A method for resource utilization of all particle sizes of slurry shield slag

Through the precipitation and grading treatment system, the problem of insufficient full particle size treatment in the existing technology is solved, and efficient and economical waste soil resource utilization and waste slurry treatment are achieved, reducing environmental pollution and improving Reuse rate and utilization value of waste soil.

CN117920732BActive Publication Date: 2024-11-29OCEAN UNIV OF CHINA

Patent Information

Application Number
CN202410165250.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2024-11-29
Estimated Expiration
2044-02-05

AI Technical Summary

Technical Problem

The existing technology has failed to effectively treat and refine the full particle size of sludge-water shield slag, resulting in a single treatment method, high energy consumption, low reuse rate, and a lack of efficient waste slurry treatment methods, which has negative impact on the environment.

Method used

Using precipitation treatment system, slag grading system and grading utilization system, the mud-water shield slag is graded according to the full particle size, and is passed through quicklime, aluminum sulfate precipitation, vibrating screen, grinding, cyclone sand detergent, drying, and airflow Equipment such as graders and centrifuges are refined to separate slags of different particle sizes, and their utilization value is enhanced by additives such as soda ash and humic acid.

Benefits of technology

The full-particle size resource utilization of mud-water shield slag has been realized, the reuse rate of slag has been improved, environmental pollution has been reduced, and a variety of suitable slag products and planting soil have been provided, with good economic and environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117920732B_ABST
    Figure CN117920732B_ABST
Patent Text Reader

Abstract

The invention discloses a method for resource utilization of full-particle size of slurry shield slag. The method comprises the following steps: firstly, the slag generated during the construction of the slurry shield is collected and added with a flocculant for precipitation; after precipitation, the slag is subjected to particle size classification by a vibrating screen, a cyclone desander, an air flow splitter, and a centrifuge, so as to separate the slag from the slurry; the slag after classification can be roughly divided into 74μm~2 mm, 2~3 mm sandy slag and 0~20μm, 20μm~74μm sticky slag, the sandy slag can be used as a sand source for synchronous grouting, concrete coarse aggregate, and asphalt mixture, and the sticky slag can be used as clay, bentonite, or replace part of cement for grouting; after screening out the slag, the remaining waste slurry is added with humic acid, biochar, and straw for fermentation, and after drying, it forms planting soil. The invention can realize the resource utilization of full-particle size of slurry shield slag.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of shield slag improvement, and relates to a method for resource utilization of all particle sizes of slurry shield slag. Background Art

[0002] Due to the advantages of shield method such as fast construction speed, high efficiency and little impact on urban life, it has been widely used in the construction of underground projects such as tunnels and subways. With the development of urbanization, the construction of urban rail transit is also accelerating, and with it comes the problem of a large amount of waste soil generated by the construction of subway tunnels. How to effectively and standardizedly dispose of and recycle these shield soil is a major problem facing today's society.

[0003] Shield slag refers to the abandoned soil and mud generated during the construction of shield tunnels. Slurry shields will produce a lot of waste mud. After dehydration, the abandoned slurry of slurry shields will become slag for subsequent treatment. Most projects have waste slurry pools for storage. As my country pays more and more attention to environmental protection, the treatment of shield slag during construction has become more stringent and standardized. From the perspective of law and management, the slag and mud generated by shield tunnel construction should be classified as construction waste. The amount of construction slag and mud in my country's annual construction waste accounts for more than half, among which the amount of shield tunnel slag and mud increases year by year. Generally, these slag and mud are disposed of by stacking and simple landfill, which has a serious negative impact on the urban environment. Although my country's shield slag recycling has made great progress, the recycling rate of slag is not high due to the single reuse method and high energy consumption.

[0004] Compared with the earth pressure balance shield, the slag is mainly composed of clay and coarse particles (silt, sand and gravel), so it is necessary to add foaming agent to transform the slag. The products of the slurry shield are mainly composed of slag and mud in a state close to sand and silty sand, and no additional modifier is needed. At present, the resource utilization of the slurry shield is mainly separated from the fine mud by grading. The sand and gravel can be used as concrete raw materials to generate economic benefits, but the graded fine mud is still mainly treated by landfill method, or used in the preparation of building materials, ceramsite, fill materials and concrete aggregates.

