Oxygen-enriched hydrogel compounded with acellular skeletal muscle matrix as well as preparation method and application of oxygen-enriched hydrogel
Through the cross-linking reaction of the composite acellular skeletal muscle matrix and perfluorotri-n-butylamine emulsion, an oxygen-rich hydrogel is formed, which solves the problems of hypoxia and excessive ROS in skeletal muscle repair materials and provides a microenvironment similar to natural skeletal muscle. , promotes skeletal muscle regeneration and repair, and has good biocompatibility and mechanical properties.
Patent Information
- Application Number
- CN202410771580.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-15
- Publication Date
- 2024-10-18
AI Technical Summary
Existing skeletal muscle repair materials are hypoxic in the early stage of damaged tissue and may produce excessive superoxide radicals in the later stage of repair. They do not consider the microenvironmental differences between the implanted material and the damaged tissue, resulting in low cell survival rate and immune response. .
Oxygen-rich hydrogel using a composite acellular skeletal muscle matrix is used to form a structure and biological phase similar to natural skeletal muscle through the cross-linking reaction of methacrylic gelatin, acellular skeletal muscle matrix fluid and perfluorotri-n-butylamine emulsion. Capacitive hydrogel provides sufficient oxygen and simulates the microenvironment of skeletal muscle.
The hydrogel provides sufficient oxygen in the early stage of tissue repair, promotes vascularization and cell proliferation, reduces ROS production, improves cell survival rate, provides the closest natural microenvironment, is conducive to the regeneration and repair of skeletal muscle, and has good biological properties. Compatibility and mechanical properties.
Smart Images

Figure BDA0004894201160000061 
Figure HDA0004894201170000011 
Figure HDA0004894201170000012
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of skeletal muscle tissue repair materials, and in particular to an oxygen-enriched hydrogel of a composite decellularized skeletal muscle matrix and a preparation method and application thereof. Background Art
[0002] Skeletal muscle is abundant in the human body, accounting for about 40% of the body weight of an adult. Slightly injured skeletal muscle has a very high regenerative capacity, but due to large-scale loss of skeletal muscle due to combat injuries, traffic accidents, etc., including loss of essential regenerative components such as satellite cells and perivascular stem cells, the endogenous self-repair ability will be severely impaired. Insufficient muscle regeneration will lead to excessive fibrosis and scar formation, resulting in muscle dysfunction or even loss of function, which greatly affects the patient's quality of life. At present, healthy autologous skeletal muscle tissue can be used clinically to replace damaged or missing muscles, but autologous tissue transplantation is expensive and accompanied by great risks, and complete functional recovery cannot be guaranteed after successful surgery. Therefore, in the field of biomedicine, the repair and regeneration of skeletal muscle tissue has attracted much attention. In recent years, attempts have been made to use decellularized biological scaffolds, growth factors, stem cells and other natural and synthetic materials for the regeneration and functional recovery of skeletal muscle. However, in the case of severe damage to the structural integrity of muscle tissue, simple cell delivery or cytokine injection has problems such as poor survival of implanted cells and short cell retention time at the implantation site.
[0003] Oxygen is a nutrient necessary for the survival of multicellular organisms. It can regulate cell activities, promote angiogenesis and collagen synthesis during tissue repair and wound healing, and kill anaerobic bacteria, so that some antibiotics can exert a certain antibacterial effect. Studies have shown that ischemia and hypoxia are common after the interruption of blood flow in fractures. Hypoxia can lead to abnormal bone metabolism. Hypoxia in the bone marrow microenvironment has a great influence on the dynamic balance between bone formation and bone resorption. Especially in the process of tissue repair or cell transplantation, the damaged tissue will gradually become vascularized, thereby providing oxygen for activities such as cell proliferation and cell migration. However, before this, the damaged tissue cannot provide enough oxygen to maintain cell proliferation and migration. Therefore, it is necessary to provide enough oxygen in the early 4-7 days of tissue repair. Cells are very sensitive to hypoxic environments. A large lack of oxygen will eventually lead to cell death and tissue necrosis, which to a certain extent also limits the practical application of tissue engineering products.
