Battery
By using fluoronitrile compounds and a combination design of lithium cobalt oxide and nickel cobalt manganese ternary materials in lithium-ion batteries, the problems of lithium precipitation and insufficient overcharge resistance of the battery core are solved, and high cycle stability and cost-effectiveness are achieved. promote.
Patent Information
- Application Number
- CN202410838566.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-29
AI Technical Summary
Lithium-ion batteries are prone to safety problems such as lithium deposition and overcharge under high-voltage and fast-charging conditions, and it is difficult to effectively reduce costs with existing technology while improving cycle stability and overcharge resistance.
Fluoronitrile compounds are used as solvents in the electrolyte, and lithium cobalt oxide and nickel cobalt manganese ternary materials are doped into the positive active material. By adjusting the content and particle size of nickel, the combination of fluoronitrile compounds and positive active materials is improved. The degree of complexation reaction enhances the protection effect of electrochemical active sites.
It significantly improves the problem of lithium precipitation in the battery core, improves the cycle stability and overcharge resistance of the battery, while reducing the battery cost and achieving high energy density and high cost performance.
Smart Images

Figure BDA0004913822730000111 
Figure BDA0004913822730000121 
Figure BDA0004913822730000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of energy storage, and in particular to a battery. Background Art
[0002] In recent years, the competition in lithium-ion batteries has reached a white-hot stage. Leading enterprises will gradually expand their market share by virtue of their advantages in technology, quality, scale and environmental protection, and the industry concentration will further increase. Among them, reducing costs and increasing efficiency of products is the core driving force for the long-term development of lithium-ion batteries. Therefore, it is necessary to innovate the design of lithium-ion batteries in the system, update and iterate materials, and continuously optimize the cost performance, so as to meet the requirements of lithium-ion batteries for high energy density and high cost performance. However, for the products after the above optimization, safety problems such as lithium deposition and overcharging caused by high voltage and fast charging are still common. Summary of the invention
[0003] The present invention provides a battery, which comprises a positive electrode and an electrolyte. The battery of the present invention can significantly improve the problem of lithium deposition in the battery core; the battery of the present invention has high cycle stability and high overcharge resistance; and the battery of the present invention can significantly reduce costs.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0005] The present invention provides a battery, comprising a positive electrode and an electrolyte.
[0006] The electrolyte includes a fluoronitrile solvent; the fluoronitrile solvent is a fluoronitrile compound;
[0007] The positive electrode includes a positive electrode active material, which includes lithium cobalt oxide and a nickel-cobalt-manganese ternary material, wherein the mass content of the nickel element is k wt%, 0wt%<k wt%≤24wt%, based on the total mass of the positive electrode active material.
[0008] Through the above technical solution, the present invention has at least the following advantages compared with the prior art:
[0009] The fluoronitrile solvent in the electrolyte of the present invention is a fluoronitrile compound, which can not only make the lithium ions in the electrolyte smoothly deintercalate under the conditions of high voltage and high current, but also can complex with the metal ions of the positive electrode active material, reduce the dissolution of metal ions under high voltage conditions, protect the stability of the positive electrode structure, and reduce the occurrence of negative electrode side reactions, and significantly improve the problem of lithium precipitation in the battery core; moreover, the compound has particularly strong oxidation resistance and high voltage resistance, so that the lithium ion battery can simultaneously achieve high cycle performance and excellent overcharge resistance; moreover, the present invention can further improve the degree of complex reaction of the electrochemical active sites formed by the carbon-nitrogen triple bond in the fluoronitrile compound and the metal ions on the surface of the positive electrode active material by reasonably adjusting the content k wt% of the nickel element in the positive electrode active material, so that the metal ions are more closely combined with the fluoronitrile compound, and the dissolution of metal ions is reduced, so that the positive electrode active material mixed with nickel-cobalt-manganese ternary material can be effectively protected by the fluoronitrile solvent, and the cycle performance and overcharge resistance of the battery are further improved. In addition, the positive electrode active material of the present invention adopts the form of a mixture of lithium cobalt oxide and nickel-cobalt-manganese ternary material, which can make the battery have high energy density and high cost performance, thereby significantly reducing the cost of the battery.
[0010] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. DETAILED DESCRIPTION
[0011] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0012] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0013] Lithium cobalt oxide, commonly used as positive electrode active material, has a theoretical capacity of about 274 mAh / g and an actual compaction density of 3.6 to 4.2 g / cm 3 , has a very high volume energy density, and the Co-O bond force is stronger than the Li-O bond, which helps Li + During the release and embedding of CoO2 interlayers, the layered structure of lithium cobalt oxide is not easy to collapse, thus ensuring that the material has good cycle stability and safety. However, since cobalt is an expensive metal, the preparation cost of lithium cobalt oxide positive electrode materials is relatively high, which limits its popularity in large-scale applications. As a positive electrode active material with a theoretical gram capacity equivalent to that of lithium cobalt oxide, the preparation cost of nickel-cobalt-manganese ternary materials is significantly lower than that of lithium cobalt oxide. Therefore, by doping nickel-cobalt-manganese ternary materials in positive electrode active materials, the cost of positive electrode materials can be effectively reduced. Moreover, since the actual compaction density of nickel-cobalt-manganese ternary materials is 3.4-3.8 g / cm 3 , slightly lower than lithium cobalt oxide. By adopting a combination design of lithium cobalt oxide and nickel-cobalt-manganese ternary materials, the positive electrode active material can have both high energy density and high cost performance, thereby reducing costs; however, the positive electrode protection additives commonly used in the electrolyte have a much lower binding ability with the nickel-cobalt-manganese ternary material than lithium cobalt oxide. Therefore, during the cycle, the nickel ions and manganese ions of the positive electrode active material cannot be well protected, causing the transition metal ions to dissolve into the negative electrode to react, destroying the interface film of the negative electrode, resulting in intensified side reactions of the electrolyte, and continuous deterioration of the battery's cycle performance. In addition, safety issues such as lithium plating and overcharging caused by high voltage and fast charging are still common.
