond coagulant for simultaneously and efficiently removing organic arsenic by integrating oxidation and adsorption, and the preparation and application thereof. Background Art

[0002] Arsenic, a priority pollutant, enters the natural environment mainly through natural weathering and industrial production (such as wood preservatives, alloy materials, pesticides, and feed chemicals). The ubiquitous presence of arsenic in natural water bodies seriously threatens the health of tens of millions of people around the world, and water quality standards are becoming increasingly stringent. With the focus on detecting and analyzing arsenic species in food supplies (such as meat, rice, and seafood), organic arsenic has gradually become a new focus of arsenic research. Organic arsenic preparations are widely used as feed additives because of their multiple functions such as improving feed utilization, inhibiting pathogens, and similar to antibiotics. Among them, roxarsone (ROX) and arsanilic acid (ASA) are the most commonly used feed additives. The molecular structure of the additive is hardly destroyed by animal digestion, and it is excreted with excrement and accumulated in compost. With the agricultural application of compost, organic arsenic pollutants are introduced into the environment; in solid / water environments, organic arsenic compounds can be converted into toxic and more mobile inorganic arsenic (As(III) / As(V)) through a series of biodegradation, and ultimately endanger human health through the food chain or drinking water sources.

[0003] Activated carbon adsorption is widely used to adsorb organic arsenic due to its advantages of simple operation, stable operation and low cost. However, the removal rate of organic arsenic by activated carbon adsorption alone is extremely low, and the head loss is too large, making solid-liquid separation difficult, and easily causing blockage of structures, pipes or equipment, which limits its industrial application. Summary of the invention

[0004] The purpose of the present invention is to provide an activated carbon material modified by an iron-loaded aluminum covalent bond coagulant, which can simultaneously remove organic arsenic by oxidation and adsorption and efficiently, and its preparation and application. The activated carbon material modified by an iron-loaded aluminum covalent bond coagulant prepared by the present invention has the ability to adsorb and oxidize organic arsenic at the same time, has a high removal rate for organic arsenic, is easy to settle, and has a low carbon loss rate.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing an activated carbon material modified by an iron-aluminum covalent bond coagulant, comprising the following steps:

[0007] Mixing a silane coupling agent, an aluminum salt solution and an iron salt solution to obtain a mixed solution;

[0008] mixing the mixed solution and an alkaline solution to obtain an alkaline mixed solution;

[0009] The alkaline mixed solution, acrylamide, methacryloyloxyethyl trimethyl ammonium chloride and a thermal initiator are mixed to carry out an initiation reaction and ripen to obtain an iron-aluminum covalent bond coagulant;

[0010] Dissolving the iron-loaded aluminum covalent bond coagulant in water to obtain an iron-loaded aluminum covalent bond coagulant solution;

[0011] The activated carbon powder is immersed in the iron-loaded aluminum covalent bond coagulant solution to carry out a modification reaction, thereby obtaining the iron-loaded aluminum covalent bond coagulant modified activated carbon material.

[0012] Preferably, the silane coupling agent includes vinyltriethoxysilane, vinyltrimethoxysilane or vinyltri(β-methoxyethoxy)silane; the ratio of the total molar amount of aluminum in the aluminum salt solution and the iron in the iron salt solution to the molar amount of silicon in the silane coupling agent is 1:(0.2-0.6); the molar ratio of aluminum in the aluminum salt solution and iron in the iron salt solution is (7-9):1.

[0013] Preferably, the alkaline solution comprises a sodium hydroxide solution; and the alkalinity of the alkaline mixed solution is 1.9 to 2.1.

[0014] Preferably, the mass ratio of acrylamide to methacryloyloxyethyltrimethylammonium chloride is (1.7-2.3):1; the mass ratio of the silane coupling agent to acrylamide is (1.1-1.3):1.

[0015] Preferably, the thermal initiator comprises ammonium persulfate solution; the initiation reaction temperature is 38-42° C. and the reaction time is 24-30 hours.

[0016] Preferably, the aging time is 24 to 48 hours.

[0017] Preferably, the ratio of the mass of the activated carbon powder to the volume of the iron-loaded aluminum covalent bond coagulant in the iron-loaded aluminum covalent bond coagulant solution is 1 g: (2 to 8) mL.

[0018] Preferably, the modification reaction is carried out at a temperature of 24 to 26° C. and for a time of 23 to 25 hours.

[0019] The present invention provides an activated carbon material modified by an iron-aluminum covalent bond coagulant prepared by the preparation method described in the above scheme.

[0020] The present invention provides the use of the iron-aluminum covalent bond coagulant modified activated carbon material described in the above scheme in the treatment of organic arsenic wastewater.

