Method for growing indium antimonide crystal

By using dopants in indium antimonide crystals and using lifting crystal growth technology, the pinning effect is formed, which solves the problem of highlight defects in indium antimonide crystal processing and significantly improves the crystal Strength and chip stability.

CN118880434APending Publication Date: 2024-11-01GUANGDONG JINGZHI OPTOELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410959240.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Indium antimonide crystals are prone to form bright spot defects during processing, which affects their performance and increases the chance of cracking in the chip process. The existing methods have limited improvement effects.

Method used

Doping of dopants such as GaN, GaP, InP, GaAs, InAs, GaSb and InSb polycrystalline materials is used to form a pinning effect through lifting crystal growth technology, which improves the strength of indium antimonide crystals and reduces highlight defects.

Benefits of technology

It effectively improves the strength of indium antimonide crystals, significantly reduces the number of highlight defects generated in substrate processing, and improves the stability and process reliability of the chip.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880434A_ABST
    Figure CN118880434A_ABST
Patent Text Reader

Abstract

The growth method of the indium antimonide crystal comprises the following steps: S1, loading, namely paving dopant particles at the bottom of a crucible, paving an InSb polycrystal material on the dopant particles, wherein the doping ratio of a dopant to the InSb polycrystal material is (0.5-1) g / 10kg, the purity of the dopant is more than 5N, the purity of the InSb polycrystal material is more than 7.5 N, and the dopant is selected from one or more of GaN, GaP, InP, GaAs, InAs and GaSb; s2, vacuumizing the Czochralski crystal growth equipment, driving air, and detecting leakage so as to enable the interior of the Czochralski crystal growth equipment to be vacuum; s3, introducing a nitrogen-hydrogen mixed gas into the Czochralski method crystal growth equipment, and maintaining the pressure of 0.1 MPa; s4, material melting; s5, after the melt is formed, the temperature of the crucible is kept unchanged when the pressure is increased to 0.15 MPa; s6, carrying out crystal growth by straight pulling to form a crystal bar; and S7, after crystal growth is completed, stopping heating and cooling, after gas in the Czochralski method crystal growth equipment is replaced with nitrogen, starting the Czochralski method crystal growth equipment, and cutting off the crystal bar from the crystal pulling rod.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of indium antimonide crystals, and more specifically to a method for growing indium antimonide crystals. Background Art

[0002] InSb is a narrow-bandgap III-V semiconductor material with a bandgap width of 0.232eV at 77K. It has intrinsic absorption in the 3-5μm band and has extremely high electron mobility. It is currently one of the best materials for medium-wave infrared detectors. The melting point of inSb is 525℃. Compared with other III-V compounds, it is easy to purify and grow single crystals, so it is often the object of choice in theoretical research on III-V compound solids.

[0003] Among the many InSb defects, bright spot defects (irregular defects or damage on the surface of the InSb substrate in microscopy shine slightly in the bright field, so they are called bright spots) are one of the main defects that affect the performance of InSb. In essence, the chip hardness is not enough and it is easy to be damaged during the crystal processing. These damages will not only cause blind pixels to form in the InSb detector, but also increase the probability of cracking of the InSb substrate during the chip manufacturing process. "Research on Surface Polishing and Corrosion of InSb Chips" (Guo Sheng et al., Infrared Technology, Vol. 40, No. 2, pp. 133-138, February 2018) proposed a method to reduce the bright spots of InSb substrates by changing the processing method, but the improvement effect of this method is limited and cannot effectively solve the bright spot problem of InSb substrates. Therefore, it is necessary to find a way to reduce the bright spot defects of InSb detectors. Summary of the invention

[0004] In view of the problems existing in the background technology, an object of the present disclosure is to provide a method for growing an indium antimonide crystal, which can effectively improve the bright spot defects caused by damage in the process of making an indium antimonide substrate from an indium antimonide crystal.

