Positive plate and lithium ion battery
By adopting a double-layer structure of the cathode active layer in lithium-ion batteries and utilizing specific lithium metal oxide composition and structural design, the problem of degradation of discharge capacity and cycle performance of lithium-ion batteries at high rates is solved, and low internal resistance is achieved. and high energy density effects.
Patent Information
- Application Number
- CN202410839946.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-25
AI Technical Summary
The discharge capacity and cycle performance of lithium-ion batteries deteriorate at high rates, and the increase in positive active materials will lead to polarization phenomena and affect the overall performance of the battery.
It adopts a double-layer structure of the cathode active layer, including the first cathode active layer and the second cathode active layer. It uses a specific lithium metal oxide composition and structural design to reduce internal resistance and improve the deintercalation efficiency of lithium ions to prevent polarization phenomena. occurrence.
It achieves excellent discharge capacity and cycle performance of lithium-ion batteries at high rates, extends battery life, reduces internal resistance, and improves battery energy density.
Smart Images

Figure CN118841513A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an electrode sheet, in particular to a positive electrode sheet and a lithium ion battery, belonging to the technical field of secondary batteries. Background Art
[0002] High-voltage digital batteries are currently developing rapidly and are widely used in 3C consumer digital fields such as mobile phones, laptops, tablets, and Bluetooth small batteries. The requirements for lithium-ion battery capacity are getting higher and higher. At present, the methods to increase battery capacity mainly include increasing its charging voltage and increasing the amount of positive electrode active materials used.
[0003] However, as the charging voltage increases, the crystal structure of the positive electrode active material will collapse, which will lead to a series of problems such as rapid capacity decay and significant reduction in cycle performance. Especially when the battery is discharged at a high rate (not less than 0.7C), the degradation of the discharge capacity and cycle performance of the battery is more prominent. The increase in the amount of positive electrode active material used will increase the polarization of the battery.
[0004] Therefore, how to improve battery capacity while maintaining the normal electrical performance of lithium-ion batteries is a challenge faced in the research process of consumer lithium-ion batteries. Summary of the invention
[0005] The present invention provides a positive electrode sheet, which can not only enable a lithium-ion battery to have excellent discharge capacity at a high rate, but also has a lower internal resistance, inhibiting the occurrence of polarization, thereby facilitating fast charging of the battery and extending the cycle life of the battery.
[0006] The present invention also provides a battery, which includes the above-mentioned positive electrode sheet and has excellent performance in discharge capacity, cycle performance and rate performance.
[0007] The present invention provides a positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector and a positive electrode active layer arranged on at least a portion of the surface of the positive electrode current collector, the positive electrode active layer comprising a first positive electrode active layer and a second positive electrode active layer stacked in a direction away from the positive electrode current collector;
[0008] The first positive electrode active material in the first positive electrode active layer includes a first lithium metal oxide shown in Formula 1 and / or a second lithium metal oxide shown in Formula 2;
[0009] The second positive electrode active material in the second positive electrode active layer includes a third lithium metal oxide represented by Formula 3;
[0010] Wherein, the first lithium metal oxide is a cubic crystal of Cmca space group;
[0011] The second lithium metal oxide is a cubic crystal with a P63mc space group;
[0012] The third lithium metal oxide C is a cubic crystal of R3-m space group;
[0013] Li n-y Na y Co c-a-b M1 b M2 a O2 Formula 1
[0014] In formula 1, 0.6≤n≤0.98, 0<y≤0.05, 0≤a≤0.1, 0<b≤0.1, 0.9<c<1.1, 0.95<a+b+c<1.15; M1 includes at least one of Al, Mg, Ti, Zr, La, and Y; M2 is a doping element different from M1, and M2 includes at least one of B, Te, W, and K;
[0015] Li m-x Na x Co d-y1 D y1 O2 Formula 2
[0016] In formula 2, 0.9≤m≤1.05, 0<x≤0.05, 0≤y1≤0.2, 0.95<d<1.1, 0.99<d+y1<1.12, D includes at least one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, Te, B, and K;
[0017] Li e Co f E g O2 Formula 3
[0018] In formula 3, 0.9≤e≤1.1, 0.95<f≤1.05, 0≤g≤0.15, 0.95≤f+g≤1.2, and E includes at least one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, Te, B, and K.
[0019] The positive electrode sheet as described above, wherein the X-ray diffraction spectrum of the positive electrode active layer includes a first diffraction peak and a second diffraction peak with 2θ of 17.6° to 19.5°, and the difference in 2θ between the first diffraction angle and the second diffraction angle is 0.3° to 1.0°;
[0020] Preferably, the intensity ratio of the second diffraction peak to the first diffraction peak is (1-5):1, and the 2θ of the second diffraction peak is greater than the 2θ of the first diffraction peak.
[0021] The positive electrode sheet as described above, wherein the half-cell composed of the positive electrode sheet and the lithium metal negative electrode is charged to 4.55V at a current rate of ≤0.1C, then charged at a constant voltage to 0.025C and then discharged to 3.0V at a current rate of ≤0.1C, the number N of discharge peaks in the capacity-voltage differential curve of the half-cell within the range of 3.0 to 4.0V is not less than 2.
[0022] The positive electrode sheet as described above, wherein the second positive electrode active material comprises spherical or quasi-spherical particles;
[0023] The Dv50 of the first positive electrode active material is 3-10 μm; the Dv50 of the second positive electrode active material is 14-20 μm;
[0024] The Dv50 of the first positive electrode active material is less than the Dv50 of the second positive electrode material.
[0025] The positive electrode sheet as described above, wherein the first positive electrode active material includes a first crack whose extension direction has an angle of less than 15° with the first direction, and the second positive electrode active material in the second positive electrode active layer includes a second crack whose extension direction has an angle of less than 15° with the first direction;
[0026] Preferably, the number of the first cracks is greater than the number of the second cracks.