[0014] Based on the above problems in the prior art, the present invention provides a battery, which includes a positive electrode and an electrolyte.
[0015] The electrolyte includes a fluoronitrile solvent; the fluoronitrile solvent is a fluoronitrile compound;
[0016] The positive electrode includes a positive electrode active material, which includes lithium cobalt oxide and a nickel-cobalt-manganese ternary material, wherein the mass content of the nickel element is k wt%, 0wt%<k wt%≤24wt%, based on the total mass of the positive electrode active material.
[0017] The electrolyte provided by the present invention includes the fluoronitrile solvent, which is a fluoronitrile compound. The compound structure has a carbon-nitrogen triple bond with a relatively high bond energy, and the introduction of fluorine atoms further enhances the electronic attraction of the nitrogen atom on the cyano group, making the carbon-nitrogen bond more solid and enhancing the polarity of the carbon-nitrogen triple bond, which can form a high-speed lithium ion solvation sheath with lithium ions, allowing lithium ions to be smoothly deintercalated under high voltage and high current conditions, and can also enhance the degree of electrochemical active site complexation reaction formed by the carbon-nitrogen triple bond and the metal ions on the surface of the positive electrode active material, thereby reducing the side reaction between the electrolyte and the active site, and reducing the nickel ion and manganese ion gold in the positive electrode active material under high voltage conditions. The dissolution of metal ions protects the stability of the positive electrode structure and avoids the destruction of the interface film of the negative electrode, thereby significantly improving the lithium plating problem of the battery core, so that the battery provided by the present invention can achieve high cycle performance; moreover, since the compound structure has a carbon-nitrogen triple bond with a high bond energy, its oxidation resistance and high voltage resistance are particularly strong, which can improve the voltage window of the electrolyte, and the electrolyte using fluoronitrile compounds has a wide temperature range, a high dielectric constant, and a high conductivity, and can better dissolve lithium salts and additives, so that the electrolyte has a high stability, and the high voltage resistance and high temperature resistance of the battery are also effectively improved, so that the lithium ion battery can simultaneously achieve high cycle performance and excellent overcharge resistance.
[0018] Furthermore, since the nickel element on the surface of the positive electrode active material has a stronger ability to bind to the fluoronitrile compound than the manganese element, by reasonably adjusting the content k wt% of the nickel element in the positive electrode active material, the degree of complexation reaction between the carbon-nitrogen triple bond in the fluoronitrile compound and the electrochemical active site formed by the metal ions on the surface of the positive electrode active material can be further improved, so that the metal ions and the fluoronitrile compound are more tightly bound, and the dissolution of the metal ions is reduced, so that the positive electrode active material mixed with the nickel-cobalt-manganese ternary material can be effectively protected by the fluoronitrile solvent, thereby further improving the battery's cycle performance and overcharge resistance.
[0019] In addition, the positive electrode active material can make the battery have high energy density and high cost performance by blending lithium cobalt oxide and nickel-cobalt-manganese ternary materials, thereby significantly reducing the cost of the battery.
[0020] In a specific embodiment, based on the total mass of the positive electrode active material, the mass content of nickel in the positive electrode active material is k wt%, 0wt%<k wt%≤24wt%. In a specific embodiment, k wt% can be 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt% or a range consisting of any two of these values. When the mass content k wt% of the nickel element is equal to 0, it is equivalent to that the positive electrode active material is basically all lithium cobalt oxide, and does not contain the mixed ternary material. Therefore, although the material has a high compaction density and a high volume energy density, its thermal stability is poor, and its overcharge resistance under high voltage and high current conditions is poor, and the preparation cost is high; when the mass content k wt% of the nickel element is greater than 24wt%, it means that the content of nickel element in the nickel-cobalt-manganese ternary material is high, which will cause some nickel ions that are not complexed by fluoronitrile compounds to dissolve into the negative electrode to react, destroy the interface film of the negative electrode, and cause the stability of the positive electrode active material to decrease, thereby causing the capacity loss of the battery cycle charge and discharge and the accelerated capacity decay under high temperature environment, affecting the capacity retention rate of the battery, and also causing the deterioration of the lithium precipitation problem of the battery core. Therefore, it is necessary to control the content k wt% of the nickel element in the positive electrode active material within a suitable range. In a preferred embodiment, 0wt% < k wt% ≤ 15wt%. In the present invention, the mass content of nickel in the positive electrode active material is measured by inductively coupled plasma emission spectrometry (ICP).
[0021] In the present invention, the positive electrode active material blended with lithium cobalt oxide and nickel cobalt manganese ternary material, in addition to reducing the material cost, the cobalt element in the nickel cobalt manganese ternary material can also prevent Li-Ni mixing, thereby improving the orderliness of lithium ion deintercalation, and the manganese element can maintain the stability of the structure of the positive electrode active material. The nickel element is the main force for the positive electrode active material to achieve high capacity, but the content of the above-mentioned transition metal elements should not be too much. Excessive cobalt elements will lead to a significant increase in the cost of the material and a decrease in gram capacity; excessive manganese and nickel elements are easily dissolved into the negative electrode to react. Therefore, by further adjusting the mass ratio between the elements in the positive electrode active material, the reversible specific capacity and cycle stability of the battery can be significantly improved, and the cost can be significantly reduced. In a specific embodiment, the mass ratio between the elements in the positive electrode active material is Ni:Co:Mn=(2~24):(0.5~8):(0.6~9). In a specific embodiment, Ni:Co:Mn can be 2:0.5:0.6, 2:0.5:9, 2:8:0.6, 2:8:9, 24:0.5:0.6, 24:0.5:9, 24:8:0.6, 24:8:9, 12:4.2:5. In a preferred embodiment, Ni:Co:Mn=(4-10):(1.2-3.6):(1.13-3.37).