[0005] Compared with the existing technology, there are a series of deficiencies in the resource utilization of slurry shield slag:

[0006] 1. In the current patented technology for resource utilization of slurry shield slag, the treatment and classification of slurry shield slag are simple, and only some particle sizes are taken into consideration, such as 20-74μm and 2-3mm shield slag, and the full-size slag cannot be graded according to the full-size size.

[0007] 2. The existing patented technology is rather vague in the classification of different particle sizes and fails to fully distinguish the viscosity and sand characteristics of slag with different particle sizes, so that resource utilization cannot achieve the optimal effect.

[0008] 3. In the current patented technology for resource utilization of slurry shield slag, the slurry shield slag treatment method uses individual mesh slag for backfilling, grouting or direct disposal. There are few treatment methods and a lack of efficient and thorough treatment methods.

[0009] 4. Among the current patent technologies for resource utilization of slurry shield slag, there is a technology that replaces bentonite with 20-74μm clay slag. However, compared with bentonite, its water absorption rate is too low. There are few studies on the comprehensive treatment of 20-74μm and 0-20μm clay slag and its optimized use in combination with water absorption rate.

[0010] 5. At present, most of the remaining mud in the patented technology of slurry shield slag resource utilization is dehydrated by plate and frame filter press and converted into mud cake for discharge or directly discarded, which will cause a certain burden on the environment. It is urgent to find a green and environmentally friendly way to deal with waste mud. Summary of the invention

[0011] In view of the problems caused by the above situation, the present invention proposes a method for resource utilization of all particle sizes of slurry shield slag. The main purpose is to separate the mud and slag in the slurry shield slag and process the slag in each particle size range. Through the treatment of the sedimentation treatment system, the slag classification system, and the classification utilization system, the resource utilization of all particle sizes of the slurry shield slag is realized.

[0012] In order to achieve the above object, the present invention adopts the following technical solutions:

[0013] (1) Collect the slurry shield waste, add quicklime and aluminum sulfate to precipitate for 6 hours, and remove the upper water.

[0014] (2) After removing the upper layer of water, the remaining mud, water and slag mixture is sent to the vibrating screen to separate the coarse slag particles with a particle size greater than 3 mm and other impurities at a speed of 800-900 r / min.

[0015] (3) The coarse particles of slag with a particle size greater than 3 mm in (2) are placed in a grinder, ground and sieved to a particle size of 2.25 to 2.5 mm to obtain product I.

[0016] (4) The product of (2) is passed through a cyclone desander at a water inlet pressure of 0.2 to 1.2 MPa and a rotation speed of 3000 to 5000 r / min to screen out sandy slag with a particle size of 2 to 3 mm.

[0017] (5) The sandy slag in (4) is placed in a dryer and dried at 80-100° C. for 24 h to reduce the internal moisture content to less than 10%, thereby obtaining product II.

[0018] (6) After removing the 2-3 mm sandy soil in step (4), the remaining soil is placed in a dryer and dried at 60-80° C. for 24 h.

[0019] (7) The product in (6) is passed through a first-stage air classifier at a speed of 6 to 8 m 3 / min ventilation volume and 3500-4000r / min rotation speed can screen out sandy particles of 74μm-2mm.

[0020] (8) The sieved sandy particles of 74 μm to 2 mm were placed in a drying oven and dried at 60 to 80 °C for 12 h to obtain product III.

[0021] (9) The remaining slag in (7) is passed through a two-stage air classifier at a rate of 10 to 12 m 3 / min ventilation volume and 4000-4200r / min rotation speed can screen out the sticky shield slag of 20μm-74μm.

[0022] (10) The sieved viscous shield slag with a size of 20 μm to 74 μm is placed in a dryer and dried at 70 to 80° C. for 8 h to obtain product IV.

[0023] (11) The remaining product in (9) is passed through a centrifuge at a speed of 5000 to 6000 r / min to separate the viscous slag with a size of 0 to 20 μm.

[0024] (12) The 0-20 μm sticky slag is placed in a dryer and dried at 70-80 °C for 8 h to obtain product V.

[0025] (13) The obtained products IV and V were placed in a blender at a mass ratio of 1:3, 3% of a soda ash reagent was added, and the mixture was stirred at 200-300 r / min for 10 min to obtain a product VI.

[0026] (14) The remaining waste slurry is added with humic acid, biochar, and straw in a mass ratio of 1:1:5-7, and fermented for 48 hours. After fermentation, the soil is naturally dried to obtain a planting soil.