[0004] Research has found that using oxygen-releasing materials to transport oxygen to implanted body tissues to avoid hypoxia is one of the most effective ways. Oxygen-releasing materials are systems that achieve controlled release of oxygen by loading oxygen source compounds on carrier materials. In recent years, regulating the local or systemic oxygen microenvironment to promote wound repair and regeneration has gradually become an emerging direction. For example, invention patent CN115887781B discloses a method for preparing an injectable hydrogel for cartilage damage repair. Silk protein solution, E7 peptide solution, bovine serum albumin nanoparticle dispersion loaded with 2-([1,1-biphenyl]-4-ylcarbamoyl)benzoic acid, horseradish peroxidase aqueous solution and hydrogen peroxide solution are mixed to obtain an injectable hydrogel for cartilage damage repair. Invention patent CN115536920B discloses a chitosan derivative-based wound repair hydrogel and its preparation method and application. The method first uses chitosan as a raw material, couples epoxypropyl trimethyl ammonium chloride at its C6-OH, and then couples caffeic acid at its amino group to obtain O-epoxypropyl trimethyl ammonium chloride-N-caffeoyl chitosan; then, dopamine is used as a raw material to prepare polydopamine; finally, the chitosan derivative and polydopamine are compounded and cross-linked into a gel through a mixed cross-linking agent system of hydrogen peroxide and horseradish peroxidase. However, the oxygen-releasing material peroxide used in the above method will be affected by many factors during the release of oxygen, such as pH, temperature, and peroxide microstructure, which will affect the release time and amount of oxygen. At the same time, peroxide will produce ROS (superoxide radicals) when releasing oxygen. A certain amount of superoxide radicals has a killing effect on bacteria, but excessive ROS will mediate cell oxidative stress response, produce certain toxicity on cells, and lead to low cell survival rate. More importantly, the current system is almost all pure oxygen release without considering the impact of the microenvironment on the repair of damaged tissues. If the biological scaffold has functions and microenvironment similar to natural skeletal muscle, it will be more conducive to cell adhesion and growth, myoblast proliferation and differentiation, and promote the ability of vascular regeneration. It can simulate the development process of skeletal muscle through a combination of exogenous and endogenous pathways to complete skeletal muscle repair, and repair skeletal muscle defects quickly and evenly through inherent myogenesis mechanisms.
[0005] Hydrogel is a three-dimensional network scaffold material formed by cross-linking hydrophilic polymers. It has a water content of up to 90%, has excellent biocompatibility and degradability, and is a commonly used type of biomaterial for the treatment of ischemic tissue. When hydrogel is used as a cell carrier to treat ischemic tissue, the hypoxia inside the large hydrogel will hinder cell vitality, function and tissue repair. Therefore, using hydrogel as a carrier to encapsulate or mix oxygen-releasing substances to prepare an oxygen-releasing hydrogel has good development prospects. How to prepare a hydrogel that has similar properties and biocompatibility to natural skeletal muscle, and can release enough oxygen in the early stage of tissue repair to complete the vascularization of damaged skeletal muscle and promote skeletal muscle regeneration and repair has become an urgent problem to be solved. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide an oxygen-enriched hydrogel of a composite decellularized skeletal muscle matrix and a preparation method and application thereof, so as to solve the problems of existing repair materials such as hypoxia in the early stage of damaged tissue or excessive ROS generation in the late stage of repair, and failure to consider the differences between implanted materials and damaged tissue.
