Efficient hemostatic material as well as preparation method and application thereof
Microgels modified with phthalaldehyde groups overcome the shortcomings of existing hemostatic materials in terms of tissue adhesion and mechanical properties, achieving efficient and rapid hemostasis, and are suitable for various hemostasis scenarios.
Patent Information
- Application Number
- CN202310404763.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-22
AI Technical Summary
Existing hemostatic materials have shortcomings in terms of tissue adhesion and mechanical properties after fluid absorption, making them particularly difficult to effectively address active or pressure bleeding and unable to achieve rapid and safe hemostasis in various hemostatic scenarios.
Microgels modified with phthalaldehyde groups are covalently linked to water-soluble or hydrophilic polymers to form highly efficient hemostatic materials, including hemostatic sponges, hemostatic powders, and flowable hemostatic agents. The rapid coupling of phthalaldehyde groups with free amine groups in blood and chemical bonding with amine groups on tissue surfaces enhances mechanical properties and adhesion strength.
It achieves effective sealing of bleeding points, enhances the mechanical properties and tissue adhesion of the material, and can quickly and effectively stop bleeding in a variety of hemostasis scenarios without additional pressure. It is particularly suitable for irregular surfaces, active or pressure bleeding, and minimally invasive surgery.
Smart Images

Figure CN118806965A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new medical materials, and in particular relates to a highly effective hemostatic material and a preparation method and application thereof. Technical Background
[0002] Uncontrollable bleeding is one of the main causes of death after trauma, during surgery and in emergency situations. Timely and effective hemostasis can greatly reduce mortality and the risk of complications. Therefore, the development of hemostatic materials has attracted much attention.
[0003] Early hemostasis is mainly achieved by cotton gauze assisted compression, but cotton gauze has a long hemostasis time and is non-degradable, so its application is limited. In recent years, new hemostatic materials have been developed mainly inorganic and hydrophilic polymer hemostatic materials. Inorganic hemostatic materials mainly include zeolite, clay and kaolin, which have strong water absorption capacity and good hemostatic effect, but because they are difficult to absorb in the body and may generate heat and cause damage to surrounding tissues while stopping bleeding, they are only used in emergency situations such as bleeding control in pre-hospital environments of war trauma. Hydrophilic polymer hemostatic materials refer to hydrophilic natural or synthetic polymers that are directly or cross-linked and processed into sponges, powders, hydrogels, films or gauze. These materials have excellent biocompatibility, adjustable degradation and strong water absorption. They can quickly absorb water in the blood to concentrate blood cells and coagulation factors and other blood components, and can also promote the adhesion, aggregation and activation of platelets, thereby accelerating the formation of blood clots and playing a hemostatic role. However, current polymer hemostatic materials generally have defects such as inability to adhere to tissues and weak mechanical properties after fluid absorption, so their hemostatic effects are limited, especially they are unable to cope with the treatment scenarios of active or pressure bleeding.
[0004] In response to the above problems, researchers are committed to modifying and modifying hemostatic materials to improve the hemostatic effect. For example, the Celox hemostatic gauze developed by MedTrade has chitosan particles impregnated on the surface of the gauze. The positive charge on chitosan increases the adhesion and aggregation of blood cells and platelets through electrostatic action, further enhancing the hemostatic effect. Johnson & Johnson has developed oxidized cellulose gauze Surgicel, and the carboxyl groups on cellulose can acidify blood to form a gel, which can also further enhance the hemostatic effect. The above strategy introduces cations or anions into the hemostatic material to increase the interaction between the hemostatic material and the blood components and tissue surface, but this force comes from weak physical interactions and still cannot solve the problem of blocking active or pressure bleeding. When stopping bleeding, the gauze needs to be continuously pressed on the bleeding site, which is difficult to apply to irregularly shaped and non-pressable bleeding wounds. In order to further improve the tissue adhesion strength of hemostatic materials and the mechanical properties after absorbing blood, some researchers modified chitosan hemostatic materials with catechol, and used highly active catechol to quickly cross-link a large amount of plasma proteins to form a second cross-linking network with the hemostatic material. At the same time, catechol bonded with tissue surface groups to form a hemostatic barrier with a certain mechanical strength within a few seconds (K. Kim et al., Coagulopathy-independent, bioinspired hemostatic materials: A full research story from preclinical models to a human clinical trial. Sci. Adv. 2021); some researchers also used carboxylic acid activated esters modified on polyacrylic acid to react with plasma proteins and amino groups on the tissue surface to form a hemostatic material and blood clot complex with a certain strength at the bleeding site, which covalently adheres to the tissue while quickly stopping bleeding, thereby achieving effective blocking of the bleeding point (H. Yuk et al., Rapid and coagulation-independent haemostatic sealing by a paste inspired by barnacle glue. Nat. Biomed. Eng. 2021). However, the oxidizability of catechol groups, the pH dependence of their tissue adhesion properties, and the non-specific binding to proteins all pose challenges to their hemostatic applications; defects such as the generation of byproducts during use and low cross-linking efficiency at low concentrations of carboxylic acid activated esters also limit their biomedical applications. Therefore, it is urgent to seek an ideal (i.e., stable, efficient, fast, and highly selective) bioactive reactive group to construct hemostatic materials with excellent tissue adhesion and mechanical properties to cope with a variety of hemostatic scenarios and achieve rapid and safe hemostasis. Summary of the invention
[0005] In view of the defects of current hemostatic materials, namely weak tissue adhesion and poor mechanical properties after absorbing blood, the present invention proposes a series of high-efficiency hemostatic materials and preparation methods and applications thereof.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] The first aspect of the present invention provides a type of microgel modified with o-phthalaldehyde groups.
[0008] The microgel modified with o-phthalaldehyde groups has a structure as shown in Formula 1:
[0009]
[0010] In Formula 1, MG represents microgel, which is a gel microparticle formed by cross-linking water-soluble or hydrophilic polymers, with a particle size of 5 mesh to 1000 mesh and a solid content of 0.01% to 50%;
[0011] In formula 1, n≥2, which means that the average number of o-phthalaldehyde functional groups on a single microgel is greater than or equal to 2;
[0012] In Formula 1, the o-phthalaldehyde group is connected to the microgel via a covalent bond.
[0013] The water-soluble or hydrophilic polymer of the microgel is selected from natural polymers or synthetic polymers.
[0014] The water-soluble or hydrophilic natural polymer is selected from one or more of hyaluronic acid, alginate, dextran, chondroitin sulfate, heparin, polyglutamic acid, tragacanth gum, xanthan gum, agarose, gellan gum, guar gum, gum arabic, locust bean gum, starch, starch hydrolysate or starch derivative, cellulose or cellulose derivative.
[0015] Wherein, the starch derivative can be selected from oxidized starch, esterified starch, etherified starch or alkylated starch;
[0016] The cellulose derivative may be selected from cellulose ethers, including but not limited to methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose and the like.
[0017] The water-soluble or hydrophilic synthetic polymer refers to an artificially synthesized polymer containing a large number of hydrophilic groups.
[0018] The hydrophilic groups include, but are not limited to, cationic groups (such as tertiary amines, quaternary amines, etc.), anionic groups (such as carboxylic acids, sulfonic acids, phosphoric acids and sulfuric acids, etc.) and polar nonionic groups (such as hydroxyl groups, ether groups, etc.).
[0019] In some embodiments of the present invention, the water-soluble or hydrophilic synthetic polymer can be selected from homopolymers or copolymers of (meth)acrylic acid and its esters containing the above-mentioned hydrophilic groups, homopolymers or copolymers of (meth)acrylamides, homopolymers or copolymers of polyvinyl alcohol, homopolymers or copolymers of polyethylene glycol, and homopolymers or copolymers of vinyl pyrrolidone.
[0020] Optionally, the homopolymer or copolymer of (meth)acrylic acid and its esters is selected from the homopolymer or copolymer of (meth)acrylic acid, the homopolymer or copolymer of hydroxyethyl (meth)acrylate, the homopolymer or copolymer of hydroxypropyl (meth)acrylate, the homopolymer or copolymer of glucose (meth)acrylate, the homopolymer or copolymer of polyethylene glycol (meth)acrylate and the copolymer of polyethylene glycol methyl ether (meth)acrylate, etc.;
[0021] Optionally, the homopolymer or copolymer of (meth)acrylamide is selected from copolymers of (meth)acrylamide, copolymers of N,N-dimethylacrylamide, homopolymers or copolymers of N-hydroxymethylacrylamide, homopolymers or copolymers of N-hydroxyethyl(meth)acrylamide, homopolymers or copolymers of N-hydroxypropyl(meth)acrylamide, copolymers of N-isopropylacrylamide and copolymers of 2-acrylamido-2-methylpropanesulfonic acid (AMPS), etc.
[0022] The above-mentioned (meth)acrylic acid refers to acrylic acid or methacrylic acid; the above-mentioned (meth)acrylamide refers to acrylamide or methacrylamide, and hereinafter, (meth)acrylic acid also refers to acrylic acid or methacrylic acid, and (meth)acrylamide also refers to acrylamide or methacrylamide.
[0023] In some embodiments of the present invention, more specifically, the water-soluble or hydrophilic polymer of the microgel is preferably one or more of hyaluronic acid, alginate, carboxymethyl starch, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyglutamic acid, polyacrylic acid and carboxylated polyethylene glycol.
[0024] In some embodiments of the present invention, further, the microgel modified with o-phthalaldehyde groups has a structure selected from one of the following structures:
[0025]
[0026]
[0027] In Formula 1-1 to Formula 1-12, MG represents microgel,
[0028] Wherein, 1≤r≤20, 1≤s≤20, 1≤t≤50, and n≥2. Preferably, 1≤r≤6, 1≤s≤10, 1≤t≤30, and n≥2.
[0029] The second aspect of the present invention provides a method for preparing the o-phthalaldehyde group-modified microgel, and the specific method is as follows:
[0030] (1) preparing microgels;
[0031] (2) covalently linking the aldehyde-preprotected o-phthalaldehyde precursor derivative to the active groups on the microgel to prepare the o-phthalaldehyde precursor derivative-modified microgel;
[0032] (3) Deprotecting the aldehyde groups to obtain microgels modified with o-phthalaldehyde groups.
[0033] In some embodiments of the present invention, the method for preparing microgel in step (1) comprises: 1) preparing microgel by direct crosslinking of water-soluble or hydrophilic polymers; or, 2) preparing microgel by polymerizing and crosslinking monomers.
[0034] Specifically, 1) refers to cross-linking a water-soluble or hydrophilic polymer into a gel by a specific cross-linking method, and then physically breaking it by mechanical force and sieving it through sieve holes of different sizes to obtain microgels with different particle size distributions; or preparing a water-soluble or hydrophilic polymer into an oil-water emulsion under the action of an emulsifier, and further cross-linking it by a specific cross-linking method to obtain a microgel with a certain particle size.
[0035] Wherein, the specific cross-linking method includes chemical cross-linking and radiation cross-linking.
[0036] When the specific cross-linking method is chemical cross-linking, it includes the following three methods:
[0037] Based on multifunctional acrylic or methacrylic acid modified polymers cross-linked via free radical chain polymerization;
[0038] Covalent crosslinking based on multifunctional crosslinkers (functionality ≥ 2) in the presence or absence of catalysts;
[0039] In the presence or absence of a catalyst, the polymer chain itself contains two or more reactive functional groups (such as hydroxyl, carboxyl, etc.) condensation cross-linking.
[0040] The chemical crosslinking is preferably covalent crosslinking based on a multifunctional crosslinking agent in the presence or absence of a catalyst.
[0041] Wherein, the multifunctional cross-linking agent can be selected from one or more of glutaraldehyde, polyamine, multifunctional epoxy, epichlorohydrin, divinyl sulfone (DVS), phosphorus oxychloride or sodium trimetaphosphate;
[0042] The multifunctional epoxy can be selected from one or more of 1,4-butanediol diglycidyl ether (BDDE), 1,6-hexanediol diglycidyl ether, ethylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, polyethylene glycol diglycidyl ether and polypropylene glycol diglycidyl ether; further, the multifunctional epoxy is preferably 1,4-butanediol diglycidyl ether;
[0043] The polyamine is a multifunctional crosslinking agent containing one or more functional groups of primary amine, diamine, hydrazide and hydroxylamine; further, the polyamine is selected from adipic acid dihydrazide (ADH) or hexamethylenediamine.
[0044] When the specific crosslinking method is radiation crosslinking, it includes electron beam radiation crosslinking or gamma ray radiation crosslinking.
[0045] Wherein, when the radiation crosslinking is selected from electron beam radiation crosslinking, the radiation dose rate is selected from 10 to 1000 Gy / s, and the radiation time is selected from 5 to 100 minutes;
[0046] When the radiation cross-linking is selected from gamma-ray radiation cross-linking, the radiation dose is selected from 10 to 100 kGy.
[0047] Specifically, 2) refers to copolymerizing and cross-linking monomers with multifunctional double bond cross-linking agents or cross-linking monomers into gels through a specific cross-linking method after polymerization, and further physically breaking them by mechanical force and then sieving them through sieve holes of different sizes to obtain microgels with different particle size distributions; or emulsion polymerization or precipitation polymerization of monomers with multifunctional double bond cross-linking agents to obtain microgels with a certain particle size, or first emulsion polymerization or precipitation polymerization of monomers and then cross-linking by a specific cross-linking method to obtain microgels with a certain particle size.
[0048] The monomer may be selected from one or more water-soluble monomers, or may be selected from one or more water-soluble monomers and other copolymerizable monomers.
[0049] The water-soluble monomer may be further selected from (meth)acrylic acid, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, glucose (meth)acrylate, polyethylene glycol methyl ether (meth)acrylate and polyethylene glycol (meth)acrylate, (meth)acrylamide, N,N-dimethylacrylamide, N-hydroxymethylacrylamide, N-hydroxyethyl (meth)acrylamide, N-hydroxypropyl (meth)acrylamide, N-isopropylacrylamide and 2-acrylamido-2-methylpropanesulfonic acid (AMPS), vinyl pyrrolidone, etc.;
[0050] The other copolymerizable monomers can be selected from (meth)acrylate monomers, (meth)acrylamide monomers, styrene monomers, vinyl acetate and acrylonitrile.
[0051] The multifunctional double bond crosslinking agent refers to a crosslinking agent containing two or more polymerizable double bond functional groups, including but not limited to glucose acrylate, 2,9-decadiene, 2-hexadecenoic acid, N,N'-methylenebisacrylamide and glycerol acrylate.
[0052] The specific cross-linking method is selected from the following two methods:
[0053] Condensation crosslinking of polymer chains containing two or more reactive functional groups in the presence or absence of a catalyst;
[0054] Irradiation cross-linking.
[0055] In some embodiments of the present invention, the aldehyde-preprotected o-phthalaldehyde precursor derivative in step (2) comprises an aldehyde-preprotected o-phthalaldehyde group and a substituent R that can be connected to an active group on the microgel, and the structure is shown in Formula 2:
[0056]
[0057] In Formula 2, R includes, but is not limited to, carboxyl substituents, vinyl sulfone substituents, epoxy substituents, halogenated alkane substituents, isocyanate substituents, and amine substituents.
[0058] In Formula 2, optionally, R can be directly connected to the benzene ring, or can be connected to the benzene ring through a single or multiple alkylene chains or alkoxy chains, and the multiple alkylene chains and alkoxy chains are connected through ether bonds, amide bonds, ester bonds, carbamate bonds or urea bonds.
[0059] In some embodiments of the present invention, the aldehyde group pre-protected o-phthalaldehyde precursor derivative is specifically selected from one or a combination of the following structures:
[0060]
[0061]
[0062] Wherein, 1≤r≤20, 1≤s≤20, 1≤t≤50. Preferably, 1≤r≤6, 1≤s≤10, 1≤t≤30.
[0063] In some embodiments of the present invention, the active groups on the microgel are selected from hydroxyl groups or carboxyl groups.
[0064] The covalent bond connection between the aldehyde group pre-protected o-phthalaldehyde precursor derivative and the active group on the microgel is selected from ether bond, amide bond, ester bond, carbamate bond or urea bond, preferably ether bond, amide bond and carbamate bond.
[0065] More specifically, when the active groups on the microgel are selected from hydroxyl groups, the covalent bond connection is an ether bond connection between vinyl sulfone substituents, epoxy substituents and halogenated alkane substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel, an ester bond connection between carboxyl substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel, and a carbamate bond connection between isocyanate substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel;
[0066] When the active groups on the microgel are selected from carboxyl groups, the covalent bond connection is based on an amide bond connection between the amino substituents on the o-phthalaldehyde precursor derivative and the carboxyl groups on the microgel.
[0067] In some embodiments of the present invention, the covalent bond connection is preferably selected from an ether bond connection between a vinyl sulfone substituent on an o-phthalaldehyde precursor derivative and a hydroxyl group on a microgel, an ether bond connection between an epoxy substituent on an o-phthalaldehyde precursor derivative and a hydroxyl group on a microgel, a carbamate bond connection between an isocyanate substituent on an o-phthalaldehyde precursor derivative and a hydroxyl group on a microgel, an ester bond connection between a carboxyl substituent on an o-phthalaldehyde precursor derivative and a hydroxyl group on a microgel, and an amide bond connection between an amino substituent on an o-phthalaldehyde precursor derivative and a carboxyl group on a microgel.
[0068] The present invention provides some specific covalent bond connection methods for preparing microgels modified with o-phthalaldehyde precursor derivatives, specifically: using the carboxyl groups on the microgels as active groups, and performing an amidation reaction with the amine substituents on the o-phthalaldehyde precursor derivatives pre-protected by aldehyde groups. The carboxyl groups on the microgels are activated by carbodiimide, 2-chloro-4,6-dimethyl-1,3,5-triazine (CDMT), 2-chloro-1-methyl iodopyridine (CMPI), 1,1'-carbonyldiimidazole (CDI) and 4-(4,6-dimethoxytriazine-2-yl)-4-methylmorpholine hydrochloride (DMTMM), and then reacting efficiently with the amine substituents on the o-phthalaldehyde precursor derivatives pre-protected by aldehyde groups to form amide bonds.
[0069] In some embodiments of the present invention, the deprotection in step (3) refers to deprotecting the pre-protected o-phthalaldehyde functional group of the aldehyde group connected to the microgel under acidic conditions to obtain a microgel modified with o-phthalaldehyde groups.
[0070] The structures of the o-phthalaldehyde group-modified microgels provided by Formula 1-1 to Formula 1-12 of the first aspect of the present invention are merely exemplary illustrations of the o-phthalaldehyde group-modified microgels that can be obtained by a certain preparation method of the above-mentioned aldehyde group-preprotected o-phthalaldehyde precursor derivatives and microgels. Based on the contents of the present application, those skilled in the art can imagine that other aldehyde group-preprotected o-phthalaldehyde precursor derivative structures can be used to realize the o-phthalaldehyde group-modified microgels.
[0071] The third aspect of the present invention provides a variety of highly effective hemostatic materials.
[0072] In some embodiments of the present invention, the highly efficient hemostatic material is a highly efficient hemostatic sponge having a pore structure obtained by drying the microgel modified with o-phthalaldehyde groups provided by the first aspect of the present invention.
[0073] In some embodiments of the present invention, the microgel modified with o-phthalaldehyde groups can be placed in a mold and dried according to the required specifications and sizes.
[0074] In some embodiments of the present invention, the drying method is vacuum freeze drying.
[0075] Preferably, the vacuum freeze-drying conditions are freezing at -20°C for 6 hours, followed by freeze-drying at -60°C for 48 hours.
[0076] In some embodiments of the present invention, the highly effective hemostatic material is a highly effective hemostatic powder obtained by dehydrating and drying the microgel modified with o-phthalaldehyde groups provided by the first aspect of the present invention.
