Production process of formaldehyde-free shaving board for furniture production
By using biomass materials such as silicon-containing corn stalks, nitrogen-containing corn starch adhesives and boron-containing sunflower seed oil, the problems of high formaldehyde content and poor flame retardant performance of particleboard are solved, and high-efficiency flame retardant and mechanical properties are improved. In furniture production.
Patent Information
- Application Number
- CN202411285359.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing particleboard has high formaldehyde content, poor flame retardant performance, easy to release a large amount of thick smoke during combustion, and poor static bending strength and elastic modulus, which limits its breadth of application in furniture and other furniture.
Using biomass materials such as silicon-containing corn stalks, nitrogen-containing corn starch adhesives and boron-containing sunflower seed oil additives, it forms highly efficient flame-retardant particle boards to enhance its static curvature strength through drying, stirring, pre-pressing, and hot pressing processes. and elastic modulus.
Effectively reduce the formaldehyde emission of particleboard, improve flame retardant performance, reduce smoke density level, improve personal safety, and enhance the mechanical properties of particleboard.
Smart Images

Figure BDA0005042973100000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of artificial boards, and in particular relates to a production process of formaldehyde-free particleboard for furniture production. Background Art
[0002] At present, there are two main types of boards on the market: solid wood boards and artificial boards. Since furniture made of solid wood boards is generally expensive, the artificial board industry has broad development prospects. Particleboard is a typical artificial board product. It is a kind of artificial board made by cutting wood and other raw materials into pieces of certain specifications, drying, mixing with adhesives, additives, etc., and pressing at a certain temperature. The raw materials of particleboard are widely available, and the amount of glue used in the production process is small. The product has the characteristics of greater strength and higher stability, etc., and has a very broad development space in my country.
[0003] However, the existing particleboards are generally prepared by gluing wood particles, wood particles or wood powder with phenolic adhesives, urea-formaldehyde adhesives, acetal adhesives, and the furniture made therefrom has the problem of high formaldehyde content, which will cause serious pollution to human health and the environment; in addition, the particleboard material has poor flame retardancy and is prone to release a large amount of thick smoke when burned, posing a potential threat to people's life, property, safety and health. At the same time, the particleboard has low static bending strength and elastic modulus, and poor mechanical properties, which greatly limit the application of particleboard in furniture and other aspects.
[0004] Therefore, how to use formaldehyde-free raw materials to prepare particleboard, improve the static bending strength of particleboard during use, expand the application scenarios, and at the same time improve the flame retardant ability, reduce the smoke density level under combustion and decomposition conditions, thereby improving personal safety, has become a direction that needs to be focused on. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a formaldehyde-free particleboard production process for furniture production, aiming to solve the problems of high formaldehyde content, poor flame retardant performance, easy release of large amounts of thick smoke when burning, and poor static bending strength and elastic modulus of the existing particleboard.
[0006] The present invention uses silicon-containing corn straw shavings, nitrogen-containing corn starch adhesive, and nitrogen-containing corn starch adhesive. The raw materials are all biomass materials, which can effectively reduce the formaldehyde emission of the particle board. At the same time, through the synergistic effect of boron-silicon-nitrogen, the particle board can achieve high-efficiency flame retardancy and effectively reduce the smoke density level. In addition, the static bending strength and elastic modulus of the particle board are increased and enhanced through modification treatment.
[0007] The technical solution of the present invention is as follows:
[0008] The present invention provides a production process of formaldehyde-free particleboard for furniture production, which is characterized by comprising the following production steps:
[0009] Step S1: weighing 60 to 100 parts of wood chips, 30 to 50 parts of nitrogen-containing corn starch adhesive, and 2 to 10 parts of biomass additives;
[0010] Step S2: placing the wood shavings in an oven for drying to obtain dried wood shavings;
[0011] Step S3: fully stirring the dried wood chips, nitrogen-containing corn starch adhesive, and biomass additive to obtain a mixture;
[0012] Step S4: spray 0.2 to 1 part of release agent evenly on the mold;
[0013] Step S5: spreading the mixture evenly in the mold;
[0014] Step S6: pre-pressing the mixture together with the mold on a flat vulcanizer to obtain a pre-pressed sample;
[0015] Step S7: hot-pressing the pre-pressed sample together with the mold on a flat vulcanizer to obtain a hot-pressed sample;
[0016] Step S8: shaping the hot pressed sample together with the mold on a flat vulcanizer, releasing the pressure, and keeping the temperature constant at 80-100° C. for 2-5 minutes;
[0017] Step S9: naturally cool to room temperature, demould the product from the mold, and obtain a formaldehyde-free particleboard for furniture production.