[0007] In order to solve the above technical problems, the present invention adopts the following technical scheme: an oxygen-enriched hydrogel of a composite decellularized skeletal muscle matrix, the hydrogel comprising methacrylate gelatin, decellularized skeletal muscle matrix liquid and oxygen-carrying perfluorotri-n-butylamine emulsion, the hydrogel using methacrylate anhydride-modified gelatin hydrogel as a matrix, perfluorotri-n-butylamine and decellularized matrix liquid cross-linked with methacrylate gelatin. Among them, after the natural skeletal muscle is treated, the cellular components in the skeletal muscle tissue are effectively removed, the immunogenicity of the heterologous tissue is eliminated, the active components of the skeletal muscle extracellular matrix are retained, and the major histocompatibility complex class I and class II antigens are not contained, and it has the characteristics of anti-inflammatory and immunosuppressive effects, etc. The skeletal muscle extracellular matrix contains rich cytokines that can promote the regeneration of skeletal muscle. After decellularization, the skeletal muscle can be used as a natural scaffold for tissue engineering, providing a good microenvironment for skeletal muscle repair. Gelatin is a protein extracted from collagen, mainly from animal bones and skin, and also found in some insects. Compared with collagen, gelatin has many advantages such as low price, good biocompatibility, and biodegradability. The gelatin derivative methacrylate gelatin has the characteristics of photocrosslinking, excellent mechanical properties, degradability and biocompatibility. The hydrogel scaffold material prepared by methacrylate gelatin is also a good delivery carrier.
[0008] Preferably, the mass-to-volume ratio of the methacrylate gelatin, the decellularized skeletal muscle matrix fluid and the perfluorotri-n-butylamine emulsion is 0.05-0.3 g: 200-800 μL: 400-800 μL.
[0009] Preferably, the Young's modulus of the hydrogel is 5-20 kPa, and the porosity is 20%-90%. The Young's modulus of the hydrogel can be made close to that of natural skeletal muscle (10 kPa) by adjusting the content of methacrylate gelatin, thus providing a suitable microenvironment for the growth of skeletal muscle cells.
[0010] Another object of the present invention is to provide a method for preparing the above-mentioned composite decellularized skeletal muscle matrix oxygen-enriched hydrogel, comprising the following steps:
[0011] 1) adding a benchtop liquid solution to egg yolk lecithin (purity 99%), ultrasonically treating the mixture for multiple times, then adding perfluorotri-n-butylamine, and ultrasonically treating the mixture for multiple times, and filtering the emulsion after ultrasonication to obtain a perfluorotri-n-butylamine emulsion;
[0012] 2) placing the perfluorotri-n-butylamine emulsion obtained in step 1) in an oxygen-rich environment to dissolve enough oxygen;
[0013] 3) adding methacrylic anhydride to the gelatin solution for reaction and then freeze-drying to obtain modified methacrylic acid-gelatin, dispersing the obtained decellularized skeletal muscle matrix liquid in the methacrylic acid-gelatin, and then adding a photoinitiator to obtain a composite liquid;
[0014] 4) adding the perfluorotri-n-butylamine emulsion treated in step 2) to the composite solution obtained in step 3) to obtain a reaction solution, and obtaining the oxygen-enriched decellularized skeletal muscle matrix hydrogel after irradiation with ultraviolet light to form a gel.
[0015] Preferably, in step 1), the mass volume ratio of egg yolk phosphatidylcholine to perfluorotri-n-butylamine is 80-110 mg: 300-600 μL.
[0016] Preferably, in the ultrasonic treatment process in step 1), the ultrasonic power is greater than 200 W, the ultrasonic time is greater than 10 s, the ultrasonic interval is greater than 1 min, and the number of ultrasonic times is greater than 2 times. Preferably, the ultrasonic power is 200-500 W, the ultrasonic time is 5-60 s, the ultrasonic interval is 30-300 s, and the number of ultrasonic times is 1-30 times.
[0017] Preferably, the pH value of the decellularized skeletal muscle matrix fluid in step 3) is 6.8-7.5.
[0018] Preferably, the photoinitiator in step 3) is 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone (I2959) or phenyl-2, 4, 6-trimethylbenzoyl phosphite lithium (LAP), 2,2′-azobis[2-methyl-N-(2-hydroxyethyl)propionamide] (VA-086), diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (TPO), 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone (HMPP) or 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone (PI).