[0005] Thus, a method for growing indium antimonide crystals comprises the following steps: S1, loading, spreading dopant particles on the bottom of a crucible, spreading InSb polycrystalline material on the dopant particles, the doping ratio of the dopant to the InSb polycrystalline material being (0.5-1) g / 10 kg, the purity of the dopant being 5N or more, the purity of the InSb polycrystalline material being 7.5N or more, and the dopant being selected from one or more of GaN, GaP, InP, GaAs, InAs, and GaSb; S2, evacuating, removing gas, and leak checking a CZ crystal growth device to achieve a vacuum in the CZ crystal growth device; S3, introducing a nitrogen-hydrogen mixed gas into the CZ crystal growth device to maintain a pressure of 0.1 MPa in the CZ crystal growth device; S4, melting the material, turning on the heating of the crucible, heating up and melting the InSb in the crucible; Polycrystalline material and dopant particles; S5, after the InSb polycrystalline material and dopant particles are completely melted to form a melt, the temperature of the crucible is maintained unchanged when the pressure in the CZC crystal growth equipment rises to 0.15MPa; S6, after step S5, the crystal pulling rod drives the seed crystal to move downward into the crucible and immerse it from the surface of the melt, and then the crystal pulling rod is pulled upward to grow the crystal to form a crystal rod. During the crystal growth process, the crucible and the crystal pulling rod maintain opposite rotation speeds, the rotation speed of the crucible is 0.5-1.5rpm, the rotation speed of the crystal pulling rod is 2-4rpm, the seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant at 5-15mm / h; S7, after the crystal growth is completed, stop heating, cool down, replace the gas in the CZC crystal growth equipment with nitrogen, open the CZC crystal growth equipment, and cut the crystal rod from the crystal pulling rod.

[0006] The beneficial effects of the present disclosure are as follows: in the method for growing indium antimonide crystals according to the present disclosure, doping is performed with one or more dopants selected from GaN, GaP, InP, GaAs, InAs, and GaSb in step S1 at a doping ratio of (0.5-1) g / 10 kg to the InSb polycrystalline material, and after a melt is formed in step S5, the indium antimonide crystal is grown by the pulling method in step S6, so that the dopant forms a pinning effect in the lattice of the formed indium antimonide crystal, thereby improving the strength of the indium antimonide crystal, and effectively improving the bright spot defects caused by damage to the indium antimonide crystal during the processing of the indium antimonide crystal to make the indium antimonide substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] Figure 1 Schematic diagram of an exemplary Czochralski crystal growth device used in the method for growing indium antimonide crystals according to the present disclosure.

[0008] Figure 2 This is a photograph of the indium antimonide substrate made in Example 1 doped with GaAs observed under a 100x microscope in a bright field state.

[0009] Figure 3This is a photograph of the undoped indium antimonide substrate made in Comparative Example 1 observed under a 100x microscope in a bright field state.

[0010] Figure 4 This is a photograph of the indium antimonide substrate made in Example 2 doped with GaP observed under a 100x microscope in a bright field state.

[0011] Figure 5 This is a photograph of the indium antimonide substrate made in Example 3 using InP doping observed under a 100x microscope in a bright field state.

[0012] Figure 6 This is a photograph of the indium antimonide substrate made in Example 4 using GaN doping observed under a 100x microscope in a bright field state.

[0013] Figure 7 This is a photograph of the indium antimonide substrate made in Example 5 using InAs doping observed under a 100x microscope in a bright field state.

[0014] Figure 8 This is a photograph of the indium antimonide substrate made in Example 6 doped with GaSb observed under a 100x microscope in a bright field state. DETAILED DESCRIPTION

[0015] It will be understood that the disclosed embodiments are merely examples of the present disclosure, which may be implemented in various forms, and therefore, the specific details disclosed herein should not be interpreted as limiting, but merely as a basis for the claims and as a representative basis for teaching one of ordinary skill in the art to implement the present disclosure in various ways.

[0016] [Method for growing indium antimonide crystals]

[0017] Reference Figure 1 According to the present disclosure, the method for growing indium antimonide crystals comprises the steps of:

[0018] S1, loading, spreading dopant particles on the bottom of the crucible, spreading InSb polycrystalline material on the dopant particles, the doping ratio of the dopant to the InSb polycrystalline material is (0.5-1) g / 10 kg, the purity of the dopant is 5N or more, the purity of the InSb polycrystalline material is 7.5N or more, and the dopant is selected from one or more of GaN, GaP, InP, GaAs, InAs, and GaSb;

[0019] S2, evacuating the CZC crystal growth device, removing air, and checking for leaks, so that the CZC crystal growth device reaches a vacuum;