[0018] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.
[0019] As a preferred technical solution of the present invention, the wood shavings in step S1 are silicon-containing corn stalk shavings.
[0020] Preferably, the preparation method of the silicon-containing corn straw shavings is as follows: weigh 50 parts of corn straw shavings, 30 parts of sodium silicate, and 100 parts of deionized water, add them into an impregnation tank, stir evenly, and evacuate to -0.1 MPa, and maintain the pressure for 1 hour; add 5 parts of polyethylene glycol to 100 parts of deionized water, stir and dissolve to obtain a polyethylene glycol solution, decompress the above-mentioned impregnation tank, add 20 parts of the polyethylene glycol solution, evacuate to -0.1 MPa, and maintain the pressure for 2 hours; after decompression, take out the impregnation, rinse the impregnation with deionized water 3 times, put it into a drying oven and set the temperature to 90°C, and treat it for 24 hours to obtain silicon-containing corn straw shavings.
[0021] After the corn straw shavings are impregnated with the sodium silicate modifier, a silicon dioxide network skeleton is formed in the duct by means of solidification and dehydration, thereby enhancing the static bending strength and elastic modulus of the particleboard; when the silicon-containing corn straw shavings are heated, the sodium silicate decomposes and removes the crystal water, turning into water vapor that absorbs most of the heat, dilutes the combustible gas, and forms inorganic silicon slag at high temperature that covers the surface of the particleboard to block the conduction of heat, thus having a good flame retardant effect.
[0022] As a preferred technical solution of the present invention, the preparation method of the nitrogen-containing corn starch adhesive in step S1 is: add 30 parts of corn starch to 300 parts of deionized water, stir evenly at a temperature of 65°C, then adjust the pH to 5, add 4 parts of sodium periodate to react for 1 hour; after the reaction is completed, adjust the pH to 2.5 to precipitate, repeatedly centrifuge and wash with deionized water, and vacuum dry to obtain oxidized corn starch; mix 10 parts of oxidized corn starch, 1 part of sodium hydroxide and 160 parts of deionized water, stir evenly, add 10 parts of polyethyleneimine to react for 48 hours, then adjust the pH to 2, centrifuge, wash, and dry to obtain the nitrogen-containing corn starch adhesive.
[0023] Corn starch is a biomass adhesive. It is modified with polyethyleneimine to obtain nitrogen-containing corn starch biomass adhesive. After hot pressing, the nitrogen-containing corn starch adhesive can be evenly dispersed in the gaps of the wood chips, wrapping and interpenetrating with the wood chips, filling most of the gaps, making the internal bonding of the particleboard tighter, thereby improving the mechanical strength of the particleboard. The nitrogen element in the nitrogen-containing corn starch adhesive can obtain a hindered amine structure with a quenching effect at high temperature, forming a non-flammable gas, and exerting a gas phase dilution effect, thereby improving the flame retardant efficiency.
[0024] As a preferred technical solution of the present invention, the biomass additive is a boron-containing sunflower oil additive.
[0025] Preferably, the preparation method of the boron-containing sunflower oil additive is: 100 parts of sunflower oil and 50 parts of diethanolamine are mixed evenly, the temperature is set to 160°C, and the reaction is stirred for 4 hours; then 10 parts of boric acid powder and 50 parts of solvent benzene are added, and the temperature is set to 75°C under a nitrogen atmosphere, and the reaction is carried out for 4 hours; after the reaction is completed, the solvent benzene is evaporated by reduced pressure distillation to obtain the boron-containing sunflower oil additive.
[0026] Preferably, the drying temperature in step S2 is 80-120° C., the drying time is 5-10 hours, and the moisture content of the wood chips after drying is 5-8%.