[0019] Preferably, the amount of the photoinitiator added is 0.5-5% of the mass of the reaction solution.
[0020] Another object of the present invention is to provide the use of the oxygen-enriched hydrogel of the composite decellularized skeletal muscle matrix or the oxygen-enriched hydrogel prepared by the above method in the regeneration and repair of skeletal muscle tissue.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The oxygen-enriched hydrogel provided by the present invention uses methacrylate gelatin as the base material of the hydrogel, and is also compounded with decellularized skeletal muscle and oxygen-carrying perfluorotri-n-butylamine emulsion to form a hydrogel scaffold material with uniform structure. During the compounding process of the raw materials, there are mutual reactions and chemical bond breakage and recombination between the materials, rather than simple physical mixing. The decellularized skeletal muscle matrix added therein removes the cellular components in the tissue, so that the obtained hydrogel not only has a three-dimensional porous structure similar to natural skeletal muscle, but also contains natural fiber components such as collagen fibers and a variety of cell growth factors, etc., which can provide the closest natural microenvironment for tissue repair without causing immune rejection, which is conducive to the adhesion and growth of cells, and is also conducive to the proliferation and differentiation of skeletal muscle cells, etc., and can promote the repair and regeneration of skeletal muscle tissue. The oxygen-enriched hydrogel prepared by the present invention not only has good hydrophilicity, but also has a three-dimensional network structure and mechanical properties similar to natural skeletal muscle, and is an ideal material for soft tissue repair with great potential.
[0023] 2. The oxygen-enriched hydrogel prepared by the present invention is compounded with acellular skeletal muscle matrix and perfluorotri-n-butylamine emulsifier, which can promote the repair and regeneration of damaged skeletal muscle tissue from both exogenous and endogenous sources. On the one hand, the growth factors contained in the decellularized skeletal muscle matrix can well promote the adhesion, proliferation and differentiation of satellite cells in skeletal muscle, and recruit endogenous stem cells to induce their differentiation into new skeletal muscle cells. On the other hand, the present invention is also compounded with perfluorotri-n-butylamine emulsifier, and the exogenous oxygen dissolved in it can well promote the proliferation and growth of cells. The present invention combines the improvement of the internal microenvironment with the delivery of exogenous oxygen, which can promote the repair and regeneration of damaged skeletal muscle from two aspects at the same time, and has good application prospects.
[0024] 3. The present invention uses gelatin and decellularized skeletal muscle matrix as raw materials, both of which are natural biomaterials, with low price, good biocompatibility, and simple preparation method. The prepared hydrogel can provide an appropriate amount of oxygen when a vascularized structure is formed in the early stage of skeletal muscle damaged tissue repair, and the hydrogel has a dense porous structure with macropores and small pores staggered, which is more conducive to the release and transportation of oxygen, and solves the problem of hypoxia in the early stage of damaged tissue or excessive ROS in the later stage of repair. Therefore, the hydrogel of the present invention is a very safe and easily available biomaterial, which is expected to provide a new research method and approach for the preparation of a new oxygen-releasing hydrogel, and has a good application scenario for skeletal muscle tissue repair. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A is a comparison of skeletal muscle tissue before and after decellularization; A is a general observation of skeletal muscle before and after decellularization; B is the DNA quantification result before and after decellularization; C is the HE staining result of fresh skeletal muscle; D is the HE staining result after decellularization; E is the Masson staining result of fresh skeletal muscle; F is the Masson staining result after decellularization.
[0026] Figure 2 These are photos of the oxygen-enriched hydrogels prepared in the present invention, A is Comparative Example 2, and B is Comparative Example 1.
[0027] Figure 3 It is a mechanical property diagram of the oxygen-enriched hydrogel prepared in the present invention; A is Young's modulus; B is the stress-strain curve.