[0077] In some embodiments of the present invention, the water removal is to replace the water in the microgel modified with the o-phthalaldehyde group with an organic solvent, so that the water content of the microgel is reduced and precipitated in the form of solid particles.
[0078] Wherein, the organic solvent is selected from methanol, ethanol, acetone, isopropanol, acetonitrile, etc. Preferably, the organic solvent is selected from ethanol.
[0079] In some embodiments of the present invention, the drying is direct drying and vacuum freeze drying followed by drying.
[0080] Preferably, the drying conditions are freezing at -20°C for 6 hours, freeze-drying at -60°C for 48 hours, and then drying at 30°C for 12 hours.
[0081] In some embodiments of the present invention, the particle size distribution of the high-efficiency hemostatic powder is 20 mesh to 500 mesh.
[0082] In some embodiments of the present invention, the highly efficient hemostatic material is a highly efficient flowing hemostatic agent directly obtained by uniformly dispersing the o-phthalaldehyde group-modified microgel provided by the first aspect of the present invention in a solvent; or, the highly efficient hemostatic material is a highly efficient flowing hemostatic agent obtained by uniformly dispersing a highly efficient hemostatic sponge or a highly efficient hemostatic powder in a solvent.
[0083] Wherein, the solvent is selected from water, physiological saline, buffer solution, decellularized matrix or cell culture medium solution containing or not containing polyol, and the polyol is preferably one or more of propylene glycol, butanediol, 1,2-pentanediol, 1,2-hexanediol or glycerol;
[0084] The uniform dispersion process can utilize mechanical stirring or a mixer.
[0085] In some embodiments of the present invention, the solid content of the high-efficiency flowable hemostat is 1% to 20% (w / v). Preferably, the solid content of the high-efficiency flowable hemostat is selected from 5% to 12% (w / v).
[0086] The fourth aspect of the present invention provides a composite sponge.
[0087] The composite sponge is a composite sponge based on microgel modified with o-phthalaldehyde groups. The composite sponge is obtained by layering microgel modified with o-phthalaldehyde groups and microgel not modified with o-phthalaldehyde groups in a mold and drying them to obtain a composite sponge with a pore structure.
[0088] Wherein, the o-phthalaldehyde group-modified microgel is provided by the first aspect of the present invention;
[0089] The microgel without the modification of the o-phthalaldehyde group refers to a microgel prepared from a water-soluble or hydrophilic polymer or a microgel prepared by polymerization and cross-linking of monomers. That is, the microgel without the modification of the o-phthalaldehyde group is the microgel prepared in step (1) of the second aspect of the present invention;
[0090] The conditions such as the polymer skeleton, water content, particle size and pH value of the microgel modified with o-phthalaldehyde groups and the microgel not modified with o-phthalaldehyde groups may be the same or different.
[0091] The layering refers to spreading the microgel modified with o-phthalaldehyde groups and the microgel not modified with o-phthalaldehyde groups in layers in a mold to form a multilayer structure with different components distributed on different horizontal planes, and further drying to obtain a composite sponge with a multilayer structure.
[0092] In some embodiments of the present invention, preferably, the composite sponge has a double-layer structure, wherein one side is composed of microgels modified with o-phthalaldehyde groups, and the other side is composed of microgels not modified with o-phthalaldehyde groups.
[0093] In some embodiments of the present invention, a composite sponge with a double-layer structure can be applied to a variety of biomedical scenarios, wherein the side containing the microgel modified with o-phthalaldehyde groups can be used in a variety of application scenarios such as hemostasis or tissue adhesion and sealing, and the side containing the microgel not modified with o-phthalaldehyde groups can achieve applications such as postoperative anti-adhesion due to the lubrication and low inflammatory stimulation properties of the corresponding polymer skeleton.
[0094] The fifth aspect of the present invention provides the use of the high-efficiency hemostatic material based on the third aspect of the present invention.
[0095] When the efficient hemostatic material is an efficient hemostatic sponge, the application of the efficient hemostatic sponge is selected from one of the following applications:
[0096] Application of the highly efficient hemostatic sponge in the preparation of non-compressive hemostatic products for penetrating wounds;
[0097] Application of the highly efficient hemostatic sponge in the preparation of liver hemostatic products;
[0098] Application of the highly efficient hemostatic sponge in the preparation of spleen hemostatic products;
[0099] Application of the high-efficiency hemostatic sponge in the preparation of surface arterial hemostatic products;
[0100] Application of the highly efficient hemostatic sponge in the preparation of surface venous hemostasis products;
[0101] Application of the high-efficiency hemostatic sponge in the preparation of femoral artery hemostatic products;
[0102] Application of the high-efficiency hemostatic sponge in preparing abdominal aorta hemostasis products;
[0103] Application of the high-efficiency hemostatic sponge in the preparation of carotid artery hemostasis products;
[0104] Application of the highly efficient hemostatic sponge in the preparation of cardiac hemostatic products;
[0105] Application of the highly efficient hemostatic sponge in the preparation of coronary artery hemostasis products;
[0106] Application of the highly effective hemostatic sponge in the preparation of hemostatic products for tooth extraction wounds;
[0107] Application of the highly efficient hemostatic sponge in the preparation of spinal hemostatic products;
[0108] The application of the high-efficiency hemostatic sponge in preparing uterine wall hemostatic products.
[0109] When the efficient hemostatic material is efficient hemostatic powder, the application of the efficient hemostatic powder is selected from one of the following applications:
[0110] Application of the highly effective hemostatic powder in the preparation of liver hemostatic products;
[0111] Application of the highly effective hemostatic powder in the preparation of spleen hemostatic products;
[0112] Application of the highly effective hemostatic powder in the preparation of venous hemostatic products;
[0113] Application of the highly effective hemostatic powder in the preparation of surface arterial hemostatic products;
[0114] Application of the highly effective hemostatic powder in the preparation of surface vein hemostatic products;
[0115] Application of the highly effective hemostatic powder in the preparation of intestinal hemostatic products;
[0116] Application of the highly effective hemostatic powder in the preparation of skin hemostatic products;
[0117] Application of the highly effective hemostatic powder in the preparation of oral mucosal hemostatic products;
[0118] Application of the highly effective hemostatic powder in the preparation of hemostatic products for hysterectomy;
[0119] The application of the high-efficiency hemostatic powder in preparing spinal hemostatic products.
[0120] When the highly efficient hemostatic material is a highly efficient flowing hemostatic agent, the application of the highly efficient flowing hemostatic agent is selected from one of the following applications:
[0121] Application of the highly efficient mobile hemostatic agent in the preparation of non-compressive hemostatic products for penetrating wounds;
[0122] The high-efficiency mobile hemostatic agent is used in the preparation of digestive tract hemostatic products;
[0123] Application of the highly efficient mobile hemostatic agent in the preparation of hemostatic products during and after partial nephrectomy;
[0124] Application of the highly efficient mobile hemostatic agent in the preparation of hemostatic products for narrow cavities of organisms;
[0125] Application of the highly efficient mobile hemostatic agent in the preparation of spinal hemostatic products;
[0126] The high-efficiency mobile hemostatic agent is used in the preparation of hemostatic products for percutaneous puncture.
[0127] The applications provided above are merely exemplary of the application of the high-efficiency hemostatic material to various hemostatic scenarios. A person skilled in the art can imagine, based on the contents of this application, that the high-efficiency hemostatic material can be applied to hemostatic applications in other scenarios.
[0128] The sixth aspect of the present invention provides an application of the composite sponge based on the fourth aspect of the present invention, selected from one of the following applications:
[0129] Application of the composite sponge in preparing postoperative anti-adhesion products;
[0130] Application of the composite sponge in the preparation of tissue leakage blocking products;
[0131] The composite sponge is used in preparing tissue fluid leakage blocking products.
[0132] Among them, the postoperative adhesion prevention includes but is not limited to abdominal wall adhesion prevention, pericardial adhesion prevention, tendon adhesion prevention and intrauterine adhesion prevention, etc.; the tissue leakage blocking includes but is not limited to lung parenchyma leakage blocking, etc.; the tissue fluid leakage blocking includes but is not limited to intestinal leakage blocking, pancreatic leakage blocking, cerebrospinal fluid leakage blocking, gastric leakage blocking, etc.
[0133] The reaction of o-phthalaldehyde with primary amines is characterized by high efficiency, rapidity and high selectivity, and has been proven to be used for quantitative detection of the content of amines and amino acids (MH Joseph, P. Davies, Electrochemical detection of aminoacids, Curr. Sep. 1982), efficient coupling of biomacromolecules (CLTung, CT Wong, EY Fung, X. Li, Traceless and chemoselective amine bioconjugation via phthalimidine formation in native protein modification, Organic Letters 2016) and rapid cross-linking construction of hydrogel materials (Z. Zhang, C. He, Y. Rong, H. Ren, T. Wang, Z. Zou, et al., A fast and versatile cross-linking strategy via o-phthalaldehyde condensation for mechanically strengthened and functional hydrogels, National Science Review 2021), etc. It can be seen that o-phthalaldehyde is expected to be used as a modified group of current polymer hemostatic materials to achieve efficient coupling between hemostatic materials and plasma proteins, form a second cross-linked network to enhance mechanical properties, and simultaneously bond with amine groups on the tissue surface to improve the adhesion strength between the hemostatic material and the tissue, thus overcoming the defects of weak tissue adhesion and poor mechanical properties of current hemostatic materials. However, there is no related technology in the prior art for modifying o-phthalaldehyde groups on microgels and using them to prepare hemostatic materials.
[0134] The present invention provides a type of microgel modified with o-phthalaldehyde groups and a preparation method thereof, and also provides a variety of different forms of hemostatic materials prepared based on the microgel modified with o-phthalaldehyde groups, including hemostatic sponges, hemostatic powders, and mobile hemostatic agents. Compared with existing hemostatic materials, the hemostatic material involved in the present invention has a highly efficient hemostatic function. On the one hand, the o-phthalaldehyde group achieves efficient and rapid coupling with the protein containing free amine groups abundant in the blood, forming a second cross-linked network to enhance the mechanical properties of the material itself, achieving effective blocking of bleeding points and resisting its continuous bleeding; on the other hand, the highly active o-phthalaldehyde group is chemically bonded with the amine groups on the surface of the tissue synchronously, providing a long-term and stable adhesion effect to prevent the occurrence of re-bleeding. Due to its excellent tissue adhesion performance and mechanical strength, the hemostatic material of the present invention does not require additional pressing when used, can cope with a variety of hemostatic scenarios to achieve rapid and effective hemostasis, and is particularly suitable for the treatment of hemostatic scenarios such as irregular surfaces, active or pressure bleeding, and minimally invasive surgery, and has important clinical application value and significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0135] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the degradation product of the hyaluronic acid microgel (i.e., microgel HA-2) in Example 2.
[0136] Figure 2 These are the results of in vitro hemostasis tests on the hemostatic sponges with different o-phthalaldehyde derivative labeling rates, the control sponge and the commercial absorbable gelatin sponge in Example 22.
[0137] Figure 3 Microscope images (left) and in vitro hemostatic test results (right) of the hemostatic powder modified with o-phthalaldehyde groups of different particle sizes in Example 23.
[0138] Figure 4 These are scanning electron microscope morphology images of the surface adhesion, aggregation, activation of platelets (left picture) and adsorption of red blood cells (right picture) of the hemostatic sponge of the present invention in Example 26.
[0139] Figure 5 These are photographs of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge (group c) in Example 27 used for non-compression hemostasis of penetrating wounds and visual photographs of blood loss.
[0140] Figure 6 These are photos of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge (group c) used for liver hemostasis in Example 28 and visual photos of the amount of blood loss.
[0141] Figure 7These are photos of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge group (group c) in Example 30 being applied to rabbit ear artery hemostasis.
[0142] Figure 8 These are photos of the hemostatic powder of the present invention (group a), control powder (group b) and commercial chitosan hemostatic granules (group c) used for liver hemostasis in Example 40.
[0143] Fig. 9 A comparison chart of hemoglobin content measured in blood clots collected from the hemostatic powder of the present invention (group a), control powder (group b), commercial chitosan hemostatic powder (group c) and blank group (group d) in Example 45.
[0144] Fig.10 These are photographs of the mobile hemostatic agent of the present invention (group a), control fluid (group b) and commercial fluid gelatin (group c) in Example 50 applied to non-compression hemostasis of penetrating wounds.
[0145] Fig.11 These are photos of the mobile hemostatic agent of the present invention (group a), control fluid (group b) and commercial fluid gelatin (group c) in Example 55 applied to percutaneous puncture hemostasis of the spleen.
[0146] Fig.12 These are the H&E staining results of the composite sponge (group a) and the control group (group b) used for postoperative abdominal adhesion prevention in Example 57 (I represents the small intestine, L represents the liver, and S represents the composite sponge material). DETAILED DESCRIPTION
[0147] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0148] Example 1: Synthesis of aldehyde-preprotected o-phthalaldehyde precursor derivatives (i.e. compounds 1 to 12)
[0149] (I) Synthesis of compounds 1 to 3 (s = 2, t = 7)
[0150]
[0151] (1) Synthesis of compound 1: The synthesis process was based on the method disclosed in Zhen Zhang, Chaoliang He, Yan Rong, Hui Ren, Tianran Wang, Zheng Zou, Xuesi Chen, National Science Review, Volume 8, Issue 4, April 2021, nwaa128. 1H NMR (400MHz, DMSO-d6): δ = 12.74 (brs, 1H), 8.29 (d, J = 7.6Hz, 1H), 8.12 (s, 1H), 7.65 (d, J = 7.6Hz, 1H), 6.30 (s, 1H), 6.11 (s, 1H), 3.40-3.30 (m, 6H).
[0152] (2) Synthesis of Compound 2: Compound 1 (10 g, 45 mmol) was dissolved in 10 mL of anhydrous dichloromethane (DCM), and 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide (EDC, 10.38 g, 67 mmol) and N-hydroxysuccinimide (NHS, 7.69 g, 67 mmol) were added, and stirred at room temperature for 30 minutes. Ethylene diamine (27.05 g, 0.45 mmol) was dissolved in anhydrous DCM and stirred, and the above reaction system was quickly added dropwise to the ethylenediamine solution, and the reaction was stirred at room temperature for 12 h. After the reaction was completed, most of the solvent was removed, and the residual compound was extracted three times with ethyl acetate, the organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was purified by silica gel chromatography to obtain Compound 2 (9.0 g, yield 75%). 1 H NMR (400MHz, DMSO-d6): δ=8.18(t,1H),8.07(d,1H),7.80(dd,1H),7.56(dd,1H),6.05(h,2 H),4.59(dt,1H),4.25(dt,1H),3.38(tt,J=5.1Hz,2H),3.34(s,3H),3.03(tt,J=6.3,2H).
[0153] (3) Synthesis of compound 3: α,ω-dicarboxyl polyethylene glycol (COOH-PEG-COOH, t=7, 8.26 g) was dissolved in 100 mL of anhydrous DCM, and EDC (3.52 g, 22.7 mmol) and NHS (2.61 g, 22.7 mmol) were added, and stirred at room temperature for 30 minutes. Compound 2 (5 g, 18.8 mmol) was dissolved in anhydrous DCM (50 mL), and gradually added dropwise to the above system, and stirred at room temperature for 12 h. After the reaction was completed, most of the solvent was removed, and the residual compound was extracted three times with ethyl acetate, the organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was purified by silica gel chromatography to obtain compound 3 (10.5 g, yield 79%). 1H NMR (400MHz, DMSO-d6): δ = 8.86 (s, 1H), 8.21 (d, J = 7.6Hz, 1H), 7.93 (s, 1H), 7.61 ( d,J=7.6Hz,1H),6.38(s,1H),6.30(s,1H),3.80-3.48(m,28H),3.40-3.30(m,6H).
[0154] (II) Synthesis of compounds 4 to 8 (r = 2, s = 6, t = 7)
[0155]
[0156] (1) Synthesis of compound 4: The synthesis process was based on the method disclosed in Chun Ling Tung, Clarence TT Wong, Eva Yi Man Fung and Xuechen Li. Org. Lett. 2016, 18, 11, 2600-2603. 1 H NMR (400MHz, DMSO-d6): δ = 11.82 (s, 1H), 7.56 (dq, 1H), 7.43 (dd, 1H), 7.16 (ddt, 1H), 6.05 (m, 1H), 5.97 (q, 1H), 3.53 (dt, 2H), 3.40-3.30 (m, 6H).
[0157] (2) Synthesis of Compound 5: The synthesis process was similar to that of Compound 2. 1 H NMR (400MHz, DMSO-d6): δ = 7.56 (t, 1H), 7.48 (m, 2H), 7.14 (ddt, 1H), 6.06 (s, 1H), 5.97 (q, 1H), 3.40-3.30 (m, 6H), 3 .07(q,2H),2.90-2.72(m,4H),2.38(t,J=8.2Hz,2H),1.87(t,J=6.5Hz,2H),1.59-1.43(m,4H),1.46-1.30(m,4H).
[0158] (3) Synthesis of Compound 6: Compound 5 (5 g, 14.3 mmol) was dissolved in 100 mL of toluene, and succinic anhydride (1.5 g, 15 mmol) and triethylamine (TEA, 2.1 mL, 15 mmol) were added and stirred at room temperature for 4 h. After the reaction was completed, the solvent was removed by rotary evaporation, and the crude product was purified by silica gel column chromatography to obtain Compound 6 (5.2 g, yield 80%). 1H NMR (400MHz, DMSO-d6): δ=11.87(s,1H),7.62(t,1H),7.56(t,1H),7.44-7.36(m,2H),7.14(ddt,1H),6.08-6.02(m,1H),5.97(q,1H), 3.40-3.30(m,6H),3.19-3.03(m,4H),2.77(tt,J=8.7Hz,2H),2.55(dd,2H),2.48-2.34(m,4H),1.56-1.43(m,4H),1.40-1.27(m,4H).
[0159] (4) Synthesis of compound 7: α,ω-diaminopolyethylene glycol (NH2-PEG-NH2, t=7, 8.8 g) was dissolved in 50 mL of anhydrous DCM. Compound 4 (5 g, 19.8 mmol) was dissolved in anhydrous DCM (50 mL), and EDC (4.65 g, 30 mmol) and NHS (3.45 g, 30 mmol) were added and stirred at room temperature for 30 minutes. The above reaction system was gradually added dropwise to the NH2-PEG-NH2 solution and stirred at room temperature for 12 h. After the reaction was completed, most of the solvent was removed, and the residual compound was extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was purified by silica gel chromatography to obtain compound 7 (10.4 g, yield 81%). 1 H NMR (400MHz, DMSO-d6): δ=7.43-7.36(m,2H),7.14(ddt,1H),3.61-3.43(m,28H),3.36-3.26(m,6H),2.88-2.71(m,2H),2.54-2.36(m,2H).
[0160] (5) Synthesis of Compound 8: Hexamethylene diisocyanate (HDI, 1.28 g, 7.6 mmol) was dissolved in anhydrous tetrahydrofuran (THF, 50 mL). Compound 7 (5 g, 7.6 mmol) was dissolved in anhydrous THF (50 mL) and slowly added dropwise to the rapidly stirred HDI solution. The mixture was stirred and reacted at room temperature for 2 h. After the solvent was removed by rotary evaporation, it was redissolved in a small amount of DCM and poured into n-pentane to precipitate a solid. This was repeated twice and then dried to obtain Compound 8 (5.5 g, yield 92%). 1H NMR (400MHz, DMSO-d6): δ = 7.53 (t, 1H), 7.44-7.36 (m, 2H), 7.14 (ddt, 1H), 6.047 (s,1H),5.97(s,1H),5.87(t,1H),5.65(t,1H),3.63-3.51(m,32H),3.36-3.28(m ,4H),3.39-3.32(m,6H),3.31-3.18(m,4H),3.10(tdd,J=5.7,4.7,1.0Hz,2H),2. 90-2.71(m,4H),2.41(t,J=8.3Hz,2H),1.87(t,J=6.5Hz,2H),1.59-1.27(m,8H).