[0021] The invention provides a preparation method of an activated carbon material modified by an iron-loaded aluminum covalent bond coagulant, comprising the following steps: mixing a silane coupling agent, an aluminum salt solution and an iron salt solution to obtain a mixed solution; mixing the mixed solution and an alkaline solution to obtain an alkaline mixed solution; mixing the alkaline mixed solution, acrylamide, methacryloyloxyethyltrimethylammonium chloride and a thermal initiator, performing an initiation reaction, and aging to obtain an iron-loaded aluminum covalent bond coagulant; dissolving the iron-loaded aluminum covalent bond coagulant in water to obtain an iron-loaded aluminum covalent bond coagulant solution; and impregnating activated carbon powder into the iron-loaded aluminum covalent bond coagulant solution to perform a modification reaction to obtain the iron-loaded aluminum covalent bond coagulant modified activated carbon material.

[0022] The present invention immerses activated carbon powder into the iron-aluminum covalent bond coagulant solution for modification. The iron-aluminum covalent bonds generated after the iron-aluminum covalent bond coagulant is dissolved in water are successfully loaded on the activated carbon, thereby generating rich iron-aluminum substances. Electron transfer occurs between the iron-aluminum substances and the activated carbon, so that the modified activated carbon has adsorption capacity and advanced oxidation capacity at the same time, greatly improving the removal effect of organic arsenic. The activated carbon can be reused after recovery and treatment, and the modified activated carbon is very easy to settle, which not only improves the synchronous and efficient removal of organic arsenic, but also solves the problems that the removal rate of organic arsenic is not good when using coagulants alone or activated carbon alone in practice, and the extremely fine particle size of activated carbon in the adsorption method leads to excessive head loss in actual application, difficulty in solid-liquid separation, easy blockage of structure pipelines or equipment, and limitation of its industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 For PAC, CAFM 0.6 @PAC and CAFM after adsorption of 6.6 mg / L (30 μM) arsanilic acid 0.6 @PACXPS full spectrum (a) and PAC, CAFM 0.2 @PAC, CAFM 0.4 @PAC, CAFM 0.6 @PAC X-ray diffraction pattern (b);

[0024] Figure 2 In the above figure, (a) is PAC, CAFM 0.2 @PAC, CAFM 0.4 @PAC, CAFM 0.6 Fourier transform infrared absorption spectrum of @PAC; (b) PAC and CAFM 0.6 @PAC’s voltammetric linear curve Tafel diagram; (c) CAFM 0.6 @PAC was added to ultrapure water and the EPR spectra of hydroxyl radicals generated by constant temperature oscillation at 0min, 5min, and 60min; (d) CAFM0.6 @The X-ray photoelectron spectrum of arsenic on the surface of the material after PAC was added to a 30μM arsanilic acid solution;

[0025] Figure 3 To measure CAFM using the horseradish method 0.6 @PAC The amount of H2O2 produced and the amount of iron and aluminum leached in the reaction solution (a) and the change of the total arsenic content in the reaction solution (b);

[0026] Figure 4 It is an iron-aluminum covalent coagulant CAFM 0.6 EPR spectrum of hydroxyl radicals;

[0027] Figure 5 This is the EPR spectrum of hydroxyl radicals of the composite coagulant prepared in Comparative Example 1. DETAILED DESCRIPTION

[0028] The present invention provides a method for preparing an activated carbon material modified by an iron-aluminum covalent bond coagulant, comprising the following steps:

[0029] Mixing a silane coupling agent, an aluminum salt solution and an iron salt solution to obtain a mixed solution;

[0030] mixing the mixed solution and an alkaline solution to obtain an alkaline mixed solution;

[0031] The alkaline mixed solution, acrylamide, methacryloyloxyethyl trimethyl ammonium chloride and a thermal initiator are mixed to carry out an initiation reaction and ripen to obtain an iron-aluminum covalent bond coagulant;

[0032] Dissolving the iron-loaded aluminum covalent bond coagulant in water to obtain an iron-loaded aluminum covalent bond coagulant solution;

[0033] The activated carbon powder is immersed in the iron-loaded aluminum covalent bond coagulant solution to carry out a modification reaction, thereby obtaining the iron-loaded aluminum covalent bond coagulant modified activated carbon material.

[0034] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.

[0035] The invention mixes a silane coupling agent, an aluminum salt solution and an iron salt solution to obtain a mixed solution.

[0036] In the present invention, the silane coupling agent preferably includes vinyl triethoxysilane, vinyl trimethoxysilane or vinyl tri(β-methoxyethoxy)silane, more preferably vinyl triethoxysilane (VTES). In the present invention, the silane coupling agent functions to combine inorganic and organic components through different functional groups.