[0027] The positive electrode sheet as described above, wherein the content of sodium element in the positive electrode active layer is 20-1000 ppm.
[0028] The positive electrode sheet as described above, wherein the positive electrode active layer contains Na element, and the ratio of the sodium element content in the first positive electrode active layer to the sodium element content in the second positive electrode active layer is greater than 10.
[0029] The positive electrode sheet as described above, wherein the thickness ratio of the first positive electrode active layer to the second positive electrode active layer is 1:1 to 1:5;
[0030] Preferably, the thickness of the first positive electrode active layer is not less than 5 μm, and the total thickness of the positive electrode active layer is greater than 85 μm.
[0031] The positive electrode sheet as described above, wherein the single-side surface density of the positive electrode active layer is not less than 17 mg / cm 2 ;
[0032] And / or; the internal resistance of the positive electrode sheet is not higher than 0.4 kΩ*cm.
[0033] The present invention provides a lithium ion secondary battery, wherein the lithium ion battery comprises the positive electrode sheet described in any one of the above items.
[0034] The positive electrode sheet of the present invention, the positive electrode active layer includes a first positive electrode active layer and a second positive electrode active layer of special composition, wherein the first positive electrode active material and the second positive electrode active material shown in Formula 1 and / or Formula 2 have a special combination of double-layer structures, so that the positive electrode sheet has a lower internal resistance, thereby providing a guarantee for the rapid insertion and extraction of lithium ions, and thus has a considerable promoting effect on the rate performance and cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Schematic diagram of crack direction of the positive electrode sheet of the present invention;
[0036] Figure 2 This is a single-sided CP-SEM image of the non-rolled positive electrode sheet of Example 1 of the present invention;
[0037] Figure 3 This is the XRD diagram of the positive electrode sheet of Example 1 of the present invention;
[0038] Figure 4 Capacity-voltage differential curves of half-cells of Example 1 and Comparative Example 1 of the present invention;
[0039] Figure 5 This is a single-sided CP-SEM image of the positive electrode sheet of Example 2 of the present invention. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] A first aspect of the present invention provides a positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector and a positive electrode active layer disposed on at least a portion of the surface of the positive electrode current collector, the positive electrode active layer comprising a first positive electrode active layer and a second positive electrode active layer in sequence in a direction away from the positive electrode current collector; the first positive electrode active material in the first positive electrode active layer comprises a first lithium metal oxide as shown in Formula 1, and / or a second lithium metal oxide as shown in Formula 2; the second positive electrode active material in the second positive electrode active layer comprises a third lithium metal oxide as shown in Formula 3; wherein the first lithium metal oxide is a cubic system Cmca space group; the second lithium metal oxide is a cubic system P63mc space group; the third lithium metal oxide C is a cubic system R3-m space group;
[0042] Li n-y Na y Co c-a-bM1 b M2 a O2 Formula 1
[0043] In formula 1, 0.6≤n≤0.98, 0<y≤0.05, 0≤a≤0.1, 0<b≤0.1, 0.99<c<1.01, 0.95<a+b+c<1.15; M1 includes at least one of Al, Mg, Ti, Zr, La, and Y; M2 is a doping element different from M1, and M2 includes at least one of B, Te, W, and K;
[0044] Li m-x Na x Co d-y1 D y1 O2 Formula 2
[0045] In formula 2, 0.94≤m≤1.05, 0<x≤0.05, 0≤y1≤0.2, 0.95<d<1.01, 0.99<d+y1<1.12, and D includes at least one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, Te, B, and K.
[0046] In order to match the first positive electrode active material, the second positive electrode active material includes a third lithium metal oxide; the third lithium metal oxide C is a cubic system R3-m space group.
[0047] Li e Co f E g O2 Formula 3
[0048] In formula 3, 0.9≤e≤1.1, 0.95<f≤1.05, 0≤g≤0.15, 0.95≤f+g≤1.2, and E includes at least one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, Te, B, and K.
[0049] It should be noted that n and m in Formula 1 and Formula 2 are parameters related to the molar amount of elemental lithium in the first lithium metal oxide and the second lithium metal oxide, respectively.
[0050] The present invention does not limit the detection method of n and m. For example, an inductively coupled plasma spectrometer (ICP) can be used to detect the positive electrode active material. Alternatively, when the positive electrode active material in the positive electrode sheet is detected, the discharged battery is disassembled and the positive electrode sheet is taken out. The positive electrode sheet is soaked in dimethyl carbonate (DMC) for 1-3 hours or rinsed with DMC, and then naturally dried in a drying room. It is then placed in a muffle furnace and calcined at 300-600° C. for 2-5 hours. After that, the active layer falls off the current collector, and the powder to be detected is obtained after being sieved with 200 mesh. Subsequently, the metal elements in the powder to be detected are detected by ICP, and the values of n and m are calculated.
[0051] The positive electrode sheet of the present invention includes a positive electrode current collector and a positive electrode active layer arranged on at least one functional surface of the positive electrode current collector, wherein the functional surface refers to a plane in the direction of the length and width of the current collector, and each current collector includes two functional surfaces arranged opposite to each other. At least one functional surface of the positive electrode current collector includes a first positive electrode active layer and a second positive electrode active layer stacked, wherein the first positive electrode active layer is closer to the positive electrode current collector. Generally, the positive electrode current collector is an aluminum foil or a composite aluminum foil with a thickness of 5 to 12 μm.