[0161] (III) Synthesis of Compounds 9 to 12
[0162]
[0163] (1) Synthesis of Compound 9: Intermediate 1 (5 g, 25.5 mmol) was dissolved in anhydrous DCM (40 mL), 0.2 M NaOH solution (85 mL) was added, followed by tetrabutylammonium bromide (TBAB, 0.82 g, 2.55 mmol), and the mixture was stirred at room temperature for 30 min. 1-Bromo-2-chloroethane (8.41 mL, 0.102 mol) was added dropwise, and the mixture was stirred at room temperature for 48 h. Subsequently, the phases were separated, and the organic phase was washed with brine in sequence, dried over anhydrous sodium sulfate, filtered, and concentrated under reduced pressure. The crude product was purified by silica gel chromatography to obtain Compound 9 (5.6 g, yield 85%). 1 H NMR (400MHz, DMSO-d6): δ = 7.45 (dd, 1H), 7.15 (dd, 1H), 6.88 (dd, 1H), 6.07-5.97 (m, 2H), 4.24 (q, J = 2.2Hz, 2H), 3.81 (t, J = 2.2Hz, 2H), 3.37-3.34 (s, 6H).
[0164] (2) Synthesis of Compound 10: HDI (6.43 g, 38.3 mmol) was dissolved in anhydrous DCM. Intermediate 1 (5 g, 25.5 mmol) was dissolved in anhydrous DCM, and TEA (3.53 mL, 25.5 mmol) was added. The above mixture was slowly added dropwise to the rapidly stirred HDI solution, and the reaction was stirred at room temperature for 30 min. After removing the solvent by rotary evaporation, it was redissolved in a small amount of DCM and poured into n-pentane to precipitate a solid. After repeating twice, Compound 10 (9.76 g, yield 70%) was obtained. 1H NMR (400MHz, DMSO-d6): δ = 7.56 (dd, J = 8.4, 1H), 7.40 (s, 1H), 7.07 (dd, J = 8.3, 1H), 6.34 (t, J = 5.3Hz, 1 H),6.03–5.93(m,2H),3.38-3.31(s,6H),3.20-3.13(m,2H),3.06(q,J=5.5Hz,2H),1.67-1.27(m,8H).
[0165] (3) Synthesis of compound 11: Under anhydrous and oxygen-free conditions, intermediate 1 (5 g, 25.5 mmol) was dissolved in anhydrous DCM. 2-Chloroethanesulfonyl chloride (5 g, 30.6 mmol) was slowly added dropwise to the above solution under an ice bath at 0°C. After reacting for 10 min, anhydrous TEA (4.23 mL, 30.6 mmol) was slowly added dropwise and reacted at room temperature for 12 h. After the reaction was completed, the solvent was removed by rotary evaporation, and the obtained crude product was purified by silica gel column chromatography to obtain compound 11 (6.9 g, yield 95%). 1 H NMR (400MHz, DMSO-d6): δ=7.48-7.41(m,1H),7.35(s,1H),7.08(dd,J=8.2,1H),6.26( dd,J=18.5,1H),6.15(dd,J=18.4,1H),6.03(dq,J=2.9,1.7Hz,2H),3.41-3.33(s,6H).
[0166] (4) Synthesis of Compound 12: Intermediate 1 (5 g, 25.5 mmol) was suspended in 30 mL of water, and a 1.5 M NaOH aqueous solution (10 mL) was added, and the system gradually became clear. After stirring for 40 minutes, epichlorohydrin (7.1 g, 76.5 mmol) was added, and the mixture was stirred at room temperature for 24 h. After the reaction was completed, most of the solvent was removed, and the residual compound was extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was purified by silica gel chromatography to obtain Compound 12 (5.8 g, yield 90%). 1 H NMR (400MHz, DMSO-d6): δ = 7.45 (s, 1H), 7.14 (s, 1H), 6.91 (dd, J = 8.3, 1H), 6.07-5.9 9(m,2H),4.11(d,J=3.3Hz,2H),3.42(s,1H),3.38-3.32(m,6H),2.91-2.78(m,2H).
[0167] Embodiment 2 to Embodiment 8:
[0168] Preparation of microgels
[0169] Example 2: Preparation of hyaluronic acid microgels (i.e. microgels HA-1 to HA-4)
[0170]
[0171] (1) Preparation of microgel HA-1: Hyaluronic acid (HA, 10 g, 890 kDa) was dissolved in 90 mL of 0.25 M NaOH solution and stirred until completely dissolved. Divinyl sulfone (DVS, 1.5 g, 13 mmol) was weighed and dissolved in 10 mL of 0.25 M NaOH solution and then added to the above reaction solution, stirred at 40° C. for 2 h, and then left to stand overnight at room temperature. The hydrogel after the reaction was dialyzed with physiological saline (pH=7) for 2-3 days, and then physically crushed and sieved to obtain microgels with mesh sizes of 20 to 300. The microgel was resuspended in 150 IU / mL hyaluronidase solution and incubated at 37°C for 24 h to observe the degradation. If it was not completely degraded, the enzyme solution was replaced and the incubation was continued. If it was completely degraded, the solution was boiled, centrifuged, and the supernatant was freeze-dried. According to the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linking agent to polymer repeating unit) of the microgel HA-1 was calculated to be approximately 31.3%.
[0172]
[0173] (2) Preparation of microgel HA-2: HA (10 g, 1.2 MDa) was dissolved in 90 mL of 0.25 M NaOH solution and stirred until completely dissolved. 1,4-Butanediol diglycidyl ether (BDDE, 2.2 g, 11 mmol) was weighed and dissolved in 10 mL of 0.25 M NaOH solution and then added to the above reaction solution. The mixture was stirred at 40 °C for 2 h and then placed under constant temperature reaction conditions at 40 °C overnight. The hydrogel after the reaction was dialyzed with physiological saline (pH = 7) for 2-3 days, and then physically broken and sieved to obtain microgels with mesh sizes of 20 to 300. The microgel was resuspended in 150 IU / mL hyaluronidase solution and incubated at 37 °C for 24 h. The degradation was observed. If it was not completely degraded, the enzyme solution was replaced and incubation continued. If it was completely degraded, the solution was boiled, centrifuged, and the supernatant was obtained and freeze-dried. In this embodiment, the nuclear magnetic resonance hydrogen spectrum of the hyaluronic acid microgel degradation product is as follows: Figure 1 As shown, based on the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linking agent to polymer repeating unit) of the microgel HA-2 can be calculated to be approximately 36.8%.
[0174]
[0175] (3) Preparation of microgel HA-3: HA (1 g, 1.2 MDa) was dissolved in 10 mL of 0.25 M NaOH solution and stirred until completely dissolved. 40 mL of liquid paraffin and 2% of emulsifier Span80 were uniformly mixed as the oil phase. The stirring speed of the oil phase was adjusted to 1800 rpm, and 10 mL of HA solution was added dropwise to the oil phase. BDDE (0.4 g, 2 mmol) was weighed and added to the above emulsion, stirred at room temperature for 30 min, and reacted at 45°C for 12 h. After the cross-linking reaction was completed, the emulsion was washed with the same volume of ethyl acetate and anhydrous ethanol, respectively, and the above operation was repeated 2 to 3 times. The gel particles after standing and stratification were collected and dried to obtain microgel HA-3. The microgel was resuspended in 150 IU / mL hyaluronidase solution and incubated at 37°C for 24 h. The degradation was observed. If it was not completely degraded, the enzyme solution was replaced and incubated continuously. If it was completely degraded, the solution was boiled, centrifuged, and the supernatant was obtained and freeze-dried. According to the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linking agent to polymer repeating unit) of the microgel HA-3 can be calculated to be approximately 35.0%.
[0176]
[0177] (4) Preparation of microgel HA-4: HA (0.1 g, 1.2 MDa) was dissolved in 10 mL of deionized water and stirred until completely dissolved. 40 mL of liquid paraffin was uniformly mixed with 5% of emulsifier Span80 as the oil phase. Under the conditions of stirring the oil phase at 500 rpm and 30% ultrasound, 10 mL of HA solution was added dropwise to the oil phase, and the pH of the mixed solution was adjusted to 4.0-5.0. 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride (EDC-HCl, 50 mg, 0.26 mmol) and adipic acid dihydrazide (ADH, 0.1 g, 57.4 mmol) were quickly added, the rotation speed was increased to 800 rpm, the pH of the system was maintained at 4.0-5.0, and the reaction was carried out at room temperature for 6 hours. After the reaction is completed, let it stand for 30 minutes, add the same volume of isopropanol to the system, stir, let it stand, remove the supernatant, repeat the operation 2 to 3 times, and ultrasonicate for 20 minutes, drain the solid to obtain microgel HA-4. The microgel was resuspended in a 150IU / mL hyaluronidase solution and incubated at 37°C for 24 hours to observe the degradation. If it is not completely degraded, the enzyme solution is replaced and incubated. If it is completely degraded, the solution is boiled, centrifuged, and the supernatant is obtained and freeze-dried. According to the nuclear magnetic hydrogen spectrum, the cross-linking degree (molar ratio of cross-linking agent to polymer repeating unit) of the microgel HA-4 can be calculated to be approximately 25.0%.
[0178] Example 3: Preparation of carboxymethyl cellulose microgels (i.e., microgels CMC-1 and CMC-2)
[0179]
[0180] (1) Preparation of microgel CMC-1: Carboxymethyl cellulose (CMC, 10 g, viscosity 1200 mPa·s (25°C, 2%), DS: 0.7) was dissolved in 100 mL of 0.25 M NaOH solution and stirred until completely dissolved. BDDE (2.2 g, 11 mmol) was weighed and dissolved in 25 mL of 0.25 M NaOH solution and then added to the above reaction solution, stirred at 40°C for 2 h, and then left to stand overnight at room temperature. The hydrogel after the reaction was dialyzed with physiological saline (pH = 7) for 2-3 days, and then physically crushed and sieved to obtain microgels with mesh sizes of 20 to 300. The microgel was resuspended in 100 IU / mL lysozyme solution and incubated at 37°C for 24 h to observe the degradation. If it was not completely degraded, the enzyme solution was replaced and the incubation was continued. If it was completely degraded, the solution was boiled, centrifuged, and the supernatant was freeze-dried. According to the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linking agent to polymer repeating unit) of the microgel CMC-1 was calculated to be approximately 21.5%.
[0181]
[0182] (2) Preparation of microgel CMC-2: Carboxymethyl cellulose (CMC, 10 g, viscosity 2000 mPa·s (25°C, 2%), DS: 0.85) was dissolved in 100 mL of 0.5 M NaOH solution and stirred until completely dissolved. The system was heated to 50°C, and epichlorohydrin (ECH, 1.5 g, 16 mmol) was weighed and added dropwise to the reaction system. The mixture was stirred at 50°C for 2 h and then left to stand overnight at room temperature. The hydrogel after the reaction was dialyzed with physiological saline (pH = 7) for 2-3 days, and then physically crushed and sieved to obtain microgels of 20 to 300 meshes. The microgel was resuspended in 100 IU / mL lysozyme solution and incubated at 37°C for 24 h to observe the degradation. If it was not completely degraded, the enzyme solution was replaced and the incubation was continued. If it was completely degraded, the solution was boiled, centrifuged, and the supernatant was freeze-dried. According to the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linking agent to polymer repeating unit) of the microgel CMC-2 was calculated to be approximately 18.5%.
[0183] Example 4: Preparation of Alginate Microgel (i.e. Microgel Alg-1)
[0184]
[0185] Alginic acid (Sodium alginate, Alg, 10g, viscosity 1000mPa·s (25℃, 2%)) was dissolved in 100mL 0.5M NaOH solution, stirred until completely dissolved, the system was heated to 50℃, epichlorohydrin (ECH, 1.5g, 16mmol) was weighed and added dropwise to the reaction system, stirred at 50℃ for 2h, and then left at room temperature overnight. The hydrogel after the reaction was dialyzed with physiological saline (pH=7) for 2-3d, and then physically broken and sieved to obtain microgels of 20 to 300 meshes. The microgel was resuspended in 20 IU / mL alginate lyase solution and incubated at 37°C for 24 h to observe the degradation. If it was not completely degraded, the enzyme solution was replaced and the incubation was continued. If it was completely degraded, the solution was boiled, centrifuged, and the supernatant was freeze-dried. According to the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linking agent to polymer repeating unit) of the microgel Alg-1 was calculated to be approximately 15.8%.
[0186] Example 5: Preparation of cross-linked sodium carboxymethyl starch microgels (i.e. microgels CMS-1 and CMS-2)
[0187]
[0188] (1) Preparation of microgel CMS-1: 25 g of cassava starch and 48 mL of 95% ethanol were placed in a 500 mL three-necked flask, condensed and refluxed, and stirred thoroughly to form a uniform starch emulsion. Then, the pH was adjusted to 11 with 5% NaOH solution, heated to 55°C in a water bath, 0.09 g of ECH was added, and the reaction was continued for 1 h to obtain cross-linked starch. The cross-linked starch was cooled to 25°C, and 11 g of NaOH solid was added for pretreatment for 30 min. After the pretreatment, 11 g of chloroacetic acid was added, heated to 55°C, and the reaction was continued for 4 h. After the reaction was completed, it was neutralized with hydrochloric acid to pH = 7. The solution was filtered while hot, and the filter cake was washed with 95% ethanol until there was no white floc in the filtrate. Then, it was vacuum dried at 50°C, and the filter cake was crushed to obtain a white powder. A certain amount of sample was taken and weighed at 105°C, and its carboxymethyl substitution degree was measured by copper salt precipitation method to be 0.8.
[0189]
[0190] (2) Preparation of microgel CMS-2: 10 g of soluble starch was dissolved in NaOH solution (1%, w / w, 100 mL) to obtain a starch solution. Sodium trimetaphosphate (2 g) was added to the above starch solution and stirred until completely dissolved. Emulsifier Span80 (7.5 mL) and oil phase cyclohexane (150 mL) were added to a 250 mL three-necked flask, stirred and condensed at 50°C. When the emulsifier was completely dissolved and the system temperature was stabilized at 50°C, 15 mL of the prepared starch / sodium trimetaphosphate solution was taken and added dropwise to the three-necked flask at a speed of 800 rpm. Stirring was maintained at this speed for 5 h. After the reaction was completed, the lower layer of solid was collected by centrifugation and washed several times with acetone, petroleum ether and deionized water respectively. Finally, it was dehydrated with anhydrous ethanol and vacuum dried at 40°C for 5 h to obtain a white powder, which was cross-linked starch. The preparation process of sodium carboxymethyl starch was referred to the preparation process of microgel CMS-1. A certain amount of the white powder was taken and weighed at 105°C, and then the degree of carboxymethyl substitution was measured by the copper salt precipitation method to be 0.8.
[0191] Example 6: Preparation of polyglutamic acid microgel (i.e. microgel PGA-1)
[0192] Dissolve poly-γ-glutamic acid (PGA, 6 g) in 100 mL of deionized water and place in a sealable 10 mL radiation tube, filled with nitrogen for protection. 60 Co-γ-ray irradiation (1.0 kGy / h, 10 kGy) The hydrogel after the reaction was dialyzed with physiological saline (pH=7) at 4°C for 2-3 days, and then physically broken and sieved to obtain microgels of 20 to 300 meshes, namely microgel PGA-1.
[0193] Example 7: Preparation of polyacrylic acid microgels (i.e. microgels PAA-1 and PAA-2)
[0194]
[0195] (1) Preparation of microgel PAA-1: Weigh acrylic acid (AA, 60 g) and add it to a beaker, stir, add about 40 mL of 30% sodium hydroxide solution to neutralize part of AA, weigh N,N'-methylenebisacrylamide (BIS, 0.5 g) and ammonium persulfate (APS, 0.4 g), dissolve them in a small amount of water and add them to the above system, mix them evenly, and stand at 75°C for polymerization and crosslinking for 3 hours. Collect the polyacrylic acid (PAA) hydrogel and fully swell and balance it in physiological saline, then obtain microgel PAA-1 by physical crushing and sieving.
[0196]
[0197] (2) Preparation of microgel PAA-2: Weigh 5 g of acrylic acid into a beaker, stir, add about 5 mL of 30% sodium hydroxide solution to neutralize part of AA, and add a small amount of ammonium acrylate (0.1 g) and sodium acetate (0.05 g). Mix 40 mL of kerosene and 9% of emulsifier octoxynol (Op-10) as the oil phase. Add 5 mL of HA solution dropwise to the oil phase while stirring at 1000 rpm, stir for 10 to 15 minutes, and obtain a white emulsion. The emulsion was added to a four-necked flask equipped with a stirrer, a thermometer, a dropping funnel and a gas guide tube. After nitrogen was passed through the flask for 20 minutes under stirring to deoxygenate, an aqueous solution of azodiisobutyronitrile (AIBN, 0.1 g) and sodium bisulfite (0.05 g) was added dropwise, followed by an ethylene glycol dimethacrylate (EGDMA, 0.5 g) solution, and the reaction was maintained at 40°C for 4 hours. After the reaction was completed, ethanol was added for precipitation, the precipitate was filtered under reduced pressure, washed with acetone 2 to 3 times, and dried to obtain microgel PAA-2.
[0198] Example 8: Preparation of carboxylated polyethylene glycol microgel (i.e. microgel PEG-1)
[0199]
[0200] 40mL of liquid paraffin and 2% of emulsifier Span80 were uniformly mixed as the oil phase. A certain amount of carboxyl-terminated four-arm polyethylene glycol (20kDa, n=113, 1g) was weighed and dissolved in 5mL of 0.01mol / L MES buffer solution (pH 5.2), and EDC (38mg) and NHS (20mg) were added; a 5% DMSO aqueous solution containing hexamethylenediamine (12mg) was prepared, and the two solutions were mixed and quickly added to the rapidly stirred liquid paraffin, and the stirring speed of the oil phase was adjusted to 1800rpm, and stirred at room temperature for 2h. A large amount of n-hexane was added to the emulsion, and after the microspheres and the solvent were naturally separated, the supernatant was poured out, and the microgel PEG-1 was obtained after being washed with n-hexane for 2 to 3 times. The gel particles after standing and separation were collected and dried.
[0201] Embodiment 9 to Embodiment 15:
[0202] Synthesis of Microgels Modified with O-Phthalaldehyde Groups
[0203] Example 9: Synthesis of hyaluronic acid microgels modified with o-phthalaldehyde groups (i.e. microgels HA-2.1 to HA-2.4)
[0204]
[0205] (1) Synthesis of microgel HA-2.1: The swollen microgel HA-2 (100 g) was resuspended in 100 mL of 0.01 mol / L 2-(N-morpholine)ethanesulfonic acid (MES) buffer solution (pH = 5.2) and dispersed by stirring. Compound 2 (110 mg, 0.41 mmol, s = 2) was weighed and dissolved in 10 mL of dimethyl sulfoxide (DMSO) and then added to the above reaction solution. 4-(4,6-dimethoxytriazine-2-yl)-4-methylmorpholine hydrochloride (DMTMM, 4.1 g, 15 mmol) was weighed three times, dissolved in 3 mL of MES buffer solution respectively, added to the above reaction solution, and reacted at 37°C for 24 h. The pH of the reaction liquid system was adjusted to 8-9, and then dialyzed with physiological saline for 2-3 days, and the microgel was collected and added with 10% trifluoroacetic acid, and reacted for 1 hour, and then the reaction system was dialyzed with deionized water for 1 day, and the HA microgel modified with o-phthalaldehyde groups, i.e., microgel HA-2.1, was collected. The supernatant of the reaction system was collected, and the amount of residual compound 2 in the supernatant was determined by high performance liquid chromatography, and the labeling rate of compound 2 was calculated to be approximately 4.67% (w / w).