[0027] In the above-mentioned method for resource utilization of all-particle sizes of slurry shield slag, the flocculants mostly used in step (1) are quicklime and aluminum sulfate, and the amount used is 0.1% of the mass of the slurry shield slag.

[0028] In the above-mentioned method for resource utilization of all-particle sizes of slurry shield slag, the frequency of the vibrating screen in step (2) is 800-900 r / min.

[0029] In the above-mentioned method for resource utilization of all-particle sizes of slurry shield slag, in step (4), the water inlet pressure of the cyclone desander is 0.2-1.2 MPa and the rotation speed is 3000-5000 r / min.

[0030] In the above-mentioned method for resource utilization of all-particle sizes of slurry shield slag, in step (5), the oven temperature is 80-100° C. and the slurry is dried for 24 hours.

[0031] In the above-mentioned method for resource utilization of all-particle size slurry shield slag, in step (6), the slurry is dried in an oven at a temperature of 60 to 80° C. for 24 hours to make the internal water content less than 40%.

[0032] In the above-mentioned method for resource utilization of all-particle size slurry shield slag, the ventilation volume of the first-stage air classifier in step (7) is 6 to 8 m 3 / min, the speed is 3500~4000r / min.

[0033] In the above-mentioned method for resource utilization of all-particle sizes of slurry shield slag, in step (8), the temperature of the drying machine is 60-80° C. and the duration is 12 hours.

[0034] In the above-mentioned method for resource utilization of all-particle size slurry from slurry shield tunneling, the ventilation volume of the second-stage air classifier in step (9) is 10 to 12 m 3 / min, the speed is 4000~4200r / min.

[0035] In the above-mentioned method for resource utilization of all-particle sizes of slurry shield slag, in step (10), the temperature of the drying machine is 70-80° C. and the duration is 8 hours.

[0036] In the above-mentioned method for resource utilization of all-particle size slurry shield slag, the centrifuge speed in step (11) is 5000-6000 r / min.

[0037] In the above-mentioned method for resource utilization of all-particle sizes of slurry shield slag, in step (12), the temperature of the drying machine is 70-80° C. and the duration is 8 hours.

[0038] In the above-mentioned method for resource utilization of all-particle sizes of slurry shield slag, the moisture content of product IV and product V in step (10) and step (12) is 15-25%.

[0039] In the above-mentioned method for resource utilization of all-particle sizes of slurry shield slag, in step (13), the stirring speed of the mixer is 200-300 r / min, and the stirring is carried out for 10 minutes.

[0040] In the above-mentioned method for resource utilization of all-particle sizes of slurry shield slag, in step (14), the slag is naturally aired until the moisture content reaches 15-25%.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] 1. The present invention uses different devices to refine the slurry shield slag to the full particle size, separates the slag of different particle sizes from the mud, separates the coarse slag particles larger than 3mm by a vibrating screen; screens out the sandy particles of 2-3mm by a cyclone desander; separates the viscous shield slag of 74μm-2mm by a first-level airflow classifier; separates the viscous shield slag of 20μm-74μm by a second-level airflow classifier; separates the viscous shield slag of 0-20μm by a centrifuge. Compared with other patented technologies that only separate a small amount of slag, this patent can combine multiple facilities to separate the slurry shield slag of all particle size ranges to the maximum extent, and recycle it, so as to achieve stable and efficient resource utilization of all particle sizes, and has good economic benefits.

[0043] 2. Product I in this patent has a larger particle size and can be used in concrete coarse aggregate, asphalt mixture, etc.; Product II can be directly used as a source of coarse sand and applied to synchronous grouting projects; Product III can be used as a source of fine sand and directly applied to synchronous grouting projects; Product IV and Product V can be used as clay or replace part of the cement in grouting after mixing, and after drying, they can serve as a component of bentonite in grouting. In summary, this patent selects a more effective treatment method for different slurry shield slag products, involves multiple fields, and forms a complete full-size shield slag treatment method, which improves utilization while reducing pollution to the environment.

[0044] 3. Compared with other patented technologies that directly use one type of slag to replace bentonite in grouting, the present invention mixes 20μm-74μm sticky shield slag with 0-20μm sticky shield slag in a mass ratio of 1:3 and then adds soda ash to make sticky shield slag. While increasing the compactness of the sticky shield slag, the state and ability of its surface adsorption molecules are improved, making it closer to the water absorption of bentonite.