[0052] The positive electrode sheet of the present invention has a lower internal resistance, which helps to improve the cycle performance and rate performance of the lithium-ion battery. The reason may be that the first positive electrode active material having the structure of Formula 1 or Formula 2 has a larger interlayer spacing. After it is matched with the second positive electrode active material having the structure of Formula 3, the lithium ion transmission channel inside the positive electrode active layer is smoother, which improves the efficiency of lithium ion deintercalation. Therefore, during the charge and discharge process, the internal resistance of the electrode sheet is lower and the electronic conductivity is higher, so it can show excellent cycle performance and rate performance. In addition, the special structure of the double-layer setting also helps to reduce the polarization phenomenon of the positive electrode sheet, further reduce the internal resistance of the electrode sheet, and help to further improve the energy density of the lithium-ion battery under high voltage.
[0053] In a specific embodiment, the X-ray diffraction spectrum of the positive electrode active layer includes a first diffraction peak and a second diffraction peak with 2θ of 17.6° to 19.5°, and the difference in 2θ between the first diffraction angle and the second diffraction angle is 0.3° to 1.0°. The inventors have found that by further controlling the ratio of the positive electrode active materials in the first positive electrode active layer and the second positive electrode active layer, it is helpful to make the positive electrode active layer have the above-mentioned diffraction characteristics. The inventors have found that when the positive electrode sheet including the first positive electrode active material and the second positive electrode active material has the above-mentioned diffraction characteristics, the resistance to lithium ion insertion and extraction is lower, which is conducive to further reducing the polarization phenomenon of the battery. It should be noted that the difference here in the present invention refers to the absolute value.
[0054] Furthermore, 2θ of the second diffraction peak is greater than 2θ of the first diffraction peak, and an intensity ratio of the second diffraction peak to the first diffraction peak is 1-5.
[0055] In detail, the peak 2θ of the second diffraction peak is greater than the peak 2θ of the first diffraction peak, and the peak intensity P2 of the second diffraction peak is not less than the peak intensity P1 of the first diffraction peak, and P2 / P1 is (1-5): 1. At this time, the internal crystalline phase structures of the first positive electrode active material and the second positive electrode active material may support each other, further showing higher material stability. On the one hand, the resistance of the lithium ion deintercalation channel is reduced, which helps to obtain a positive electrode sheet with lower internal resistance. On the other hand, the voltage resistance of the positive electrode sheet is also more outstanding, and the discharge capacity of the battery can be increased by appropriately increasing the charging voltage, as well as the ion conduction efficiency of lithium ions.
[0056] In addition, when the half-cell consisting of the positive electrode sheet and the lithium metal negative electrode is charged to 4.55V at a current rate of ≤0.1C, and then charged at a constant voltage to 0.025C and cut off, and then discharged to 3.0V at a current rate of ≤0.1C, the number N of discharge peaks in the capacity-voltage differential curve of the half-cell in the range of 3.0 to 4.0V is not less than 2.
[0057] In the above-mentioned charging and discharging process, as long as the charging rate and the discharging rate of the half-cell do not exceed 0.1C, the capacity-voltage differential curve of the battery has no less than 2 discharge peaks in the range of 3.0-4.0V. It should be noted that the above-mentioned battery refers to a battery with a cycle number of no more than 10 cycles, and the present invention does not impose any restrictions on the electrolyte constituting the above-mentioned battery. In addition, after charging is completed, it is necessary to stand for 3 minutes before performing the above-mentioned discharge operation.
[0058] Specifically, the capacity-voltage differential curve is obtained by performing capacity-voltage differential processing on the charge and discharge curve of the battery. Specifically, the capacity-voltage differential curve includes two parts: a capacity-voltage differential charge curve and a capacity-voltage differential discharge curve. The above discharge peaks are all located in the capacity-voltage differential discharge curve. During the charging and discharging process of the battery, the charge rate and the discharge rate do not exceed 0.1C and the two can be the same or different.
[0059] The inventors found that when the positive electrode of the present invention is applied to a lithium-ion battery, as the charging voltage increases, the lithium-ion battery can release more capacity, and as the number of charge and discharge cycles increases and the discharge rate increases, the lithium-ion discharge capacity remains stable. The number of discharge peaks is related to the energy of lithium deintercalation and the reversibility of the material. The positive electrode of the present invention has a large number of discharge peaks in the range of 3.0 to 4.0V, which means that the double-layer structure of the special material of the positive electrode of the present invention has a lower lithium ion transmission resistance, which in turn makes it have a lower lithium deintercalation potential at low voltage. Therefore, the positive electrode of the present invention requires lower energy during lithium deintercalation and can improve the material reversibility. Therefore, the positive electrode is easier to deintercalate lithium at the same voltage, so it has a higher capacity, better cycle performance and rate performance.
[0060] It can be understood that the positive electrode sheet in the above half-cell is a single-sided positive electrode sheet, that is, the positive electrode active layer is only provided on one functional surface of the positive electrode current collector.
[0061] In addition, the above-mentioned half-cell can also be prepared by disassembling the lithium-ion battery including the positive electrode sheet of the present invention. Specifically, a lithium-ion battery including the positive electrode sheet of the present invention and having a cycle number of no more than 10 cycles is selected, and after discharging to 3.0V at a current of 1 / 10 of the rated capacity, its voltage is tested to confirm that its voltage is 3.0 to 3.6V, and then the lithium-ion battery is disassembled, the positive electrode sheet is taken out, and it is soaked in dimethyl carbonate (DMC) for 3 hours, and after baking in an oven below 100°C for 12 hours, after ensuring that the solvent has completely evaporated, the single-sided positive electrode sheet is taken out for the corresponding half-cell assembly.
[0062] In a specific embodiment, the Dv50 of the first positive electrode active material is 3-10 μm, and the particle size Dv50 of the second positive electrode active material is 14-20 μm. The Dv50 referred to here is the particle size when the cumulative volume reaches 50% of the total volume of all the second positive electrode active materials.