[0027] Preferably, the release agent in step S4 is dimethyl silicone oil.
[0028] Preferably, the pre-pressing temperature in step S6 is 80-100° C., the pressure is 1-2 MPa, and the time is 2-5 min.
[0029] Preferably, the hot pressing temperature in step S7 is 110-170° C., the pressure is 10-20 MPa, and the time is 30-50 min.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The wood chips, adhesives and additives of the present invention are all made of biomass materials. Biomass materials have the advantages of being green and environmentally friendly and renewable raw materials. There is no problem of formaldehyde and volatile organic pollutants being released during the preparation process and the use process. The formaldehyde emission of particleboard can be effectively reduced, meeting the demand for formaldehyde-free particleboard for furniture production.
[0032] (2) The boron element in the boron-containing biomass additive of the present invention decomposes under heat to produce boric anhydride or boric acid to form a glassy melt that covers the surface of the material, isolating the propagation of oxygen and heat, and can inhibit the generation of thick smoke and molten droplets. The silicon element in the silicon-containing corn stalk shavings has a low surface energy and is easy to migrate to the surface of the material to form a silicon-containing protective layer, thereby improving the thermal stability of the carbon layer on the surface of the material. The nitrogen element in the nitrogen-containing corn starch adhesive produces flame-retardant nitrogen-containing compounds at high temperatures to dilute the concentration of the combustion gas near the flame and exert a flame retardant effect. Through the synergistic effect of boron, silicon and nitrogen, efficient flame retardancy of the particleboard is achieved, and the smoke density level is effectively reduced. DETAILED DESCRIPTION
[0033] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0034] The sources of some components in the embodiments and comparative examples are as follows:
[0035] Wood shavings: poplar wood shavings (purchased from Wanhua Jingzhou Company), corn straw shavings (purchased from Wanhua Jingzhou Company);
[0036] Adhesive: corn starch adhesive (purchased from Shandong Pingdu Starch Co., Ltd.), urea-formaldehyde resin adhesive (purchased from Zibo Huasen Adhesive Co., Ltd.);
[0037] Additive: Formamide (CAS No. 75-12-7);
[0038] Release agent: dimethyl silicone oil (CAS No. 63148-62-9).
[0039] Preparation of silicon-containing corn straw shavings: weigh 50 parts of corn straw shavings (purchased from Wanhua Jingzhou Company), 30 parts of sodium silicate (CAS No. 1344-09-8), and 100 parts of deionized water, add them into an impregnation tank, stir evenly, and evacuate to -0.1 MPa, and maintain the pressure for 1 hour; add 5 parts of polyethylene glycol (brand CHPEG-1500, purchased from Changhua Chemical Technology Co., Ltd.) to 100 parts of deionized water, stir and dissolve to obtain a polyethylene glycol solution, depressurize the above-mentioned impregnation tank, add 20 parts of the polyethylene glycol solution, evacuate to -0.1 MPa, and maintain the pressure for 2 hours; after decompression, take out the impregnation, rinse the impregnation 3 times with deionized water, put it into a drying oven and set the temperature to 90°C, and obtain silicon-containing corn straw shavings after treating for 24 hours.
[0040] Preparation of nitrogen-containing corn starch adhesive: 30 parts of corn starch (purchased from Shandong Pingdu Starch Co., Ltd.) are added to 300 parts of deionized water, stirred evenly at a temperature of 65°C, then the pH is adjusted to 5, and 4 parts of sodium periodate (CAS No. 7790-28-5) are added to react for 1 hour; after the reaction is completed, the pH is adjusted to 2.5 to precipitate, and the precipitate is repeatedly centrifuged and washed with deionized water, and vacuum dried to obtain oxidized corn starch; 10 parts of oxidized corn starch, 1 part of sodium hydroxide (CAS No. 1310-73-2) and 160 parts of deionized water are mixed, stirred evenly, 10 parts of polyethyleneimine (CAS No. 9002-98-6) are added to react for 48 hours, and then the pH is adjusted to 2, centrifuged, washed, and dried to obtain a nitrogen-containing corn starch adhesive.
