Polyurethane adhesive and preparation method thereof
By introducing flame-retardant microcapsules and modified isocyanates into the polyurethane adhesive, a polyurethane adhesive with excellent anti-ultraviolet and flame retardant properties is formed, which solves the problems of insufficient anti-ultraviolet aging performance and poor antibacterial properties in the prior art, and achieves safety and environmental protection Adhesive applications.
Patent Information
- Application Number
- CN202411215142.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In use, existing polyurethane adhesives have problems such as insufficient anti-ultraviolet aging performance, poor antibacterial properties and organic solvent emissions, especially in the medical and food processing fields.
Polyurethane adhesives of component A and component B are used, wherein component A is obtained by reacting polyester polyol, polyether polyol and 4,4-diphenylmethane diisocyanate, and component B is obtained by toluene diisocyanate and modified isocyanate. It consists of flame retardant microcapsules. The flame retardant microcapsules are made of polyurethane prepolymer as the wall material and ammonium polyphosphate as the core material. Nano calcium carbonate and quaternary ammonium structurally modified isocyanate participate in the reaction, forming excellent UV resistance and flame retardant properties. Adhesive.
It improves the UV aging resistance, flame retardant properties and antibacterial properties of polyurethane adhesives. It is suitable for special occasions and does not require the addition of small molecule antibacterial agents, avoiding organic solvent emissions.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of adhesives, and in particular to a polyurethane adhesive and a preparation method thereof. Background Art
[0002] Polyurethane adhesives contain highly polar and chemically active carbamate and isocyanate groups, so they have excellent chemical adhesion to smooth surfaces of materials containing active hydrogen, such as paper, plastics, and metals. Solvent-based polyurethane adhesives will cause a large amount of organic solvent emissions, which are flammable and explosive, not only polluting the air, but also having adverse effects on people's health. In recent years, with the rapid development of science and technology and the deepening and strengthening of people's environmental protection awareness, the call for the use of safer, more environmentally friendly and efficient adhesive products has become increasingly strong.
[0003] Two-component waterborne polyurethane adhesives are more outstanding in the adhesive field because of their advantages such as safety, environmental protection and high quality. Two-component waterborne polyurethane is mainly composed of a waterborne polyol component (component A) containing hydroxyl (OH) and a polyisocyanate component (component B) containing isocyanate groups (NCO) in combination with some other special-purpose additives. Components A and B are packaged separately. Mix the two components evenly before use. By adjusting the ratio of components A and B, the strength, curing time and other properties of the polyurethane material can be changed. Additives include desiccants, flame retardants, coupling agents, antioxidants, UV inhibitors, colorants, adhesion promoters, fillers, plasticizers, etc.
[0004] The patent with application number 202110699008.1 discloses a bio-based flame retardant microcapsule and a preparation method thereof. The modified microcapsule uses a bio-based expanded phosphorus-nitrogen synergistic flame retardant as the core material and an intrinsically flame-retardant modified polyurethane as the wall material to prepare flame-retardant microcapsules with flame-retardant properties in both the core and the core. However, the following shortcomings still exist: Although the intrinsically flame-retardant modified polyurethane used as the wall material enhances the flame retardant properties of the polymer, the anti-ultraviolet aging properties of the polymer are not mentioned, which is not conducive to the storage and use of the microcapsules. When polyurethane adhesives are used in medical, food processing and other fields, antibacterial properties become an important performance indicator. Commonly used inorganic nanoparticles are used as reinforcing fillers and are directly added to polymers to enhance the mechanical properties of adhesives. They have problems such as poor compatibility with polymers and easy self-agglomeration. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a polyurethane adhesive and a preparation method thereof.
[0006] The purpose of the present invention can be achieved through the following technical solutions: A polyurethane adhesive comprises a component A and a component B, wherein the molar ratio of the OH functional group of the component A to the NCO functional group of the component B is 1:1.3-1.7; Component A includes 100 parts of polyester polyol, 50-60 parts of polyether polyol, 10-20 parts of 4,4-diphenylmethane diisocyanate, and 1-3 parts of molecular sieve; component B includes 90 parts of toluene diisocyanate, 50-60 parts of polyether polyol, 10 parts of modified isocyanate, and 10-12 parts of flame retardant microcapsules; the molecular weight of the polyester polyol is 2000-3000, and the average functionality is 2-3; the polyether polyol is polypropylene glycol 600, and the molecular sieve is 3A type molecular sieve; The preparation of the polyurethane adhesive comprises the following steps: Step S1: Add polyester polyol and polyether polyol to a reaction kettle, stir at 110° C. under vacuum for 2 h, cool to 50° C., then add 4,4-diphenylmethane diisocyanate under stirring, heat to 80-90° C. and stir for 4-5 h, then add molecular sieves and stir under vacuum for 30-40 min to obtain component A; Step S2: Add polyether polyol to a reaction kettle, stir at 110° C. under vacuum for 1 hour, cool to 50° C., then add toluene diisocyanate and modified isocyanate under stirring, heat to 80-90° C. and stir to react for 3-4 hours, then add flame retardant microcapsules and stir under vacuum for 25-35 minutes to obtain component B; Step S3: Package component A and component B in double tubes, add components A and B into a reaction kettle and stir for 1-2 hours before use to obtain a polyurethane adhesive.