[0206]
[0207] (2) Synthesis of microgel HA-2.2 with different labeling rates: The swollen microgel HA-2 (100 g) was resuspended in 100 mL of 0.01 mol / L MES buffer solution (pH = 5.2), stirred and dispersed, and different masses (20, 50, 100, 175 mg) of compound 5 (r = 2, s = 6) were weighed and dissolved in 10 mL of DMSO and added to the above reaction solution. The rest of the reaction process was referred to the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected, and the amount of residual compound 5 in the supernatant was determined by high performance liquid chromatography. The labeling rates of compound 5 were calculated to be 0.58%, 1.12%, 2.03% and 4.21% (w / w), respectively, and recorded as microgels HA-2.2 (0.58), HA-2.2 (1.12), HA-2.2 (2.03) and HA-2.2 (4.21), respectively.
[0208]
[0209] (3) Synthesis of microgel HA-2.3: The swollen equilibrium microgel HA-2 (100 g) was resuspended in 50 mL of 0.25 M NaOH solution and stirred to disperse. Compound 11 (68.6 mg, 0.24 mmol) was weighed and added to the above system. React at 50°C for 8 h. After the reaction, the pH of the reaction solution was neutralized to 7, and then dialyzed with saline for 2-3 days. The microgel was collected and added with 10% trifluoroacetic acid, reacted for 1 h, and then the reaction system was dialyzed with deionized water for 1 day to collect the HA microgel modified with o-phthalaldehyde groups, i.e., microgel HA-2.3. The supernatant of the reaction system was collected, and the amount of residual compound 11 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 11 was calculated to be approximately 2.78% (w / w).
[0210]
[0211] (4) Synthesis of microgel HA-2.4: The swollen equilibrium microgel HA-2 (100 g) was resuspended in 50 mL of 0.25 M NaOH solution and stirred to disperse. Compound 12 (60 mg, 0.24 mmol) was weighed and added to the above system. The reaction was carried out at 40°C for 12 h. After the reaction was completed, the pH of the reaction solution was neutralized to 7, and then dialyzed with saline for 2-3 days. The microgel was collected and 10% trifluoroacetic acid was added to react for 1 h. The reaction system was then dialyzed with deionized water for 1 day, and the HA microgel modified with o-phthalaldehyde groups, i.e., microgel HA-2.4, was collected. The supernatant of the reaction system was collected, and the amount of residual compound 12 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 12 was calculated to be approximately 3.04% (w / w).
[0212] The above structural formula and examples provide exemplary structures of hyaluronic acid microgels modified with o-phthalaldehyde groups and methods for synthesizing them. Based on the contents of this application, those skilled in the art can imagine that other hyaluronic acid microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the o-phthalaldehyde group-modified hyaluronic acid microgels.
[0213] Example 10: Synthesis of carboxymethyl cellulose microgels modified with o-phthalaldehyde groups (i.e. microgels CMC-1.1 to CMC-1.3)
[0214]
[0215] (1) Synthesis of microgel CMC-1.1: The swollen equilibrium microgel CMC-1 (100 g) was resuspended in 20 mL of deionized water and stirred to disperse. Compound 1 (54 mg, 0.24 mmol, s = 2), EDC (1.12 g, 7.2 mmol) and dimethylaminopyridine p-toluenesulfonate (DPTS, 1.8 g, 7.2 mmol) were added to the above system in sequence and reacted at room temperature for 24 h. After the reaction was completed, it was dialyzed with sodium chloride aqueous solution (pH = 4) containing dilute hydrochloric acid for 2-3 days, and the microgel was collected and added with 10% trifluoroacetic acid to react for 1 h. The reaction system was then dialyzed with deionized water for 1 day, and the CMC microgel modified with o-phthalaldehyde groups, i.e., microgel CMC-1.1, was collected. The supernatant of the reaction system was collected, and the amount of residual compound 1 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 1 was calculated to be approximately 2.15% (w / w).
[0216]
[0217] (2) Synthesis of microgel CMC-1.2: The swollen microgel CMC-1 (100 g) was resuspended in 20 mL of 0.01 mol / L MES buffer solution (pH = 5.2), stirred and dispersed, compound 5 (175 mg, 0.5 mmol, r = 2, s = 6) was weighed and dissolved in 10 mL of DMSO and added to the above reaction solution, and the rest of the reaction process was referred to the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected, and the amount of residual compound 5 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 5 was calculated to be approximately 3.14% (w / w).
[0218]
[0219] (3) Synthesis of microgel CMC-1.3: The swollen microgel CMC-1 (100 g) was resuspended in 20 mL of 0.01 mol / L MES buffer solution (pH = 5.2), stirred and dispersed, compound 7 (156 mg, 0.24 mmol, r = 2, t = 7) was weighed and dissolved in 10 mL and directly added to the above reaction solution, and the rest of the reaction process was referred to the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected, and the amount of residual compound 7 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 7 was calculated to be approximately 4.69% (w / w).
[0220] The above structural formula and examples provide the structure of an exemplary o-phthalaldehyde group-modified carboxymethyl cellulose microgel and its synthesis method. Based on the contents of this application, a person skilled in the art can imagine that other carboxymethyl cellulose microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the o-phthalaldehyde group-modified carboxymethyl cellulose microgel.
[0221] Example 11: Synthesis of alginate microgels modified with o-phthalaldehyde groups (i.e., microgels Alg-1.1 to Alg-1.3)
[0222]
[0223] (1) Synthesis of microgel Alg-1.1: The swollen equilibrium microgel Alg-1 (100 g) was resuspended in 20 mL of deionized water and stirred to disperse. Compound 3 (160 mg, 0.24 mmol, s=2, t=7), EDC (1.12 g, 7.2 mmol) and DPTS (1.8 g, 7.2 mmol) were added to the above system in sequence, and the rest of the reaction process was referred to the synthesis of microgel CMC-1.1. The supernatant of the reaction system was collected, and the amount of residual compound 3 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 3 was calculated to be approximately 4.88% (w / w).
[0224]
[0225] (2) Synthesis of microgel Alg-1.2: The swollen microgel Alg-1 (100 g) was resuspended in 20 mL of 0.01 mol / L MES buffer solution (pH = 5.2), stirred and dispersed, compound 5 (175 mg, 0.5 mmol, r = 2, s = 6) was weighed and dissolved in 10 mL of DMSO and added to the above reaction solution, and the rest of the reaction process was referred to the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected, and the amount of residual compound 5 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 5 was calculated to be approximately 3.47% (w / w).
[0226]
[0227] (3) Synthesis of microgel Alg-1.3: The swollen equilibrium microgel Alg-1 (100 g) was resuspended in 50 mL of 0.25 M NaOH solution and stirred for dispersion. Compound 11 (68.6 mg, 0.24 mmol) was weighed and added to the above system. The rest of the reaction process was referred to the synthesis of microgel HA-2.3. The supernatant of the reaction system was collected, and the amount of residual compound 11 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 11 was calculated to be approximately 2.44% (w / w).
[0228] The above structural formula and examples provide exemplary structures of alginate microgels modified with o-phthalaldehyde groups and methods for synthesizing them. Based on the contents of this application, those skilled in the art can imagine that other alginate microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the alginate microgels modified with o-phthalaldehyde groups.
[0229] Example 12: Synthesis of Sodium Carboxymethyl Starch Microgels Modified with O-Phthalaldehyde Groups (i.e. Microgels CMS-1.1 to CMS-1.3)
[0230]
[0231] (1) Synthesis of microgel CMS-1.1: The dried cross-linked sodium carboxymethyl starch (i.e., microgel CMS-1, 10 g) was uniformly dispersed in 100 mL of deionized water and stirred for dispersion. Compound 4 (0.6 g, 2.4 mmol, r=2), EDC (1.12 g, 7.2 mmol) and DPTS (1.8 g, 7.2 mmol) were added to the above system in sequence, and the rest of the reaction process was referred to the synthesis of microgel CMC-1.1. The supernatant of the reaction system was collected, and the amount of residual compound 4 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 4 was calculated to be approximately 2.17% (w / w).
[0232]
[0233] (2) Synthesis of microgel CMS-1.2: The dried cross-linked sodium carboxymethyl starch (i.e., microgel CMS-1, 10 g) was uniformly dispersed in 50 mL of 0.25 M NaOH solution, stirred and dispersed, and compound 9 (0.65 g, 2.5 mmol) was weighed and added to the above reaction solution, and reacted at 40° C. for 12 h. After the reaction was completed, the pH was adjusted to 7, and 10 volumes of anhydrous ethanol were used to reprecipitate a white powder. The white powder was resuspended in a 10% trifluoroacetic acid solution, stirred at room temperature for 1 h, and reprecipitated with 10 volumes of anhydrous ethanol to precipitate a white powder, i.e., cross-linked sodium carboxymethyl starch microgel modified with o-phthalaldehyde groups (i.e., microgel CMS-1.2). The supernatant of the reaction system was collected, and the amount of residual compound 9 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 9 was calculated to be approximately 2.43% (w / w).
[0234]
[0235] (3) Synthesis of microgel CMS-1.3: The dried cross-linked sodium carboxymethyl starch (i.e., microgel CMS-1, 10 g) was uniformly dispersed in anhydrous DMSO and stirred for dispersion. A solution of compound 10 (0.87 g, 2.4 mmol) in anhydrous DMSO was added dropwise to the above system, and dibutyltin dilaurate (13 μL, 20 μmol) was added as a catalyst, and nitrogen was filled for protection. The reaction was stirred at 70°C for 24 h. After the reaction was completed, the reaction system was allowed to stand, the microgel was collected, and dialyzed in physiological saline (pH = 7) for 2-3 days. The microgel was collected and a 10% trifluoroacetic acid solution was added, and the mixture was stirred at room temperature for 1 h. After the reaction was completed, it was reprecipitated with 10 times the volume of anhydrous ethanol to precipitate a white powder, i.e., cross-linked sodium carboxymethyl starch microgel modified with o-phthalaldehyde groups (i.e., microgel CMS-1.3). The supernatant of the reaction system was collected, and the amount of residual compound 10 in the supernatant was determined by high performance liquid chromatography. It was calculated that the labeling rate of compound 10 was approximately 3.21% (w / w).
[0236] The above structural formula and examples provide the structure of exemplary o-phthalaldehyde group-modified carboxymethyl starch microgel and its synthesis method. According to the contents of this application, those skilled in the art can imagine that other carboxymethyl starch microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the o-phthalaldehyde group-modified carboxymethyl starch microgel.
[0237] Example 13: Synthesis of polyglutamic acid microgel modified with o-phthalaldehyde groups (i.e. microgel PGA-1.1)
[0238]
[0239] The microgel PGA-1 (100 g) was resuspended in 500 mL of 0.01 mol / L MES buffer solution (pH = 5.2), stirred and dispersed, compound 2 (1.6 g, 6 mmol, s = 2) and DMTMM (5 g, 18 mmol) were weighed and dissolved in 20 mL of DMSO and added to the above reaction solution, and the rest of the reaction process was referred to the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected, and the amount of residual compound 2 in the supernatant was determined by high performance liquid chromatography, and the labeling rate of compound 2 was calculated to be approximately 0.88% (w / w).
[0240] The above structural formula and examples provide exemplary structures of polyglutamic acid microgels modified with o-phthalaldehyde groups and their synthesis methods. Based on the contents of this application, those skilled in the art can imagine that other polyglutamic acid microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the o-phthalaldehyde group-modified polyglutamic acid microgels.
[0241] Example 14: Synthesis of polyacrylic acid microgel modified with o-phthalaldehyde groups (i.e. microgel PAA-2.1)
[0242]
[0243] The microgel PAA-2 (100 g) was resuspended in 50 mL of 0.01 mol / L MES buffer solution (pH = 5.2), stirred and dispersed, EDC (10.38 g, 67 mmol) and N-hydroxysuccinimide (NHS, 7.69 g, 67 mmol) were weighed and added to the above system, and stirred at room temperature for 30 minutes. Compound 2 (53 mg, 0.2 mmol) was weighed and dissolved in 10 mL of DMSO and added to the above reaction solution, and reacted at room temperature for 24 hours. The pH of the reaction solution system was adjusted to 8-9, and then dialyzed with physiological saline for 2-3 days, and the microgel was collected and added with 10% trifluoroacetic acid, reacted for 1 hour, and then the reaction system was dialyzed with deionized water for 1 day, and the PAA microgel modified with o-phthalaldehyde group was collected, that is, microgel PAA-2.1. The supernatant of the reaction system was collected, and the amount of residual compound 2 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 2 can be calculated to be approximately 2.68% (w / w).
[0244] The above structural formula and examples provide exemplary structures of polyacrylic acid microgels modified with o-phthalaldehyde groups and their synthesis methods. Based on the contents of this application, those skilled in the art can imagine that other polyacrylic acid microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the polyacrylic acid microgels modified with o-phthalaldehyde groups.
[0245] Example 15: Synthesis of carboxylated polyethylene glycol microgels modified with o-phthalaldehyde groups (i.e. microgels PEG-1.1 and PEG-1.2)
[0246]
[0247] (1) Synthesis of microgel PEG-1.1: Microgel PEG-1 (10 g) was uniformly dispersed in 200 mL of deionized water and stirred for dispersion. Compound 2 (1.6 g, 6 mmol, s=2) and DMTMM (5 g, 18 mmol) were weighed and dissolved in 20 mL of DMSO and then added to the above reaction solution. The rest of the reaction process was referred to the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected, and the amount of residual compound 2 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 2 was calculated to be approximately 6.05% (w / w).
[0248]
[0249] (2) Synthesis of microgel PEG-1.2: Disperse microgel PEG-1 (10 g) uniformly in 200 mL of deionized water and stir to disperse. Weigh EDC (1.04 g, 6.7 mmol) and NHS (0.77 g, 6.7 mmol) and add them to the above system, and stir at room temperature for 30 minutes. Weigh compound 5 (0.35 g, 1 mmol, r=2, s=6) and dissolve it in 20 mL of DMSO and add it to the above reaction solution. The rest of the reaction process refers to the synthesis of microgel HA-2.1. Collect the supernatant of the reaction system, and determine the amount of residual compound 5 in the supernatant by high performance liquid chromatography. The labeling rate of compound 5 can be calculated to be approximately 1.10% (w / w).
[0250] The above structural formula and examples provide the structure of exemplary o-phthalaldehyde group-modified polyethylene glycol microgel and its synthesis method. According to the contents of this application, those skilled in the art can imagine that other polyethylene glycol microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the o-phthalaldehyde group-modified polyethylene glycol microgel.
[0251] Embodiment 16 to Embodiment 21:
[0252] Preparation of the hemostatic material of the present invention and its control material
[0253] Example 16: Preparation of hemostatic sponge
[0254] Taking the microgel HA-2.2 in Example 9 as an example, the microgel was fully dispersed in deionized water to obtain a suspension with a solid content of 0.5% to 1.5% (w / v). The suspension was poured into a mold, frozen at -20°C for 6 hours, and then freeze-dried at -60°C for 48 hours to obtain the hemostatic sponge of the present invention.
[0255] Microgels modified with other o-phthalaldehyde groups can also be used to prepare hemostatic sponges.
[0256] Comparative Example 17: Synthesis of Control Sponge
[0257] Taking the microgel HA-2 in Example 2 as an example, the microgel was fully dispersed in deionized water to obtain a suspension with a solid content of 0.5% to 1.5% (w / v). The suspension was poured into a mold, frozen at -20°C for 6 hours, and then freeze-dried at -60°C for 48 hours to obtain a control sponge without modification of o-phthalaldehyde groups.
[0258] Example 18: Preparation of hemostatic powder
[0259] Taking the microgel CMC-1.2 synthesized in Example 10 as an example, the microgel was fully dispersed in deionized water, replaced with 75%, 90% and anhydrous ethanol respectively, and the precipitated solid was collected and freeze-dried at -60°C for 48 hours, and then vacuum-dried at 30°C for 12 hours. After sieving with sieves of different mesh sizes, powders of different mesh sizes were obtained, which were the hemostatic powder of the present invention.
[0260] Other microgels modified with o-phthalaldehyde groups can also be used for the preparation of the hemostatic powder of the present invention.
[0261] Comparative Example 19: Synthesis of Control Powder
[0262] Taking the microgel CMC-1 synthesized in Example 3 as an example, the microgel was fully dispersed in deionized water, replaced with 75%, 90% and anhydrous ethanol respectively, and the precipitated solid was collected and freeze-dried at -60°C for 48 hours, and then vacuum-dried at 30°C for 12 hours. After sieving with sieves of different mesh sizes, powders of different mesh sizes were obtained, which were the control powders of the present invention.
[0263] Example 20: Preparation of fluid hemostatic agent
[0264] Taking the microgel HA-2.2 synthesized in Example 9 as an example, the microgel was frozen at -20°C for 6 hours, then freeze-dried at -60°C for 48 hours, redispersed in physiological saline containing 5% glycerol, and homogenized using a high-speed homogenizer to obtain a paste fluid with a solid content of 5% to 10% (w / v) and a certain fluidity, namely the mobile hemostatic agent of the present invention.
[0265] Other microgels modified with o-phthalaldehyde groups can also be used to prepare the mobile hemostatic agent of the present invention.
[0266] Comparative Example 21: Synthesis of Control Fluid
[0267] Taking the microgel HA-2 synthesized in Example 2 as an example, the microgel was frozen at -20°C for 6 hours, then freeze-dried at -60°C for 48 hours, redispersed in physiological saline containing 5% glycerol, and homogenized using a high-speed homogenizer to obtain a paste fluid with a solid content of 5% to 10% (w / v) and a certain fluidity, i.e., the control fluid.
[0268] Embodiment 22 to Embodiment 26:
[0269] Verification experiment of hemostasis, tissue adhesion and mechanical property enhancement after blood absorption of the hemostatic material of the present invention Example 22: In vitro thrombosis experiment of hemostatic sponges with different o-phthalaldehyde group labeling rates
[0270] In this example, the hemostatic ability of the hemostatic sponge of the present invention is characterized by a thrombus formation experiment. The specific experimental method is as follows:
[0271] The microgels HA-2.2 (0.58), HA-2.2 (1.12), HA-2.2 (2.03) and HA-2.2 (4.21) with the labeling rates of phthalaldehyde groups of 0.58%, 1.12%, 2.03% and 4.21% (w / w) in Example 9 were selected for in vitro thrombosis experiment, and the control sponge (i.e., the labeling rate was 0) and the commercial absorbable gelatin sponge were selected as the control group. The materials were placed in a clean container and preheated at 37°C, and 100 μL of 37°C fresh EDTA anticoagulated sheep blood was dripped on the surface of the materials. For the blank group, the blood was directly dripped on the wall of the container and left to stand at 37°C for 5 minutes. Then pour 4 mL of deionized water into the container and shake it slightly to rupture the red blood cells that have not been absorbed by the material. Aspirate the supernatant to detect the characteristic absorption of red blood cell hemoglobin at 540 nm, and calculate the thrombosis index according to the formula below. The lower the thrombosis index, the stronger the material's ability to form thrombus.
[0272]
[0273] In this example, the in vitro hemostatic properties of the control group and the hemostatic sponges with different o-phthalaldehyde group labeling rates, the control sponge and the commercial absorbable gelatin sponge are as follows: Figure 2 As shown, the experimental results show that after labeling with o-phthalaldehyde groups, the thrombosis ability of the hemostatic sponge is significantly improved, and the higher the o-phthalaldehyde group labeling rate on the hemostatic sponge, the stronger the thrombosis ability, indicating that the hemostatic effect of the sponge is better. It can be seen that the o-phthalaldehyde groups modified on the hemostatic sponge in the present invention can effectively improve the hemostatic performance of the hemostatic material.