[0037] In the present invention, the aluminum salt solution preferably includes an aluminum chloride solution; the iron salt solution preferably includes a ferric chloride solution; the concentration of aluminum ions in the aluminum salt solution and the concentration of iron ions in the iron salt solution are independently preferably 0.5 to 1 mol / L, more preferably 1 mol / L.

[0038] In the present invention, the molar ratio of the aluminum element in the aluminum salt solution to the iron element in the iron salt solution is preferably (7-9):1, more preferably (7.5-8.5):1; the ratio of the total molar amount of the aluminum element in the aluminum salt solution and the iron element in the iron salt solution to the molar amount of the silicon element in the silane coupling agent is preferably 1:(0.2-0.6), specifically 1:0.2, 1:0.3, 1:0.4, 1:0.5 or 1:0.6, and most preferably 1:0.6.

[0039] In the present invention, the mixing is preferably carried out under magnetic stirring conditions, the mixing time is preferably 20 to 40 minutes, and the stirring rate is preferably 350 to 500 r / min.

[0040] After obtaining the mixed solution, the present invention mixes the mixed solution with an alkaline solution to obtain an alkaline mixed solution.

[0041] In the present invention, the alkaline solution preferably includes a sodium hydroxide solution; the concentration of the sodium hydroxide solution is preferably 0.48-0.53 mol / L, more preferably 0.5 mol / L. In the present invention, the amount of the alkaline solution preferably satisfies the alkalinity of the alkaline mixed solution to be 1.9-2.1, more preferably to be 2. In the present invention, the alkalinity is defined as (OH) / n(M), wherein OH represents the equivalent number of -OH bound to the metal ion, M represents the equivalent number of the metal ion, and n is the compound of the metal ion.

[0042] In the present invention, mixing the mixed solution and the alkaline solution preferably includes: adding the alkaline solution dropwise to the mixed solution at 38-42° C. and under stirring conditions, so that the solution always presents a dark orange color, and after the addition is completed, continuing to stir for 1.5-2 hours to obtain an alkaline mixed solution. Under alkaline conditions, FeCl3 and AlCl3 form Fe(OH)3 and Al(OH)3 with NaOH, thereby generating Fe-OH bonds and Al-OH bonds, providing material raw materials for subsequent bonding through a silane coupling agent.

[0043] After obtaining the alkaline mixed solution, the present invention mixes the alkaline mixed solution, acrylamide, methacryloyloxyethyl trimethyl ammonium chloride and a thermal initiator, performs an initiation reaction, and ripens to obtain an iron-aluminum covalent bond coagulant.

[0044] In the present invention, the acrylamide (AM) is used as an organic monomer, and the methacryloyloxyethyltrimethylammonium chloride (DMC) is used as a cationic monomer.

[0045] In the present invention, the mass ratio of acrylamide to methacryloyloxyethyltrimethylammonium chloride is preferably (1.7-2.3):1, more preferably 2:1; the mass ratio of the silane coupling agent used to prepare the alkaline mixed solution to acrylamide is preferably (1.1-1.3):1.

[0046] In the present invention, the thermal initiator is preferably an ammonium persulfate solution; in an embodiment of the present invention, the concentration of the ammonium persulfate solution is preferably 0.075 g / mL. The present invention does not specifically limit the amount of the thermal initiator, as long as it can initiate the polymerization reaction.

[0047] In the present invention, mixing the alkaline mixed solution, acrylamide, methacryloyloxyethyl trimethyl ammonium chloride and thermal initiator preferably comprises: adding acrylamide and methacryloyloxyethyl trimethyl ammonium chloride to the alkaline mixed solution and stirring until dissolved, and dropping the thermal initiator into the obtained solution.

[0048] In the present invention, the temperature of the initiation reaction is preferably 38-42°C, more preferably 40°C; the time is preferably 24-30h, more preferably 26-28h. In the present invention, the initiation reaction is preferably carried out under stirring conditions, and the stirring speed is preferably 350-400r / min. The present invention intensifies the breaking and synthesis of chemical bonds between the silane coupling agent and the Fe-OH and Al-OH formed under alkaline conditions by adding a thermal initiator, thereby producing a more stable Si-O-Fe, Si-O-Al iron-aluminum covalent bond structure, which is intuitively manifested in that the synthesized substance changes from a liquid to a colloidal state, presenting a more stable structure.

[0049] In the present invention, the aging is preferably carried out under room temperature and static conditions; the aging time is preferably 24 to 48 hours, more preferably 30 to 40 hours. In the aging process of the present invention, the synthesized iron-aluminum covalent bond material continues to fully react for a certain period of time to achieve the best composite strength.

[0050] In the present invention, the iron-aluminum covalent bond coagulant is in a colloid state with a certain viscosity.

[0051] After obtaining the iron-loaded aluminum covalent bond coagulant, the present invention dissolves the iron-loaded aluminum covalent bond coagulant into water to obtain an iron-loaded aluminum covalent bond coagulant solution.