[0028] Figure 4 is the hydrophilic property of the oxygen-enriched hydrogel prepared in the present invention; A is the swelling property; B is the water absorption property; and C is the water retention property.
[0029] Figure 5 This is the infrared spectrum of the oxygen-enriched hydrogel prepared in the present invention.
[0030] Figure 6 The figure is a curve showing the change of dissolved oxygen content of the oxygen-enriched hydrogel prepared in the present invention in PBS.
[0031] Figure 7 The scanning electron microscope images are of the surface and cross-section of the oxygen-enriched hydrogel prepared in the present invention, with a scale of 200 μm. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below with reference to the examples. The reagents used in the examples are commercially available unless otherwise specified.
[0033] Example 1
[0034] An oxygen-enriched hydrogel composited with acellular skeletal muscle matrix is prepared by the following method:
[0035] 1) Collect fresh porcine skeletal muscle tissue and place it in a sterile culture dish, add enough phosphate buffer to completely cover the tissue, remove the muscle membrane and fat on the surface of the skeletal muscle tissue, and cut the skeletal muscle tissue into small pieces of about 0.5 cm, then place the small pieces of skeletal muscle in a centrifuge tube filled with phosphate buffer, and perform freeze-thaw cycles (freeze the tissue in a -80°C refrigerator for more than 6 hours, then thaw in a 37°C constant temperature water bath for about 30 minutes) 3 times to destroy the cell structure, and rinse the tissue 2-3 times with phosphate buffer after each thawing.
[0036] The skeletal muscle pieces after repeated freezing and thawing were transferred into a conical flask, and a mixture of 1% Triton and 0.1% ammonia water was added (need to be sterilized by filtering with a 0.22 μm filter membrane), and the mixture was submerged in the tissue, and the mixture was shaken at a speed of 50 r / min for 12 hours, and the water was changed every 4 hours. The solution was changed after observing that the solution became turbid after a period of time until the skeletal muscle pieces were milky white (3-4 days), and the periosteum was washed with distilled water 2-3 times after 12 hours, and the skeletal muscle was defatted with methanol for 24 hours (the methanol solution was changed twice during this period). The skeletal muscle pieces were washed with deionized water until there was no foam. Pour out the deionized water, put the skeletal muscle tissue into a -20°C refrigerator for pre-freezing for 2 hours, and then put it into a -80°C refrigerator for freezing for 8 hours, and then put it into a freeze dryer for freeze drying for 3-4 days.
[0037] The lyophilized tissue was cut into pieces, and 10 mL of 0.5 M glacial acetic acid, 100 mg of pepsin (1:10000) and 5 mg of phosphate buffer powder were added to each 100 mg of tissue for digestion. After digestion, the digested mixture was centrifuged to remove cell debris and other impurities to obtain dmECM matrix liquid, which was stored in a -20 ° C refrigerator for use. When using decellularized skeletal muscle, NaOH was used to adjust the pH to 7.4 in an ice bath environment to obtain a decellularized skeletal muscle matrix liquid, which was a milky white transparent gel.
[0038] 2) At 60°C, 10 g of gelatin was dissolved in 100 mL of PBS, stirred vigorously for 1 h using a magnetic bar, and then 8 mL of methacrylic anhydride was added dropwise, and the solution was stirred for another 3 h in the dark. The solution was then diluted by adding 400 mL of preheated phosphate buffer to terminate the reaction. The prepared sample was collected and dialyzed in a dialysis bag (8-14 kDa molecular weight cutoff) at 40°C for 7 days, and the solution after dialysis was freeze-dried to obtain a gel in the form of a white solid foam, i.e., methacrylic acid-gelatin.
[0039] 3) Take 0.5 g of freeze-dried methacrylic acid-gelatin and 0.05 g of 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone (I2959) and add them to a 10 mL centrifuge tube, then add 5 mL of decellularized skeletal muscle matrix solution (dmECM) with a pH of 7.4, and oscillate using a vortex mixer until GelMA is completely dissolved. Then, use a syringe to inject an equal amount of it into a 96-well plate and let it stand for 1 hour to eliminate excess bubbles. After the bubbles are eliminated, a composite solution is obtained.