[0274] Other hemostatic sponges or other different forms of hemostatic materials prepared based on microgels modified with o-phthalaldehyde groups also have excellent hemostatic properties.
[0275] Example 23: In vitro thrombosis experiment of hemostatic powder with different particle size distribution
[0276] In this embodiment, the hemostatic performance of the hemostatic powder is characterized by the thrombosis index. The specific experiment is as follows: the hemostatic powder with the same o-phthalaldehyde group labeling rate prepared in Example 18 is passed through sieves with different mesh sizes to collect hemostatic powder materials with different particle size distributions, and the materials are divided into five groups (Group 1: mesh size less than 20 mesh, Group 2: 20-32 mesh, Group 3: 32 mesh-80 mesh, Group 4: 80 mesh-200 mesh, Group 5: mesh size greater than 200 mesh), observed under a microscope, and an in vitro thrombosis experiment was conducted: a certain mass (10 mg) of material was placed in a clean centrifuge tube and preheated at 37°C, 50 μL of 37°C fresh EDTA anticoagulated sheep blood was dripped on the surface of the material, and the blank control group was directly dripped with blood on the wall of the container and allowed to stand at 37°C for 5 minutes. Subsequently, 2 mL of deionized water was poured into the container and slightly shaken, the supernatant was aspirated to detect the absorbance at 540 nm, and the thrombosis index was calculated according to the formula in Example 22.
[0277] In this example, the microscopic images (left) and thrombosis test results (right) of hemostatic powder modified with o-phthalaldehyde groups of different particle sizes are shown in FIG. Figure 3 As shown, the results show that within a certain particle size range, the thrombosis ability of the hemostatic powder is closely related to its particle size. The smaller the particle size, the larger the specific surface area of the hemostatic powder, the larger the surface area in contact with the blood, and the stronger the ability to form a thrombus, indicating that the hemostatic effect of the hemostatic powder is better.
[0278] Other hemostatic powders prepared based on microgels modified with o-phthalaldehyde groups also have excellent hemostatic properties.
[0279] Example 24: In vitro tissue adhesion test of hemostatic materials
[0280] The tissue adhesion of the hemostatic material is a property required for it to block bleeding points, effectively control bleeding in a timely manner, and reduce the risk of venous thrombosis over a long period of time. This example tests the tissue adhesion of the hemostatic sponge of the present invention by a standard lap shear test (ASTM F2255), and the specific experimental method is as follows:
[0281] The adhesion strength of the above-mentioned hemostatic materials of different formulations on pigskin was measured by a standard lap shear test using a tensile machine (Germany INSTRON), and the control hemostatic material and commercial Fibrin glue (fibrinogen glue) in the present invention were selected as the control group. The pigskin was cut into rectangular pigskins of 20 mm wide and 40 mm long. During the mechanical test, a transparent polymethyl methacrylate film was used as a hard backing for the tissue. For the sponge material, the sponge was cut into different formula hemostatic sponges or control sponges of the same thickness (3 mm) and the same area (20 mm × 20 mm), and attached to one end of a piece of pigskin (the adhesion area was 20 mm × 20 mm). Immediately press another piece of pigskin on top of the sponge material on the other pigskin, press evenly for 2 minutes with a force of 100 kPa, and immediately perform a tensile test to evaluate the instantaneous tissue adhesion strength of the above-mentioned sponge material. Subsequently, the pigskin was soaked in physiological saline for 12 hours, and the surface liquid was wiped and then the tensile test was performed to evaluate the long-term tissue adhesion strength of the above-mentioned sponge material. For powder materials, the hemostatic powder or control powder was evenly spread on one end of the pigskin (adhesion area was 20mm×20mm) with a thickness of 1mm. Immediately press another piece of pigskin on top of the powder material on the other pigskin, press evenly with a force of 100kPa for 2 minutes, and immediately perform a tensile test to evaluate the instantaneous tissue adhesion strength of the above powder material. Subsequently, soak the pigskin in saline for 12h, wipe the surface liquid and then perform a tensile test to evaluate the long-term tissue adhesion strength of the above powder material. For fluid materials, 0.2mL of flowing hemostatic agent or control fluid was evenly spread on one end of the pigskin (adhesion area was 20mm×20mm), immediately press another piece of pigskin on top of the fluid, press evenly with a force of 100kPa for 2 minutes, and immediately perform a tensile test to evaluate the instantaneous tissue adhesion strength of the fluid material. Subsequently, soak the pigskin in saline for 12h, wipe the surface liquid and then perform a tensile test to evaluate the long-term tissue adhesion strength of the above fluid material. For the Fibrin glue control group, the two-component solution was sprayed on one end of a piece of pig skin (adhesion area of 20mm×20mm) through a double mixer, and another piece of pig skin was immediately pressed on the glue, and pressed evenly with a force of 100kPa for 2 minutes, and a tensile test was immediately performed to evaluate the instantaneous tissue adhesion strength of Fibrin glue. Subsequently, the pig skin was soaked in saline for 12h, and the surface liquid was wiped off and then a tensile test was performed to evaluate the long-term tissue adhesion strength of Fibrin glue. The adhesion strength was calculated by the following formula, where Fmax is the maximum force value. To ensure the reliability of the data, three samples under each condition were measured.
[0282]
[0283] In this embodiment, the instantaneous tissue adhesion strength and long-term tissue adhesion strength of different materials are shown in Table 1. The results show that the sponge material modified by the o-phthalaldehyde group in the present invention has excellent tissue adhesion performance compared to commercial Fibrin glue and the control sponge without o-phthalaldehyde group modification (i.e., the control sponge prepared based on microgel HA-2), and the higher the o-phthalaldehyde group labeling rate on the sponge material, the stronger its instantaneous and long-term tissue adhesion; in a wet environment, the tissue adhesion of the sponge material without o-phthalaldehyde group modification is greatly attenuated, and it is difficult to achieve long-term stable tissue adhesion, while the sponge material modified by the o-phthalaldehyde group has stable and long-term tissue adhesion. At the same time, other forms of hemostatic materials of the present invention also embody stronger instantaneous tissue adhesion strength and long-term tissue adhesion strength than the control material and commercial Fibrin glue (fibrinogen glue).
[0284] Table 1
[0285]
[0286] Example 25: Rheological test of hemostatic materials
[0287] Blocking bleeding points with a physical barrier is a strategy for controlling bleeding using hemostatic materials. However, the mechanical properties of common hemostatic materials, such as gauze, sponges, hydrogels and powders, are often weakened in the presence of blood (wet environment), making it difficult to block bleeding points in a timely and long-term manner, especially to block active or pressure bleeding points. The hemostatic material prepared by the present invention is based on the chemical reaction of o-phthalaldehyde and amine groups, and can react with a large amount of plasma proteins in the blood to form a complex of material and thrombus, enhance the mechanical properties of the material, achieve compression blocking of bleeding points, and resist continuous bleeding. This example studies the changes in mechanical properties (storage modulus) of the hemostatic material of the present invention before and after the reaction with blood through rheological testing, and the specific experimental method is as follows:
[0288] A HAAKE MARS rheometer was used to perform rheological tests on a test platform (20 mm in diameter) at 37°C. For sponge materials, the hemostatic sponge in Example 16 (components selected from microgel HA-2.2 (4.21)) and the control sponge in Comparative Example 17 (components selected from microgel HA-2) were used for testing: the sponges were pre-cut into circles of the same size (thickness 0.5 mm, diameter 20 mm), placed on the test platform, and 200 uL of physiological saline or fresh EDTA anticoagulated sheep blood was dripped on the top of the materials, fully absorbed at 37°C for 5 minutes, and then immediately subjected to rheological tests to record their storage modulus (G'). For powder materials, the hemostatic powder in Example 18 (the component is selected from microgel HA-2.2 (4.21)) and the control powder in Comparative Example 19 (the component is selected from microgel HA-2) were tested: the same mass (50 mg) of powder was evenly spread on the test platform, 200 uL of saline or fresh EDTA anticoagulated sheep blood was dripped on the top of the material, fully absorbed at 37°C for 5 minutes, and then the rheological test was immediately performed to record its storage modulus (G'). For fluid materials, the mobile hemostatic agent in Example 20 (the component is selected from microgel HA-2.2 (4.21)) and the control fluid in Comparative Example 21 (selected from microgel HA-2) were tested: the same volume (200 μL) of fluid was spread on the test platform, 200 uL of saline or fresh EDTA anticoagulated sheep blood was dripped on the top of the material, fully absorbed at 37°C for 5 minutes, and then the rheological test was immediately performed to record its storage modulus (G'). To ensure the reliability of the data, three samples were measured in each condition.
[0289] Table 2
[0290]
[0291]
[0292] In this embodiment, the changes in mechanical properties of different hemostatic materials of the present invention before and after the reaction with blood are shown in Table 2. The results show that the storage modulus of the hemostatic material of the present invention after absorbing blood and saline is significantly different, and the storage modulus of the hemostatic material after absorbing blood is significantly improved; while for the unlabeled control group material, there is no obvious difference in the storage modulus after absorbing blood or saline. The above results show that the hemostatic material of the present invention can increase its storage modulus after contacting and reacting with blood, that is, enhance the mechanical properties.
[0293] Other hemostatic materials prepared based on microgels modified with o-phthalaldehyde groups can also increase their storage modulus and enhance their mechanical properties after contact and reaction with blood.
[0294] Example 26: Scanning electron microscope image of the interaction between hemostatic sponge and blood cells
[0295] Platelet adhesion is the initial step of thrombus formation and plays an important role in the hemostasis process; in addition, the rapid adhesion and aggregation of red blood cells also contribute to the formation of thrombus. The adhesion of platelets and red blood cells is one of the indicators for evaluating the quality of hemostatic performance. This example uses scanning electron microscopy (SEM) to characterize the adhesion of the hemostatic material of the present invention to platelets and red blood cells. The specific experimental method is as follows:
[0296] A NOVA NanoSEM 230 low vacuum ultra-high resolution field emission scanning electron microscope was used to observe the surface morphology in the fast electron backscatter diffraction EBSD mode. Fresh EDTA anticoagulated sheep blood was centrifuged at 1500rpm for 12 minutes at room temperature. After centrifugation, the upper layer was platelet-rich plasma, and the lower layer was packed white blood cells and red blood cells. The blood cells in the lower layer were collected. The platelet-rich plasma was transferred to a plastic test tube and centrifuged at 3500rpm for 5 minutes to collect the platelets in the lower layer. The collected blood cells and platelets were resuspended in phosphate buffered saline (PBS) respectively, added dropwise to the sponge sample (the hemostatic sponge in Example 16, the component was selected from microgel HA-2.2 (4.21)), and reacted at 37°C for 5 minutes. The sample was washed 3 times with PBS and fixed with 5% glutaraldehyde solution for 4 hours. The fixed sample was washed 3 times with PBS. Then, the sample was replaced with 30%, 50%, 70%, 90%, 95% ethanol solution and anhydrous ethanol respectively, each for 10 minutes; then, the ethanol was replaced with tert-butyl alcohol at room temperature for more than 3 times, each for 15 minutes, and the sample was frozen and crystallized at 4°C and freeze-dried. The sample was subjected to Pt metal coating.
[0297] In this embodiment, the scanning electron microscopic morphology of the surface adhesion, aggregation, activation of platelets (left figure) and adsorption of red blood cells (right figure) of the hemostatic sponge of the present invention is shown in FIG. Figure 4 As shown in the figure, it can be clearly observed that the platelets on the surface of the hemostatic sponge of the present invention are tightly adhered to the surface of the material, and the shape of the platelets changes from spheres to a multi-pseudopodal mesh structure after being activated; a large number of red blood cells are adsorbed and aggregated in the porous structure of the material. The above experimental results prove that the hemostatic sponge of the present invention can adhere to, aggregate and activate platelets, adsorb red blood cells, and help thrombosis.
[0298] Embodiment 27 to Embodiment 39:
[0299] Hemostatic application of the hemostatic sponge of the present invention
[0300] Example 27: Application of hemostatic sponge in non-compression hemostasis of penetrating wounds
[0301] A SD rat liver perforation model was selected and divided into three groups for non-compressive hemostasis experiments on penetrating injuries, with 3 rats in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which is selected from microgel HA-2.2 (4.21)); a sponge control group of the present invention (group b, the control sponge in comparative example 17, the component of which is selected from microgel HA-2); and a commercial absorbable gelatin sponge group (group c). After anesthetizing the SD rats, their abdominal cavities were opened, the liver was lifted and placed on a pre-weighed filter paper, and then a penetrating wound with a diameter of 5 mm was established on the liver to cause bleeding. Subsequently, different groups of hemostatic materials were stuffed into the penetrating wound. The amount of blood loss was measured by the weight gain of the hemostatic material and the filter paper, and the hemostasis time was recorded by a timer. In this example, photographs of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge (group c) used for non-compressive hemostasis of penetrating injuries are shown in the following figure. Figure 5 The experimental results show that group a has the least blood loss (group a 0.5±0.1g, group b 1.0±0.2g, group c 1.2±0.2g), and group a has the shortest hemostasis time (group a 45±10s, group b 60±12s, group c 80±15s). It can be seen that the hemostatic sponge in the present invention can be used for non-compression hemostasis of penetrating wounds.
[0302] Hemostatic sponges made of other different materials can also be used for non-compression hemostasis of penetrating wounds.
[0303] Example 28: Application of hemostatic sponge to stop bleeding in liver
[0304] A liver cross-sectional trauma model of SD rats was selected and divided into three groups for liver hemostasis experiments, with 3 rats in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which was selected from microgel HA-2.4); a sponge control group of the present invention (group b, the control sponge in comparative example 17, the component of which was selected from microgel HA-2); and a commercial absorbable gelatin sponge group (group c). After anesthetizing the SD rats, their abdominal cavities were opened, the liver was lifted and placed on a pre-weighed filter paper, and then a cross-sectional section with a diameter of 10 mm was established on the liver to cause bleeding. Subsequently, the hemostatic materials of different groups were lightly pressed on the cross-sectional wound surface. The amount of blood loss was measured by the weight gain of the hemostatic material and the filter paper, and the hemostasis time was recorded by a timer. In this example, photographs of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge (group c) used for liver hemostasis are shown in the figure. Figure 6 As shown. The experimental results show that group a has the least blood loss (group a 0.3±0.1g, group b 0.7±0.3g, group c 1.2±0.2g), and group a has the shortest hemostasis time (group a 15±10s, group b 60±20s, group c 150±13s). It can be seen that the hemostatic sponge in the present invention can be used for liver hemostasis.
[0305] Hemostatic sponges made of other different materials can also be used to stop liver bleeding.
[0306] Example 29: Application of hemostatic sponge to spleen hemostasis
[0307] A spleen incision bleeding model of New Zealand white rabbits was selected, and the spleen hemostasis experiment was carried out in three groups, with 3 rabbits in each group: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component is selected from microgel HA-2.1); the sponge control group of the present invention (group b, the control sponge in comparative example 17, the component is selected from microgel HA-2); commercial absorbable hemostatic gauze (group c). After the New Zealand white rabbits were anesthetized and fixed, the abdominal hair was shaved, and the midline of the abdomen was incised to open the abdominal cavity and expose the spleen. An incision (8mm wide and 2mm deep) was made in the spleen to cause spleen damage, and bleeding continued for 30s. Then, different groups of hemostatic materials were placed on the bleeding site and pressed for 60 seconds and then observed. If the bleeding was not successfully stopped, the pressure was continued. The experimental results show that the hemostasis time of group a is the shortest (80±20s in group a, 3 rabbits in group b failed to stop bleeding after more than 5 minutes, and 240±45s in group c), and the blood loss in group a is the least (1.3±0.3g in group a, 5±0.8g in group b within 5 minutes, and 4±0.65g in group c). It can be seen that the hemostatic sponge in the present invention can be applied to spleen hemostasis.
[0308] Hemostatic sponges made of other different materials can also be used to stop spleen bleeding.
[0309] Example 30: Application of hemostatic sponge to hemostasis of superficial arteries
[0310] A New Zealand white rabbit ear artery bleeding model was selected and divided into three groups for surface artery hemostasis experiments, with 3 rabbits in each group: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component is selected from microgel CMC-1.2); the sponge control group of the present invention (group b, the control sponge in comparative example 17, the component is selected from microgel CMC-1); the commercial absorbable gelatin sponge group (group c). After the rabbit was anesthetized, the rabbit ear artery was punctured with a needle, and then the hemostatic materials of different groups were lightly pressed on the wound, and the hemostasis time was recorded by a timer. In this example, photos of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge group (group c) used for rabbit ear artery hemostasis are shown in the figure. Figure 7 As shown. The experimental results show that the hemostatic time of group a is the shortest (group a 13±10s, group b 65±15s, group c 85±13s) and the blood loss of group a is the least (group a 0.2±0.1g, group b 1.2±0.5g, group c 1.0±0.4g). It can be seen that the hemostatic sponge in the present invention can be used for hemostasis of superficial arteries.
[0311] Hemostatic sponges composed of other different materials can also be used to stop bleeding in superficial arteries.
[0312] Example 31: Application of hemostatic sponge to stop bleeding in body surface veins
[0313] A New Zealand white rabbit ear vein bleeding model was selected and divided into three groups for surface vein hemostasis experiments, with 3 rabbits in each group: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component is selected from microgel CMC-1.1); the sponge control group of the present invention (group b, the control sponge in comparative Example 17, the component is selected from microgel CMC-1); the commercial absorbable gelatin sponge group (group c). After the rabbit was anesthetized, the rabbit ear vein was pierced with a needle tube, and then the hemostatic materials of different groups were gently pressed on the wound, and the hemostasis time was recorded by a timer. The experimental results showed that the hemostasis time of group a was the shortest (group a 20±10s, group b 50±12s, group c 55±15s), and the blood loss of group a was the least (group a 0.5±0.1g, group b 1.5±0.3g, group c 1.5±0.2g). It can be seen that the hemostatic sponge in the present invention can be used for surface vein hemostasis.
[0314] Hemostatic sponges made of other different materials can also be used for superficial venous hemostasis.
[0315] Example 32: Application of hemostatic sponge to hemostasis of femoral artery
[0316] A femoral artery bleeding model of SD rats was selected and divided into three groups for femoral artery hemostasis experiment, with 3 rats in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component is selected from microgel Alg-1.2); a sponge control group of the present invention (group b, the control sponge in comparative example 17, the component is selected from microgel Alg-1); a commercial absorbable gelatin sponge group (group c). After the SD rats were anesthetized and fixed, the hair on the left leg was shaved, and the covering muscles of the groin were opened to expose the femoral artery. A dissecting needle was used for puncture with a depth of 0.5 mm. Subsequently, the hemostatic materials of different groups were lightly pressed on the wound, and the hemostatic time was recorded by a timer. The hemostatic material was gently lifted every 5 seconds to observe the bleeding situation until the bleeding was completely stopped. The amount of blood loss was calculated by the weight gain of the pre-weighed hemostatic material. The experimental results show that the hemostasis time of group a is the shortest (120±25s in group a, 1 rat in group b successfully stopped bleeding in 280s, the other 2 rats failed to stop bleeding within 5 minutes, and 3 rats in group c failed to stop bleeding within 5 minutes), and the blood loss in group a is the least (1.5±0.4g in group a, 3.5±0.7g in group b within 5 minutes, and 4.0±1.0g in group c within 5 minutes). It can be seen that the hemostatic sponge in the present invention can be applied to femoral artery hemostasis.
[0317] Hemostatic sponges composed of other different materials can also be used for femoral artery hemostasis.