[0020] S3, introducing a nitrogen-hydrogen mixed gas into the CZC crystal growth device to maintain a pressure of 0.1 MPa in the CZC crystal growth device;

[0021] S4, melting the material, starting the heating of the crucible, heating up and melting the InSb polycrystalline material and dopant particles in the quartz crucible;

[0022] S5, after the InSb polycrystalline material and the dopant particles are completely melted to form a melt, the pressure in the Czochralski crystal growth device is raised to 0.15 MPa while maintaining the temperature of the quartz crucible unchanged;

[0023] S6, after step S5, the pulling rod drives the seed crystal to move downward into the crucible and immerse into the melt from the surface, and then the pulling rod pulls the crystal upward to grow the crystal to form a crystal rod. During the crystal growth process, the quartz crucible and the pulling rod maintain opposite rotation speeds, the rotation speed of the crucible is 0.5-1.5 rpm, the rotation speed of the pulling rod is 2-4 rpm, the seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant at 5-15 mm / h;

[0024] S7, after the crystal growth is completed, the heating and cooling are stopped, the gas in the Czochralski crystal growth equipment is replaced with nitrogen, the Czochralski crystal growth equipment is opened, and the crystal rod is cut off from the crystal pulling rod.

[0025] In the growth method of indium antimonide crystal according to the present disclosure, doping is performed with one or more dopants selected from GaN, GaP, InP, GaAs, InAs, and GaSb in step S1 at a doping ratio of (0.5-1) g / 10kg to InSb polycrystalline material, and after forming a melt in step S5, the indium antimonide crystal is grown by the pulling method in step S6, so that the dopant forms a pinning effect in the lattice of the formed indium antimonide crystal, thereby improving the strength of the indium antimonide crystal, and effectively improving the bright spot defects caused by damage to the indium antimonide crystal during the processing of the indium antimonide substrate.

[0026] In one example, in step S1 , the crucible is a quartz crucible.

[0027] In one example, in step S1, the InSb polycrystalline material is a zone melting polycrystalline material, which is cleaned with aqua regia, rinsed with deionized water for more than 3 times, and dried in a vacuum oven for later use.

[0028] In one example, in step S2 , the vacuum pressure achieved is 10 Pa.

[0029] In one example, in step S2, the flushing gas is 7N nitrogen.

[0030] In one example, in step S3, after the pressure in the Czochralski crystal growth apparatus reaches 0.1 MPa, the gas inlet in the Czochralski crystal growth apparatus is closed.

[0031] In one example, in step S4, the heater used for heating includes a graphite heater, a graphite double-layer insulation cover and carbon felt. The graphite heater is arranged around the crucible, the graphite double-layer insulation cover is arranged around the graphite heater, and the carbon felt is filled between the inner layer and the outer layer of the graphite double-layer insulation cover. The heater for heating the quartz crucible is the only heating device in the Czochralski crystal growth equipment.

[0032] In one example, in step S5, when the pressure in the Czochralski crystal growth device is raised to 0.15 MPa, the gas inlet and the vacuum port in the Czochralski crystal growth device are closed.

[0033] [test]

[0034] Example 1

[0035] Reference Figure 1 , Example 1 adopts the following steps:

[0036] S1, loading, spreading dopant particles on the bottom of the crucible, spreading the dried InSb polycrystalline material on the dopant particles, the doping ratio of the dopant to the InSb polycrystalline material is 0.75g / 10kg, the purity of the dopant is 5N, the purity of the InSb polycrystalline material is 7.5N, the dopant is selected from GaAs, wherein the crucible is a quartz crucible, the InSb polycrystalline material is cleaned with aqua regia, rinsed with deionized water for more than 3 times, and dried in a vacuum oven for later use;

[0037] S2, evacuate the CZC crystal growth device, remove gas, and check for leaks, so that the CZC crystal growth device reaches a vacuum, and the vacuum pressure reached is 10Pa. The evacuation and removal of gas are performed alternately 2-3 times by using a vacuum pump to evacuate the CZC crystal growth device and fill nitrogen into the CZC crystal growth device. The evacuation interface is set at the bottom of the CZC crystal growth device, and nitrogen (purity 7N) is used to remove gas. The nitrogen gas inlet is set at the top of the CZC crystal growth device;