[0040] 4) Add 600 μL of desktop liquid to 95 mg of egg yolk lecithin (purity ~99%), sonicate twice at 300 W, with an interval of 1 min between each sonication, and continue for 15 s. Then add 400 μL of perfluorotri-n-butylamine, and sonicate 10 times in the same way. Then filter the sonicated emulsion through a 0.8 μm filter membrane to obtain a perfluorotri-n-butylamine emulsion. Then place the perfluorotri-n-butylamine emulsion in an oxygen-rich environment (hyperbaric oxygen chamber for more than 8 minutes) to dissolve enough oxygen.
[0041] 5) The prepared perfluorotri-n-butylamine emulsion and the composite liquid were mixed in a mass ratio of 4:6, and oscillated using a vortex mixer. After complete mixing, an equal amount of the mixture was injected into a 96-well plate using a syringe and allowed to stand for 1 hour to eliminate excess bubbles. After the bubbles were eliminated, an ultraviolet lamp was used to irradiate the mixture for 10 minutes to gelate the mixture, thereby preparing an oxygen-enriched hydrogel of a composite decellularized skeletal muscle matrix.
[0042] 2. Example 2. Comparative Examples 1 to 3 have the same operating steps as Example 1, except that the concentrations of methacrylate gelatin, decellularized skeletal muscle matrix and perfluorotri-n-butylamine emulsion in the reaction system are different, as shown in Table 1.
[0043] Table 1
[0044]
[0045] 2. Performance Testing
[0046] 1. HE staining, MASSON staining and DNA quantitative analysis were performed on the fresh porcine skeletal muscle tissue before and after decellularization. The results were as follows: Figure 1 shown.
[0047] As can be seen from the figure, compared with the control group, the outer color of the skeletal muscle after decellularization changes from red before treatment to white. In HE staining, there are a large number of blue-purple nuclei and pink cytoplasm in fresh pig skeletal muscle tissue, while almost no blue-purple nuclei are seen in the decellularized sections, only pink cytoplasm. This result shows that the present invention can effectively remove cells in skeletal muscle tissue while retaining its natural extracellular matrix. In MASSON staining, the content of collagen fibers does not change much after decellularization, indicating that the cells are effectively removed after decellularization while retaining the matrix structure and collagen. At the same time, the DNA quantification results also show that the DNA content per milligram of tissue after decellularization is 3.9% of that in fresh tissue. Most of the deoxyribonucleic acid is removed from the natural tissue, and the decellularization effect is good.
[0048] 2. The hydrogel materials obtained in Comparative Example 1 and Comparative Example 2 were observed. The results are as follows: Figure 2 shown.
[0049] As can be seen from the figure, the gel scaffolds of different concentrations of methacrylate gelatin can be formed into cylinders with relatively smooth surfaces, with better forming performance and better gelling effect. In addition, there are obvious differences in the colors of the gel scaffolds with different methacrylate gelatin contents. The gel scaffold of comparative example 1 is lighter in color, milky white and translucent; the gel scaffold of comparative example 2 is darker in color, yellow-white and opaque.
[0050] 3. The mechanical properties of the hydrogels obtained in Comparative Examples 1 and 2 were tested using a microcomputer-controlled mechanical testing machine (DNS20) produced by Changchun Institute of Mechanical Science Co., Ltd. The results are as follows: Figure 3 shown.
[0051] As can be seen from the figure, when the concentration of methacrylate gelatin in the hydrogel is 10%, its average Young's modulus is 0.56±0.01kPa; when the concentration of methacrylate gelatin in the hydrogel is 20%, its average Young's modulus is 7.02±0.11kPa. This shows that the content of methacrylate gelatin can change the mechanical properties of the hydrogel, and the Young's modulus of the 20% methacrylate gelatin group is close to the Young's modulus of natural skeletal muscle (10kPa), which can provide a suitable microenvironment for the growth of skeletal muscle cells. On the contrary, too high or too low Young's modulus often affects bone tissue ingrowth and bone interface integration.