[0052] In the present invention, the water is preferably ultrapure water. The present invention has no special requirements for the amount of water, as long as the iron-aluminum covalent bond coagulant can be completely dissolved. In an embodiment of the present invention, the volume ratio of the iron-aluminum covalent bond coagulant to water is preferably 1:50. In the present invention, the dissolution is preferably carried out under stirring conditions, and the stirring rate is preferably 100-150rpm; the present invention has no special requirements for the stirring time, as long as the iron-aluminum covalent bond coagulant is fully dissolved until no obvious colloidal suspended matter is observed by the naked eye.

[0053] After obtaining the iron-loaded aluminum covalent bond coagulant solution, the present invention immerses activated carbon powder into the iron-loaded aluminum covalent bond coagulant solution to perform a modification reaction to obtain the iron-loaded aluminum covalent bond coagulant modified activated carbon material.

[0054] Before the impregnation, the present invention preferably washes the activated carbon powder with ultrapure water for more than 3 times, and the washed activated carbon powder is vacuum dried at 60-65°C for 10-24h, and then ground and sieved through a 200-mesh sieve. In an embodiment of the present invention, the activated carbon powder has an analytical purity, an iodine value of 1000mg / g, a methylene blue value of 120mg / g, a moisture content of 10%, and an ash content of 9%.

[0055] In the present invention, the ratio of the mass of the activated carbon powder to the volume of the iron-loaded aluminum covalent coagulant in the iron-loaded aluminum covalent coagulant solution is preferably 1g:(2-8)mL, more preferably 1g:(3-6)mL. In the present invention, the temperature of the modification reaction is preferably 24-26°C, and the time is preferably 23-25h. In the present invention, the modification reaction is preferably carried out under constant temperature water bath oscillation conditions. During the modification process of the present invention, the iron-loaded aluminum covalent coagulant dissolved in water is wrapped and composited on the surface of the powdered activated carbon, and its covalent bonds react and bond with the functional groups on the surface of the powdered activated carbon, thereby activating the redox ability of the functional groups on the surface of the powdered activated carbon.

[0056] After the modification reaction is completed, the present invention performs solid-liquid separation on the obtained modified system, and washes it with ultrapure water until the supernatant is clarified. The obtained solid is vacuum dried at 60-65° C. for 10-24 hours, and after grinding, an iron-aluminum covalent coagulant modified activated carbon material that integrates oxidation and adsorption to simultaneously and efficiently remove organic arsenic is obtained, which is recorded as CAFM@PAC.

[0057] The present invention provides an activated carbon material modified by an iron-aluminum covalent bond coagulant and capable of simultaneously and efficiently removing organic arsenic by integrating oxidation and adsorption, which is prepared by the preparation method described in the above scheme.

[0058] The present invention immerses activated carbon powder into the iron-aluminum covalent bond coagulant solution for modification. The iron-aluminum covalent bonds generated after the iron-aluminum covalent bond coagulant is dissolved in water are successfully loaded on the activated carbon, thereby generating rich iron-aluminum substances. Electron transfer occurs between the iron-aluminum substances and the activated carbon, so that the modified activated carbon has adsorption capacity and advanced oxidation capacity at the same time, greatly improving the removal effect of organic arsenic. The activated carbon can be reused after recovery and treatment, and the modified activated carbon is very easy to settle, which not only improves the synchronous and efficient removal of organic arsenic, but also solves the problems that the removal rate of organic arsenic is not good when using coagulants alone or activated carbon alone in practice, and the extremely fine particle size of activated carbon in the adsorption method leads to excessive head loss in actual application, difficulty in solid-liquid separation, easy blockage of structure pipelines or equipment, and limitation of its industrial application.

[0059] The present invention provides the use of the iron-aluminum covalent bond coagulant modified activated carbon material described in the above scheme in the treatment of organic arsenic wastewater.

[0060] In an embodiment of the present invention, the conditions for treating the organic arsenic wastewater include: the pH value of the organic arsenic wastewater is 4, the temperature is 25°C, and the dosage of the iron-aluminum covalent bond coagulant modified activated carbon material is 0.5 g / L. The concentration of organic arsenic in the organic arsenic wastewater is preferably 5 to 50 μM.

[0061] The following detailed description of the iron-aluminum covalent coagulant modified activated carbon material for simultaneously and efficiently removing organic arsenic by oxidation and adsorption provided by the present invention and its preparation and application are combined with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0062] Preparation of the iron-aluminum covalent bond coagulant CAFM used in Examples 1 to 3:

[0063] (1) 1 mol / L AlCl3 and 1 mol / L FeCl3 solutions were added with VTES (vinyl triethoxysilane) at a molar ratio of 9:1 according to different Si / (Al+Fe) molar ratios (ranging from 0.2 to 0.6), and the mixture was stirred magnetically to be fully mixed to obtain a mixed solution.