[0007] The flame retardant microcapsules are prepared by the following steps: Step A1: Add ethyl 3-butenylphosphine carboxylate to dichloromethane, start stirring, then add 3-chloroperbenzoic acid, and stir at room temperature for 4-5 hours to obtain an epoxy product; Further, the usage ratio of 3-butenylphosphine carboxylic acid ethyl ester, dichloromethane and 3-chloroperoxybenzoic acid is 0.1 mol: 80-90 mL: 0.1 mol; During the reaction of step A1, the carbon-carbon double bond in ethyl 3-butenylphosphinothric acid ester is oxidized to an epoxy group to obtain an epoxy product; Step A2: In a nitrogen atmosphere, add thiophene-2,4-dicarboxylic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 8-10h, then heat to 110-120°C, stir for 1-2h to obtain diol; Further, the ratio of thiophene-2,4-dicarboxylic acid, toluene, pyridine and epoxy product is 0.1 mol: 150-160 mL: 0.010-0.015 mol: 0.1 mol; During the reaction of step A2, the carboxyl group of thiophene-2,4-dicarboxylic acid reacts with the epoxy group of the epoxy product to form a diol containing a phosphoric acid ester and a thiophene ring; Step A3: Stir polyethylene glycol 600 at 110° C. under vacuum for 1-2 hours for later use; add toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dimethylol propionic acid to a reaction bottle in a nitrogen atmosphere; stir and react at 80-85° C. for 4-6 hours to obtain the wall material; add ammonium polyphosphate to 1,4-dioxane and stir for 10-15 minutes to obtain dispersion 1; then add the wall material to 1,4-dioxane and stir for 30-35 minutes to obtain dispersion 2; then add dispersion 1 to dispersion 2, stir for 10 minutes, add dibutyltin dilaurate, stir and react at 80° C. for 4-5 hours to obtain flame retardant microcapsules; Further, the dosage ratio of toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dimethylol propionic acid is 10-20g: 10-15g: 9-11g: 4-6g; the dosage ratio of ammonium polyphosphate and 1,4-dioxane is 1g: 5-7mL; the dosage ratio of wall material and 1,4-dioxane is 1g: 10-14mL; the dosage ratio of dispersion 1, dispersion 2 and dibutyltin dilaurate is 6-8mL: 15-20mL: 0.02-0.04g; In the reaction process of step A3, toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dimethylol propionic acid are reacted to generate polyurethane prepolymer as wall material, ammonium polyphosphate as core material, and the wall material is coated with the core material to obtain flame retardant microcapsules.
[0008] The modified isocyanate is prepared by the following steps: Step B1: Add 2-(4-methylpiperidinyl)-5-nitroaniline, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution 1, then add succinyl dichloride to dimethyl sulfoxide to obtain a mixed solution 2, slowly dropwise add the mixed solution 2 into the mixed solution 1 in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, and stir the mixture at constant temperature for 10 hours to obtain an amide product; Further, the usage ratio of 2-(4-methylpiperidinyl)-5-nitroaniline, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.015 mol: 50-60 mL; the usage ratio of succinyl dichloride and dimethyl sulfoxide is 0.1 mol: 30-40 mL; the usage ratio of mixed solution 1 and mixed solution 2 is 55-65 mL: 35-45 mL; During the reaction of step B1, the amino group of 2-(4-methylpiperidinyl)-5-nitroaniline reacts with succinyl dichloride to generate an amide product containing a tertiary amino group and a nitro group; Step B2: Add nano-calcium carbonate to anhydrous ethanol, add bromobutyltrimethoxysilane and sulfuric acid solution, heat to 30°C, stir and react for 4-5h to obtain surface-modified nano-calcium carbonate; put the amide product and ethanol in a flask, start stirring, then add the surface-modified nano-calcium carbonate, heat to 50-60°C, stir and react at constant temperature for 10-12h, recrystallize with acetone after rotary evaporation, and filter to obtain quaternary ammonium salt; Further, the dosage ratio of nano-calcium carbonate, anhydrous ethanol, bromobutyltrimethoxysilane and sulfuric acid solution is 10g: 50-60mL: 5-7g: 10-12mL, and the concentration of sulfuric acid solution is 0.5mol / L; the dosage ratio of amide product, ethanol and surface-modified nano-calcium carbonate is 56-60g: 135-145mL: 15-16g, and the volume fraction of ethanol is 95%; In the reaction process of step B2, silanol obtained by hydrolysis of bromobutyltrimethoxysilane reacts with hydroxyl groups on the surface of nano-calcium carbonate to obtain surface-modified nano-calcium carbonate; tertiary amine groups of the amide product react with bromine atoms of the surface-modified nano-calcium carbonate to generate quaternary ammonium salt containing nano-calcium carbonate and nitro groups; Step B3: Add quaternary ammonium salt and ethyl acetate to a three-necked flask, heat to 45-55°C, start reflux stirring, then add sodium dithionite, and reflux stirring to react for 1-1.5h to obtain aromatic primary amine; add xylene to a four-necked flask, pass nitrogen, add aromatic primary amine and triphosgene at 75°C, and after the addition is complete, heat to 125°C and continue to react for 3.5h to obtain modified isocyanate; Further, the usage ratio of quaternary ammonium salt, ethyl acetate, and sodium dithionite is 58-62 g: 150-160 mL: 20-25 g; the usage ratio of xylene, aromatic primary amine, and triphosgene is 220 mL: 63-65 g: 40-45 g; During the reaction of step B3, the nitro group in the quaternary ammonium salt is reduced to an amino group to obtain an aromatic primary amine; the amino group of the aromatic primary amine reacts with triphosgene to generate chloroamide, which is then heated to dehydrochlorinate to generate a modified isocyanate.