[0022] In addition, in order to further improve the degree of complexation reaction and binding ability of fluoronitrile compounds in the electrolyte and metal ions in the nickel-cobalt-manganese ternary material, and solve the problem that fluoronitrile compounds cannot efficiently bind to manganese ions on the surface of the positive electrode active material, the average particle size of the primary particles (single crystal or polycrystalline) of the nickel-cobalt-manganese ternary material can be controlled within a certain range; because the small particles of the nickel-cobalt-manganese ternary material have a larger specific surface area, the contact area between the ternary material and the fluoronitrile compounds will be increased, effectively improving the degree of complexation reaction between the fluoronitrile compounds and the manganese ions, thereby strengthening the protective effect of the fluoronitrile solvent on the transition metal ions on the positive electrode surface, and further reducing the dissolution of manganese ions. In a specific embodiment, the average particle size Dv50 of the primary particles of the nickel-cobalt-manganese ternary material is 0.1μm to 6μm. In a specific embodiment, the average particle size of the primary particles of the nickel-cobalt-manganese ternary material can be 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm , 2μm, 2.2μm, 2.4μm, 2.6μm, 2.8μm, 3μm, 3.1μm, 3.3μm, 3.5μm, 3.7μm, 3.9μm, 4μm, 4.2μm, 4.4μm, 4.6μm, 4.8μm, 5μm, 5.1μm, 5.3μm, 5.5μm, 5.7μm, 5.9μm, 6μm or a range consisting of any two of these values. In a preferred embodiment, the average particle size Dv50 of the primary particles of the nickel-cobalt-manganese ternary material is 0.12μm to 3μm. In the present invention, the average particle size Dv50 of the primary particles of the nickel-cobalt-manganese ternary material can be obtained by observing the size of the particles using a scanning electron microscope (SEM).
[0023] In the present invention, based on the total mass of the electrolyte, the mass content of the fluoronitrile solvent is c wt%, 3wt%≤c wt%≤40wt%. In a specific embodiment, c wt% can be 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt% or a range consisting of any two of these values. When the mass content c wt% of the fluoronitrile solvent is less than 3wt%, it means that the content of the fluoronitrile solvent in the electrolyte is too low. After consuming part of the fluoronitrile solvent that participates in the complexing of transition metal ions on the surface of the positive electrode, it is no longer possible to efficiently transport a large amount of lithium ions under fast charging conditions, so that the lithium ions accumulate on the surface of the negative electrode, destroying the SEI film of the negative electrode, increasing the risk of internal short circuit of the battery, resulting in a decrease in battery safety, while accelerating electrode loss and reducing the capacity retention rate of the battery; and when the mass content c wt% of the fluoronitrile solvent is greater than 40wt%, the content of the fluoronitrile solvent is too high, the viscosity of the electrolyte increases, resulting in poor fluidity, which is not conducive to lithium ion transportation, and the problem of lithium precipitation is easy to occur during the deintercalation process. Therefore, by regulating the mass content c of the fluoronitrile solvent within a specific range, the occurrence of lithium precipitation can be further avoided, and the requirements of lithium ion batteries for high safety (such as furnace temperature and overcharge) and high cycle capacity retention rate under high voltage or fast charging conditions can be met; and by further regulating the mass content c of the fluoronitrile solvent wt%, can make the concentration of carbon-nitrogen triple bonds in fluoronitrile compounds reach an appropriate level, further enhance the complexation reaction effect with metal ions at electrochemical active sites, make the metal ions and fluoronitrile compounds more closely combined, further reduce the dissolution of metal ions, and improve the cycle performance and overcharge resistance of lithium-ion batteries using nickel-cobalt-manganese ternary materials mixed positive electrodes. In a preferred embodiment, 4wt%≤cwt%≤30wt%, and can be further preferably 4wt%≤cwt%≤20wt%.
[0024] In addition to the fluoronitrile solvent, the electrolyte of the present invention also includes other basic electrolyte solvents such as ethylene carbonate, propylene carbonate and carboxylic acid ester solvents.
[0025] In a specific embodiment, based on the total mass of the electrolyte, the mass content of the ethylene carbonate (EC) is w1 wt%, w1 wt%≤20wt%. In a specific embodiment, the mass content w1wt% of the ethylene carbonate can be 20wt%, 19wt%, 18wt%, 17wt%, 16wt%, 15wt%, 14wt%, 13wt%, 12wt%, 11wt%, 10wt%, 9wt%, 8wt%, 7wt%, 6wt%, 5wt%, 4wt%, 3wt%, 2wt%, 1wt%, 0wt% or a range consisting of any two of these values. The high dielectric constant ethylene carbonate and LiPF6 have a solvation-desolvation process, which can form a uniform and dense SEI film rich in organic-inorganic in the first charge and discharge, but the overly dense SEI film usually has a slightly larger impedance, which is not conducive to high current fast charging. Therefore, the amount of ethylene carbonate should not be too much, so it is necessary to control the mass content of ethylene carbonate within a suitable range. In a preferred embodiment, 0wt%≤w1wt%≤15wt%;
[0026] In a specific embodiment, based on the total mass of the electrolyte, the mass content of propylene carbonate (PC) is w2 wt%, w2 wt%≤20wt%. In a specific embodiment, the mass content w2wt% of propylene carbonate can be 20wt%, 19wt%, 18wt%, 17wt%, 16wt%, 15wt%, 14wt%, 13wt%, 12wt%, 11wt%, 10wt%, 9wt%, 8wt%, 7wt%, 6wt%, 5wt%, 4wt%, 3wt%, 2wt%, 1wt%, 0wt% or a range consisting of any two of these values. There is no solvation combination between propylene carbonate and lithium ions, but its high dielectric constant is usually used in combination with ethylene carbonate, which can significantly enhance the conductivity of the electrolyte and is conducive to high-rate charge and discharge. However, the mass content of propylene carbonate should not be too much, which will cause it to undergo continuous reduction and decomposition before the lithium insertion potential (~0.7V), and eventually cause the carbon material (such as graphite) in the negative electrode to collapse in structure and be unable to insert and extract lithium normally, thereby causing a decrease in the energy density of the battery and affecting the overall performance of the battery. Therefore, the mass content of propylene carbonate also needs to be controlled within an appropriate range. In a preferred embodiment, 0wt%≤w2 wt%≤15wt%;
[0027] In a specific embodiment, based on the total mass of the electrolyte, the mass content of the carboxylate solvent is w3 wt%, w3 wt%≤70wt%. In a specific embodiment, the mass content w3wt% of the carboxylate solvent can be 60wt%, 55wt%, 50wt%, 45wt%, 40wt%, 35wt%, 30wt%, 25wt%, 20wt%, 19wt%, 18wt%, 17wt%, 16wt%, 15wt%, 14wt%, 13wt%, 12wt%, 11wt%, 10wt%, 9wt%, 8wt%, 7wt%, 6wt%, 5wt%, 4wt%, 3wt%, 2wt%, 1wt%, 0wt% or a range consisting of any two of these values. Carboxylate solvents are excellent solvents that can dissolve lithium salts and various additives at room temperature and do not precipitate at low temperatures. In a preferred embodiment, 20wt%≤w3 wt%≤60wt%. In the present invention, the carboxylic acid ester solvent includes at least one of propyl propionate (PP), ethyl propionate (EP), ethyl acetate (EA) or ethyl butyrate (EB).