[0063] When the positive electrode sheet includes the above structure, on the one hand, the side reaction between the positive electrode sheet and the electrolyte can be reduced, which not only prolongs the cycle life of the battery, but also helps to ensure the safety of the battery during long cycles; on the other hand, in the process of roller pressing preparation of the positive electrode sheet, the above structure can effectively utilize the roller pressing pressure, which can not only avoid the crushing and collapse of the positive electrode active material while ensuring the surface density, but also help to create channels inside the positive electrode active material that are conducive to the transmission of lithium ions, thereby ensuring the cycle performance and rate performance of the battery.
[0064] Furthermore, the Dv50 of the first positive electrode active material is less than the Dv50 of the second positive electrode material. At this time, it is more conducive to the electrolyte to infiltrate the positive electrode sheet, reduce the migration resistance of lithium ions, and further improve the cycle performance and rate performance.
[0065] In a specific embodiment, the first positive electrode active material is a block material, and the second positive electrode active material in the second positive electrode active layer is spherical or quasi-spherical. Specifically, the first positive electrode active material and the second positive electrode active have different morphologies. Specifically, the first positive electrode active material is a block material, that is, the ratio of the length to the thickness, and the ratio of the width to the thickness of the first positive electrode active material are both greater than 1.
[0066] Furthermore, the first positive electrode active material includes a first crack whose extension direction has an angle of less than 15° with the first direction, and the second positive electrode active material includes a second crack whose extension direction has an angle of less than 15° with the first direction, wherein the first direction is the length direction of the current collector.
[0067] The first crack and the second crack with special angles have obvious regular orientation and can be used as transmission channels for lithium ions to realize charge and discharge operations.
[0068] Furthermore, the number of the first cracks can be controlled to be greater than the number of the second cracks. The reason is that since the first cracks are located in the first positive electrode active layer far away from the electrolyte, more lithium ions in the first positive electrode active layer can be involved in the deintercalation by making the first positive electrode active layer have more first cracks, thereby improving the gram capacity and cycle performance of the battery.
[0069] by Figure 1 For example, Figure 1 The positive electrode sheet in the embodiment includes a first positive electrode active layer and a second positive electrode active layer arranged on a functional surface of an aluminum foil layer, wherein the first crack in the first positive electrode active layer is substantially parallel to the length direction of the aluminum foil layer (i.e., the angle is 0°), and the second positive electrode active layer includes a second crack with an angle less than 15° to the length direction of the aluminum foil layer, and a third crack with an angle greater than 15° to the length direction of the aluminum foil layer. Obviously, the number of the first cracks is greater than the number of the second cracks.
[0070] Specifically, the cross-section CP (cross-section) technology can be used for SEM imaging test and observation (CP-SEM). It should be noted that the positive electrode sheet having the above-mentioned relationship between the number of the first crack and the second crack refers to the positive electrode sheet that has not been assembled into a battery after rolling or the positive electrode sheet in a lithium-ion battery with a cycle number of no more than 10 cycles.
[0071] In addition, the present invention also defines the sodium content of the positive electrode active layer in the positive electrode sheet. Specifically, the total sodium content in the positive electrode active layer is 20-1000ppm. For example, when both functional surfaces of the positive electrode sheet include a first positive electrode active layer and a second positive electrode active layer stacked, the total sodium content of all active layers on the two functional surfaces is 20-1000ppm.
[0072] Since the radius of sodium ions is larger than that of lithium ions, the sodium ions in the positive electrode active layer play a supporting role in the material structure, which can significantly improve the insertion and extraction of lithium ions, thereby improving the cycle performance.
[0073] In a specific embodiment, when the positive electrode sheet has the structure as described above, that is, including the first positive electrode active layer and the second positive electrode active layer, the ratio of the sodium content in the first positive electrode active layer to the sodium content in the second positive electrode active layer is greater than 10. At this time, the Na content in the first positive electrode active layer is higher than that in the second positive electrode active layer, indicating that the first positive electrode active material has a better lithium ion deintercalation channel than the second positive electrode active material, which is more conducive to the free deintercalation of lithium during the charge and discharge process, thereby improving the cycle performance to a certain extent, and can reduce the polarization phenomenon of the electrode sheet and improve the rate performance.
[0074] The present invention does not limit the source of the sodium element in the positive electrode active layer, and the sodium element may come from, for example, the positive electrode active material, the dispersant, the binder, and the like.
[0075] Furthermore, a thickness ratio of the first positive electrode active layer to the second positive electrode active layer is 1:1 to 1:5.
[0076] When the first positive electrode active layer and the second positive electrode active layer have the above chemical composition and the thickness ratio of the two also satisfies 1:1 to 1:5, it helps to further reduce the internal resistance of the positive electrode sheet. Even if the energy density of the battery is increased by increasing the thickness of the positive electrode active layer or the surface density of the positive electrode sheet, it will not affect the ionic conductivity of lithium ions, which helps to maintain the cycle performance and rate performance of the battery.
[0077] Furthermore, the thickness of the first positive electrode active layer is not less than 5 μm. In the prior art, in order to reduce the migration resistance of lithium ions, the thickness of the active layer is often controlled to avoid the obstruction of lithium ion migration due to excessive thickness. However, the inventors found that when the positive electrode sheet of the present invention includes a first positive electrode active material and a second positive electrode active material, the mutual synergy between the first positive electrode active material and the second positive electrode active material increases with the increase in the thickness of the first active layer, not only the energy density of the battery increases, but also it helps to further ensure the cycle performance and rate performance of the lithium ion battery.
[0078] In a specific embodiment, the total thickness of the positive electrode active layer is greater than 85 μm, which can provide more positive electrode active materials for the battery to participate in the deintercalation of lithium ions. The total thickness of the positive electrode active layer here refers to the sum of the thickness of the first positive electrode active layer and the second positive electrode active layer.