[0009] Beneficial effects of the invention: The invention discloses a polyurethane adhesive, comprising component A and component B, wherein component A is obtained by adding a molecular sieve to an OH-terminated product obtained by reacting a polyester polyol, a polyether polyol and 4,4-diphenylmethane diisocyanate; and component B is formed by adding a flame-retardant microcapsule to an NCO-terminated product obtained by reacting toluene diisocyanate, a polyether polyol and a modified isocyanate.
[0010] The flame retardant microcapsules are obtained by coating an essential polyurethane prepolymer as a wall material with ammonium polyphosphate as a core material. The essential polyurethane prepolymer is obtained by reacting toluene diisocyanate, polyethylene glycol 600, diol and the like. The diols including thiophene ring and phosphate structure are added to the molecular chain of the intrinsic polyurethane prepolymer through chain extension reaction with toluene diisocyanate, etc. When exposed to ultraviolet rays, the thiophene ring can effectively absorb ultraviolet energy and convert it into lower-energy heat energy for release, thereby reducing the damage caused by ultraviolet rays; when burning, the phosphate structure decomposes, and the generated acetal and gaseous phosphate free radicals react with oxygen molecules in the air to form phosphate oxides that cover the surface, isolate oxygen, and thus inhibit continued combustion; therefore, the use of diols enhances the ultraviolet resistance and flame retardancy of the flame retardant microcapsule wall material, facilitates the storage and transportation of the flame retardant microcapsules, and also enhances the ultraviolet aging resistance and flame retardancy of component B. The flame retardant microcapsules are more evenly dispersed in the polyurethane adhesive due to the polyurethane structure in their wall material, thereby making the polyurethane adhesive have excellent ultraviolet resistance and flame retardancy.
[0011] The modified isocyanate contains nano calcium carbonate and quaternary ammonium salt structure. After the surface of the nano calcium carbonate is modified, its compatibility with the matrix is increased and it is not easy to agglomerate. The modified isocyanate is grafted into the molecular chain of component B through the reaction of the modified isocyanate with polyether polyol, etc., which is more conducive to improving the mechanical properties of the polyurethane adhesive formed by components B and A. When bacteria come into contact with the adhesive containing the quaternary ammonium salt, the negatively charged bacteria will be attracted by the cations on its surface, resulting in the restriction of the freedom of movement of the bacteria, which inhibits the respiratory function of the bacteria. The quaternary ammonium salt structure is grafted into the molecular chain of component B through the reaction of the modified isocyanate with polyether polyol, etc., which avoids the lack of antibacterial persistence caused by the addition of small molecule antibacterial agents, is more conducive to improving the antibacterial property of the polyurethane adhesive, and can be applied to special occasions. Therefore, the modified isocyanate is used to enhance the mechanical properties and antibacterial property of the polyurethane adhesive. DETAILED DESCRIPTION
[0012] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0013] Embodiment 1: A flame retardant microcapsule, the preparation of which comprises the following steps: Step A1: Add ethyl 3-butenylphosphinothioate to dichloromethane, start stirring, then add 3-chloroperbenzoic acid, and stir at room temperature for 4 hours to obtain an epoxy product; the amount ratio of ethyl 3-butenylphosphinothioate, dichloromethane and 3-chloroperbenzoic acid is 0.1 mol: 80 mL: 0.1 mol; Step A2: In a nitrogen atmosphere, add thiophene-2,4-dicarboxylic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 8-10h, then heat to 110°C, stir for 1h to obtain diol; the amount ratio of thiophene-2,4-dicarboxylic acid, toluene, pyridine and epoxy product is 0.1mol:150mL:0.010mol:0.1mol; Step A3: Stir polyethylene glycol 600 at 110°C under vacuum for 1 hour for later use; add toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dimethylol propionic acid to a reaction bottle in a nitrogen atmosphere, and stir and react at 80°C for 4 hours to obtain the wall material; add ammonium polyphosphate to 1,4-dioxane and stir for 10 minutes to obtain dispersion 1; then add the wall material to 1,4-dioxane and stir for 30 minutes to obtain dispersion 2; then add dispersion 1 to dispersion 2 and stir for 10 minutes After that, dibutyltin dilaurate was added, and the reaction was stirred at 80°C for 4 hours to obtain flame retardant microcapsules; the dosage ratio of toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dihydroxymethylpropionic acid was 10g:10g:9g:4g; the dosage ratio of ammonium polyphosphate and 1,4-dioxane was 1g:5mL; the dosage ratio of wall material and 1,4-dioxane was 1g:10mL; the dosage ratio of dispersion 1, dispersion 2 and dibutyltin dilaurate was 6mL:15mL:0.02g.