[0028] Further, as mentioned above, appropriately increasing the amount of fluoronitrile solvent in the electrolyte can enhance the degree of complexation reaction between the carbon-nitrogen triple bond in the fluoronitrile compound and the metal ions at the electrochemical active site, but too much fluoronitrile solvent will increase the viscosity of the electrolyte and reduce the fluidity, especially the free fluorine ions in the fluoronitrile solvent are easy to combine with the protons in the electrolyte to form Lewis acids that are easy to destroy the active substances on the positive electrode surface. Therefore, in order to maintain the fluidity of the electrolyte and at the same time ensure the protection of the transition metal on the positive electrode surface, in a specific embodiment, the mass content c wt% of the fluoronitrile solvent, the mass content k wt% of the nickel element and the mass content w3 wt% of the carboxylic acid ester solvent satisfy the relationship: 56≤0.1k+0.7c+w3≤70. Exemplarily, 0.1k+0.7c+w3 can be 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70. Among them, the mass content of carboxylate solvents refers to the total mass content of all carboxylate solvents in the electrolyte. For example, when the carboxylate solvents include propyl propionate and ethyl acetate, the mass content of the carboxylate solvents is equal to the sum of the mass content of propyl propionate and the mass content of ethyl acetate. By satisfying the above relationship, the metal ions in the positive electrode surface active material can be effectively protected by the fluoronitrile solvent, and the fluoronitrile solvent and the carboxylate solvent can be ensured to work at the same time, thereby enhancing the fluidity of the electrolyte, helping the lithium ion fluoronitrile solvent to transport lithium ions, and further improving the cycle performance of the battery. In a preferred embodiment, 58≤0.1k+0.7c+w3≤68.
[0029] In a specific embodiment, the fluoronitrile compound includes a fluorinated mononitrile compound, and the fluorinated mononitrile compound includes at least one of the following compounds:
[0030]
[0031]
[0032] Due to their specific structure, fluoronitrile compounds can also undergo solvation and desolvation with the lithium ions released from the positive electrode to form an SEI film. Moreover, because the molecular weight of fluorinated mononitrile compounds is low, they can transport lithium ions faster and more efficiently, and the degree of solvation with lithium ions is lighter, making it easier to desolvate, thereby forming a thin SEI film. Therefore, it can further reduce the occurrence of negative electrode side reactions, improve the problem of lithium plating in the battery cell, and enhance the battery's cycle performance and overcharge resistance.
[0033] Furthermore, in order to improve the problem of the binding ability of the fluoronitrile solvent with the metal ions in the nickel-cobalt-manganese ternary material, the electrolyte of the present invention may also include an additive A. The additive A can switch the coordination mode arbitrarily with the variable number and orientation of the ligand point, and can include one or more coordination sites starting from the phosphorus center, and has rich coordination connection capabilities, which is conducive to its full interaction with the metal ions. Moreover, the phosphorus-oxygen double bonds and / or phosphorus-nitrogen double bonds it possesses can make its structural skeleton more flexible and flexible, and can further enhance its degree of interaction with the metal ions. Therefore, by adding such additives to the electrolyte of the present invention, the effective binding of the electrolyte with the nickel, cobalt, and manganese ions in the nickel-cobalt-manganese ternary material is enhanced, and the dissolution of manganese ions and nickel ions in the nickel-cobalt-manganese ternary material is further inhibited, thereby avoiding the destruction of the interface film of the negative electrode; in addition, the additive method can also be used to supplement part of the positive electrode sites that are ignored by the fluoronitrile solvent due to the formation of an ionization sheath with lithium ions, thereby further enhancing the stability of the positive electrode active material.
[0034] In a specific embodiment, the additive A comprises at least one of the compounds represented by the following formula (I) and formula (II):
[0035]
[0036] Wherein, R1, R2, and R3 may be the same or different, and are independently selected from substituted or unsubstituted C1-C8 alkyl, substituted or unsubstituted C2-C5 alkenyl, substituted or unsubstituted C2-C4 alkynyl, substituted or unsubstituted C1-C8 alkoxy, wherein when substituted, the substituents are independently selected from phenyl, halogen, sulfur, phosphorus, silicon, methoxy, hydroxyl, carboxyl, aldehyde, carbonyl, and cyano; the compound represented by formula (I) has at least one carbon-nitrogen triple bond;
[0037]
[0038] Wherein, R4, R5, R6, R7, R8, and R9 may be the same or different, and are independently selected from substituted or unsubstituted C1-C8 alkyl, substituted or unsubstituted C2-C5 alkenyl, substituted or unsubstituted C2-C4 alkynyl, substituted or unsubstituted C1-C8 alkoxy, substituted or unsubstituted C6-C 12 The phenoxy group, when substituted, is independently selected from phenyl, halogen, sulfur, phosphorus, silicon, methoxy, hydroxyl, carboxyl, aldehyde, carbonyl, and cyano.