[0052] 4. The hydrogels of Comparative Example 1 and Comparative Example 2 were tested for swelling rate and water absorption. The hydrogels were dissolved in PBS solution, taken out at different time points, and then the surface water was absorbed and weighed for analysis. The results are as follows: Figure 4 shown.
[0053] As can be seen from the figure, the swelling rate, water absorption and water retention of the hydrogel in Comparative Example 2 are better than those in Comparative Example 1, indicating that the increase in the content of methacrylate gelatin will reduce the hydrophilicity of the material, but the statistical analysis results show that there is a difference but no significant difference (0.01 <p<0.05)。
[0054] 5. The oxygen-enriched hydrogel material prepared in Example 1 was analyzed by infrared spectroscopy using a Fourier transform infrared spectrometer from Perkin Elmer, USA. The results are as follows: Figure 5 shown.
[0055] It can be clearly seen from the figure that methacrylate gelatin has a peak at 1633 cm -1 , 1539cm -1 and 1231cm -1 There are obvious absorption peaks at 1633cm -1 The characteristic peak is attributed to the vibration of the C=O bond of the amino acid side chain, 1539 cm -1 and 1231cm -1 The characteristic peaks that appear correspond to the stretching vibration of the NH bond, and the characteristic absorption peaks of the corresponding wavelengths can also be seen in the oxygen-enriched hydrogel of Example 1, but the peak intensities and areas are different between groups, and there is a certain offset, indicating that there is a chemical bond breakage and recombination between the various materials composited by the oxygen-enriched hydrogel, rather than a simple physical mixture.
[0056] 6. The hydrogels prepared in Example 1 and Comparative Example 1 were placed in PBS solutions respectively, and dissolved oxygen was measured using a JPB-607A portable dissolved oxygen meter produced by Shanghai Yidian Scientific Instrument Co., Ltd. The blank PBS solution was used as the control group. The results are shown in FIG. Figure 6 shown.
[0057] As can be seen from the figure, the dissolved oxygen content in the control group continued to change little because the control group was in a closed environment and there was no oxygen exchange. The addition of hydrogel in Comparative Example 1 will absorb the PBS solution to a certain extent and then consume the oxygen dissolved in the PBS solution, resulting in a decrease in the dissolved oxygen content in the PBS solution, and the dissolved oxygen in Comparative Example 1 decreased rapidly, and the dissolved oxygen content decreased to 0.12 ± 0.13 mg / L on the 5th day; and although the dissolved oxygen in Example 1 also decreased, its decreasing trend was more gentle, and it was still 1 ± 0.16 mg / L on the 7th day, which was about 9 times the dissolved oxygen in Comparative Example 1. It can be seen that the continuous release of oxygen from perfluorotributylamine in the hydrogel of Example 1 can reach at least 7 days, and this time period just covers the time of vascularization in the early stage of tissue repair. After that, because the damaged tissue has formed a vascularized structure, the dependence on external oxygen sources will also be reduced. The results show that the addition of perfluorotributylamine in Example 1 can improve the hypoxic state inside the GelMA gel compared with Comparative Example 1.
[0058] 7. The microscopic morphology of the hydrogels prepared in Example 1, Comparative Example 1 and Comparative Example 3 was observed using a Quattro S scanning electron microscope produced by Thermo Fisher Scientific Brno Ltd. Figure 7 shown.
[0059] As can be seen from the figure, the surface and cross-sectional SEM morphology observations of the hydrogel materials of Example 1, Comparative Example 1 and Comparative Example 3 all show porous structures. Among them, Comparative Example 1 has a uniform porous structure, Comparative Example 3 shows a sparse pore structure, and the network structure of Example 1 shows a staggered distribution of large and small pores, a more compact porous distribution structure, and this pore structure is more conducive to the release and transportation of oxygen.