[0014] Embodiment 2: A flame retardant microcapsule, the preparation of which comprises the following steps: Step A1: Add ethyl 3-butenylphosphine carboxylate to dichloromethane, start stirring, then add 3-chloroperbenzoic acid, and stir at room temperature for 4.5 hours to obtain an epoxy product; the amount ratio of ethyl 3-butenylphosphine carboxylate, dichloromethane and 3-chloroperbenzoic acid is 0.1 mol: 85 mL: 0.1 mol; Step A2: In a nitrogen atmosphere, add thiophene-2,4-dicarboxylic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 9 hours, then heat to 115°C, stir for 1.5 hours to obtain diol; the amount ratio of thiophene-2,4-dicarboxylic acid, toluene, pyridine and epoxy product is 0.1 mol: 155 mL: 0.013 mol: 0.1 mol; Step A3: Stir polyethylene glycol 600 at 110°C under vacuum for 1.5h for later use; add toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dimethylol propionic acid to a reaction bottle in a nitrogen atmosphere, and stir at 80°C for 5 minutes to obtain the wall material; add ammonium polyphosphate to 1,4-dioxane and stir for 13 minutes to obtain dispersion 1; then add the wall material to 1,4-dioxane and stir for 33 minutes to obtain dispersion 2; then add dispersion 1 to dispersion 2 and stir for 10 minutes; , add dibutyltin dilaurate, stir and react at 80°C for 4.5h to obtain flame retardant microcapsules; the dosage ratio of toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dihydroxymethylpropionic acid is 15g:13g:10g:5g; the dosage ratio of ammonium polyphosphate and 1,4-dioxane is 1g:6mL; the dosage ratio of wall material and 1,4-dioxane is 1g:12mL; the dosage ratio of dispersion 1, dispersion 2 and dibutyltin dilaurate is 7mL:18mL:0.03g.
[0015] Embodiment 3: A flame retardant microcapsule, the preparation of which comprises the following steps: Step A1: Add ethyl 3-butenylphosphinothioate to dichloromethane, start stirring, then add 3-chloroperbenzoic acid, and stir at room temperature for 5 hours to obtain an epoxy product; the amount ratio of ethyl 3-butenylphosphinothioate, dichloromethane and 3-chloroperbenzoic acid is 0.1 mol:90 mL:0.1 mol; Step A2: In a nitrogen atmosphere, add thiophene-2,4-dicarboxylic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 10 hours, then heat to 120°C, stir for 2 hours to obtain diol; the amount ratio of thiophene-2,4-dicarboxylic acid, toluene, pyridine and epoxy product is 0.1 mol: 160 mL: 0.015 mol: 0.1 mol; Step A3: Stir polyethylene glycol 600 at 110°C under vacuum for 2 hours for later use; add toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dimethylol propionic acid to a reaction bottle in a nitrogen atmosphere, and stir and react at 80-85°C for 6 hours to obtain the wall material; add ammonium polyphosphate to 1,4-dioxane and stir for 15 minutes to obtain dispersion 1; then add the wall material to 1,4-dioxane and stir for 35 minutes to obtain dispersion 2; then add dispersion 1 to dispersion 2 and stir for 10 minutes. n, dibutyltin dilaurate was added, and the reaction was stirred at 80°C for 5 hours to obtain flame retardant microcapsules; the dosage ratio of toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dihydroxymethylpropionic acid was 20g:15g:11g:6g; the dosage ratio of ammonium polyphosphate and 1,4-dioxane was 1g:7mL; the dosage ratio of wall material and 1,4-dioxane was 1g:14mL; the dosage ratio of dispersion 1, dispersion 2 and dibutyltin dilaurate was 8mL:20mL:0.04g.