[0064] (2) Slowly add an appropriate amount of 0.5 mol / L NaOH solution according to a certain alkalinity by the alkalinity method, control the dripping rate, temperature 40°C and stirring speed 350-400 r / min, so that the solution always appears dark orange. After the addition is completed, continue stirring for 1.5 hours to obtain an alkaline mixed solution with an alkalinity of 2.

[0065] (3) Weigh 3 g of acrylamide (AM) and 1.5 g of methyl methacrylate trimethyl ammonium chloride (DMC) monomers and add them into 120 mL of alkaline mixed solution. Stir magnetically for 40 min to fully dissolve them.

[0066] (4) Weigh a certain amount of thermal initiator according to the ratio of monomers. Thermal initiation requires excess. The amount of thermal initiator used in the embodiment is: weigh 1.5g of ammonium persulfate and dissolve it in 20mL of ultrapure water. Add the solution dropwise, and initiate the reaction at 40°C±1°C at a certain stirring speed for 24 hours. After the stirring is completed, the solution is taken out and left to stand at room temperature for 24 hours until the mixed solution presents a colloidal state with a certain viscosity. The colloidal substance after aging is the iron-aluminum covalent bond coagulant CAFM.

[0067] When the Si / (Al+Fe) molar ratio is 0.2, the obtained iron-aluminum covalent bond coagulant is recorded as CAFM. 0.2 When the Si / (Al+Fe) molar ratio is 0.4, the obtained iron-aluminum covalent bond coagulant is denoted as CAFM 0.4 When the Si / (Al+Fe) molar ratio is 0.6, the obtained iron-aluminum covalent bond coagulant is denoted as CAFM 0.6 .

[0068] Example 1

[0069] (1) Select activated carbon powder with analytical purity, particle size of about 200 mesh, iodine value of 1000 mg / g, methylene blue value of 120 mg / g, particle size of more than 200 mesh accounting for 90%, moisture content of 10%, and ash content of 9%. Wash the activated carbon powder with ultrapure water at room temperature for more than 3 times. Stir and soak it fully during the washing process to reduce its alkalinity and remove ash and impurities on the surface of the activated carbon powder. After filtering, place the washed activated carbon powder in a vacuum drying oven at 60°C and dry it for 10 hours. The ground sample is recorded as PAC and set aside.

[0070] (2) At room temperature, take 1 g of the activated carbon powder PAC obtained in step (1) and absorb 2 mL of the iron-aluminum covalent bond coagulant CAFM 0.2 In a beaker, add 100 mL of ultrapure water and stir magnetically for 10 minutes. After it is fully dissolved, pour it into a conical flask together with activated carbon powder PAC and shake it at a constant temperature of 25°C and 150 rpm for 24 hours. After the immersion is completed, the solid and liquid are separated, and the obtained solid is washed with ultrapure water until the supernatant is clear and then vacuum dried at 60°C for 10 hours. After grinding, the iron-aluminum covalent coagulant modified activated carbon material is obtained, which is recorded as CAFM. 0.2 @PAC.

[0071] Example 2

[0072] (1) Select activated carbon powder with analytical purity, particle size of about 200 mesh, iodine value of 1000 mg / g, methylene blue value of 120 mg / g, particle size of more than 200 mesh accounting for 90%, moisture content of 10%, and ash content of 9%. Wash the activated carbon powder with ultrapure water at room temperature for more than 3 times. Stir and soak it fully during the washing process to reduce its alkalinity and remove ash and impurities on the surface of the activated carbon powder. After filtering, place the washed activated carbon powder in a vacuum drying oven at 60°C and dry it for 10 hours. The ground sample is recorded as PAC and set aside.

[0073] (2) At room temperature, take about 1 g of the activated carbon powder PAC obtained in step (1) and absorb 2 mL of the iron-aluminum covalent bond coagulant CAFM. 0.4 In a beaker, add 100 mL of ultrapure water and stir magnetically for 10 minutes. After it is fully dissolved, pour it into a conical flask together with activated carbon powder PAC, and oscillate at a constant temperature of 25°C and 150 rpm for 24 hours. After the immersion is completed, the solid and liquid are separated, and the obtained solid is washed with ultrapure water until the supernatant is clear, and then vacuum dried at 60°C for 10 hours. After grinding, the iron-aluminum covalent coagulant modified activated carbon material is obtained, which is recorded as CAFM. 0.4 @PAC.