[0079] Furthermore, in order to make the lithium-ion battery have a better energy density, the total thickness of the positive electrode active layer can be controlled to be 85-150 μm.
[0080] In one embodiment of the present invention, the single-surface density of the positive electrode active layer is not less than 17 mg / cm 2 ; Wherein, the internal resistance of the positive electrode sheet is not higher than 0.4 kΩ*cm. The single-sided surface density of the positive electrode active layer refers to the surface density of the positive electrode active layer on each functional surface of the positive electrode current collector.
[0081] On the one hand, the single-sided surface density of the positive electrode active layer of the positive electrode sheet of the present invention is not less than 17 mg / cm 2 Therefore, more positive electrode active materials participate in the deintercalation of lithium ions per unit time, thereby making the lithium ion battery including the positive electrode sheet have an advantage in discharge capacity. On the other hand, the internal resistance of the positive electrode sheet of the present invention is not higher than 0.4 kΩ*cm, so the deintercalation resistance of lithium ions is lower, the deintercalation pathway is smoother, and no serious polarization phenomenon occurs, thereby ensuring the rate performance and cycle performance of the lithium ion battery.
[0082] It can be understood that in addition to the positive electrode active material, the positive electrode active layer also includes a conductive agent and a binder. Exemplarily, the positive electrode active layer includes 70-99wt% of the positive electrode active material, 0.5-15wt% of the conductive agent, and 0.5-15wt% of the binder according to the mass percentage, and further includes 80-98wt% of the positive electrode active material, 1-10wt% of the conductive agent, and 1-10wt% of the binder.
[0083] The selection of the conductive agent and the binder is not special and can be conventionally selected in the art. For example, the conductive agent is selected from at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotube, single-walled carbon nanotube, multi-arm carbon nanotube, and carbon fiber, and the binder is selected from at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyacrylate lithium (PAALi).
[0084] Furthermore, in order to improve safety performance, a safety layer can be provided between the positive electrode active layer and the current collector. The material of the safety layer is generally a non-conductive safety material, such as an iron-containing compound (such as lithium iron phosphate, iron phosphate, etc.), an aluminum-containing compound (such as ceramic alumina), etc. Of course, the safety layer also includes a binder, and the ratio of the binder to the safety material can be further determined according to specific needs.
[0085] Furthermore, when the compaction density of the positive electrode sheet is not less than 3.5 g / cm 3 When the battery is heated, the cycle performance and capacity of the battery can be further improved.
[0086] The second aspect of the present invention also provides a lithium ion battery, which includes the above-mentioned positive electrode sheet and thus has outstanding performance in terms of cycle performance, rate performance and specific capacity.
[0087] The present invention does not limit the specific structure of the lithium-ion battery, for example, it can be a square shell battery, a cylindrical battery, etc.
[0088] According to the present invention, the lithium ion battery further comprises a negative electrode sheet, a separator and an electrolyte.
[0089] For example, the conventional electrolyte of the electrolyte lithium salt and the solvent contains ethylene carbonate (abbreviated as EC), diethyl carbonate (abbreviated as DEC), propylene carbonate (abbreviated as PC), fluoroethylene carbonate (abbreviated as FEC). Further, an additive represented by formula T is also included.
[0090]
[0091] In a specific embodiment, when the electrolyte includes 5-10% of the additive shown in the above formula T in terms of mass percentage, under the above-mentioned positive electrode active material system, the additive can enable the non-lithium salt components in the electrolyte to preferentially form a SEI film at the negative electrode, and the stability of the SEI film is improved to a certain extent, thereby improving the performance of the lithium-ion battery in terms of cycle performance and rate performance.
[0092] Furthermore, the electrolyte comprises, by mass percentage, 4-20% fluoroethylene carbonate, 10-30% lithium hexafluorophosphate, and 2-10% additives. In this case, the cycle performance and rate performance of the lithium-ion battery are more prominent.
[0093] Exemplarily, the negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on at least one functional surface of the negative electrode current collector. Wherein, the negative electrode active layer includes a negative electrode active material, a conductive agent and a binder. In a specific embodiment, the negative electrode active layer includes 70-99wt% of negative electrode active material, 0.5-15wt% of conductive agent, 0.5-15wt% of binder according to mass percentage, and further includes 80-98wt% of negative electrode active material, 1-10wt% of conductive agent, and 1-10wt% of binder. Wherein, the negative electrode active material is selected from one or more of artificial graphite, natural graphite, hard carbon, mesophase carbon microspheres, lithium titanate, silicon carbon, and silicon oxide. Further, the negative electrode sheet can also be a lithium metal negative electrode including lithium metal, which is beneficial to provide more lithium sources for the battery, wherein the lithium metal can be disposed on the surface of the negative electrode active layer away from the current collector, or lithium foil can be directly used as the negative electrode sheet. In detail, when the first positive electrode active material described in Formula 1 is included, a negative electrode sheet containing lithium metal is preferred, which is beneficial to improving lithium deintercalation and lithium transport of the positive electrode first active material.
[0094] Exemplarily, the diaphragm is a material with polypropylene as the base material, or a rubber-coated diaphragm with ceramic coated on one side or both sides thereof.
[0095] The lithium ion battery of the present invention is suitable for high voltage systems, and has good rate performance, cycle stability and high gram capacity at higher voltages such as 4.50V, and can meet the demand for lightweight and thin use of high-end digital products.
[0096] The present invention is further described below through specific embodiments.
[0097] Example 1
[0098] The method for preparing the positive electrode sheet of this embodiment comprises the following steps:
[0099] 1) The first metal oxide numbered A1, the conductive agent SP and the binder PVDF-900 are mixed in a mass ratio of 97%:1.5%:1.5%, and the mixture is dispersed in NMP, and a first active material layer slurry is obtained by double planetary stirring. The first active material layer slurry is coated on the two functional surfaces of the aluminum foil current collector with a thickness of 10 μm, and dried after coating. The thickness of the single-side coating layer is about 15 μm, and a positive electrode sheet containing the first active material layer is obtained.