[0039] In a preferred embodiment, the additive A comprises at least one of the following compounds: cyclotriphosphazene, tris(cyanoethyl) phosphate, ethoxypentafluorocyclotriphosphazene, hexafluorocyclotriphosphazene, pentafluoro(phenoxy)cyclotriphosphazene.
[0040] In addition, in order to further enhance the protective effect of additive A on the surface metal ions of the positive electrode active material. In a specific embodiment, based on the total mass of the electrolyte, the mass content of the additive A is y wt%, 0.5wt%≤y wt%≤4.5wt%. In a specific embodiment, y wt% can be 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or a range consisting of any two of these values. When the mass content y wt% of additive A is less than 0.5wt%, the content of additive A is too low and cannot completely cover the transition metal on the surface of the positive electrode, which will cause the probability of additive A forming an effective combination with transition metal nickel, cobalt, and manganese ions to decrease, affecting the cycle stability of the battery; and when the mass content y wt% of additive A is greater than 4.5wt%, the content of additive A is too high, and the complex film formed at the positive electrode is thick, resulting in a large impedance between the electrodes, which is not conducive to the transmission of lithium ions and is prone to lithium precipitation problems in the battery core. In a preferred embodiment, 0.6 wt%≤y wt%≤2.5 wt%, and more preferably 0.8 wt%≤y wt%≤2 wt%. In the present invention, the mass content of the additive A can be obtained by liquid chromatography testing.
[0041] Furthermore, the fluoronitrile solvent and the additive A in the electrolyte can cooperate with each other to form a complex on the surface of the positive electrode active material to form a protective effect on the metal ions. Specifically, when the battery encounters external force majeure factors such as high temperature, overcharging, etc., a large amount of heat will be generated inside the battery, causing the positive electrode material to decompose and produce active oxygen, and the active oxygen produced by the decomposition will also react with the electrolyte to continue to generate a large amount of heat, thereby causing a sharp increase in heat inside the battery, generating more gas, and ultimately causing the battery to have a risk of gas explosion; and the electrolyte provided by the present invention, because it includes both the fluoronitrile solvent and the additive A, can cooperate with each other to form a complex on the surface of the positive electrode active material to form a protective effect on the metal ions, thereby further improving the high temperature resistance and overcharge resistance of the battery, mainly because the fluoronitrile solvent and the additive A both have a special nitrile structure, the fluoronitrile solvent contains a carbon-nitrogen triple bond, and the additive A contains Carbon-nitrogen triple bond and / or phosphorus-nitrogen triple bond, this kind of special nitrile structure can interact with the active material on the surface of the positive electrode as an electron pair donor and an electron docking acceptor respectively, and when the fluoronitrile solvent and additive A are simultaneously in the electrolyte, the nitrile structure in the additive A forms a protective layer in a point-to-point form, and the nitrile structure in the fluoronitrile solvent forms a protective layer in a face-to-face form, thereby synergistically improving the degree of complexation on the surface of the positive electrode active material, enhancing the protective effect of the fluoronitrile solvent and additive A on the surface of the positive electrode active material, so that the high temperature resistance and overcharge resistance of the battery are further effectively improved, and the additive A can further strengthen the protection of the transition metal nickel ions and manganese ions in the nickel-cobalt-manganese ternary material, thereby preventing the active oxygen in the positive electrode material from escaping under heating and being catalyzed by the dissolved transition metal ions, aggravating the side reactions in the electrolyte, and deteriorating the cycle performance of the battery.
[0042] In addition, in order to further enhance the synergistic effect between the fluoronitrile solvent and the additive A in the electrolyte. In a specific embodiment, based on the total mass of the electrolyte, the mass content c wt% of the fluoronitrile solvent and the mass content y wt% of the additive A satisfy the relationship of 4.8≤y+c≤43. In a specific embodiment, y+c can be 3.5, 4, 4.5, 5, 6, 7, 8, 9, 10, 13, 15, 17, 19, 21, 23, 25, 27, 29, 31, 33, 35, 37, 39, 41, 43 or a range consisting of any two of these values. In a preferred embodiment, 5≤y+c≤12.
[0043] In a specific embodiment, the nickel-cobalt-manganese ternary material includes LiNi 0.3 Co 0.3 Mn 0.3 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi0.5 Co 0.3 Mn 0.2 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.6 Mn 0.3 Co 0.1 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.9 Co 0.05 Mn 0.05 At least one of O2.
[0044] In a specific embodiment, the positive electrode active material also includes at least one of the following doped metals: Mg, Al, W, Zn, Ca, Fe, Ba, Sr, B, Cr, V, Zr, Ti, Sn, Mo, Ru, Si, Sb, Nb, Te.
[0045] In a specific embodiment, the gram capacity of the positive electrode active material is 170 mAh / g to 195 mAh / g. Exemplarily, the gram capacity of the positive electrode active material can be 170 mAh / g, 175 mAh / g, 180 mAh / g, 185 mAh / g, 190 mAh / g, 195 mAh / g.
[0046] In one embodiment, the compaction density of the positive electrode active material is 2.8 g / cm 3 ~4.8g / cm 3 For example, the compaction density of the positive electrode active material may be 2.8 g / cm 3 , 3g / cm 3 、3.2g / cm 3 、3.4g / cm 3 、3.6g / cm 3 、3.8g / cm 3 、3.9g / cm 3 , 4g / cm 3 , 4.1g / cm 3 , 4.2g / cm 3 , 4.25g / cm 3 , 4.3g / cm 3 4.4g / cm 3 , 4.5g / cm 3 , 4.7g / cm 3 , 4.8g / cm 3 In a preferred embodiment, the compaction density of the positive electrode active material is 3.8 g / cm 3~4.25g / cm 3 .