[0038] S3, after the completion of step S2, the top cover and the middle tube are locked by corresponding screws, and the middle tube and the base are locked by corresponding screws, then the vacuum interface and the gas inlet are closed, and a nitrogen-hydrogen mixed gas is introduced into the CZC crystal growth device to maintain the pressure in the CZC crystal growth device at 0.1 MPa (monitored by a pressure gauge), and then the gas inlet is closed;

[0039] S4, chemical material, start heating the crucible, heat up and melt the InSb polycrystalline material and dopant particles in the crucible, wherein the heater used for heating includes a graphite heater, a graphite double-layer insulation cover and carbon felt, the graphite heater is arranged around the crucible, the graphite double-layer insulation cover is arranged around the graphite heater, and the carbon felt is filled between the inner layer and the outer layer of the graphite double-layer insulation cover. The heater for heating the quartz crucible is the only heating device in the Czochralski crystal growth equipment;

[0040] S5, after the InSb polycrystalline material and the dopant particles are completely melted to form a melt, the temperature of the crucible is maintained constant when the pressure in the Czochralski crystal growth apparatus rises to 0.15 MPa (monitored by a pressure gauge), wherein the formation of the melt is confirmed by observing through an observation window (not shown, disposed on the top cover);

[0041] S6, after step S5, the pulling rod drives the seed crystal to move downward into the crucible and immerse into the melt from the surface, and then the pulling rod pulls the crystal upward to grow the crystal to form a crystal rod. During the crystal growth process, the crucible and the pulling rod maintain opposite rotation speeds, the rotation speed of the crucible is 1 rpm, the rotation speed of the pulling rod is 3 rpm, the seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant at 12 mm / h;

[0042] S7, after the crystal growth is completed, the heating and cooling are stopped, the gas in the Czochralski crystal growth equipment is replaced with nitrogen, the Czochralski crystal growth equipment is opened, and the crystal rod is cut off from the crystal pulling rod.

[0043] Comparative Example 1

[0044] Except that the dopant in step S1 is eliminated and the corresponding steps S4 and S5 do not involve dopant, the rest is the same as in embodiment 1.

[0045] Example 2

[0046] Except that the dopant in step S1 is selected from GaP, the rest is the same as in Example 1.

[0047] Example 3

[0048] Except that the dopant in step S1 is selected from InP, the rest is the same as in Example 1.

[0049] Example 4

[0050] Except that the dopant in step S1 is selected from GaN, the rest is the same as in Example 1.

[0051] Example 5

[0052] Except that the dopant in step S1 is selected from InAs, the rest is the same as in Example 1.

[0053] Example 6

[0054] Except that the dopant in step S1 is selected from GaSb, the rest is the same as in Example 1.

[0055] The middle part of the crystal rods prepared in Examples 1-6 and Comparative Example 1 after removing the head and tail parts was cut by diamond single wire to produce indium antimonide crystal sheets as indium antimonide substrates. The indium antimonide substrates were ground and polished using a double-sided grinder. The polishing liquid was prepared by mixing SiO2 sol at room temperature and pure water in a volume ratio of 1:1. The grinding and polishing time was 30 seconds. Afterwards, the surface of the indium antimonide substrate after grinding and polishing was observed under a 100x microscope in a bright field state.

[0056] Figure 2 This is a photograph of the indium antimonide substrate made in Example 1 doped with GaAs observed under a 100x microscope in a bright field state. Figure 3 This is a photograph of the undoped indium antimonide substrate made in Comparative Example 1 observed under a 100x microscope in a bright field state.

[0057] from Figure 2 and Figure 3 The comparison shows that Figure 2 The number of bright spot defects on the indium antimonide substrate of Example 1 is very small, only a few.

[0058] Figure 4 This is a photograph of the indium antimonide substrate made in Example 2 doped with GaP observed under a 100x microscope in a bright field state. Figure 5 This is a photograph of the indium antimonide substrate made in Example 3 using InP doping observed under a 100x microscope in a bright field state. Figure 6 This is a photograph of the indium antimonide substrate made in Example 4 using GaN doping observed under a 100x microscope in a bright field state. Figure 7 This is a photograph of the indium antimonide substrate made in Example 5 using InAs doping observed under a 100x microscope in a bright field state. Figure 8 This is a photograph of the indium antimonide substrate made in Example 6 doped with GaSb observed under a 100x microscope in a bright field state.