[0074] Example 3

[0075] (1) Select activated carbon powder with analytical purity, particle size of about 200 mesh, iodine value of 1000 mg / g, methylene blue value of 120 mg / g, particle size of more than 200 mesh accounting for 90%, moisture content of 10%, and ash content of 9%. Wash the activated carbon powder with ultrapure water at room temperature for more than 3 times. Stir and soak it fully during the washing process to reduce its alkalinity and remove ash and impurities on the surface of the activated carbon powder. After filtering, place the washed activated carbon powder in a vacuum drying oven at 60°C and dry it for 10 hours. The ground sample is recorded as PAC and set aside.

[0076] (2) At room temperature, take 1 g of the activated carbon powder PAC obtained in step (1) and absorb 2 mL of the iron-aluminum covalent coagulant CAFM. 0.6 In a beaker, add 100 mL of ultrapure water and stir magnetically for 10 minutes. After it is fully dissolved, pour it into a conical flask together with activated carbon powder PAC, and oscillate at a constant temperature of 25°C and 150 rpm for 24 hours. After the immersion is completed, the solid and liquid are separated, and the obtained solid is washed with ultrapure water until the supernatant is clear, and then vacuum dried at 60°C for 10 hours. After grinding, the iron-aluminum covalent coagulant modified activated carbon material is obtained, which is recorded as CAFM. 0.6 @PAC.

[0077] Comparative Example 1

[0078] The composite coagulant A was prepared by referring to the preparation method disclosed in Example 6 of CN 112939167A. The specific preparation steps are as follows:

[0079] S1: Take 1.33 g aluminum chloride powder and 8.11 g ferric chloride solid respectively, stir at a stirring rate of 150 rpm and room temperature and pressure for 3 h, dissolve in distilled water and adjust the volume to 100 mL to obtain a flocculation intermediate;

[0080] S2: Take 0.112 g of cationic polyacrylamide solid and 2.8 g of calcium oxide, add them to the flocculation intermediate at a stirring rate of 150 rpm and normal temperature and pressure, and stir and mix to obtain a flocculation semi-finished product;

[0081] S3: Take 0.56g of powdered activated carbon and add it to the flocculation semi-finished product. Stir for 5 hours at a stirring rate of 100rpm, a heating temperature of 45°C and normal pressure to obtain a flocculation product. Then, age the flocculation product at normal temperature and pressure for 24 hours to obtain a composite coagulant.

[0082] Performance characterization:

[0083] (1) Prepare the iron-aluminum covalent bond coagulant CAFM 0.6 It was applied to organic arsenic of different concentrations to investigate its removal effect. The results are shown in Table 1.

[0084] Table 1 Treatment effect of the iron-aluminum covalent bond coagulant obtained in Example 1 on organic arsenic

[0085]

[0086]

[0087] The results in Table 1 show that the prepared iron-aluminum covalent coagulant CAFM 0.6 The removal rate of organic arsenic was poor under different concentrations of organic arsenic. When the dosage was 0.5 g / L and the concentration of arsenic acid (ρ-ASA) was 30 μM (6.6 mg / L), the removal rate was only 16.5%. 0.6 Not suitable as a removal material for organic arsenic ρ-ASA.

[0088] (2) The prepared unmodified powdered activated carbon PAC and iron-aluminum covalently bonded activated carbon CAFM 0.6 @PAC was applied to 30μM arsenic acid (ρ-ASA) organic arsenic wastewater at 25°C to investigate its adsorption effect on organic arsenic. The results are shown in Table 2.

[0089] Table 2 PAC, CAFM 0.6 and CAFM0.6 @PAC treatment effect on wastewater containing organic arsenic

[0090] Adsorbent Dosage(g / L) Initial concentration (mg / L) Removal rate (%) Adsorption capacity (mg / g) PAC 0.5 6.6 29.68 3.87 CAFM0.6 0.5 6.6 16.5% — <![CDATA[CAFM 0.2 @PAC]]> 0.5 6.6 74.88 9.75 <![CDATA[CAFM 0.4 @PAC]]> 0.5 6.6 75.72 9.86 <![CDATA[CAFM 0.6 @PAC]]> 0.5 6.6 89.57 11.67

[0091] The results in Table 2 show that the unmodified powdered activated carbon PAC and the iron-aluminum covalent bond coagulant CAFM 0.6 The removal rates of organic arsenic were low, at 29.68% and 16.5% respectively. 0.6 @PAC has a significant effect in removing organic arsenic, among which CAFM 0.6 @PAC has the best organic arsenic removal effect, reaching 89.57%, achieving efficient removal of organic arsenic in water by combining oxidation and adsorption simultaneously.

[0092] (3) Prepared iron-aluminum covalently bonded activated carbon CAFM 0.6 @PAC was applied to organic arsenic at different concentrations to investigate its removal effect. The results are shown in Table 3.