[0041] Preparation of boron-containing sunflower oil additive: 100 parts of sunflower oil (purchased from Shanghai Kerry Grain and Oil Industry Co., Ltd.) and 50 parts of diethanolamine (CAS No. 111-42-2) were mixed evenly, the temperature was set to 160°C, and the reaction was stirred for 4 hours; then 10 parts of boric acid powder (CAS No. 10043-35-3) and 50 parts of solvent benzene (CAS No. 71-43-2) were added, and the temperature was set to 75°C under a nitrogen atmosphere, and the reaction was carried out for 4 hours; after the reaction was completed, the solvent benzene was distilled off under reduced pressure to obtain a boron-containing sunflower oil additive.
[0042] Example 1
[0043] This embodiment provides a production process of formaldehyde-free particleboard for furniture production, comprising the following production steps:
[0044] Step S1: weighing 100 parts of silicon-containing corn straw shavings, 50 parts of nitrogen-containing corn starch adhesive, and 10 parts of boron-containing sunflower oil additive;
[0045] Step S2: putting the wood shavings into an oven for drying at a drying temperature of 120° C. for a drying time of 5 hours to obtain dried wood shavings having a moisture content of 5%;
[0046] Step S3: fully stirring the dried wood chips, the nitrogen-containing corn starch adhesive, and the boron-containing sunflower oil additive to obtain a mixture;
[0047] Step S4: spraying 1 part of mold release agent dimethyl silicone oil evenly on the mold;
[0048] Step S5: spreading the mixture evenly in the mold;
[0049] Step S6: pre-pressing the mixture together with the mold on a flat vulcanizer at a pre-pressing temperature of 100° C., a pressure of 2 MPa, and a time of 2 min to obtain a pre-pressed sample;
[0050] Step S7: hot-pressing the pre-pressed sample together with the mold on a flat vulcanizer at a temperature of 170° C., a pressure of 20 MPa, and a time of 30 min to obtain a hot-pressed sample;
[0051] Step S8: shaping the hot-pressed sample together with the mold on a flat vulcanizer, releasing the pressure, and keeping the temperature constant at 100° C. for 2 minutes;
[0052] Step S9: naturally cool to room temperature, demould the product from the mold, and obtain a formaldehyde-free particleboard for furniture production.
[0053] Example 2
[0054] This embodiment provides a production process of formaldehyde-free particleboard for furniture production, comprising the following production steps:
[0055] Step S1: weighing 60 parts of silicon-containing corn straw shavings, 30 parts of nitrogen-containing corn starch adhesive, and 2 parts of boron-containing sunflower oil additive;
[0056] Step S2: putting the wood shavings into an oven for drying at a drying temperature of 80° C. for a drying time of 10 h to obtain dried wood shavings having a moisture content of 8%;
[0057] Step S3: fully stirring the dried wood chips, the nitrogen-containing corn starch adhesive, and the boron-containing sunflower oil additive to obtain a mixture;
[0058] Step S4: spray 0.2 parts of release agent dimethyl silicone oil evenly on the mold;
[0059] Step S5: spreading the mixture evenly in the mold;
[0060] Step S6: pre-pressing the mixture together with the mold on a flat vulcanizer at a pre-pressing temperature of 80° C., a pressure of 1 MPa, and a time of 5 min to obtain a pre-pressed sample;
[0061] Step S7: hot-pressing the pre-pressed sample together with the mold on a flat vulcanizer at a temperature of 110° C., a pressure of 10 MPa, and a time of 50 min to obtain a hot-pressed sample;
[0062] Step S8: shaping the hot-pressed sample together with the mold on a flat vulcanizer, releasing the pressure, and keeping the temperature constant at 80° C. for 5 minutes;
[0063] Step S9: naturally cool to room temperature, demould the product from the mold, and obtain a formaldehyde-free particleboard for furniture production.