[0045] 4. Compared with other patented technologies that directly abandon waste pulp treatment, the present invention adds humic acid, biochar, and straw for fermentation to increase the content of microorganisms and organic matter in the soil, and applies it to planting soil after drying. The raw material processing method is simple and efficient, and has good economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION

[0047] The present invention proposes a method for resource utilization of all particle sizes of slurry shield slag. In order to make the advantages and technical solutions of the present invention clearer and more specific, the present invention is further described below in conjunction with specific embodiments.

[0048] The raw materials described in the present invention can be purchased through commercial channels.

[0049] The structures and working principles of the vibrating screen, cyclone desander, air flow splitter and centrifuge described in the present invention can be realized by referring to the existing technology.

[0050] The main technical concept of the present invention is to use a practical method to utilize the slurry shield waste in all particle sizes, and to convert the cheap and readily available slurry shield waste into valuable resource products as much as possible, that is, to transform it from low value-added to high value-added products, and the method used is simple and easy to operate.

[0051] Specifically, the present invention provides a method for resource utilization of all-particle size slurry shield slag, comprising the following steps:

[0052] (1) Collect the slurry shield waste, add quicklime and aluminum sulfate to precipitate for 6 hours, and remove the upper water.

[0053] (2) After removing the upper layer of water, the remaining mud, water and slag mixture is sent to the vibrating screen to separate the coarse slag particles with a particle size greater than 3 mm and other impurities at a speed of 800-900 r / min.

[0054] (3) The coarse particles of slag with a particle size greater than 3 mm in (2) are placed in a grinder, ground and sieved to a particle size of 2.25 to 2.5 mm to obtain product I.

[0055] (4) The product of (2) is passed through a cyclone desander at a water inlet pressure of 0.2 to 1.2 MPa and a rotation speed of 3000 to 5000 r / min to screen out sandy slag with a particle size of 2 to 3 mm.

[0056] (5) The sandy slag in (4) is placed in a dryer and dried at 80-100° C. for 24 h to reduce the internal moisture content to less than 10%, thereby obtaining product II.

[0057] (6) After removing the 2-3 mm sandy soil in step (4), the remaining soil is placed in a dryer and dried at 60-80° C. for 24 h.

[0058] (7) The product in (6) is passed through a first-stage air classifier at a speed of 6 to 8 m 3 / min ventilation volume and 3500-4000r / min rotation speed can screen out sandy particles of 74μm-2mm.

[0059] (8) The sieved sandy particles of 74 μm to 2 mm were placed in a drying oven and dried at 60 to 80 °C for 12 h to obtain product III.

[0060] (9) The remaining slag in (7) is passed through a two-stage air classifier at a rate of 10 to 12 m 3 / min ventilation volume and 4000-4200r / min rotation speed can screen out the sticky shield slag of 20μm-74μm.

[0061] (10) The sieved viscous shield slag with a size of 20 μm to 74 μm is placed in a dryer and dried at 70 to 80° C. for 8 h to obtain product IV.

[0062] (11) The remaining product in (9) is passed through a centrifuge at a speed of 5000 to 6000 r / min to separate the viscous slag with a size of 0 to 20 μm.

[0063] (12) The 0-20 μm sticky slag is placed in a dryer and dried at 70-80° C. for 8 h to obtain product V.

[0064] (13) The obtained products IV and V were placed in a blender at a mass ratio of 1:3, 3% of a soda ash reagent was added, and the mixture was stirred at 200-300 r / min for 10 min to obtain a product VI.

[0065] (14) The remaining waste slurry is added with humic acid, biochar, and straw for fermentation for 48 hours, and then naturally dried after fermentation to obtain a planting soil.

[0066] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application:

[0067] 1000 kg of slurry shield slag produced in the same place were respectively taken, and the implementation method of the present invention was used for comparison with the currently popular implementation method.

[0068] Embodiment 1:

[0069] (1) Collect the slurry shield waste, add quicklime and aluminum sulfate to precipitate for 6 hours, and remove the upper layer of moisture.

[0070] (2) After removal, the slag is sent to a vibrating screen at a frequency of 800 r / min to separate coarse slag particles with a particle size greater than 3 mm and other impurities.

[0071] (3) The coarse particles of slag with a particle size greater than 3 mm in (2) are placed in a grinder, ground to a particle size of 2.25 to 2.5 mm, and sieved to obtain product I.