[0318] Example 33: Application of hemostatic sponge to hemostasis of abdominal aorta
[0319] The abdominal aorta bleeding model of SD rats was selected and divided into three groups for abdominal aorta hemostasis experiment, with 3 rats in each group: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component is selected from microgel HA-2.4); the sponge control group of the present invention (group b, the control sponge in comparative example 17, the component is selected from microgel HA-2); the commercial absorbable gelatin sponge group (group c). After the SD rats were anesthetized and fixed, the abdominal hair was shaved, the abdominal cavity was opened, and the internal organs were exposed. Use a small piece of filter paper to gently push the intestine and fat to the left abdomen of the mouse, separate the two larger blood vessels in front of the spine, and the slightly whiter one on the right is the abdominal aorta. Use a dissecting needle for puncture, with a depth of 0.5mm. Subsequently, the hemostatic materials of different groups were lightly pressed on the wound surface, and the hemostasis time was recorded by a timer. The hemostatic material was gently lifted every 5 seconds to observe the bleeding situation until the bleeding was completely stopped. The amount of blood loss was calculated by the weight gain of the pre-weighed hemostatic material. During the experiment, the hemostasis time of group a was the shortest (155±45s in group a, and the three rats in groups b and c did not achieve hemostasis within 5 minutes), and the blood loss in group a was the least (1.3±0.5g in group a, and the blood loss in groups b and c within 5 minutes was 2.4±0.8g and 2.8±0.9g, respectively). It can be seen that the hemostatic sponge in the present invention can be used for hemostasis of the abdominal aorta.
[0320] Hemostatic sponges composed of other different materials can also be used to stop bleeding in the abdominal aorta.
[0321] Example 34: Application of hemostatic sponge to carotid artery hemostasis
[0322] The SD rat carotid artery bleeding model was selected and divided into three groups for carotid artery hemostasis experiment, with 3 rats in each group: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component is selected from microgel HA-2.3); the sponge control group of the present invention (group b, the control sponge in comparative example 17, the component is selected from microgel HA-2); the commercial absorbable gelatin sponge group (group c). The SD rats were anesthetized, the neck hair was shaved and fixed, and the rats were wiped and disinfected with iodine tincture. A longitudinal incision of about 2 cm was made in the middle of the neck, and then a complete transsection of the common carotid artery was performed. Subsequently, the hemostatic material was immediately applied to the bleeding site and the same pressure was applied. The wound was observed approximately every 10 seconds, and the hemostasis time was recorded immediately after the bleeding stopped completely. The hemostatic material was weighed before and after use, and the difference was the total blood loss. The experimental results show that the hemostatic sponge (group a) of the present invention firmly adheres to the transverse section of the carotid artery. Compared with other groups, the hemostatic time of group a is the shortest (group a 250±22s, group b and group c failed to stop bleeding after more than 5 minutes), and group a has the least blood loss (group a 1.6±0.5g, group b and group c lost 2.8±0.9g and 3.2±1.1g within 5 minutes, respectively). It can be seen that the hemostatic sponge in the present invention can be applied to carotid artery hemostasis.
[0323] Hemostatic sponges composed of other different materials can also be used for carotid artery hemostasis.
[0324] Example 35: Application of hemostatic sponge to cardiac hemostasis
[0325] A SD rat heart bleeding model was selected and divided into three groups for a heart hemostasis experiment, with 3 rats in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component is selected from microgel PAA-2.1); a sponge control group of the present invention (group b, the control sponge in comparative Example 17, the component is selected from microgel PAA-2); a commercial absorbable hemostatic gauze group (group c). The SD rats were anesthetized and fixed, and the chest hair was shaved. The chest cavity was opened and the heart was exposed, and the pericardium was removed using fine tweezers. A biopsy punch was used to create a 2 mm diameter injury to the left or right ventricular wall of the heart. Subsequently, the hemostatic material was immediately applied to the bleeding site and a certain amount of pressure was applied. The wound was observed approximately every 10 seconds, and the hemostasis time was recorded immediately after the bleeding stopped completely. The hemostatic material was weighed before and after use, and the difference was the total blood loss. For rats that failed to successfully stop bleeding within 5 minutes, the rats were euthanized by bleeding. The experimental results show that the hemostatic sponge (group a) of the present invention is firmly adhered to the ventricular wound surface. Compared with other groups, the hemostatic time of group a is the shortest (80 ± 12s in group a, 200 ± 35s in group b, and 3 rats in group c failed to stop bleeding within 5 minutes), and the blood loss in group a is the least (1.6 ± 0.3g in group a, 2.0 ± 0.5g in group b, and 3.7 ± 0.8g in group c within 5 minutes). After surgery, all (3) SD rats in group a survived successfully, and rats in groups b and c died within 30 minutes during or after the experiment. It can be seen that the hemostatic sponge in the present invention can be applied to cardiac hemostasis.
[0326] Hemostatic sponges made of other different materials can also be used to stop cardiac bleeding.
[0327] Example 36: Application of hemostatic sponge in coronary artery hemostasis
[0328] A Bama pig coronary artery injury model was selected and divided into three groups for coronary artery hemostasis experiments, with 3 pigs in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component is selected from microgel HA-2.2 (4.21)); a sponge control group of the present invention (group b, the control sponge in comparative example 17, the component is selected from microgel HA-2); a commercial absorbable hemostatic gauze group (group c). The Bama pig was anesthetized, the chest cavity was opened and the heart was exposed, the coronary artery was isolated and clamped on both sides, and a dissecting needle was used to puncture in the middle of the clamped ends on both sides with a depth of 1 mm. Subsequently, the hemostatic material was immediately applied to the bleeding site, and a certain pressure was applied. The wound was observed approximately every 20 seconds, and the hemostasis time was recorded immediately after the bleeding stopped completely. The hemostatic material was weighed before and after use, and the difference was the total blood loss. The experimental results show that the hemostasis time of group a is the shortest (group a 155±25s, group b 380±110s, group c failed to stop bleeding for more than 10 minutes), and the blood loss of group a is the least (group a 10±3.5g, group b 23±8.2g, group c blood loss within 10 minutes is 45±9.0g). It can be seen that the hemostatic sponge in the present invention can be used for coronary artery hemostasis.
[0329] Hemostatic sponges composed of other different materials can also be used for coronary artery hemostasis.
[0330] Example 37: Application of hemostatic sponge to hemostasis of tooth extraction wound
[0331] A beagle dog tooth extraction wound model was selected and divided into four groups for a tooth extraction wound hemostasis experiment: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component is selected from microgel PEG-1.1); the sponge control group of the present invention (group b, the control sponge in comparative Example 17, the component is selected from microgel PEG-1); the commercial absorbable gelatin sponge group (group c); and the blank group (group d). The beagle dogs were anesthetized and fixed, the oral cavity was disinfected, and four premolars were symmetrically extracted on the left and right sides, leaving tooth extraction wounds. For group a, group b and group c, the tooth extraction wounds were filled with the hemostatic sponge of the present invention, the sponge control group and the commercial absorbable gelatin sponge, respectively. Group d did not take any measures, and each group had 4 wounds. Observe the hemostasis. If the bleeding stops, it proves that the hemostasis is complete, and record the hemostasis time; if there is still fluid bleeding, continue to compress until there is no bleeding. 0.5, 1, 6, and 12 hours after complete hemostasis, observe whether there is secondary bleeding. The experimental results showed that compared with the other groups, the hemostasis time of group a was the shortest (group a 55±10s, group b 105±21s, group c 200±20s, group d 266±35s) and there was no obvious secondary bleeding in the later period. One tooth extraction wound in group b and group c had secondary bleeding 1 hour after complete hemostasis, and two tooth extraction wounds in group d had secondary bleeding 0.5 hours after complete hemostasis. It can be seen that the hemostatic sponge in the present invention can be used for hemostasis of tooth extraction wounds.
[0332] Hemostatic sponges made of other different materials can also be used to stop bleeding from tooth extraction wounds.
[0333] Example 38: Application of hemostatic sponge to hemostasis of spine
[0334] The SD rat spinal injury model was selected and divided into three groups for spinal hemostasis experiment, with 3 rats in each group: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component selected from microgel CMC-1.3); the sponge control group of the present invention (group b, the control sponge in comparative Example 17, the component selected from microgel CMC-1); the commercial absorbable gelatin sponge group (group c). The SD rats were anesthetized and fixed, the back hair was shaved, and the skin and fascia were cut in sequence with chest 13 and waist 1 as the center to expose the muscles in the surgical area. On one side, ophthalmic scissors were used to cut the muscles and tendons connected to the spinous process close to it, and an incision was created, the length of which was preferably chest 12 to waist 2, and the depth was to reach the articular process. Another parallel incision was cut about 0.5 cm outside the incision, and the length and depth were basically the same as the previous incision. The muscles between the two incisions were removed to expose 3 pairs of articular processes (chest 12 to chest 13, chest 13 to waist 1 and waist 1 to waist 2). Expose the lateral wall of the spinal canal and the intervertebral foramen at one time, cut off the two lateral walls of the spinal canal in parallel, expose the spinal cord, and create a bleeding wound. Subsequently, the hemostatic material is immediately applied to the bleeding site, and a certain pressure is applied. The wound surface is observed approximately every 10 seconds, and the hemostasis time is recorded immediately after the bleeding stops completely. The hemostatic material is weighed before and after use, and the difference is the total blood loss. The experimental results show that the hemostasis time of group a is the shortest (group a 60 ± 10s, group b 200 ± 24s, group c 250 ± 28s), and the amount of blood loss in group a is the least (group a 0.5 ± 0.2g, group b 1.2 ± 0.3g, group c 1.8 ± 0.8g). It can be seen that the hemostatic sponge in the present invention can be applied to spinal hemostasis.
[0335] Hemostatic sponges composed of other different materials can also be used for spinal hemostasis.
[0336] Example 39: Application of hemostatic sponge to uterine wall for hemostasis
[0337] A uterine incision model of female New Zealand white rabbits aged 12 to 18 weeks was selected and divided into three groups for uterine wall hemostasis experiments, with 3 rabbits in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component selected from microgel HA-2.2 (4.21)); a sponge control group of the present invention (group b, the control sponge in comparative Example 17, the component selected from microgel HA-2); a commercial absorbable gelatin sponge group (group c). After the New Zealand white rabbits were anesthetized and fixed, the skin and hair of the lower abdomen were shaved and disinfected with iodine and 75% ethanol. The abdominal wall skin was cut open, the tissue was cut layer by layer, the pelvic cavity was opened, the uterus was slowly exposed, and a 2 cm long incision was made on the right uterus 3.5 cm away from the vagina to form a bleeding wound, which was the result of model establishment. The hemostatic material was immediately applied to the bleeding site, and the upper layer was covered with pre-weighed gauze. The wound was observed approximately every 10 seconds, and the hemostasis time was recorded immediately after the bleeding stopped completely. The hemostatic material and gauze were weighed before and after use, and the difference was the total blood loss. The experimental results show that the hemostatic time of group a is the shortest (group a 30±6s, group b 60±12s, group c 50±8s), and the blood loss of group a is the least (group a 1.8±0.2g, group b 3.4±0.3g, group c 2.5±0.5g). It can be seen that the hemostatic sponge in the present invention can be used for uterine wall hemostasis.
[0338] Hemostatic sponges made of other different materials can also be used to stop bleeding in the uterine wall.
[0339] Embodiment 40 to Embodiment 49:
[0340] Hemostatic application of the hemostatic powder of the present invention
[0341] Example 40: Application of hemostatic powder to stop bleeding in the liver
[0342] A liver cross-sectional trauma model of SD rats was selected and divided into three groups for liver hemostasis experiment, with 3 rats in each group: the hemostatic freeze-dried powder group of the present invention (group a, the hemostatic powder in Example 18, the component is selected from microgel HA-2.1); the control powder group of the present invention (group b, the control powder in comparative Example 19, the component is selected from microgel HA-2); commercial chitosan hemostatic granules (group c). After the SD rats were anesthetized and fixed, the hair on the upper abdomen was shaved, the abdominal cavity was opened, the liver was lifted and placed on a pre-weighed filter paper, and then a cross-sectional section with a diameter of 10 mm was established on the liver to cause bleeding. Subsequently, a certain mass of hemostatic materials from different groups were sprayed on the cross-sectional trauma. The amount of blood loss was measured by the weight gain of the filter paper and the weight gain of the material, and the hemostasis time was recorded by a timer. In this example, photos of the hemostatic powder of the present invention (group a), the control powder (group b) and the commercial chitosan hemostatic granules (group c) used for liver hemostasis are shown in the figure. Figure 8The experimental results show that group a has the least blood loss (group a 0.1±0.05g, group b 0.8±0.1g, group c 0.5±0.2g), and group a has the shortest hemostasis time (group a 25±5s, group b 85±12s, group c 40±10s). It can be seen that the hemostatic powder of the present invention can be used for liver hemostasis.
[0343] Hemostatic powders made of other different materials can also be used to stop liver bleeding.
[0344] Example 41: Hemostatic powder is used to stop bleeding in the spleen
[0345] A spleen incision bleeding model of SD rats was selected and divided into three groups for spleen hemostasis experiment, with 3 rats in each group: the hemostatic powder group of the present invention (group a, the hemostatic powder in Example 18, the component is selected from microgel HA-2.2 (4.21)); the control powder group of the present invention (group b, the control powder in comparative example 19, the component is selected from microgel HA-2); commercial chitosan hemostatic granules (group c). After the SD rats were anesthetized and fixed, an incision was made in the midline of the abdomen, the abdominal cavity was opened, and the spleen was exposed. An incision (8 mm wide and 2 mm deep) was made in the spleen to cause spleen injury, and bleeding continued for 20 seconds. Subsequently, different groups of hemostatic materials were sprinkled on the bleeding area and covered with gauze for continuous compression for 60 seconds. The amount of blood loss was measured by the weight gain of the gauze and the material, and the hemostasis time was recorded by a timer. The experimental results showed that the hemostatic time of group a was the shortest (80±12s in group a, 3 in group b failed to stop bleeding within 5 minutes, and 180±20s in group c), and the blood loss in group a was the least (0.9±0.2g in group a, 2.2±0.8g in group b within 5 minutes, and 1.3±0.5g in group c). It can be seen that the hemostatic powder in the present invention can be applied to spleen hemostasis.
[0346] Hemostatic powders made of other different materials can also be used to stop spleen bleeding.
[0347] Example 42: Application of hemostatic powder to stop bleeding in veins
[0348] The SD rat tail amputation model was selected and divided into three groups for tail vein hemostasis experiment, with 3 rats in each group: the hemostatic powder group of the present invention (group a, the hemostatic powder in Example 18, the component is selected from microgel CMC-1.1); the control powder group of the present invention (group b, the control powder in comparative Example 19, the component is selected from microgel CMC-1); commercial chitosan hemostatic particles (group c). After the SD rats were anesthetized, the weighed filter paper was placed under their tails, and the tails of the rats were cut off with scissors to cause bleeding. Subsequently, the hemostatic materials of different groups were sprinkled on the bleeding area and covered with gauze for continuous compression. The amount of blood loss was measured by the weight gain of the filter paper, and the hemostasis time was recorded by a timer. The experimental results showed that the amount of blood loss in group a was the least (group a 0.4±0.05g, group b 1.2±0.5g, group c 0.9±0.2g), and the hemostasis time in group a was the shortest (group a 40±5s, group b 90±15s, group c 75±10s). It can be seen that the hemostatic powder of the present invention can be applied to venous hemostasis.
[0349] Hemostatic powders made of other different materials can also be used to stop venous bleeding.
[0350] Example 43: Application of hemostatic powder to stop bleeding in body surface arteries
[0351] A New Zealand white rabbit ear artery bleeding model was selected and divided into three groups for a body surface artery hemostasis experiment, with 3 rabbits in each group: the hemostatic powder group of the present invention (group a, the hemostatic powder in Example 18, the component is selected from microgel CMC-1.2); the control powder group of the present invention (group b, the control powder in comparative Example 19, the component is selected from microgel CMC-1); and commercial chitosan hemostatic particles (group c). After the rabbit was anesthetized, a weighed filter paper was placed under its ear. The rabbit ear artery was pierced with a needle, and then different groups of hemostatic materials were applied to the bleeding site. The amount of blood loss was measured by the weight gain of the filter paper, and the hemostasis time was recorded by a timer. During the experiment, the hemostasis time of group a was the shortest (group a 23±8s, group b 65±15s, group c 35±10s) and the blood loss of group a was the least (group a 0.8±0.2g, group b 3.5±0.8g, group c 1.2±0.4g). It can be seen that the hemostatic powder in the present invention can be used for body surface artery hemostasis.
[0352] Hemostatic powders made of other different materials can also be used to stop bleeding in superficial arteries.
[0353] Example 44: Application of hemostatic powder to stop bleeding in body surface veins
[0354] A New Zealand white rabbit ear vein bleeding model was selected and divided into three groups for surface vein hemostasis experiments, with 3 rabbits in each group: the hemostatic powder group of the present invention (group a, the hemostatic powder in Example 18, the component is selected from microgel CMC-1.3); the control powder group of the present invention (group b, the control powder in comparative Example 19, the component is selected from microgel CMC-1); and commercial chitosan hemostatic particles (group c). After the rabbit was anesthetized, a weighed filter paper was placed under its ear. The rabbit ear vein was pierced with a needle, and then different groups of hemostatic materials were applied to the bleeding site, and the hemostasis time was recorded by a timer. The experimental results showed that the hemostasis time of group a was the shortest (group a 40±5s, group b 80±15s, group c 45±8s) and the blood loss of group a was the least (group a 1.0±0.2g, group b 3.4±2.0g, group c 1.2±0.4g). It can be seen that the hemostatic powder in the present invention can be used for surface vein hemostasis.
[0355] Hemostatic powders made of other different materials can also be used to stop bleeding in superficial veins.
[0356] Example 45: Application of hemostatic powder to intestinal bleeding
[0357] A SD rat cecal bleeding model was selected and divided into four groups for intestinal hemostasis experiments, with 3 rats in each group: the hemostatic powder group of the present invention (group a, the hemostatic powder in Example 18, the component is selected from microgel CMC-1.2); the control powder group of the present invention (group b, the control powder in comparative Example 19, the component is selected from microgel CMC-1); commercial chitosan hemostatic granules (group c); and a blank group (group d). After the SD rats were anesthetized, their abdominal cavities were opened and the cecum was rubbed until a bleeding surface was obtained. Subsequently, different groups of hemostatic materials were placed on the bleeding surface of the cecum. The amount of blood loss was measured by the increment of the hemostatic material, and the hemostasis time was recorded by a counter. After the experiment, the blood clots on the cecum and the hemostatic material were collected, and the hemoglobin analysis kit was used to measure the absorbance at 400nm to measure the hemostatic effect. In this example, the hemoglobin content of the blood clots collected from the hemostatic powder of the present invention (group a), the control powder (group b), the commercial chitosan hemostatic powder (group c) and the blank group (group d) was measured as follows: Fig. 9 The experimental results show that group a has the least blood loss (group a 0.2±0.1g, group b 0.4±0.12g, group c 0.35±0.1g, group d 0.8±0.2g), and the hemostasis time of group a is the shortest (group a 10±4s, group b 25±5s, group c 20±2s, group d 75±15s). It can be seen that the hemostatic powder of the present invention can be used for intestinal hemostasis.
[0358] Hemostatic powders made of other different materials can also be used to stop intestinal bleeding.