[0016] Example 4: A modified isocyanate, the preparation of which comprises the following steps: Step B1: 2-(4-methylpiperidinyl)-5-nitroaniline, potassium carbonate and dimethyl sulfoxide are added to a flask to obtain a mixed solution 1, and then succinyl dichloride is added to dimethyl sulfoxide to obtain a mixed solution 2. The mixed solution 2 is slowly added dropwise to the mixed solution 1 in an ice-water bath at 0°C. After the addition is completed, the mixture is heated to 40°C and stirred at a constant temperature for 10 hours to obtain an amide product. The amount ratio of 2-(4-methylpiperidinyl)-5-nitroaniline, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.015 mol: 50 mL; the amount ratio of succinyl dichloride and dimethyl sulfoxide is 0.1 mol: 30 mL; the amount ratio of mixed solution 1 to mixed solution 2 is 55 mL: 35 mL; Step B2: Add nano calcium carbonate to anhydrous ethanol, add bromobutyltrimethoxysilane and sulfuric acid solution, heat to 30°C, stir and react for 4 hours to obtain surface-modified nano calcium carbonate; put amide product and ethanol in a flask, start stirring, then add surface-modified nano calcium carbonate, heat to 50°C, stir and react at constant temperature for 10 hours, recrystallize with acetone after rotary evaporation, filter and obtain quaternary ammonium salt; the dosage ratio of nano calcium carbonate, anhydrous ethanol, bromobutyltrimethoxysilane and sulfuric acid solution is 10g:50mL:5g:10mL, and the concentration of sulfuric acid solution is 0.5mol / L; the dosage ratio of amide product, ethanol and surface-modified nano calcium carbonate is 56g:135mL:15g, and the volume fraction of ethanol is 95%; Step B3: Add quaternary ammonium salt and ethyl acetate to a three-necked flask, heat to 45°C, start reflux stirring, then add sodium dithionite, and reflux stirring to react for 1 hour to obtain aromatic primary amine; add xylene to a four-necked flask, pass nitrogen, add aromatic primary amine and triphosgene at 75°C respectively, after the addition is completed, heat to 125°C and continue to react for 3.5 hours to obtain modified isocyanate; the usage ratio of quaternary ammonium salt, ethyl acetate and sodium dithionite is 58g:150mL:20g; the usage ratio of xylene, aromatic primary amine and triphosgene is 220mL:63g:40g.
[0017] Example 5: A modified isocyanate, the preparation of which comprises the following steps: Step B1: 2-(4-methylpiperidinyl)-5-nitroaniline, potassium carbonate and dimethyl sulfoxide are added to a flask to obtain a mixed solution 1, and then succinyl dichloride is added to dimethyl sulfoxide to obtain a mixed solution 2. In a 0°C ice-water bath, the mixed solution 2 is slowly added dropwise to the mixed solution 1. After the addition is completed, the temperature is raised to 40°C, and the reaction is stirred at a constant temperature for 10 hours to obtain an amide product; the amount ratio of 2-(4-methylpiperidinyl)-5-nitroaniline, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.015 mol: 55 mL; the amount ratio of succinyl dichloride and dimethyl sulfoxide is 0.1 mol: 35 mL; the amount ratio of mixed solution 1 to mixed solution 2 is 60 mL: 40 mL; Step B2: Add nano-calcium carbonate to anhydrous ethanol, add bromobutyltrimethoxysilane and sulfuric acid solution, heat to 30°C, stir and react for 4.5 hours to obtain surface-modified nano-calcium carbonate; put amide product and ethanol in a flask, start stirring, then add surface-modified nano-calcium carbonate, heat to 55°C, stir and react at constant temperature for 11 hours, recrystallize with acetone after rotary evaporation, and filter to obtain quaternary ammonium salt; the dosage ratio of nano-calcium carbonate, anhydrous ethanol, bromobutyltrimethoxysilane and sulfuric acid solution is 10g:55mL:6g:11mL, and the concentration of sulfuric acid solution is 0.5mol / L; the dosage ratio of amide product, ethanol and surface-modified nano-calcium carbonate is 58g:140mL:15.5g, and the volume fraction of ethanol is 95%; Step B3: Add quaternary ammonium salt and ethyl acetate to a three-necked flask, heat to 50°C, start reflux stirring, then add sodium dithionite, and reflux stirring to react for 1.3 hours to obtain aromatic primary amine; add xylene to a four-necked flask, pass nitrogen, add aromatic primary amine and triphosgene at 75°C respectively, after the addition is completed, heat to 125°C and continue to react for 3.5 hours to obtain modified isocyanate; the usage ratio of quaternary ammonium salt, ethyl acetate and sodium dithionite is 60g:155mL:23g; the usage ratio of xylene, aromatic primary amine and triphosgene is 220mL:64g:43g.
[0018] Example 6: A modified isocyanate, the preparation of which comprises the following steps: Step B1: 2-(4-methylpiperidinyl)-5-nitroaniline, potassium carbonate and dimethyl sulfoxide are added to a flask to obtain a mixed solution 1, and then succinyl dichloride is added to dimethyl sulfoxide to obtain a mixed solution 2. In a 0°C ice-water bath, the mixed solution 2 is slowly added dropwise to the mixed solution 1. After the addition is completed, the temperature is raised to 40°C, and the reaction is stirred at a constant temperature for 10 hours to obtain an amide product; the amount ratio of 2-(4-methylpiperidinyl)-5-nitroaniline, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.015 mol: 60 mL; the amount ratio of succinyl dichloride and dimethyl sulfoxide is 0.1 mol: 40 mL; the amount ratio of mixed solution 1 to mixed solution 2 is 65 mL: 45 mL; Step B2: Add nano calcium carbonate to anhydrous ethanol, add bromobutyltrimethoxysilane and sulfuric acid solution, heat to 30°C, stir and react for 5 hours to obtain surface-modified nano calcium carbonate; put amide product and ethanol in a flask, start stirring, then add surface-modified nano calcium carbonate, heat to 60°C, stir and react at constant temperature for 12 hours, recrystallize with acetone after rotary evaporation, filter and obtain quaternary ammonium salt; the dosage ratio of nano calcium carbonate, anhydrous ethanol, bromobutyltrimethoxysilane and sulfuric acid solution is 10g:60mL:7g:12mL, and the concentration of sulfuric acid solution is 0.5mol / L; the dosage ratio of amide product, ethanol and surface-modified nano calcium carbonate is 60g:145mL:16g, and the volume fraction of ethanol is 95%; Step B3: Add quaternary ammonium salt and ethyl acetate to a three-necked flask, heat to 55°C, start reflux stirring, then add sodium dithionite, and reflux stirring to react for 1.5 hours to obtain aromatic primary amine; add xylene to a four-necked flask, pass nitrogen, add aromatic primary amine and triphosgene at 75°C respectively, after the addition is completed, heat to 125°C and continue to react for 3.5 hours to obtain modified isocyanate; the usage ratio of quaternary ammonium salt, ethyl acetate and sodium dithionite is 62g:160mL:25g; the usage ratio of xylene, aromatic primary amine and triphosgene is 220mL:65g:45g.