[0093] Table 3 Treatment effect of iron-aluminum covalent bond activated carbon obtained in Example 3 on organic arsenic

[0094]

[0095]

[0096] The results in Table 3 show that the prepared Fe-Al covalently bonded activated carbon CAFM 0.6 @PAC still has a good organic arsenic removal rate in the environment of different organic arsenic concentrations. When the organic arsenic concentration is 1.1 mg / L (50 μmol / L), the arsenic removal effect is optimal, reaching 100%, realizing the efficient removal of organic arsenic in water by simultaneous oxidation and adsorption.

[0097] (4) Iron-loaded aluminum covalent bond modified activated carbon CAFM prepared in Example 3 0.6 After use, the PAC was rinsed clean, stirred and immersed in a 1.0 mol / L nitric acid solution for 24 h, and then dried at 60°C for 10 h for recovery. The iron-loaded aluminum covalent bond modified activated carbon material still had good adsorption capacity after repeated recycling and use for 2 times. The removal effect of the iron-loaded aluminum covalent bond modified activated carbon material of Example 3 on organic arsenic wastewater is shown in Table 4. In Table 4, the original dosage was 0.5 g / L, and the initial concentration of organic arsenic was 6.6 mg / L (30 μmol / L).

[0098] Table 4 Recovered CAFM 0.6 @PAC treatment effect on organic arsenic wastewater

[0099] Recycling times Removal rate of organic arsenic (%) Adsorption of organic arsenic (mg / g) 1 84.82 11.05 2 74.14 9.65

[0100] Structural characterization:

[0101] Figure 1 (a) is powdered activated carbon PAC, iron-aluminum covalent coagulant modified activated carbon material CAFM 0.6 @PAC and Fe-Al covalent bond modified activated carbon CAFM 0.6 @Full spectrum of x-ray photoelectron spectrum of PAC after adsorption of 30 μM arsanilic acid (ρ-ASA); Figure 1 (b) is PAC, CAFM 0.2 @PAC, CAFM 0.4 @PAC, CAFM 0.6 @PAC X-ray diffraction diagram. According to the full spectrum of XPS, it can be seen that the surface of the modified activated carbon is loaded with iron-aluminum-containing substances, and after the adsorption of organic arsenic, arsenic substances are detected on the surface of the activated carbon. Figure 1 From the XRD characterization analysis in (b), it can be seen that with the increase of the dosage of silane coupling agent, the iron and aluminum metal substances on the surface of the modified activated carbon are more abundant, including iron and aluminum oxides such as Al2O3, FeO, Fe2O3, and FeO(OH), which indicates that the iron and aluminum substances of CAFM@PAC are mainly loaded in the form of their oxides. When the dosage of silane coupling agent is 0.6, the conversion of Fe(II) to Fe(III) is found, which may involve oxidation process or electron transfer process.

[0102] Figure 2 (a) refers to PAC and CAFM 0.2 @PAC, CAFM 0.4 @PAC, CAFM 0.6 @PAC’s Fourier transform infrared absorption spectrum; Figure 2 (b) is PAC and CAFM 0.6 @PAC's voltammetric linear curve Tafel diagram; Figure 2 (c) is CAFM 0.6 @PAC was added to ultrapure water, and the EPR spectra of hydroxyl radicals generated by constant temperature oscillation at 0min, 5min, and 60min. The reaction conditions were: dark environment, pH=4, and 25℃; Figure 2 (d) is CAFM 0.6 @PAC is added to a 30μM arsanilic acid solution and reacts with it. This is the X-ray photoelectron spectrum of arsenic on the surface of the material.

[0103] Depend on Figure 2 (a) The mid-infrared spectrum shows that CAFM@PAC has a wavelength of 878 cm -1 、1080cm -1The Fe-OH-Fe and Fe-O-Fe / Al-O-Al metal covalent bonds were generated at 1620 cm -1 C=C was generated at the site, indicating that the surface of the newly generated activated carbon has an unsaturated structure and can be oxidized. Figure 2 In (c), it can be concluded that at 0 min, there is no DMOP-OH characteristic peak, and at 5 min, an extremely weak DMOP-OH characteristic peak is detected. At 60 min, the DMOP-OH characteristic peak is obvious, which shows that in the process of CAFM@PAC adsorbing organic arsenic, it not only has an adsorption effect, but also reactive oxygen species (ROS) play an important role in the removal of organic arsenic.