[0359] Example 46: Hemostatic powder is applied to the skin to stop bleeding
[0360] A Bama pig back skin tear and bleeding model was selected, and the back skin hemostasis experiment was carried out in three groups, with 4 wounds in each group: the hemostatic powder group of the present invention (group a, the hemostatic powder in Example 18, the component is selected from microgel Alg-1.2); the control powder group of the present invention (group b, the control powder in comparative Example 19, the component is selected from microgel Alg-1); commercial chitosan hemostatic granules (group c). Two-month-old male Bama miniature pigs (weight 1.6-1.8kg) were anesthetized, and after shaving the back hair, 4 linear incisions of 2 cm long and 1 cm deep were made on the pig's back with a scalpel to obtain skin bleeding wounds. Subsequently, the hemostatic material was immediately applied to the bleeding site, and all were covered with gauze to apply a certain pressure. The wound was observed approximately every 10 seconds, and the hemostasis time was recorded immediately after the bleeding stopped completely. The hemostatic material and gauze were weighed before and after use, and the difference was the total blood loss. The experimental results show that the hemostatic time of group a is the shortest (group a 40±10s, group b 70±14s, group c 55±12s), and the blood loss of group a is the least (group a 2.5±0.8g, group b 4.0±1.2g, group c 3.7±1.5g). Compared with other groups, the hemostatic powder of group a can form a gel layer with blood at the bleeding wound surface. It can be seen that the hemostatic powder in the present invention can be applied to skin hemostasis.
[0361] Hemostatic powders made of other different materials can also be used to stop bleeding on the skin.
[0362] Example 47: Application of hemostatic powder to oral mucosal bleeding
[0363] A SD rat hard palate mucosa injury model was selected and divided into three groups for oral mucosal hemostasis experiments, with 3 rats in each group: the hemostatic powder group of the present invention (group a, the hemostatic powder in Example 18, the component is selected from microgel Alg-1.1); the control powder group of the present invention (group b, the control powder in comparative Example 19, the component is selected from microgel Alg-1); commercial chitosan hemostatic particles (group c). After the SD rats were anesthetized, the mouths of the rats were opened with an eyelid device, and the palatal mucosa was disinfected with iodine and 75% ethanol. Then, a disposable biopsy punch (diameter 3mm) was used to create a circular full-thickness hard palate mucosa defect in the middle part of the rat's oral palate mucosa to obtain a bleeding wound. Subsequently, the hemostatic material was immediately applied to the bleeding site, and it was covered with gauze to apply a certain pressure. The wound was observed approximately every 10 seconds, and the hemostasis time was recorded immediately after the bleeding stopped completely. The hemostatic material and gauze were weighed before and after use, and the difference was the total blood loss. The experimental results show that the hemostatic time of group a is the shortest (group a 10±2s, group b 20±9s, group c 20±5s), and the blood loss of group a is the least (group a 0.1±0.02g, group b 0.4±0.03g, group c 0.3±0.02g). It can be seen that the hemostatic powder of the present invention can be used for oral mucosal hemostasis.
[0364] Hemostatic powders made of other different materials can also be used to stop bleeding in the oral mucosa.
[0365] Example 48: Application of hemostatic powder to stop bleeding during hysterectomy
[0366] A hysterectomy model of female SD rats aged 6 to 8 weeks was selected and divided into three groups for hemostasis experiment during hysterectomy, with 3 rats in each group: the hemostatic powder group of the present invention (group a, the hemostatic powder in Example 18, the component selected from microgel CMS-1.1); the control powder group of the present invention (group b, the control powder in comparative Example 19, the component selected from microgel CMS-1); Arista absorbable hemostatic microspheres (group c). After the SD rats were anesthetized and fixed, the hair on the lower abdomen was shaved and disinfected with iodine and 75% ethanol. The skin of the abdominal wall was cut longitudinally 2 to 3 cm above the pubic symphysis, and the tissue was cut layer by layer to open the abdominal cavity. The Y-shaped uterus of the rat was slowly picked out, and incisions were made in the left and right uterine horns respectively. The ophthalmic straight scissors were used to cut a 2.5 cm long incision longitudinally in the middle of the uterus to keep the uterine mesentery intact. The ophthalmic curved scissors were perpendicular to the longitudinal incision of the uterus, and the endometrium was cut off one by one, and the whole layer of the endometrium was completely removed. The depth was controlled not to break through the uterine serosal surface, that is, to ensure the integrity of the uterine serosal surface, and the uterine wall was cut off until it was thin and translucent. After the endometrial resection was completed, the hemostatic material was immediately applied to the bleeding site, and it was covered with gauze to apply a certain amount of pressure. The wound was observed about every 10 seconds, and the hemostasis time was recorded immediately after the bleeding stopped completely. The hemostatic material and gauze were weighed before and after use, and the difference was the total blood loss. The experimental results show that the hemostatic time of group a is the shortest (group a 30±6s, group b 60±12s, group c 50±8s), and the blood loss of group a is the least (group a 0.2±0.05g, group b 0.4±0.13g, group c 0.35±0.08g). It can be seen that the hemostatic powder of the present invention can be used for hemostasis during hysterectomy.
[0367] Other hemostatic powders made of different materials can also be used to stop bleeding during hysterectomy.
[0368] Example 49: Application of hemostatic powder to stop bleeding in the spine
[0369] The SD rat spinal injury model was selected and divided into three groups for spinal hemostasis experiments, with 3 rats in each group: the hemostatic powder group of the present invention (group a, the hemostatic powder in Example 18, the component is selected from microgel CMS-1.2); the control powder group of the present invention (group b, the control powder in Example 19, the component is selected from microgel CMS-1); Arista absorbable hemostatic microspheres (group c). The SD rats were anesthetized and fixed, the back hair was shaved, and the skin and fascia were cut in sequence with chest 13 and waist 1 as the center to expose the muscles in the surgical area. On one side, ophthalmic scissors were used to cut the muscles and tendons connected to the spinous process close to the spinous process to create an incision with a length of chest 12 to waist 2 and a depth to reach the articular process. Another parallel incision was cut about 0.5 cm outside the incision, and the length and depth were basically the same as the previous incision. The muscles between the two incisions were removed to expose 3 pairs of articular processes (chest 12 to chest 13, chest 13 to waist 1 and waist 1 to waist 2). Expose the lateral wall of the spinal canal and the intervertebral foramen at one time, cut off the two lateral walls of the spinal canal in parallel, expose the spinal cord, and create a bleeding wound. Subsequently, each group of hemostatic materials is immediately sprinkled on the bleeding site and the wound is continuously observed, and the hemostasis time is recorded immediately after the bleeding stops completely. The hemostatic materials are weighed before and after use, and the difference is the total blood loss. The experimental results show that the hemostasis time of group a is the shortest (group a 60 ± 8s, group b 120 ± 16s, group c 85 ± 15s), and the blood loss of group a is the least (group a 0.3 ± 0.1g, group b 1.0 ± 0.4g, group c 0.7 ± 0.25g). It can be seen that the hemostatic powder in the present invention can be applied to spinal hemostasis.
[0370] Hemostatic powders made of other different materials can also be used to stop spinal bleeding.
[0371] Embodiment 50 to Embodiment 55:
[0372] Hemostatic application of the mobile hemostatic agent of the present invention
[0373] Example 50: Application of mobile hemostatic agent in non-compression hemostasis of penetrating wounds
[0374] A New Zealand white rabbit liver perforation model was selected and divided into three groups for non-compressive penetrating wound hemostasis experiments, with 3 rabbits in each group: the flowing hemostat group of the present invention (group a, the flowing hemostat in Example 20, the component is selected from microgel HA-2.2 (4.21)); the control fluid group (group b, the control fluid in comparative Example 21, the component is selected from microgel HA-2); the commercial fluid gelatin group (group c). After the New Zealand white rabbits were anesthetized, their abdominal cavity was opened, the liver was lifted and placed on a pre-weighed gauze, and then a penetrating wound with a diameter of 6 mm was established on the liver to cause bleeding. Subsequently, different groups of hemostatic materials were injected into the penetrating wound. The amount of blood loss was measured by the weight gain of the hemostatic material and the gauze, and the hemostasis time was recorded by a timer. In this example, photographs of the flowing hemostat of the present invention (group a), the control fluid (group b) and the commercial fluid gelatin (group c) used for non-compressive hemostasis of penetrating wounds are shown in the figure. Fig.10 The experimental results show that group a has the least blood loss (group a 2.6±0.4g, group b 9.0±2.1g, group c 4.5±0.8g), and the hemostasis time of group a is the shortest (group a 25±2s, group b 135±21s, group c 85±14s). It can be seen that the flowable hemostatic agent of the present invention can be applied to non-compressive hemostasis of penetrating wounds.
[0375] Other mobile hemostatic agents composed of different materials can also be used for non-compression hemostasis of penetrating wounds.
[0376] Example 51: Application of mobile hemostatic agent in digestive tract hemostasis under endoscopy
[0377] The acute upper gastrointestinal arterial bleeding model of Bama pigs was selected and the gastrointestinal hemostasis experiment was carried out in three groups, with 2 pigs in each group: the mobile hemostat group of the present invention (group a, the mobile hemostat in Example 20, the component is selected from microgel CMC-1.2); the control fluid group (group b, the control fluid in comparative Example 21, the component is selected from microgel CMC-1); the commercial fluid gelatin group (group c). Adult female Bama pigs (weight 20-25kg) were anesthetized and cannulated in the right femoral artery to monitor blood pressure. Subsequently, within 5 minutes, the baseline blood pressure (systolic pressure) of all animals was monitored and adjusted to 90-100 mm Hg, and then heparin (10 mg / kg) was administered intravenously to achieve systemic heparinization. Under endoscopy, the mucosa was peeled off and the submucosal pulsating artery in the stomach was distinguished. The artery was then cut with an endoscopic knife to induce acute upper gastrointestinal bleeding, and natural bleeding was maintained for 4 minutes. The mobile hemostatic agent of the present invention (group a), control fluid (group b) or commercial fluid gelatin (group c) is applied to the bleeding site through the endoscopic biopsy channel via a catheter. The bleeding site is continuously observed using an endoscope within 30 minutes. Unless hemostasis is achieved, the hemostasis procedure is repeated, and the hemostasis time and the quality of the materials used are recorded. The experimental results show that compared with other groups, the hemostasis time of group a is the shortest (group a 3±1.0min, group c 13±4.0min, group b 12±3.5min), and the material used in group a is the least (group a 8±2.5g, group b 15±4.5g, group c 16±5g). It can be seen that the mobile hemostatic agent in the present invention can be applied to endoscopic hemostasis of the digestive tract.
[0378] Other mobile hemostatic agents composed of different materials can also be used for gastrointestinal hemostasis under endoscopy.
[0379] Example 52: Application of mobile hemostatic agent in hemostasis during and after laparoscopic partial nephrectomy
[0380] A Bama pig partial nephrectomy model was selected and divided into three groups for hemostasis experiments during and after partial nephrectomy, with 2 pigs in each group: the mobile hemostat group of the present invention (group a, the mobile hemostat in Example 20, the component of which is selected from microgel HA-); the control fluid group (group b, the control fluid in comparative Example 21, the component of which is selected from microgel HA-2); and the commercial fluid gelatin group (group c). Adult female Bama pigs (weight 20-25kg) were anesthetized and cannulated in the right femoral artery to monitor blood pressure. A pneumoperitoneum needle was inserted into the pararectal incision, and one-third partial nephrectomy was performed under laparoscopy. The mobile hemostat of the present invention (group a), the fluid control group (group b) or the commercial fluid gelatin (group c) was applied to the bleeding site through the endoscopic biopsy channel via a catheter. The bleeding site was continuously observed using an endoscope within 30 minutes. Unless hemostasis was achieved, the hemostasis procedure was repeated, and the hemostasis time and material quality were recorded. The experimental results showed that the hemostasis time of group a was the shortest (group a 15±3.5min, group b and group c failed to stop bleeding within 60 minutes), and group a used the least amount of material (group a 12±3g, group b and group c used more than 30g of material within 60 minutes). It can be seen that the mobile hemostatic agent of the present invention can be used for hemostasis during and after laparoscopic partial nephrectomy.
[0381] Other mobile hemostatic agents composed of different materials can also be used for hemostasis during and after laparoscopic partial nephrectomy.
[0382] Example 53: Application of mobile hemostatic agent in hemostasis of narrow cavities
[0383] A New Zealand white rabbit cochlear bleeding model was selected and divided into three groups for a narrow cavity hemostasis experiment, with 3 rabbits in each group: a mobile hemostat group of the present invention (group a, the mobile hemostat in Example 20, the component is selected from microgel Alg-1.3); a control fluid group (group b, the control fluid in comparative Example 21, the component is selected from microgel Alg-1); a commercial fluid gelatin group (group c). After the rabbits were anesthetized, they were scratched with a surgical blade at the cochlea to create a bleeding wound. Subsequently, different groups of hemostatic materials were injected into the cochlea through a syringe. The hemostasis time was recorded by a timer. The experimental results showed that the hemostasis time of group a was the shortest (group a 20±5s, group b 85±14s, group c 45±9s). It can be seen that the mobile hemostat in the present invention can be used for hemostasis in narrow cavities.
[0384] Other mobile hemostatic agents composed of different materials can also be used to stop bleeding in narrow cavities.
[0385] Example 54: Application of mobile hemostatic agent to hemostasis of spine
[0386] The SD rat spinal injury model was selected and divided into three groups for spinal hemostasis experiment, with 3 rats in each group: the mobile hemostatic agent group of the present invention (group a, the mobile hemostatic agent in Example 20, the component selected from microgel HA-2.1); the control fluid group (group b, the control fluid in comparative Example 21, the component selected from microgel HA-2); the commercial fluid gelatin group (group c). The SD rats were anesthetized and fixed, the back hair was shaved, and the skin and fascia were cut in sequence with thoracic 13 and lumbar 1 as the center to expose the muscles in the surgical area. On one side, ophthalmic scissors were used to cut the muscles and tendons connected to the spinous process close to it, and an incision was created, the length of which was preferably thoracic 12 to lumbar 2, and the depth was to reach the articular process. Another parallel incision was cut about 0.5 cm outside the incision, and the length and depth were basically the same as the previous incision. The muscles between the two incisions were removed to expose 3 pairs of articular processes (thoracic 12 to thoracic 13, thoracic 13 to lumbar 1 and lumbar 1 to lumbar 2). The lateral wall of the spinal canal and the intervertebral foramen are exposed at one time, and the two lateral walls of the spinal canal are cut in parallel to expose the spinal cord and create a bleeding wound. Subsequently, different groups of hemostatic materials are injected into the bleeding wound through a syringe. The wound is observed approximately every 10 seconds, and the hemostatic time is recorded immediately after the bleeding stops completely; if the bleeding does not stop, the hemostatic material is continued to be injected. The bleeding from the wound is collected with gauze and weighed to record the blood loss. The experimental results show that the hemostatic time of group a is the shortest (group a 30±6s, group b 105±21s, group c 60±12s), and the blood loss of group a is the least (group a 0.8±0.2g, group b 1.2±0.3g, group c 1.0±0.3g). It can be seen that the mobile hemostatic agent in the present invention can be applied to spinal hemostasis.
[0387] Other mobile hemostats composed of different materials can also be used for spinal hemostasis.
[0388] Example 55: Application of mobile hemostatic agent in percutaneous puncture hemostasis
[0389] A percutaneous puncture defect model of the spleen of a Bama pig was selected, and the percutaneous puncture hemostasis experiment was carried out in three groups, with 3 puncture defects in each group: the mobile hemostat group of the present invention (group a, the mobile hemostat in Example 20, the component is selected from microgel CMS-1.2); the control fluid group (group b, the control fluid in comparative Example 21, the component is selected from microgel CMS-1); the commercial fluid gelatin group (group c). Adult female Bama pigs (weight 20-25kg) were anesthetized, incised along the midline of the abdomen, the abdominal cavity was opened, the spleen was gradually exposed, and gauze soaked in physiological saline was used to keep the spleen moist continuously. Starting from the distal end of the spleen, a surgical biopsy punch with a diameter of 6mm was used to make a bleeding defect of similar size and cannulated the right femoral artery to monitor blood pressure. The mobile hemostat of the present invention (group a), the control fluid group (group b) or the commercial fluid gelatin (group c) was applied to the bleeding site by syringe. The hemostasis was continuously observed, and the hemostasis procedure was repeated unless hemostasis was achieved, and the hemostasis time was recorded. In this example, the mobile hemostatic agent (group a), the control fluid (group b) and the commercial fluid gelatin (group c) are used for percutaneous hemostasis. Fig.11 The experimental results show that group a quickly blocked the bleeding site, while blood in groups b and c continued to seep out from the gap between the material and the tissue; compared with other groups, group a had the shortest hemostasis time (group a 55±10s, group b 155±25s, group c 90±12s). It can be seen that the mobile hemostatic agent in the present invention can be used for percutaneous puncture hemostasis.
[0390] Other mobile hemostats composed of different materials can also be used for percutaneous puncture hemostasis.
[0391] Embodiment 56 to Embodiment 59:
[0392] Preparation and application of composite sponge of the present invention
[0393] Example 56: Preparation of composite sponge
[0394] Taking the hyaluronic acid microgel modified with o-phthalaldehyde groups prepared in Example 9 (i.e., HA-2.2 (4.21)) and the hyaluronic acid microgel without o-phthalaldehyde group modification prepared in Example 2 (i.e., HA-2) as examples, the two microgels were fully dispersed in deionized water to obtain a suspension with a solid content of 0.5% to 1.5% (w / v), and the suspensions were spread in molds in turn (constituting the a surface modified with o-phthalaldehyde groups and the b surface unmodified, respectively), frozen at -20°C for 6 hours, and then freeze-dried at -60°C for 48 hours to obtain a composite sponge.
[0395] Example 57: Application of composite sponge in postoperative adhesion prevention
[0396] An intra-abdominal adhesion model of SD rats with scraped liver surface was selected, and the postoperative intra-abdominal anti-adhesion experiment was carried out in two groups, with 3 rats in each group: the composite sponge in Example 56 (group a) and a blank control group (group b). After the SD rats were anesthetized, their abdominal cavities were opened, and the liver surface was rubbed until a bleeding wound was obtained. The a side of the sponge in group a was placed close to the liver surface and pressed evenly for 1 minute to adhere it to the liver surface, and the b side was moistened with saline; group b did not receive any treatment. 14 days after the operation, the abdominal cavity of the SD rats was opened again, and the adhesion conditions in the abdominal cavity were recorded. The experimental results showed that 2 of the 3 rats in group a had no adhesion in the abdominal cavity, and 1 had slight adhesion, which could be easily peeled off with tweezers; all 3 rats in group b had obvious adhesion. Subsequently, tissue sections and H&E staining were performed for histological analysis. In this example, the H&E staining results of the composite sponge (group a) and the blank group (group b) are shown as follows: Fig.12 As shown, I represents the small intestine, L represents the liver, and S represents the composite sponge material. The staining results show that the liver tissue in group a has a composite sponge material protective layer and has no obvious adhesion to other organs or the abdominal wall, while the liver tissue in group b has obvious adhesion to the small intestine tissue. It can be seen that the composite sponge in the present invention can be used to prevent adhesion after surgery.
[0397] Composite sponges made of other different materials can also be used to prevent adhesion after surgery.
[0398] Example 58: Application of composite sponge in blocking air leakage in lung parenchyma
[0399] The New Zealand white rabbit lung parenchyma air leakage model was used to conduct a lung parenchyma air leakage blocking experiment in two groups, each with 3 rabbits: the composite sponge in Example 56 (group a) and a blank control group (group b). The New Zealand white rabbits were injected with 1% sodium pentobarbital at a dose of 3 mL / kg, and the trachea was intubated under general anesthesia and assisted with ventilation with a ventilator (VT 80 mL, R 30 bpm). Subsequently, the thoracotomy was performed, and the marginal tissue of the lung lobe was removed. The wound surface was about 1 cm 2 , at least one bronchial stump with a diameter of about 1 mm can be seen. The experimental group evenly pressed the a surface of the composite sponge in Example 48 to the defective part of the lung, adhered it to the wound surface, closed the chest layer by layer, eliminated the residual air, and fully re-expanded the lung. The wound surface of the control group was not treated and the chest was closed directly. 14 days after surgery, the surgical side was observed for atelectasis and pleural effusion. The experimental results showed that the rabbits in group b died of respiratory failure due to continuous air leakage within 4 hours after surgery, and the rabbits in group a survived well. After 14 days, the chest was opened to observe the lung wound surface. The wound healing was good, no obvious air leakage was observed, and there was no atelectasis, peritoneal effusion, etc. It can be seen that the composite sponge in the present invention can be used for lung parenchymal air leakage blocking.