[0100] 2) The third metal oxide numbered C1, PVDF, and carbon nanotubes are mixed in a mass ratio of 97%:1.5%:1.5%, and the mixture is dispersed in NMP, and a second active material layer slurry is obtained by double planetary stirring. The second active material layer slurry is coated on the surface of the first active material layer away from the positive electrode current collector, and dried after coating. The thickness of the single-side coating layer is about 40 μm. Figure 2 This is a single-sided CP-SEM image of the non-rolled positive electrode sheet of Example 1 of the present invention.
[0101] 3) The electrode after drying in step 2) is compacted to a single-sided density of 4.05 g / cm 3 Rolling was performed to obtain a positive electrode sheet with a total thickness of 102 μm, and the thickness ratio H of the first positive electrode active layer to the second positive electrode active layer was 3:8, the thickness of the positive electrode active layer was 92 μm, and the surface density was 18.64 mg / cm 2 .
[0102] The specific parameters of the positive electrode sheet of this embodiment are shown in Table 1 and Table 2.
[0103] 4) Mix the negative electrode active materials graphite, styrene diene rubber (SBR), sodium carboxymethyl cellulose, and conductive carbon black in a weight ratio of 94.5%:3%:2%:0.5%, disperse the mixture in water, and obtain a negative electrode slurry by double planetary mixing. Apply the negative electrode slurry to both sides of the copper foil current collector, then roll and dry to obtain a negative electrode sheet for standby use.
[0104] Embodiments 2 to 11
[0105] The preparation methods of Examples 2 to 11 are substantially the same as those of Example 1. Specific parameters of the positive electrode sheets are shown in Tables 1 and 2. The parameters not shown are the same as those of Example 1.
[0106] Embodiments 12 to 13
[0107] The preparation methods of Examples 12 to 13 are basically the same as those of Example 5, except for the thickness ratio of the positive electrode active layer. The specific parameters of the positive electrode sheet are shown in Table 1 and Table 2. The parameters not shown are the same as those of Example 1.
[0108] Embodiments 14 to 15
[0109] The preparation methods of Examples 14 to 15 are basically the same as those of Example 2, except for the chemical composition of the first positive electrode active layer. Specific parameters of the positive electrode sheets are shown in Tables 1 and 2. The parameters not shown are the same as those of Example 1.
[0110] Comparative Examples 1-2
[0111] The preparation methods of Comparative Examples 1-2 are the same as those of Example 1, except that step (1) is omitted. Specific parameters of the positive electrode sheets are shown in Tables 1 and 2. The parameters not shown are the same as those of Example 1.
[0112] Comparative Examples 3-4
[0113] The preparation methods of Comparative Examples 3 to 4 are the same as those of Example 1, except that step (2) is omitted. The specific parameters of the positive electrode sheet are shown in Tables 1 and 2. In addition, the negative electrode sheet of Comparative Example 3 is also laminated by rolling on the surface of the negative electrode active layer away from the current collector to obtain a surface density of 0.5 mg / cm 2 The lithium foil is finally obtained to obtain a negative electrode sheet containing lithium metal. The parameters not shown are the same as those in Example 1.
[0114] The number of first cracks in the first positive electrode active materials in Table 1 is greater than the number of second cracks in the second positive electrode active materials.
[0115] Table 1
[0116]
[0117]
[0118] Table 2
[0119]
[0120]
[0121] Test Example 1
[0122] The surface density, total thickness of the positive electrode active layer and internal resistance of the positive electrode sheets in the embodiments and comparative examples were tested, and the results are shown in Table 3.
[0123] in,
[0124] Surface density detection method: Take the positive electrode, first confirm that the appearance of the electrode is intact, without missing materials or electrolyte residue, and then use a punching die with a diameter of 18mm to punch the double-sided electrode multiple times. Select 5 pieces of punching pieces in different positions, and weigh them accordingly to obtain the corresponding electrode weights. Calculate the surface density of the weighed electrode according to the area of the electrode, and take the average value to obtain the electrode surface density.
[0125] Total thickness of the positive electrode active layer: The thickness of the positive electrode sheet is measured with a micrometer, and then the thickness of the positive electrode current collector is subtracted.
[0126] Electrode internal resistance test method: Take the positive electrode, first confirm that the appearance of the electrode is intact, without missing materials or electrolyte residue, and then place the electrode flat on a multi-function digital four-probe tester for the corresponding electrode resistance test. The results are shown in Table 3.
[0127] Table 3
[0128]
[0129] Test Example 2
[0130] The positive electrode sheets in the embodiments and comparative examples were subjected to XRD testing, and the specific experimental method included:
[0131] The positive electrode sheets of the embodiment and the comparative example are respectively wound with the negative electrode sheets to obtain a winding core, which is then packaged in an aluminum-plastic bag, injected with electrolyte, and hot-pressed to obtain a lithium-ion battery. The capacity of the battery is tested to be 4000mAh. The negative electrode sheet includes a copper foil and a negative electrode active layer located on both sides of the copper foil. The negative electrode active layer includes 94.5% graphite, 3% styrene diene rubber (SBR), 2% sodium carboxymethyl cellulose, and 0.5% conductive carbon black in terms of mass percentage. The electrolyte is mixed in a mass ratio of ethylene carbonate (abbreviated as EC): diethyl carbonate (abbreviated as DEC): propylene carbonate (abbreviated as PC): ethyl methyl carbonate (EMC) = 3:6:2:9, and then 6% of the total mass of the electrolyte is added with fluoroethylene carbonate (abbreviated as FEC), 13% of the total mass of the electrolyte is added with lithium hexafluorophosphate (abbreviated as LiPF6), and the additive shown in formula T, and the additive content accounts for 2% of the total content of the electrolyte;
[0132] After discharging to 3.0V at a current of 1 / 10 of the rated capacity, the voltage was tested to confirm that the voltage was 3.0-3.6V. The lithium-ion battery was then disassembled, the positive electrode sheet was taken out, and it was soaked in dimethyl carbonate (DMC) for 3 hours. After naturally drying in a drying room, the positive electrode sheet was taken out for XRD testing. The scanning angle range of the XRD test was 10-90°, and the 2θ and 2θ differences of the first diffraction peak and the second diffraction peak of 17.6°-19.5° were confirmed, as shown in Table 4. Figure 3 This is the XRD diagram of the positive electrode sheet of Example 1 of the present invention.