[0019] Embodiment 7: A polyurethane adhesive comprises component A and component B, wherein the molar ratio of OH functional group of component A to NCO functional group of component B is 1:1.3; component A comprises 100 parts of polyester polyol, 50 parts of polyether polyol, 10 parts of 4,4-diphenylmethane diisocyanate, and 1 part of molecular sieve; component B comprises 90 parts of toluene diisocyanate, 50 parts of polyether polyol, 10 parts of modified isocyanate, and 10 parts of flame retardant microcapsules; the molecular weight of the polyester polyol is 2000, and the average functionality is 2; the polyether polyol is polypropylene glycol 600, and the molecular sieve is 3A type molecular sieve; The preparation of the polyurethane adhesive comprises the following steps: Step S1: Add polyester polyol and polyether polyol to a reaction kettle, stir at 110° C. under vacuum for 2 h, cool to 50° C., then add 4,4-diphenylmethane diisocyanate under stirring, heat to 80° C. and stir for 4 h, then add molecular sieves and stir under vacuum for 30 min to obtain component A; Step S2: Add the polyether polyol to a reaction kettle, stir at 110° C. under vacuum for 1 h, cool to 50° C., then add toluene diisocyanate and the modified isocyanate obtained in Example 4 under stirring, heat to 80° C. and stir for 3 h, then add the flame retardant microcapsules obtained in Example 1 and stir for 25 min under vacuum to obtain component B; Step S3: Package component A and component B in double tubes, add components A and B into a reaction kettle and stir for 1 hour before use to obtain a polyurethane adhesive.
[0020] Embodiment 8: A polyurethane adhesive comprises component A and component B, wherein the molar ratio of OH functional group of component A to NCO functional group of component B is 1:1.5; component A comprises 100 parts of polyester polyol, 55 parts of polyether polyol, 15 parts of 4,4-diphenylmethane diisocyanate, and 2 parts of molecular sieve; component B comprises 90 parts of toluene diisocyanate, 55 parts of polyether polyol, 10 parts of modified isocyanate, and 11 parts of flame retardant microcapsules; the molecular weight of the polyester polyol is 2000, and the average functionality is 2; the polyether polyol is polypropylene glycol 600, and the molecular sieve is 3A type molecular sieve; The preparation of the polyurethane adhesive comprises the following steps: Step S1: Add polyester polyol and polyether polyol to a reaction kettle, stir at 110° C. under vacuum for 2 h, cool to 50° C., then add 4,4-diphenylmethane diisocyanate under stirring, heat to 85° C. and stir for 4.5 h, then add molecular sieves and stir under vacuum for 35 min to obtain component A; Step S2: Add the polyether polyol to a reaction kettle, stir at 110° C. under vacuum for 1 h, cool to 50° C., then add toluene diisocyanate and the modified isocyanate obtained in Example 5 under stirring, heat to 85° C. and stir for 3.5 h, then add the flame retardant microcapsules obtained in Example 2 and stir under vacuum for 30 min to obtain component B; Step S3: Component A and component B are packaged in double tubes. Before use, components A and B are added to a reaction kettle and stirred for 1.5 hours to obtain a polyurethane adhesive.
[0021] Embodiment 9: A polyurethane adhesive comprises component A and component B, wherein the molar ratio of OH functional group of component A to NCO functional group of component B is 1:1.7; component A comprises 100 parts of polyester polyol, 60 parts of polyether polyol, 20 parts of 4,4-diphenylmethane diisocyanate, and 3 parts of molecular sieve; component B comprises 90 parts of toluene diisocyanate, 60 parts of polyether polyol, 10 parts of modified isocyanate, and 12 parts of flame retardant microcapsules; the molecular weight of the polyester polyol is 3000, and the average functionality is 3; the polyether polyol is polypropylene glycol 600, and the molecular sieve is 3A type molecular sieve; The preparation of the polyurethane adhesive comprises the following steps: Step S1: Add polyester polyol and polyether polyol to a reaction kettle, stir at 110° C. under vacuum for 2 h, cool to 50° C., then add 4,4-diphenylmethane diisocyanate under stirring, heat to 90° C. and stir for 5 h, then add molecular sieves and stir under vacuum for 40 min to obtain component A; Step S2: Add the polyether polyol to a reaction kettle, stir at 110° C. under vacuum for 1 h, cool to 50° C., then add toluene diisocyanate and the modified isocyanate obtained in Example 6 under stirring, heat to 90° C. and stir for 4 h, then add the flame retardant microcapsules obtained in Example 3 and stir for 35 min under vacuum to obtain component B; Step S3: Package component A and component B in double tubes, add components A and B into a reaction kettle and stir for 2 hours before use to obtain a polyurethane adhesive.