[0400] Composite sponges composed of other different materials can also be used to seal lung parenchymal air leaks.
[0401] Example 59: Application of composite sponge in blocking intestinal leakage
[0402] The New Zealand rabbit intestinal leakage model was used to conduct a cecal leakage plugging experiment in two groups, with 3 rabbits in each group: the composite sponge in Example 56 (group a) and a blank control group (group b). After the New Zealand rabbits were anesthetized, their abdominal cavities were opened and a leakage model was made at their cecum. Group a placed the a side of the composite sponge close to the wound at the leakage site, pressed evenly for 1 minute, adhered it to the abdominal wall, and moistened the b side with physiological saline; Group b did not do any treatment after making the wound. One rabbit in group b died 2 days after surgery, and the other two rabbits died 3 days after surgery. The cecum was dissected and observed, and both had obvious leakage and severe inflammation. All rabbits in group a survived for 4 weeks after surgery. After the New Zealand rabbits were euthanized in the fourth week, the cecum was extracted for observation, and there was no leakage or local inflammation. It can be seen that the composite sponge in the present invention can be used for intestinal leakage exudate plugging.
[0403] Composite sponges composed of other different materials can also be used to block intestinal leakage.
[0404] The above examples 27 to 39 give the application of the hemostatic sponge of the present invention with specific formulas in various hemostatic scenarios. These hemostatic applications mainly utilize the characteristics of the hemostatic sponge of the present invention that can react efficiently with blood and the tissue adhesion characteristics. According to the records of examples 22, 24 and 25, it can be known that the hemostatic performance of the hemostatic sponge provided by the embodiment of the present invention is positively correlated with the modified o-phthalaldehyde group, and the hemostatic sponges of multiple formulas in the embodiments of the present invention have good tissue adhesion and good mechanical properties after absorbing blood. Therefore, the hemostatic sponges prepared based on the microgels modified with various o-phthalaldehyde groups provided by the present invention can be used in various hemostatic scenarios. The above examples 40 to 49 and examples 50 to 55 respectively give the application of hemostatic powders and mobile hemostats with specific formulas in various hemostatic scenarios. Similarly, the hemostatic powders or mobile hemostats prepared based on the microgels modified with various o-phthalaldehyde groups provided by the present invention can be used in various hemostatic scenarios.
[0405] The above Examples 56 to 59 provide the preparation of composite sponges with specific formulas and corresponding biomedical applications. According to the contents of the present application, those skilled in the art can prepare composite sponges from the o-phthalaldehyde group-modified or unmodified microgels provided by the present invention as needed. Similarly, those skilled in the art can prepare composite sponges from the o-phthalaldehyde group-modified or unmodified microgels provided by the present invention as needed for applications in postoperative anti-adhesion, tissue air leakage blocking, tissue fluid leakage blocking, etc. according to the contents of the present application.
[0406] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. Microgels modified with o-phthalaldehyde groups, It is characterized in that The chemical structure of the o-phthalaldehyde group-modified microgel is shown in Formula 1: In Formula 1, MG represents microgel, which is a gel microparticle formed by cross-linking water-soluble or hydrophilic polymers, with a particle size of 5 mesh to 1000 mesh and a solid content of 0.01% to 50%; In formula 1, n≥2, that is, the average number of o-phthalaldehyde functional groups on a single microgel is greater than or equal to 2; In Formula 1, the o-phthalaldehyde group is connected to the microgel via a covalent bond.
2. The o-phthalaldehyde group-modified microgel according to claim 1, It is characterized in that The water-soluble or hydrophilic polymer forming the microgel is selected from water-soluble or hydrophilic natural polymers or water-soluble or hydrophilic synthetic polymers; The water-soluble or hydrophilic natural polymer is selected from one or more of hyaluronic acid, alginic acid, dextran, chondroitin sulfate, heparin, polyglutamic acid, tragacanth gum, xanthan gum, agarose, gellan gum, guar gum, gum arabic, locust bean gum, starch, starch hydrolysate, starch derivative, cellulose or cellulose derivative; The water-soluble or hydrophilic synthetic polymer refers to an artificial synthetic polymer containing a hydrophilic group, selected from homopolymers or copolymers of (meth)acrylic acid and its esters, homopolymers or copolymers of (meth)acrylamides, homopolymers or copolymers of polyvinyl alcohol, homopolymers or copolymers of polyethylene glycol, and homopolymers or copolymers of vinyl pyrrolidone; Preferably, the homopolymer or copolymer of (meth)acrylic acid and its esters is selected from the group consisting of homopolymer or copolymer of (meth)acrylic acid, homopolymer or copolymer of hydroxyethyl (meth)acrylate, homopolymer or copolymer of hydroxypropyl (meth)acrylate, homopolymer or copolymer of glucose (meth)acrylate, homopolymer or copolymer of polyethylene glycol (meth)acrylate and copolymer of polyethylene glycol methyl ether (meth)acrylate; Preferably, the homopolymer or copolymer of (meth)acrylamide is selected from copolymers of (meth)acrylamide, copolymers of N,N-dimethylacrylamide, homopolymers or copolymers of N-hydroxymethylacrylamide, homopolymers or copolymers of N-hydroxyethyl(meth)acrylamide, homopolymers or copolymers of N-hydroxypropyl(meth)acrylamide, copolymers of N-isopropylacrylamide or copolymers of 2-acrylamido-2-methylpropanesulfonic acid; Herein, (meth)acrylic acid refers to acrylic acid or methacrylic acid; and (meth)acrylamide refers to acrylamide or methacrylamide.
3. The o-phthalaldehyde group-modified microgel according to claim 2, It is characterized in that The water-soluble or hydrophilic polymer forming the microgel is selected from one or more of hyaluronic acid, alginic acid, starch, carboxymethyl starch, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyglutamic acid, polyacrylic acid or carboxylated polyethylene glycol.
4. The o-phthalaldehyde group-modified microgel according to claim 1, It is characterized in that The chemical structure of the microgel modified with o-phthalaldehyde groups is selected from one of the following structures: In Formula 1-1 to Formula 1-12, MG represents microgel, Among them, 1≤r≤20, 1≤s≤20, 1≤t≤50, n≥2, preferably, 1≤r≤6, 1≤s≤10, 1≤t≤30, n≥2.
5. A method for preparing a microgel modified with o-phthalaldehyde groups according to any one of claims 1 to 4, It is characterized in that The steps include: (1) preparing microgels; (2) covalently linking the aldehyde-preprotected o-phthalaldehyde precursor derivative to the active groups on the microgel to prepare the o-phthalaldehyde precursor derivative-modified microgel; (3) Deprotecting the aldehyde groups to obtain microgels modified with o-phthalaldehyde groups.
6. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 5, It is characterized in that The method for preparing the microgel in step (1) comprises: 1) preparing the microgel by directly cross-linking a water-soluble or hydrophilic polymer; or, 2) preparing the microgel by polymerizing and cross-linking a monomer.
7. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 6, It is characterized in that The preparation of microgels by direct cross-linking of water-soluble or hydrophilic polymers refers to: The water-soluble or hydrophilic polymer is cross-linked into a gel by a specific cross-linking method, and then physically broken by mechanical force and sieved through sieves of different sizes to obtain microgels with different particle size distributions; or, Water-soluble or hydrophilic polymers are prepared into an oil-water emulsion under the action of an emulsifier, and then cross-linked by a specific cross-linking method to obtain microgels with a certain particle size.
8. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 7, It is characterized in that The specific cross-linking method is chemical cross-linking; The chemical crosslinking is selected from the following three methods: Based on multifunctional acrylic or methacrylic acid modified polymers cross-linked by free radical chain polymerization; or, Covalent crosslinking based on multifunctional crosslinking agents with a functionality ≥ 2 in the presence or absence of a catalyst; or In the presence or absence of a catalyst, the polymer chain itself contains two or more reactive functional groups that undergo condensation crosslinking.
9. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 8, It is characterized in that The multifunctional crosslinking agent is selected from glutaraldehyde, polyamine, multifunctional epoxy, epichlorohydrin, divinyl sulfone, phosphorus oxychloride or sodium trimetaphosphate.
10. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 9, It is characterized in that The multifunctional epoxy is selected from 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, ethylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, polyethylene glycol diglycidyl ether or polypropylene glycol diglycidyl ether; The polyamine refers to a multifunctional crosslinking agent containing one or more functional groups of primary amine, hydrazine, hydrazide, and hydroxylamine, preferably adipic acid dihydrazide or hexamethylenediamine.
11. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 7, It is characterized in that The specific cross-linking method is radiation cross-linking; The radiation crosslinking is selected from electron beam radiation crosslinking or gamma ray radiation crosslinking; Wherein, when the radiation crosslinking is selected from electron beam radiation crosslinking, the radiation dose rate is selected from 10 to 1000 Gy / s, and the radiation time is selected from 5 to 100 minutes; When the radiation cross-linking is selected from gamma-ray radiation cross-linking, the radiation dose is selected from 10 to 100 kGy.
12. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 6, It is characterized in that The preparation of microgels by polymerization and cross-linking of monomers refers to: The monomers are copolymerized and cross-linked with multifunctional double-bond cross-linking agents or the monomers are polymerized and cross-linked into gels by a specific cross-linking method, and then physically broken by mechanical force and sieved through sieves of different sizes to obtain microgels with different particle size distributions; or, Monomers and multifunctional double-bond crosslinking agents are polymerized by emulsion polymerization or precipitation polymerization to obtain microgels with a certain particle size; or, The monomers are first emulsion polymerized or precipitated and then cross-linked by a specific cross-linking method to obtain microgels with a certain particle size; The monomer may be selected from one or more water-soluble monomers, or may be selected from one or more water-soluble monomers and other copolymerizable monomers.
13. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 12, It is characterized in that The water-soluble monomer is selected from (meth)acrylic acid, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, glucose (meth)acrylate, polyethylene glycol methyl ether (meth)acrylate and polyethylene glycol (meth)acrylate, (meth)acrylamide, N,N-dimethylacrylamide, N-hydroxymethylacrylamide, N-hydroxyethyl (meth)acrylamide, N-hydroxypropyl (meth)acrylamide, N-isopropylacrylamide and 2-acrylamido-2-methylpropanesulfonic acid (AMPS), vinyl pyrrolidone; The other copolymerizable monomers may be selected from (meth)acrylate monomers, (meth)acrylamide monomers, styrene monomers, vinyl acetate and acrylonitrile; Herein, (meth)acrylic acid refers to acrylic acid or methacrylic acid; and (meth)acrylamide refers to acrylamide or methacrylamide.
14. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 12, It is characterized in that The multifunctional double bond crosslinking agent refers to a crosslinking agent containing two or more polymerizable double bond functional groups, preferably glucose acrylate, 2,9-decadiene, 2-hexadecenoic acid, N,N'-methylenebisacrylamide or glycerol acrylate.
15. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 12, It is characterized in that The specific cross-linking method is selected from the following two methods: Condensation crosslinking of polymer chains containing two or more reactive functional groups in the presence or absence of a catalyst; Irradiation cross-linking.
16. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 5, It is characterized in that The aldehyde-preprotected o-phthalaldehyde precursor derivative described in step (2) comprises an aldehyde-preprotected o-phthalaldehyde group and a substituent R that can be connected to an active group on the microgel, and the structure is shown in Formula 2: In Formula 2, R is selected from a carboxyl substituent, a vinyl sulfone substituent, an epoxy substituent, a haloalkane substituent, an isocyanate substituent or an amine substituent; In Formula 2, R is directly connected to the benzene ring, or connected to the benzene ring through a single or multiple alkylene chains or alkoxy chains, and the multiple alkylene chains or alkoxy chains are connected through ether bonds, amide bonds, ester bonds, carbamate bonds or urea bonds.
17. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 16, It is characterized in that The aldehyde group pre-protected o-phthalaldehyde precursor derivative is selected from one or more of the following structures: Among them, 1≤r≤20, 1≤s≤20, 1≤t≤50; preferably, 1≤r≤6, 1≤s≤10, 1≤t≤30.
18. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 16, It is characterized in that The active groups on the microgel are selected from hydroxyl groups or carboxyl groups; The covalent bond connection between the aldehyde group pre-protected o-phthalaldehyde precursor derivative and the active group on the microgel is selected from ether bond, amide bond, ester bond, carbamate bond or urea bond, preferably ether bond, amide bond and carbamate bond.
19. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 18, It is characterized in that When the active groups on the microgel are selected from hydroxyl groups, the covalent bond connection is based on an ether bond connection between vinyl sulfone substituents, epoxy substituents and halogenated alkane substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel, based on an ester bond connection between carboxyl substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel, and based on a carbamate bond connection between isocyanate substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel; When the active groups on the microgel are selected from carboxyl groups, the covalent bond connection is based on an amide bond connection between the amino substituents on the o-phthalaldehyde precursor derivative and the carboxyl groups on the microgel.
20. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 5, It is characterized in that The deprotection described in step (3) refers to deprotecting the pre-protected o-phthalaldehyde functional group of the aldehyde group connected to the microgel under acidic conditions to obtain a microgel modified with o-phthalaldehyde groups.
21. Highly efficient hemostatic materials, It is characterized in that Select one of the following materials: A highly efficient hemostatic sponge having a porous structure obtained by drying the microgel modified with the o-phthalaldehyde group according to any one of claims 1 to 4; The highly effective hemostatic powder is obtained by removing water and drying the microgel modified with the o-phthalaldehyde group according to any one of claims 1 to 4; The invention is a highly efficient flowable hemostatic agent directly obtained by uniformly dispersing the microgel modified with the o-phthalaldehyde group described in any one of claims 1 to 4 in a solvent.
22. The highly effective hemostatic material according to claim 21, It is characterized in that When the high-efficiency hemostatic material is a high-efficiency hemostatic sponge, the drying method is vacuum freeze drying; When the high-efficiency hemostatic material is a high-efficiency hemostatic powder, the dehydration is to replace the water in the microgel modified by the o-phthalaldehyde group with an organic solvent, so that the water content of the microgel is reduced and precipitated in the form of solid particles; the drying is direct drying or vacuum freeze drying followed by drying; the particle size distribution of the high-efficiency hemostatic powder is 20 mesh to 300 mesh; When the highly efficient hemostatic material is a highly efficient mobile hemostatic agent, the solvent is selected from water, physiological saline, buffer solution, decellularized matrix or cell culture medium solution containing or not containing polyols, and the polyol is preferably one or more of propylene glycol, butanediol, 1,2-pentanediol, 1,2-hexanediol or glycerol; The solid content of the high-efficiency flowable hemostat is 1% to 20% (w / v); preferably, the solid content of the high-efficiency flowable hemostat is selected from 5% to 12% (w / v).
23. Composite sponge, It is characterized in that The composite sponge is a composite sponge having a porous structure obtained by layering the microgel modified with the o-phthalaldehyde group and the microgel not modified with the o-phthalaldehyde group according to any one of claims 1 to 4 in a mold, and then drying. The microgel without o-phthalaldehyde group modification refers to a microgel prepared from a water-soluble or hydrophilic polymer or a microgel prepared by polymerization and cross-linking of monomers.
24. The composite sponge according to claim 23, It is characterized in that The microgel modified with o-phthalaldehyde groups and the microgel not modified with o-phthalaldehyde groups have the same or different polymer skeleton, water content, particle size and pH value.
25. The composite sponge according to claim 23, It is characterized in that The composite sponge has a double-layer structure, one side of which is composed of microgels modified with o-phthalaldehyde groups, and the other side of which is composed of microgels not modified with o-phthalaldehyde groups.
26. Use of the high-efficiency hemostatic material according to claim 21 or 22, It is characterized in that When the efficient hemostatic material is an efficient hemostatic sponge, the application of the efficient hemostatic sponge is selected from one of the following applications: Application of the highly efficient hemostatic sponge in the preparation of non-compressive hemostatic products for penetrating wounds; Application of the highly efficient hemostatic sponge in the preparation of liver hemostatic products; Application of the highly efficient hemostatic sponge in the preparation of spleen hemostatic products; Application of the high-efficiency hemostatic sponge in the preparation of surface arterial hemostatic products; Application of the highly efficient hemostatic sponge in the preparation of surface venous hemostasis products; Application of the high-efficiency hemostatic sponge in the preparation of femoral artery hemostatic products; Application of the high-efficiency hemostatic sponge in preparing abdominal aorta hemostasis products; Application of the high-efficiency hemostatic sponge in the preparation of carotid artery hemostasis products; Application of the highly efficient hemostatic sponge in the preparation of cardiac hemostatic products; Application of the highly efficient hemostatic sponge in the preparation of coronary artery hemostasis products; Application of the highly effective hemostatic sponge in the preparation of hemostatic products for tooth extraction wounds; Application of the highly efficient hemostatic sponge in the preparation of spinal hemostatic products; Application of the highly efficient hemostatic sponge in the preparation of uterine wall hemostatic products; When the efficient hemostatic material is efficient hemostatic powder, the application of the efficient hemostatic powder is selected from one of the following applications: Application of the highly effective hemostatic powder in the preparation of liver hemostatic products; Application of the highly effective hemostatic powder in the preparation of spleen hemostatic products; Application of the highly effective hemostatic powder in the preparation of venous hemostatic products; Application of the highly effective hemostatic powder in the preparation of surface arterial hemostatic products; Application of the highly effective hemostatic powder in the preparation of surface vein hemostatic products; Application of the highly effective hemostatic powder in the preparation of intestinal hemostatic products; Application of the highly effective hemostatic powder in the preparation of skin hemostatic products; Application of the highly effective hemostatic powder in the preparation of oral mucosal hemostatic products; Application of the highly effective hemostatic powder in the preparation of hemostatic products for hysterectomy; Application of the highly effective hemostatic powder in the preparation of spinal hemostatic products; When the highly efficient hemostatic material is a highly efficient flowing hemostatic agent, the application of the highly efficient flowing hemostatic agent is selected from one of the following applications: Application of the highly efficient mobile hemostatic agent in the preparation of non-compressive hemostatic products for penetrating wounds; The high-efficiency mobile hemostatic agent is used in the preparation of digestive tract hemostatic products; Application of the highly efficient mobile hemostatic agent in the preparation of hemostatic products during and after partial nephrectomy; Application of the highly efficient mobile hemostatic agent in the preparation of hemostatic products for narrow cavities of organisms; Application of the highly efficient mobile hemostatic agent in the preparation of spinal hemostatic products; The high-efficiency mobile hemostatic agent is used in the preparation of hemostatic products for percutaneous puncture.
27. Use of the composite sponge according to any one of claims 23 to 25, It is characterized in that Select one of the following applications: Application of the composite sponge in preparing postoperative anti-adhesion products; Application of the composite sponge in the preparation of tissue leakage blocking products; Application of the composite sponge in the preparation of tissue fluid leakage blocking products; Wherein, the postoperative adhesion prevention includes abdominal wall adhesion prevention, pericardial adhesion prevention, tendon adhesion prevention and intrauterine adhesion prevention; The tissue air leakage blocking includes lung parenchyma air leakage blocking; The tissue fluid leakage blocking includes intestinal leakage blocking, pancreatic leakage blocking, cerebrospinal fluid leakage blocking, and gastric leakage blocking.
Citation Information
Cited By
Composite quick-acting styptic powder as well as preparation method and application thereof