[0059] from Figures 4 to 8 It can be seen that under different dopants, the number of bright spot defects of the indium antimonide substrates prepared in Examples 2-6 is also very small or even zero ( Figure 4 For GaP and Figure 8 The number of bright spot defects of the indium antimonide substrate prepared in comparative example 1 is also far lower than that of the indium antimonide substrate prepared in comparative example 1.

[0060] The above detailed description is used to describe multiple exemplary embodiments, but this document is not intended to be limited to the explicitly disclosed combinations. Therefore, unless otherwise stated, the various features disclosed herein can be combined together to form multiple additional combinations that are not shown for the sake of simplicity.

Claims

1. A method for growing indium antimonide crystals, characterized in that: Includes steps: S1, loading, spreading dopant particles on the bottom of the crucible, spreading InSb polycrystalline material on the dopant particles, the doping ratio of the dopant to the InSb polycrystalline material is (0.5-1) g / 10 kg, the purity of the dopant is 5N or more, the purity of the InSb polycrystalline material is 7.5N or more, and the dopant is selected from one or more of GaN, GaP, InP, GaAs, InAs, and GaSb; S2, evacuating the CZC crystal growth device, removing air, and checking for leaks, so that the CZC crystal growth device reaches a vacuum; S3, introducing a nitrogen-hydrogen mixed gas into the CZC crystal growth device to maintain a pressure of 0.1 MPa in the CZC crystal growth device; S4, melting the material, starting to heat the crucible, and heating up to melt the InSb polycrystalline material and dopant particles in the crucible; S5, after the InSb polycrystalline material and the dopant particles are completely melted to form a melt, the pressure in the Czochralski crystal growth device is raised to 0.15 MPa to maintain the temperature of the crucible unchanged; S6, after step S5, the pulling rod drives the seed crystal to move downward into the crucible and immerse into the melt from the surface, and then the pulling rod pulls the crystal upward to grow the crystal to form a crystal rod. During the crystal growth process, the crucible and the pulling rod maintain opposite rotation speeds, the rotation speed of the crucible is 0.5-1.5 rpm, the rotation speed of the pulling rod is 2-4 rpm, the seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant at 5-15 mm / h; S7, after the crystal growth is completed, the heating and cooling are stopped, the gas in the Czochralski crystal growth equipment is replaced with nitrogen, the Czochralski crystal growth equipment is opened, and the crystal rod is cut off from the crystal pulling rod.

2. The method for growing indium antimonide crystals according to claim 1, characterized in that: In step S1 , the crucible is a quartz crucible.

3. The method for growing indium antimonide crystals according to claim 1, characterized in that: In step S1, the InSb polycrystalline material is a zone melting polycrystalline material, which is cleaned with aqua regia, rinsed with deionized water for more than 3 times, and dried in a vacuum oven for later use.

4. The method for growing indium antimonide crystal according to claim 1, characterized in that: In step S2, the vacuum pressure reached is 10Pa.

5. The method for growing indium antimonide crystals according to claim 1, characterized in that: In step S2, nitrogen gas with a concentration of 7N is used as the flushing gas.

6. The method for growing indium antimonide crystals according to claim 1, characterized in that: In step S3 , after the pressure in the CZC crystal growth apparatus reaches 0.1 MPa, the gas inlet in the CZC crystal growth apparatus is closed.

7. The method for growing indium antimonide crystal according to claim 1, characterized in that: In step S4, the heater used for heating includes a graphite heater, a graphite double-layer insulation cover and carbon felt. The graphite heater is arranged around the crucible, the graphite double-layer insulation cover is arranged around the graphite heater, and the carbon felt is filled between the inner layer and the outer layer of the graphite double-layer insulation cover. The heater for heating the quartz crucible is the only heating device in the Czochralski crystal growth equipment.

8. The method for growing indium antimonide crystal according to claim 1, characterized in that: In step S5, the pressure in the Czochralski crystal growth device is raised to 0.15 MPa, and the gas inlet and vacuum port in the Czochralski crystal growth device are closed.