[0022] Comparative Example 1 This comparative example is a commercially available polyurethane adhesive.
[0023] Comparative Example 2 Compared with Example 9, the thiophene-2,4-dicarboxylic acid in the diol preparation process was replaced with succinic acid, that is, the thiophene ring was not introduced, and the rest was exactly the same as Example 9 to prepare a polyurethane adhesive.
[0024] Comparative Example 3 Compared with Example 9, the modified isocyanate was replaced with 4,4-diphenylmethane diisocyanate, that is, nano calcium carbonate and quaternary ammonium salt structure were not introduced, and the rest was exactly the same as Example 9 to prepare a polyurethane adhesive.
[0025] The polyurethane adhesive prepared by the present invention is further tested for its effect, and the test results are as follows.
[0026] In order to test the polyurethane adhesive prepared by the present invention, the tensile strength and elongation at break of the dumbbell-shaped specimen of polyurethane adhesive on the plastic substrate PET after curing for 7 days under the standard environment of reference standard GB / T528-2009 were tested; the obtained polyurethane adhesive was placed in a strength of 1000W / m2 After irradiation with ultraviolet light for 200 hours, the tensile strength retention rate was measured to test the anti-ultraviolet performance; Escherichia coli, Staphylococcus aureus, and Candida albicans were used as experimental bacteria to test the antibacterial property of the polyurethane adhesive; the flame retardant property of the polyurethane adhesive was tested according to UL-94, and the results are recorded in Table 1; UL-94 test method: The flame retardant material standard UL-94 vertical combustion test method is adopted, and the flame retardant level increases step by step from V-2, V-1 to V-0; V-0: After the sample is subjected to two 10-second combustion tests, the flame goes out within 30 seconds, and no burning objects fall off; V-1: After the sample is subjected to two 10-second combustion tests, the flame goes out within 60 seconds, and no burning objects fall off; V-2: After the sample is subjected to two 10-second combustion tests, the flame goes out within 60 seconds, and burning objects fall off; Table 1 Test results:
[0027] According to the data in Table 1, it can be seen from the comparison between Examples 7-9 and Comparative Example 1 that the polyurethane adhesive of the present invention has good mechanical properties, UV resistance, flame retardancy and antibacterial properties. It can be seen from the comparison between Example 9 and Comparative Example 2 that the introduction of thiophene rings in the wall material of the flame retardant microcapsules improves the UV resistance of the flame retardant microcapsules, which is also conducive to the improvement of the UV resistance of the polyurethane adhesive. It can be seen from the comparison between Example 9 and Comparative Example 3 that the use of modified isocyanate introduced with nano-calcium carbonate and quaternary ammonium salt to participate in the reaction and the introduction of nano-calcium carbonate and quaternary ammonium salt structure in the molecular chain of component B is more conducive to the improvement of the mechanical properties and antibacterial properties of the prepared polyurethane adhesive.
[0028] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A polyurethane adhesive, Features: It comprises component A and component B, wherein the molar ratio of OH functional group of component A to NCO functional group of component B is 1:1.3-1.7; component A comprises 100 parts of polyester polyol, 50-60 parts of polyether polyol, 10-20 parts of 4,4-diphenylmethane diisocyanate and 1-3 parts of molecular sieve; component B comprises 90 parts of toluene diisocyanate, 50-60 parts of polyether polyol, 10 parts of modified isocyanate and 10-12 parts of flame retardant microcapsules; The flame retardant microcapsules are prepared by the following steps: Step A1: Add ethyl 3-butenylphosphine carboxylate to dichloromethane, start stirring, then add 3-chloroperbenzoic acid, and stir at room temperature for 4-5 hours to obtain an epoxy product; Step A2: In a nitrogen atmosphere, add thiophene-2,4-dicarboxylic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 8-10h, then heat to 110-120°C, stir for 1-2h to obtain diol; Step A3: Stir polyethylene glycol 600 at 110° C. under vacuum for 1-2 hours for later use; in a nitrogen atmosphere, add toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dimethylol propionic acid to a reaction bottle, stir and react at 80-85° C. for 4-6 hours to obtain the wall material; add ammonium polyphosphate to 1,4-dioxane and stir for 10-15 minutes to obtain dispersion 1; then add the wall material to 1,4-dioxane and stir for 30-35 minutes to obtain dispersion 2; then add dispersion 1 to dispersion 2, stir for 10 minutes, add dibutyltin dilaurate, stir and react at 80° C. for 4-5 hours to obtain flame retardant microcapsules.
2. A polyurethane adhesive according to claim 1, Features: In step A1, the usage ratio of ethyl 3-butenylphosphine carboxylate, dichloromethane and 3-chloroperbenzoic acid is 0.1 mol: 80-90 mL: 0.1 mol.