[0047] The battery of the present invention includes a separator and a negative electrode in addition to a positive electrode and an electrolyte. The other constituent materials of the positive electrode except the materials described above can refer to conventional positive and negative electrodes in the art.
[0048] According to the battery of the present invention, the negative electrode includes a negative electrode active material, and the negative electrode active material includes a carbon-based negative electrode material.
[0049] In a specific embodiment, the carbon-based negative electrode material includes at least one of artificial graphite, natural graphite, mesophase carbon microbeads, hard carbon, and soft carbon.
[0050] According to the lithium ion battery of the present invention, the negative electrode active material may further include a silicon-based negative electrode material.
[0051] In a specific embodiment, the silicon-based negative electrode material includes at least one of a silicon-oxygen negative electrode material or a silicon-carbon negative electrode material, such as Si, SiC, SiO x (0 <x<2)。
[0052] According to the battery of the present invention, the separator may also be a separator conventionally used in the art, such as a PP film, a PE film, and the like.
[0053] The battery of the present invention can be prepared by conventional methods in the art. Specifically, the positive electrode, the separator and the negative electrode can be stacked in sequence, and then a battery cell can be obtained through a lamination or winding process, and then the above-mentioned battery can be obtained through baking, liquid injection, formation, packaging and other processes.
[0054] Hereinafter, the positive electrode sheet and the lithium-ion battery provided by the present invention are described in detail through specific embodiments.
[0055] Example 1
[0056] The lithium ion battery of the present invention is obtained by the following method:
[0057] Preparation of electrolyte
[0058] The electrolyte material of the present invention is obtained in the following manner:
[0059] In a glove box (H2O<0.01ppm, O2<0.01ppm, Ar atmosphere), EC w1 (wt%), PC w2 (wt%), PP w3 (wt%) and fluoronitrile solvent c (wt%) of fluoronitrile compound (compound (2)) based on the total mass of the electrolyte are added and mixed evenly, and then fully dried lithium hexafluorophosphate (LiPF6) is added thereto. After dissolution, additive A (tricyanoethyl phosphate) with a content of y (wt%) based on the total mass of the electrolyte is added and stirred evenly. After passing the moisture and free acid tests, the desired electrolyte is obtained.
[0060] Cathode sheet preparation
[0061] Weigh the prepared positive electrode active material (lithium cobalt oxide LiCoO2: nickel cobalt manganese ternary material LiNi 0.6 Mn 0.3 Co 0.1 =8:2, wherein Ni:Co:Mn=6.5:3.6:1.15, and the mass content of nickel element is 10wt%), conductive agent Super P, and binder polyvinylidene fluoride (PVDF) are dispersed in an appropriate amount of N-methylpyrrolidone (NMP) in a weight ratio of 97:2:1, and are fully stirred to form a uniform positive electrode slurry. The positive electrode slurry is coated on the positive electrode current collector aluminum foil, and then dried, rolled, and cut to obtain a positive electrode sheet.
[0062] Negative electrode preparation
[0063] The prepared artificial graphite, conductive agent Super P, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) were weighed in a weight ratio of 97:1:1.5:0.5, dispersed in an appropriate amount of deionized water, and fully stirred to form a uniform negative electrode slurry. The negative electrode slurry was coated on the negative electrode current collector copper foil, and then dried, rolled, and cut to obtain a negative electrode sheet.
[0064] The positive electrode, negative electrode and separator are wound into a core according to a predetermined process, and then the pole ears are welded, the electrolyte is injected, and vacuum sealing, standing, forming and other processes are carried out to prepare a lithium-ion battery.
[0065] Example 2 Group
[0066] The lithium-ion batteries of the second embodiment were all manufactured by the method of the first embodiment, except that the mass content of the fluoronitrile compound in the electrolyte was changed by c wt %, as shown in Table 1.
[0067] Example 3 Group
[0068] The lithium-ion batteries of the third embodiment were all manufactured by the method of the first embodiment, except that the type of the fluoronitrile compound in the electrolyte was changed, specifically:
[0069] In Example 3-1, the fluoronitrile compound is compound (4);
[0070] In Example 3-2, the fluoronitrile compound is compound (6);
[0071] In Example 3-3, the fluoronitrile compound is compound (9);
[0072] In Example 3-4, the fluoronitrile compound is compound (15);
[0073] In Example 3-5, the fluoronitrile compound is compound (17).
[0074] Example 4 Group
[0075] The lithium-ion batteries of the fourth embodiment were all manufactured by the method of the first embodiment, except that the mass content of the additive A was changed by y wt %, as shown in Table 1.
[0076] Example 5 Group
[0077] The lithium ion batteries of the fifth embodiment were all manufactured by the method of the first embodiment, except that the type of additive A was changed, specifically:
[0078] In Example 5-1, the additive A is cyclotriphosphazene;
[0079] In Example 5-2, the additive A is ethoxy pentafluorocyclotriphosphazene;
[0080] In Example 5-3, the additive A is hexafluorocyclotriphosphazene;
[0081] In Example 5-4, the additive A is pentafluoro(phenoxy)cyclotriphosphazene.
[0082] Example 6 Group
[0083] The lithium-ion batteries of the Example 6 group were all manufactured by the method of the Example 1, except that the ratio of lithium cobalt oxide to nickel-cobalt-manganese ternary material in the positive electrode active material was changed, thereby changing the mass content k wt % of the nickel element. For details, see Table 1.