[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An oxygen-enriched hydrogel composite with decellularized skeletal muscle matrix, characterized in that: The hydrogel comprises methacrylate gelatin, decellularized skeletal muscle matrix liquid and perfluorotri-n-butylamine emulsion carrying oxygen. The hydrogel takes methacrylate gelatin as a base and is cross-linked with the decellularized skeletal muscle matrix and the perfluorotri-n-butylamine.
2. The oxygen-enriched hydrogel of the composite decellularized skeletal muscle matrix according to claim 1, characterized in that The mass volume ratio of the methacrylate gelatin, the decellularized skeletal muscle matrix liquid and the perfluorotri-n-butylamine emulsion is 0.05-0.3 g: 200-800 μL: 400-800 μL.
3. The oxygen-enriched hydrogel of the composite decellularized skeletal muscle matrix according to claim 1, characterized in that: The Young's modulus of the hydrogel is 5 to 20 kPa, and the porosity is 20% to 90%.
4. A method for preparing the oxygen-enriched hydrogel of the composite decellularized skeletal muscle matrix according to any one of claims 1 to 3, characterized in that: The following steps are involved: 1) adding a benchtop liquid solution to egg yolk lecithin with a purity greater than 99%, ultrasonically treating the mixture for multiple times, then adding perfluorotri-n-butylamine, and continuing the ultrasonic treatment, and filtering the ultrasonicated emulsion through a 0.8 μm filter membrane to obtain a perfluorotri-n-butylamine emulsion; 2) placing the perfluorotri-n-butylamine emulsion obtained in step 1) in an oxygen-rich environment to dissolve enough oxygen; 3) adding methacrylic anhydride to the gelatin solution for reaction and then freeze-drying to obtain modified methacrylic acid-gelatin, dispersing the obtained decellularized skeletal muscle matrix liquid in the methacrylic acid-gelatin, and then adding a photoinitiator to obtain a composite liquid; 4) adding the perfluorotri-n-butylamine emulsion treated in step 2) to the composite solution obtained in step 3) to obtain a reaction solution, and obtaining the oxygen-enriched decellularized skeletal muscle matrix hydrogel after irradiation with ultraviolet light to form a gel.
5. The method for preparing the oxygen-enriched hydrogel of the composite decellularized skeletal muscle matrix according to claim 4, characterized in that: In step 1), the mass volume ratio of egg yolk lecithin to perfluorotri-n-butylamine is 80-110 mg: 300-600 μL.
6. The method for preparing the oxygen-enriched hydrogel of the composite decellularized skeletal muscle matrix according to claim 4, characterized in that: In the ultrasonic treatment process in step 1), the ultrasonic power is greater than 200 W, the ultrasonic time is greater than 10 s, the ultrasonic interval is greater than 1 min, and the number of ultrasonic times is greater than 2 times.
7. The method for preparing the oxygen-enriched decellularized skeletal muscle matrix hydrogel according to claim 4, characterized in that: The pH value of the decellularized skeletal muscle matrix solution in step 3) is 6.8-7.
5.
8. The method for preparing the oxygen-enriched decellularized skeletal muscle matrix hydrogel according to claim 4, characterized in that: The photoinitiator in step 3) is 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone, phenyl-2,4,6-trimethylbenzoyl lithium phosphinate, 2,2′-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone or 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone.
9. The method for preparing the oxygen-enriched hydrogel of the composite decellularized skeletal muscle matrix according to claim 4, characterized in that: The amount of the photoinitiator added is 0.5-5% of the mass of the reaction solution.
10. Use of the oxygen-enriched hydrogel of the composite decellularized skeletal muscle matrix according to any one of claims 1 to 3 or the oxygen-enriched hydrogel prepared by the method according to any one of claims 4 to 9 in the regeneration and repair of skeletal muscle tissue.
Citation Information
Cited By
Multispectral response oxygen-carrying artificial periosteum and preparation method thereof