[0133] Table 4
[0134]
[0135]
[0136] Test Example 3
[0137] The positive electrode sheets of the embodiment and the comparative example are respectively wound with the negative electrode sheets to obtain a winding core, which is then packaged in an aluminum-plastic bag, injected with electrolyte, and hot-pressed to obtain a lithium-ion battery. The capacity of the battery is tested to be 4000 mAh. The negative electrode sheet includes a copper foil and a negative electrode active layer located on both sides of the copper foil. The negative electrode active layer includes 94.5% graphite, 3% styrene diene rubber (SBR), 2% sodium carboxymethyl cellulose, and 0.5% conductive carbon black in terms of mass percentage. The electrolyte is mixed in a mass ratio of ethylene carbonate (abbreviated as EC): diethyl carbonate (abbreviated as DEC): propylene carbonate (abbreviated as PC): ethyl methyl carbonate (EMC) = 3:6:2:9, and then 6% of the total mass of the electrolyte is added with fluoroethylene carbonate (abbreviated as FEC), 13% of the total mass of the electrolyte is added with lithium hexafluorophosphate (abbreviated as LiPF6), and the additive shown in formula T, and the additive content accounts for 2% of the total content of the electrolyte.
[0138] Perform the following tests on lithium-ion batteries.
[0139] 1) The total content of sodium in the positive electrode active layer
[0140] After the lithium-ion battery that has not been cycled (after formation) is discharged to 3.0V at a current of 1 / 10 of the rated capacity, its voltage is tested and found to be 3.0-3.6V. Then the lithium-ion battery is disassembled, the positive electrode sheet is taken out, and it is soaked in dimethyl carbonate (DMC) for 3h, dried naturally in a drying room, and then calcined at 300℃ in a muffle furnace for 3h. After sieving through 200 mesh, the sample powder is obtained, and the sodium content is tested using an inductively coupled plasma (ICP) instrument to obtain the sodium content in the positive electrode active layer. The results are shown in Table 5.
[0141] 2) Ratio of sodium content in the first positive electrode active layer and the second positive electrode active layer
[0142] After the lithium-ion battery that has not been cycled (after formation) is discharged to 3.0V at a current of 1 / 10 of the rated capacity, its voltage is tested and found to be 3.0-3.6V. Then the lithium-ion battery is disassembled, the positive electrode sheet is taken out, and the surface of the second active material layer is adhered with tape, and then the second active material layer is separated from the first active material layer by force. Then, they are soaked in dimethyl carbonate (DMC) for 3h, dried naturally in a drying room, and placed in a muffle furnace for calcination at 300℃ for 3h. After sieving at 200 mesh, sample powders are obtained, and the sodium content is tested using an inductively coupled plasma (ICP) instrument, and the ratio of the sodium content in the first positive electrode active layer and the second positive electrode active layer is calculated. The results are shown in Table 5.
[0143] 3) Battery capacity
[0144] The lithium-ion battery was placed in an environment of 25°C, first discharged at 0.2C to 3.0V, then charged at 0.2C to 4.5V, then charged at a constant voltage until the current dropped to 0.02C, and then discharged at 0.2C to 3.0V, and the battery discharge capacity Q was obtained in mAh, and the gram capacity of the positive electrode material C mAh / g was calculated by the weight of the positive electrode active material. The results are shown in Table 6.
[0145] 4) Capacity retention rate
[0146] At 25°C, under the conditions of 0.7C charging and 0.7C discharging, the lithium ion battery in 1) was repeatedly charged and discharged for 1000 times, and the voltage ranges were 3.0-4.5V and 3.0-4.53V, respectively. The discharge capacity at the first cycle and the discharge capacity at the 1000th cycle were measured, and the capacity retention rate Re1 at a charge and discharge voltage of 3.0-4.5V and the capacity retention rate Re2 at a charge and discharge voltage of 3.0-4.53V after 1000 cycles were calculated according to the following formulas. The results are shown in Table 6.
[0147] Capacity retention rate Re1 = (discharge capacity at the 1000th cycle) / (discharge capacity at the first cycle) * 100%
[0148] Capacity retention rate Re2 = (discharge capacity at the 1000th cycle) / (discharge capacity at the first cycle) * 100%
[0149] Table 5
[0150]
[0151]
[0152] Test Example 4
[0153] A single-sided positive electrode sheet was prepared according to the method of the above embodiment and comparative example, and then the positive electrode sheet was punched into a small disc with a diameter of 12 mm using a film mold. After drying and weighing, a button battery was assembled in a glove box under Ar protective atmosphere using a 2025 button battery shell, a Li metal disc as the negative electrode, and a conventional high-voltage lithium cobalt oxide electrolyte.