[0084] Example 7 Group
[0085] The lithium-ion batteries of the embodiment 7 group were all manufactured by the method of the embodiment 1, except that the average particle size Dv50 of the primary particles of the ternary material was changed, specifically:
[0086] In Example 7-1, the average particle size Dv50 of the primary particles of the ternary material was changed to 0.12 μm;
[0087] In Example 7-2, the average particle size Dv50 of the primary particles of the ternary material is changed to 3 μm;
[0088] Example 7-3, the average particle size Dv50 of the primary particles of the ternary material is changed to 0.1 μm;
[0089] Example 7-4, the average particle size Dv50 of the primary particles of the ternary material is changed to 6 μm;
[0090] In Example 7-5, the average particle size Dv50 of the primary particles of the ternary material is changed to 8 μm.
[0091] Example 8 Group
[0092] The lithium-ion batteries of the Example 8 group were all manufactured by the method of the Example 1, except that the specific selection of the nickel-cobalt-manganese ternary material in the positive electrode active material was changed, specifically:
[0093] Example 8-1, the nickel-cobalt-manganese ternary material is LiNi 0.8 Co 0.1 Mn 0.1 O2, wherein Ni:Co:Mn=8.4:1.3:1.14;
[0094] Example 8-2, the nickel-cobalt-manganese ternary material is LiNi 0.5 Co 0.2 Mn 0.3 O2, wherein Ni:Co:Mn=5.5:2.4:3.23;
[0095] Example 8-3, the nickel-cobalt-manganese ternary material is LiNi 0.9 Co 0.05 Mn 0.05 O2, wherein Ni:Co:Mn=9.67:0.73:0.65;
[0096] Example 8-4, the nickel-cobalt-manganese ternary material is LiNi 0.3 Co 0.3 Mn 0.3 O2, among which Ni:Co:Mn=3.91:3.85:3.56.
[0097] Example 9
[0098] The lithium ion batteries of Example 9 are all manufactured by the method of Example 1, except that the additive A is not added. For details, see Table 1.
[0099] Comparative Examples 1-2
[0100] The lithium ion batteries of Comparative Examples 1-2 were manufactured using the method of Example 1, except that the ratio of lithium cobalt oxide to nickel-cobalt-manganese ternary material in the positive electrode active material was changed, thereby changing the mass content k wt % of the nickel element. For details, see Table 1.
[0101] Comparative Example 3
[0102] The lithium ion battery of Comparative Example 3 is manufactured by the method of Example 1, except that no fluoronitrile compound and additive A are added to the electrolyte. For details, see Table 1.
[0103] Table 1
[0104]
[0105]
[0106] Lithium-ion battery test example
[0107] The lithium ion batteries obtained in the above examples and comparative examples were tested by the following method, and the test results are recorded in Table 2:
[0108] Performance parameter test methods:
[0109] (1) 25℃ battery dissection and lithium deposition test
[0110] Place the lithium-ion battery at 25°C, charge it to the upper limit voltage (4.5V) at 1.5C constant current, then charge it to 0.05C at 4.5V constant voltage, and let it stand for 5 minutes; then discharge it to 3V at 1C constant current, and let it stand for 5 minutes. This is a charge and discharge cycle. After charging / discharging for a certain number of times, dissect the battery cell after it is removed from the stage, observe the state of the negative electrode surface, and determine whether lithium is deposited. The situations are divided into the following categories: no lithium deposition (there is no lithium deposition on the surface of the negative electrode sheet, the top and bottom, the arc, and the junction of the single and double sides), slight lithium deposition (there is lithium deposition only on the top and bottom of the negative electrode sheet), local lithium deposition (there is obvious lithium deposition at any of the top and bottom of the negative electrode sheet, the arc, and the junction of the single and double sides) and severe lithium deposition (lithium deposition occurs on the entire surface of the negative electrode sheet).
[0111] (2) 25℃ cycle test
[0112] Place the lithium-ion battery at 25°C, charge it to the upper limit voltage (4.5V) at 1C constant current, then charge it to 0.05C at 4.5V constant voltage, and let it stand for 5 minutes; then discharge it to 3V at 0.5C constant current, and let it stand for 5 minutes. This is a charge and discharge cycle. After charging / discharging in this way, record the capacity retention rate / % of the lithium-ion battery after 1000T cycle.
[0113] (3) 25℃ overcharge test
[0114] At 25℃±5℃, discharge at 0.2C to the lower limit voltage, let it stand for 2min, then charge at 0.7C constant current and constant voltage to the upper limit voltage, let it stand for 10min, and charge at 18.5V constant voltage for 40h. After the test, observe whether the battery surface has fire or explosion. If there is no fire or explosion, it means it has passed. Test 20 times and calculate the 25℃ overcharge test pass rate / %.
[0115] (4) Furnace temperature test
[0116] Under 25℃±5℃ environment, stand for 10min, discharge at 0.2C to the lower limit voltage; stand for 10min, charge at 0.7C to the upper limit voltage. Place the fully charged batteries prepared in the above embodiments and comparative examples in an oven, and heat them at a temperature rise rate of 5±2℃ / min. When the temperature in the box reaches 130℃±2℃, keep the temperature constant for 60min. After the test, observe whether there is fire or explosion on the surface of the battery. If there is no fire or explosion, it means it has passed. Test 20 times and calculate the pass rate of the oven temperature test.
[0117] Table 2
[0118]
[0119]
[0120] From the analysis of Table 1 and Table 2, it can be seen that the battery prepared in the embodiment of the present invention can significantly improve the problem of lithium plating in the battery cell compared with the battery prepared in the comparative example, and has high cycle stability, high overcharge resistance and excellent safety performance; in addition, the battery prepared in the present invention is composed of a mixture of lithium cobalt oxide and nickel-cobalt-manganese ternary materials, which can also significantly reduce material costs and has broader application prospects.
[0121] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A battery comprising a positive electrode and an electrolyte, It is characterized in that The electrolyte includes a fluoronitrile solvent; the fluoronitrile solvent is a fluoronitrile compound; The positive electrode includes a positive electrode active material, which includes lithium cobalt oxide and a nickel-cobalt-manganese ternary material, wherein the mass content of the nickel element is k wt%, 0wt%<k wt%≤24wt%, based on the total mass of the positive electrode active material.