[0104] In order to understand the source of oxidation during the reaction, the horseradish method was used to determine the amount of H2O2 produced in the reaction solution, the amount of iron and aluminum leached, and the change in the total arsenic content in the measured reaction solution. The results are as follows: Figure 3 shown. Figure 3 In the above example, (a) is CAFM. 0.6 @PAC is a graph showing the amount of H2O2 produced in the solution and the amount of Fe and Al residual in the solution during the reaction when the dosage is 0.5 g / L and the concentration of arsanilic acid is 30 μM; (b) is a graph showing the amount of H2O2 produced in the solution and the amount of Fe and Al residual in the solution during the reaction; 0.6 @PAC shows the content of inorganic arsenic (the sum of As(III) and As(VI)) in the solution during the reaction when the dosage is 0.5 g / L and the concentration of arsanilic acid is 30 μM.

[0105] The amount of hydrogen peroxide produced can be seen to be in a dynamic change within 140 minutes, indicating that there is H2O2 produced in the reaction solution, and the H2O2 content reaches a maximum value (7μg / L) at 60 minutes. This is consistent with the EPR detection results. Figure 3 As can be seen from the total arsenic production in (b), the total arsenic content is also in dynamic change, which indicates that in the process of CAFM@PAC treating organic arsenic, part of the organic arsenic is removed by oxidation to generate inorganic arsenic and then further removed.

[0106] Figure 4 It is an iron-aluminum covalent coagulant CAFM 0.6 EPR spectrum of hydroxyl radicals (test conditions are the same as CAFM) 0.6 @PAC) by Figure 4 It can be seen that without coupling with carbon, CAFM 0.6 No hydroxyl radical peak was detected in the solution.

[0107] Figure 5The EPR spectrum of the hydroxyl radical of the composite coagulant of Comparative Example 1 (test conditions are the same as those of CAFM 0.6 @PAC), Figure 5 Displayed by Figure 5 It can be seen that in Comparative Example 1, the composite coagulant obtained by loading conventional iron salt and aluminum salt onto activated carbon does not detect the peak of hydroxyl radicals in the solution.

[0108] From the above test results, it can be seen that the iron-aluminum covalent bond coagulant modified activated carbon material prepared by the present invention has the ability to adsorb and perform advanced oxidation on organic arsenic, while a single iron-aluminum covalent bond coagulant or activated carbon modified with ordinary iron materials and aluminum materials cannot produce free radicals and do not have advanced oxidation ability.

[0109] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an activated carbon material modified by an iron-aluminum covalent bond coagulant, comprising the following steps: Mixing a silane coupling agent, an aluminum salt solution and an iron salt solution to obtain a mixed solution; mixing the mixed solution and an alkaline solution to obtain an alkaline mixed solution; The alkaline mixed solution, acrylamide, methacryloyloxyethyl trimethyl ammonium chloride and a thermal initiator are mixed to carry out an initiation reaction and ripen to obtain an iron-aluminum covalent bond coagulant; Dissolving the iron-loaded aluminum covalent bond coagulant in water to obtain an iron-loaded aluminum covalent bond coagulant solution; The activated carbon powder is immersed in the iron-loaded aluminum covalent bond coagulant solution to carry out a modification reaction, thereby obtaining the iron-loaded aluminum covalent bond coagulant modified activated carbon material.

2. The preparation method according to claim 1, characterized in that: The silane coupling agent includes vinyl triethoxysilane, vinyl trimethoxysilane or vinyl tri(β-methoxyethoxy)silane; the ratio of the total molar amount of the aluminum element in the aluminum salt solution and the iron element in the iron salt solution to the molar amount of the silicon element in the silane coupling agent is 1:(0.2-0.6); the molar ratio of the aluminum element in the aluminum salt solution to the iron element in the iron salt solution is (7-9):

1.

3. The preparation method according to claim 1, characterized in that: The alkaline solution includes a sodium hydroxide solution; the alkalinity of the alkaline mixed solution is 1.9 to 2.

1.

4. The preparation method according to claim 1, characterized in that: The mass ratio of acrylamide to methacryloyloxyethyl trimethylammonium chloride is (1.7-2.3):1; the mass ratio of the silane coupling agent to acrylamide is (1.1-1.3):

1.

5. The preparation method according to claim 1, 3 or 4, characterized in that: The thermal initiator includes ammonium persulfate solution; the initiation reaction temperature is 38-42° C. and the time is 24-30 hours.

6. The preparation method according to claim 1, 3 or 4, characterized in that: The aging time is 24 to 48 hours.

7. The preparation method according to claim 1, characterized in that: The ratio of the mass of the activated carbon powder to the volume of the iron-loaded aluminum covalent bond coagulant in the iron-loaded aluminum covalent bond coagulant solution is 1 g: (2 to 8) mL.

8. The preparation method according to claim 1 or 7, characterized in that: The temperature of the modification reaction is 24-26° C. and the time is 23-25 ​​hours.

9. The iron-loaded aluminum covalent bond coagulant modified activated carbon material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the activated carbon material modified by the iron-aluminum covalent bond coagulant according to claim 9 in the treatment of organic arsenic wastewater.

Citation Information