[0072] (4) The product of (2) is passed through a cyclone desander to screen out sandy slag with a particle size of 2 to 3 mm at an inlet water pressure of 1 MPa and a rotation speed of 3000 r / min.

[0073] (5) The sandy slag in (4) is placed in a dryer and dried at 80° C. for 24 h to reduce the internal moisture content to less than 10%, thereby obtaining product II.

[0074] (6) The slag after the sandy slag is removed in (4) is placed in a dryer and dried at 80° C. for 24 hours to reduce the internal moisture content to less than 40%.

[0075] (7) The product in (6) is passed through a first-stage air classifier at 6 m 3 / min gas volume, 3500r / min rotation speed to screen out sandy particles of 74μm~2mm, put them into a dryer, and dry them at 60~80℃ for 12h to obtain product III.

[0076] (8) The remaining slag in (7) is passed through a two-stage air classifier at a rate of 10 m 3 / min gas volume and 4200r / min rotation speed to screen out 20μm-74μm sticky shield slag and put it into the dryer at 80℃ for 8h to obtain product IV.

[0077] (9) The remaining product in (8) was centrifuged at 6000 r / min to separate the sticky residue with a size of 0 to 20 μm, and placed in a dryer and dried at 80° C. for 8 h to obtain product V.

[0078] (10) Product IV and product V obtained in (8) and (9) were placed in a blender at a mass ratio of 1:3, and 3% soda ash reagent was added. The mixture was stirred at 200 r / min for 10 min to obtain product VI.

[0079] (11) The remaining waste slurry is added with humic acid, biochar, and straw for fermentation for 48 hours, and then naturally aired after fermentation to obtain a planting soil.

[0080] Embodiment 2:

[0081] (1) Collect the slurry shield waste, add quicklime and aluminum sulfate to precipitate for 6 hours, and remove the upper layer of moisture.

[0082] (2) After removal, the slag is sent to a vibrating screen at a frequency of 900 r / min to separate coarse slag particles with a particle size greater than 3 mm and other impurities.

[0083] (3) The coarse particles of slag with a particle size greater than 3 mm in (2) are placed in a grinder, ground to a particle size of 2.25 to 2.5 mm, and sieved to obtain product I.

[0084] (4) The product of (2) is passed through a cyclone desander to screen out sandy slag with a particle size of 2 to 3 mm at an inlet water pressure of 0.8 MPa and a rotation speed of 4500 r / min.

[0085] (5) The sandy slag in (4) is placed in a dryer and dried at 90° C. for 24 h to reduce the internal moisture content to less than 10%, thereby obtaining product II.

[0086] (6) The slag after the sandy slag is removed in (4) is passed through a dryer and dried at 65° C. for 24 hours to reduce the internal moisture content to less than 40%.

[0087] (7) The product in (6) is passed through a first-stage air classifier at 7 m 3 / min gas volume, 3800r / min rotation speed to screen out sandy particles of 74μm~2mm, put them into a dryer, and dry them at 70℃ for 12h to obtain product III.

[0088] (8) The remaining slag in (7) is passed through a two-stage air classifier at 12m 3 / min gas volume and 4200r / min rotation speed to screen out 20-74μm sticky shield slag and put it into the dryer at a temperature of 70-80℃ for 8h to obtain product IV.

[0089] (9) The remaining product in (8) was centrifuged at 6000 r / min to separate the sticky residue of 0 to 20 μm, and placed in a dryer and dried at 75° C. for 8 h to obtain product V.

[0090] (10) The products IV and V obtained in (8) and (9) were placed in a blender at a mass ratio of 1:3, 3% soda ash reagent was added and mixed thoroughly, and stirred at 210 r / min for 10 min to obtain product VI.

[0091] (11) The remaining waste slurry is added with humic acid, biochar, and straw for fermentation for 48 hours, and then naturally aired after fermentation to obtain a planting soil.

[0092] Comparative Example:

[0093] (1) Collect the slurry shield waste, add quicklime and aluminum sulfate to precipitate for 6 hours, and remove the upper layer of moisture.

[0094] (2) After removal, the slag is sent to a vibrating screen at a frequency of 800 r / min to separate coarse slag particles with a particle size greater than 3 mm and other impurities.

[0095] (3) The product of (2) is passed through a cyclone desander to screen out sandy slag with a particle size of 2 to 3 mm at a water inlet pressure of 0.2 to 1.2 MPa and a rotation speed of 3000 to 5000 r / min.