2. The battery according to claim 1, in, The mass ratio of each element in the positive electrode active material is Ni:Co:Mn=(2-24):(0.5-8):(0.6-9), Preferably, Ni:Co:Mn=(4-10):(1.2-3.6):(1.13-3.37).
3. The battery according to claim 1, in, The average particle size Dv50 of the primary particles of the nickel-cobalt-manganese ternary material is 0.1 μm to 6 μm, preferably 0.12 μm to 3 μm.
4. The battery according to claim 1, in, Based on the total mass of the electrolyte, the mass content of the fluoronitrile solvent is c wt%, 3wt%≤c wt%≤40wt%; And / or, based on the total mass of the positive electrode active material, the mass content of the nickel element is k wt%, 0wt%<k wt%≤15wt%.
5. The battery according to claim 4, in, The electrolyte satisfies at least one of the conditions (a) to (c): (a) The electrolyte comprises ethylene carbonate, and the mass content of the ethylene carbonate is w based on the total mass of the electrolyte. 1 wt%,w 1 wt%≤20wt%, preferably, 0wt%≤w 1 wt%≤15wt%; (b) The electrolyte includes propylene carbonate, and the mass content of the propylene carbonate is w based on the total mass of the electrolyte. 2 wt%,w 2 wt%≤20wt%, preferably, 0wt%≤w 2 wt%≤15wt%; (c) The electrolyte includes a carboxylic acid ester solvent, and the mass content of the carboxylic acid ester solvent is w based on the total mass of the electrolyte. 3 wt%,w 3 wt%≤70wt%, preferably, 20wt%≤w 3 wt%≤60wt%; Preferably, the mass content of the fluoronitrile solvent is c wt%, the mass content of the nickel element is k wt%, and the mass content of the carboxylic acid ester solvent is w 3 wt%, satisfying the relationship: 56≤0.1k+0.7c+w 3 ≤70.
6. The battery according to claim 1, in, The fluoronitrile compound includes a fluorinated mononitrile compound, and the fluorinated mononitrile compound includes at least one of the following compounds: H 3 C—CN(1), 7. The battery according to claim 4, in, The electrolyte includes an additive A, and the additive A includes at least one of the compounds represented by the following formula (I) and formula (II): Among them, R 1 , R 2 , R 3 may be the same or different and are independently selected from substituted or unsubstituted C 1 -C 8 Alkyl, substituted or unsubstituted C 2 -C 5 Alkenyl, substituted or unsubstituted C 2 -C 4 Alkynyl, substituted or unsubstituted C 1 -C 8 wherein, when substituted, the substituents are independently selected from phenyl, halogen, sulfur, phosphorus, silicon, methoxy, hydroxyl, carboxyl, aldehyde, carbonyl, and cyano; the compound represented by formula (I) has at least one carbon-nitrogen triple bond; Among them, R 4 , R 5 , R 6 , R 7 , R 8 , R 9 may be the same or different and are independently selected from substituted or unsubstituted C 1 -C 8 Alkyl, substituted or unsubstituted C 2 -C 5 Alkenyl, substituted or unsubstituted C 2 -C 4 Alkynyl, substituted or unsubstituted C 1 -C 8 Alkoxy, substituted or unsubstituted C 6 -C 12 phenoxy, wherein, when substituted, the substituents are each independently selected from phenyl, halogen, sulfur, phosphorus, silicon, methoxy, hydroxyl, carboxyl, aldehyde, carbonyl, and cyano; Preferably, the additive A comprises at least one of the following compounds: cyclotriphosphazene, tris(cyanoethyl) phosphate, ethoxypentafluorocyclotriphosphazene, hexafluorocyclotriphosphazene, pentafluoro(phenoxy)cyclotriphosphazene.
8. The battery according to claim 7, in, Based on the total mass of the electrolyte, the mass content of the additive A is y wt%, 0.5 wt%≤y wt%≤4.5 wt%; Preferably, based on the total mass of the electrolyte, the mass content c wt % of the fluoronitrile solvent and the mass content y wt % of the additive A satisfy the relationship 4.8≤y+c≤43.
9. The battery according to claim 1, in, The nickel-cobalt-manganese ternary material includes LiNi 0.3 Co 0.3 Mn 0.3 O 2 、LiNi 0.5 Co 0.2 Mn 0.3 O 2 、LiNi 0.5 Co 0.3 Mn 0.2 O 2 、LiNi 0.6 Co 0.2 Mn 0.2 O 2 、LiNi 0.6 Mn 0.3 Co 0.1 O 2 、LiNi 0.8 Co 0.1 Mn 0.1 O 2 、LiNi 0.9 Co 0.05 Mn 0.05 O 2 At least one of; And / or, the positive electrode active material also includes at least one of the following doped metals: Mg, Al, W, Zn, Ca, Fe, Ba, Sr, B, Cr, V, Zr, Ti, Sn, Mo, Ru, Si, Sb, Nb, Te.
10. The battery according to claim 1, in, The gram capacity of the positive electrode active material is 170 mAh / g to 195 mAh / g; And / or, the compaction density of the positive electrode active material is 2.8 g / cm 3 ~4.8g / cm 3 .
Citation Information
Patent Citations
Electrolyte and lithium-ion battery
CN109888383A
Preparation method of high-safety high-voltage electrolyte containing nitrile compounds
CN114400379A
High-voltage electrolyte suitable for fast-charging lithium battery and lithium battery
CN116799300A
Nonaqueous electrolytic solution secondary battery and nonaqueous electrolytic solution for use in the same
JP2003007336A
Nonaqueous electrolyte and lithium ion secondary battery
JP2015118852A
Cited By
Battery
WO2026001679A1
Nonaqueous electrolyte and lithium secondary battery comprising same
WO2026106235A1