[0154] After each button cell was left to stand for 4 hours under normal conditions, the first charge and discharge capacity test was conducted. The test conditions were as follows: charging to 4.55V at a current rate of ≤0.1C, charging at a constant voltage to 0.025C, and then standing for 3 minutes, and then discharging to 3.0V at a current rate of ≤0.1C to obtain the corresponding discharge capacity in grams. A portion of the graph was selected to make a curve graph, and its discharge capacity in grams was C1mAh / g. After the discharge curve was subjected to DQ / DV differential processing, the number of peaks in the range of 3.0 to 4.0V was defined as N. The results are shown in Table 6. Figure 4 The capacity-voltage differential curves of the half-cells of Example 1 and Comparative Example 1 of the present invention are shown.
[0155] Test Example 5
[0156] The lithium-ion battery was assembled according to the method of Experimental Example 2, and discharged to 3.0V at a current of 1 / 10 of the rated capacity. The voltage was tested and found to be 3.0-3.6V. The lithium-ion battery was then disassembled, the positive electrode was taken out, and it was soaked in dimethyl carbonate (DMC) for 3h. After being naturally dried in a drying room, it was processed by CP (cross-section) technology and then subjected to SEM imaging test to obtain the corresponding cross-sectional SEM image of the electrode, as shown in FIG. Figure 5 shown.
[0157] Table 6
[0158]
[0159]
[0160] It can be seen from Tables 3 to 6 that the positive electrode sheets of the embodiments of the present invention can enable the battery to have a relatively high discharge capacity while also having excellent cycle performance and internal resistance.
[0161] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A positive electrode sheet, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active layer arranged on at least a portion of the surface of the positive electrode current collector, wherein the positive electrode active layer comprises a first positive electrode active layer and a second positive electrode active layer stacked in a direction away from the positive electrode current collector; The first positive electrode active material in the first positive electrode active layer includes a first lithium metal oxide shown in Formula 1 and / or a second lithium metal oxide shown in Formula 2; The second positive electrode active material in the second positive electrode active layer includes a third lithium metal oxide represented by Formula 3; Wherein, the first lithium metal oxide is a cubic crystal of Cmca space group; The second lithium metal oxide is a cubic crystal with a P63mc space group; The third lithium metal oxide C is a cubic crystal of R3-m space group; Li n-y Na y Co c-a-b M1 b M2 a O2 type 1 In formula 1, 0.6≤n≤0.98, 0<y≤0.05, 0≤a≤0.1, 0<b≤0.1, 0.9<c<1.1, 0.95<a+b+c<1.15; M1 includes at least one of Al, Mg, Ti, Zr, La, and Y; M2 is a doping element different from M1, and M2 includes at least one of B, Te, W, and K; Li m-x Na x Co d-y1 D y1 O2 formula 2 In formula 2, 0.9≤m≤1.05, 0<x≤0.05, 0≤y1≤0.2, 0.95<d<1.1, 0.99<d+y1<1.12, D includes at least one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, Te, B, and K; Li e Co f E g O2 formula 3 In formula 3, 0.9≤e≤1.1, 0.95<f≤1.05, 0≤g≤0.15, 0.95≤f+g≤1.2, and E includes at least one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, Te, B, and K.
2. The positive electrode sheet according to claim 1, characterized in that: The X-ray diffraction spectrum of the positive electrode active layer includes a first diffraction peak and a second diffraction peak with 2θ of 17.6° to 19.5°, and the difference in 2θ between the first diffraction angle and the second diffraction angle is 0.3° to 1.0°; Preferably, the intensity ratio of the second diffraction peak to the first diffraction peak is (1-5):1, and the 2θ of the second diffraction peak is greater than the 2θ of the first diffraction peak.
3. The positive electrode sheet according to claim 1 or 2, characterized in that: The half-cell composed of the positive electrode sheet and the lithium metal negative electrode is charged to 4.55V at a current rate of ≤0.1C, then charged at a constant voltage to 0.025C and then discharged to 3.0V at a current rate of ≤0.1C. The number N of discharge peaks in the capacity-voltage differential curve of the half-cell within the range of 3.0 to 4.0V is not less than 2.
4. The positive electrode sheet according to any one of claims 1 to 3, characterized in that: The second positive electrode active material comprises spherical or quasi-spherical particles; The Dv50 of the first positive electrode active material is 3-10 μm; the Dv50 of the second positive electrode active material is 14-20 μm; The Dv50 of the first positive electrode active material is less than the Dv50 of the second positive electrode material.
5. The positive electrode sheet according to claim 1, characterized in that: The first positive electrode active material includes a first crack whose extension direction has an angle of less than 15° with the first direction, and the second positive electrode active material in the second positive electrode active layer includes a second crack whose extension direction has an angle of less than 15° with the first direction; Preferably, the number of the first cracks is greater than the number of the second cracks.
6. The positive electrode sheet according to any one of claims 1 to 5, characterized in that: The content of sodium element in the positive electrode active layer is 20-1000ppm.
7. The positive electrode sheet according to claim 1, characterized in that: The positive electrode active layer contains Na element, and the ratio of the sodium element content in the first positive electrode active layer to the sodium element content in the second positive electrode active layer is greater than 10.
8. The positive electrode sheet according to claim 1, characterized in that: The thickness ratio of the first positive electrode active layer to the second positive electrode active layer is 1:1 to 1:5; Preferably, the thickness of the first positive electrode active layer is not less than 5 μm, and the total thickness of the positive electrode active layer is greater than 85 μm.
9. The positive electrode sheet according to any one of claims 1 to 8, characterized in that: The single-surface density of the positive electrode active layer is not less than 17 mg / cm 2 ; And / or; the internal resistance of the positive electrode sheet is not higher than 0.4 kΩ*cm.
10. A lithium ion secondary battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to any one of claims 1 to 9.
Citation Information
Cited By
Positive electrode material, electrochemical device, and electronic device
WO2026174429A1
Positive electrode material, electrochemical device, and electronic device
WO2026183671A1
Positive electrode material, secondary battery, and electronic device
WO2026193690A1
Positive electrode material, secondary battery, and electronic device
WO2026213824A1