[0096] (4) The sandy soil in (3) is placed in a dryer and dried at 80° C. for 24 hours until the internal moisture content is less than 10%.

[0097] (5) The remaining slag in (4) is passed through an air classifier at a rate of 10 m 3 / min gas volume and 4000r / min rotation speed to screen out viscous shield slag with a size of 20-74μm and put it into the dryer at a temperature of 70-80℃ for 8h.

[0098] (6) The remaining waste slurry is dehydrated by a plate and frame filter press and converted into mud cake and discharged or directly discarded.

[0099]

[0100] By comparison, it is found that the method for resource utilization of all particle sizes of slurry shield slag in this patent application is better than the commonly used slag treatment method, and it can treat and utilize all particle sizes, with better utilization rate and less waste slurry. Therefore, the method for resource utilization of all particle sizes of slurry shield slag proposed in this patent is a treatment method with higher utilization rate, more refinement and greener.

[0101] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present application and are not intended to be limiting of the present application. As long as they are within the spirit and scope of the present application, appropriate changes and modifications to the above embodiments are within the scope of protection claimed in the present application.

Claims

1. A method for resource utilization of all particle sizes of slurry shield slag, characterized in that: The following steps are included in sequence: (1) Collect the slurry shield waste, add quicklime and aluminum sulfate to precipitate for 6 hours, and remove the upper water; (2) After removing the upper layer of water, the remaining mud, water and soil mixture is sent to the vibrating screen to separate the coarse soil particles with a particle size greater than 3 mm and other impurities at a speed of 800-900 r / min; (3) placing the coarse soil particles with a particle size greater than 3 mm in (2) into a grinder, grinding and sieving to a particle size of 2.25 to 2.5 mm, to obtain product I; (4) passing the product of (2) through a cyclone desander at a water inlet pressure of 0.2 to 1.2 MPa and a rotation speed of 3000 to 5000 r / min to screen out sandy slag with a particle size of 2 to 3 mm; (5) placing the sandy soil in (4) into a dryer and drying it at 80-100° C. for 24 h until the internal moisture content is less than 10%, thereby obtaining product II; (6) After removing the 2-3 mm sandy soil in (4), the remaining soil is placed in a dryer and dried at 60-80° C. for 24 h; (7) The product in (6) is passed through a first-stage air classifier at a speed of 6 to 8 m 3 / min ventilation volume, 3500-4000r / min rotation speed to screen out sandy particles of 74μm-2mm; (8) placing the sieved sandy particles of 74 μm to 2 mm into a drying oven and drying them at 60 to 80° C. for 12 h to obtain product III; (9) The remaining slag in (7) is passed through a two-stage air classifier at a rate of 10 to 12 m 3 / min ventilation volume, 4000-4200r / min rotation speed to screen out 20μm-74μm sticky shield slag; (10) The 20 μm to 74 μm viscous shield slag screened out is placed in a dryer and dried at 70 to 80° C. for 8 h to obtain product IV; (11) passing the remaining product in (9) through a centrifuge at a speed of 5000 to 6000 r / min to separate the viscous residue of 0 to 20 μm; (12) placing the 0-20 μm sticky slag into a dryer and drying it at 70-80° C. for 8 h to obtain product V; (13) Put the obtained products IV and V into a blender at a mass ratio of 1:3, add 3% soda ash reagent, stir at 200-300 r / min for 10 min to fully mix, and obtain product VI; (14) adding humic acid, biochar and straw to the remaining waste slurry at a mass ratio of 1:1:5-7, fermenting for 48 hours, and naturally drying after fermentation to obtain a planting soil; (15) The product I obtained in step 3 is directly used as coarse aggregate for concrete preparation or asphalt mixture; (16) Product II obtained in step 5 has a particle size between 2 and 3 mm and directly replaces the coarse sand source in synchronous grouting; (17) Product III obtained in step 8 has a particle size between 74 μm and 2 mm and directly replaces the fine sand source in synchronous grouting; (18) The products IV and V obtained in step 10 and step 12 replace the clay or part of the cement component in the simultaneous grouting.

Citation Information

Patent Citations

  • Shield muck recycling modifying process method

    CN113182328A

  • Urban shield muck treatment system and treatment method thereof

    CN117228884A

Cited By

  • Preparation method and application of modified shield soil recycled coarse aggregate

    CN121270131A