3. A polyurethane adhesive according to claim 1, Features: In step A2, the usage ratio of thiophene-2,4-dicarboxylic acid, toluene, pyridine and epoxy product is 0.1 mol: 150-160 mL: 0.010-0.015 mol: 0.1 mol.
4. A polyurethane adhesive according to claim 1, Features: In step A3, the usage ratio of toluene diisocyanate, polyethylene glycol 600, diol and 2,2-dimethylolpropionic acid is 10-20g:10-15g:9-11g:4-6g; the usage ratio of ammonium polyphosphate and 1,4-dioxane is 1g:5-7mL; the usage ratio of wall material and 1,4-dioxane is 1g:10-14mL; the usage ratio of dispersion 1, dispersion 2 and dibutyltin dilaurate is 6-8mL:15-20mL:0.02-0.04g.
5. A polyurethane adhesive according to claim 1, Features: The modified isocyanate is prepared by the following steps: Step B1: Add 2-(4-methylpiperidinyl)-5-nitroaniline, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution 1, then add succinyl dichloride to dimethyl sulfoxide to obtain a mixed solution 2, slowly dropwise add the mixed solution 2 into the mixed solution 1 in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, and stir the mixture at constant temperature for 10 hours to obtain an amide product; Step B2: Add nano-calcium carbonate to anhydrous ethanol, add bromobutyltrimethoxysilane and sulfuric acid solution, heat to 30°C, stir and react for 4-5h to obtain surface-modified nano-calcium carbonate; put the amide product and ethanol in a flask, start stirring, then add the surface-modified nano-calcium carbonate, heat to 50-60°C, stir and react at constant temperature for 10-12h, recrystallize with acetone after rotary evaporation, and filter to obtain quaternary ammonium salt; Step B3: Add quaternary ammonium salt and ethyl acetate to a three-necked flask, heat to 45-55°C, start reflux stirring, then add sodium dithionite, and reflux stirring to react for 1-1.5h to obtain aromatic primary amine; add xylene to a four-necked flask, pass nitrogen, add aromatic primary amine and triphosgene at 75°C respectively, after the addition is completed, heat to 125°C and continue to react for 3.5h to obtain modified isocyanate.
6. A polyurethane adhesive according to claim 5, Features: In step B1, the usage ratio of 2-(4-methylpiperidinyl)-5-nitroaniline, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.015 mol: 50-60 mL; the usage ratio of succinyl dichloride and dimethyl sulfoxide is 0.1 mol: 30-40 mL; the usage ratio of mixed solution 1 and mixed solution 2 is 55-65 mL: 35-45 mL.
7. A polyurethane adhesive according to claim 5, Features: In step B2, the dosage ratio of nano-calcium carbonate, anhydrous ethanol, bromobutyltrimethoxysilane and sulfuric acid solution is 10g:50-60mL:5-7g:10-12mL, and the concentration of sulfuric acid solution is 0.5mol / L; the dosage ratio of amide product, ethanol and surface-modified nano-calcium carbonate is 56-60g:135-145mL:15-16g, and the volume fraction of ethanol is 95%.
8. A polyurethane adhesive according to claim 5, Features: In step B3, the usage ratio of quaternary ammonium salt, ethyl acetate and sodium dithionite is 58-62 g:150-160 mL:20-25 g; the usage ratio of xylene, aromatic primary amine and triphosgene is 220 mL:63-65 g:40-45 g.
9. The polyurethane adhesive according to claim 1, Features: The molecular weight of the polyester polyol is 2000-3000, and the average functionality is 2-3; the polyether polyol is polypropylene glycol 600, and the molecular sieve is 3A type molecular sieve.
10. The method for preparing a polyurethane adhesive according to claim 1, Features: The steps include: Step S1: Add polyester polyol and polyether polyol to a reaction kettle, stir at 110° C. under vacuum for 2 h, cool to 50° C., then add 4,4-diphenylmethane diisocyanate under stirring, heat to 80-90° C. and stir for 4-5 h, then add molecular sieves and stir under vacuum for 30-40 min to obtain component A; Step S2: Add polyether polyol to a reaction kettle, stir at 110° C. under vacuum for 1 hour, cool to 50° C., then add toluene diisocyanate and modified isocyanate under stirring, heat to 80-90° C. and stir to react for 3-4 hours, then add flame retardant microcapsules and stir under vacuum for 25-35 minutes to obtain component B; Step S3: Package component A and component B in double tubes, add components A and B into a reaction kettle and stir for 1-2 hours before use to obtain a polyurethane adhesive.
Citation Information
Patent Citations
Bio-based flame retardant microcapsule and preparation method thereof
CN113214539A
Polyurethane adhesive for textile flocking
CH504522A
Preparation method of UV-curable branched polythiophene derivative conductive polymer material
CN104927029A
Temperature-resistant high-viscosity adhesive and preparation method thereof
CN118421255A
Double-shell microcapsule as well as preparation method and application thereof
CN118531641A
Cited By
High-performance modified polyurethane grouting material and preparation method thereof
CN119144163A
A high performance modified polyurethane grouting material and preparation method thereof
CN119144163B