[0064] Example 3
[0065] This embodiment provides a production process of formaldehyde-free particleboard for furniture production, comprising the following production steps:
[0066] Step S1: weighing 80 parts of silicon-containing corn straw shavings, 40 parts of nitrogen-containing corn starch adhesive, and 5 parts of boron-containing sunflower oil additive;
[0067] Step S2: putting the wood shavings into an oven for drying at a drying temperature of 90° C. for a drying time of 8 hours to obtain dried wood shavings having a moisture content of 6%;
[0068] Step S3: fully stirring the dried wood chips, the nitrogen-containing corn starch adhesive, and the boron-containing sunflower oil additive to obtain a mixture;
[0069] Step S4: spray 0.5 parts of release agent dimethyl silicone oil evenly on the mold;
[0070] Step S5: spreading the mixture evenly in the mold;
[0071] Step S6: pre-pressing the mixture together with the mold on a flat vulcanizer at a pre-pressing temperature of 90° C., a pressure of 2 MPa, and a time of 4 min to obtain a pre-pressed sample;
[0072] Step S7: hot-pressing the pre-pressed sample together with the mold on a flat vulcanizer at a temperature of 150° C., a pressure of 18 MPa, and a time of 40 min to obtain a hot-pressed sample;
[0073] Step S8: shaping the hot-pressed sample together with the mold on a flat vulcanizer, releasing the pressure, and keeping the temperature constant at 90° C. for 4 minutes;
[0074] Step S9: naturally cool to room temperature, demould the product from the mold, and obtain a formaldehyde-free particleboard for furniture production.
[0075] Example 4
[0076] This embodiment provides a production process for formaldehyde-free particleboard for furniture production. The only difference from Example 1 is that in this example, 100 parts of silicon-containing corn straw shavings are replaced with 100 parts of poplar shavings, and the rest is the same as Example 1.
[0077] Example 5
[0078] This embodiment provides a production process for formaldehyde-free particleboard for furniture production. The only difference from Example 1 is that in this example, 50 parts of nitrogen-containing corn starch adhesive are replaced with 20 parts of corn starch adhesive and 30 parts of urea-formaldehyde resin adhesive, and the rest is the same as Example 1.
[0079] Example 6
[0080] This embodiment provides a production process of formaldehyde-free particleboard for furniture production. The only difference from Embodiment 1 is that in this embodiment, 10 parts of boron-containing sunflower oil additive are replaced with 10 parts of formamide additive, and the rest is the same as Embodiment 1.
[0081] Comparative Example 1
[0082] This comparative example provides a particleboard production process, comprising the following production steps:
[0083] Step S1: weighing 100 parts of poplar wood shavings, 20 parts of corn starch adhesive, 30 parts of urea-formaldehyde resin adhesive, and 10 parts of formamide additive;
[0084] Step S2: putting the wood shavings into an oven for drying at a drying temperature of 120° C. for a drying time of 5 hours to obtain dried wood shavings having a moisture content of 5%;
[0085] Step S3: fully stirring the dried wood chips, adhesive and additives to obtain a mixture;
[0086] Step S4: spraying 1 part of mold release agent dimethyl silicone oil evenly on the mold;
[0087] Step S5: spreading the mixture evenly in the mold;
[0088] Step S6: pre-pressing the mixture together with the mold on a flat vulcanizer at a pre-pressing temperature of 100° C., a pressure of 2 MPa, and a time of 2 min to obtain a pre-pressed sample;
[0089] Step S7: hot-pressing the pre-pressed sample together with the mold on a flat vulcanizer at a temperature of 170° C., a pressure of 20 MPa, and a time of 30 min to obtain a hot-pressed sample;
[0090] Step S8: shaping the hot-pressed sample together with the mold on a flat vulcanizer, releasing the pressure, and keeping the temperature constant at 100° C. for 2 minutes;
[0091] Step S9: Cool naturally to room temperature, demould the product from the mold, and obtain a particleboard.
[0092] Comparative Example 2
[0093] This comparative example provides a particleboard production process, which differs from comparative example 1 only in that 100 parts of poplar wood shavings are replaced with 100 parts of silicon-containing corn straw shavings in this comparative example, and the rest is the same as comparative example 1.
[0094] Comparative Example 3
[0095] This comparative example provides a particleboard production process, which is different from Comparative Example 1 only in that 20 parts of corn starch adhesive and 30 parts of urea-formaldehyde resin adhesive are replaced with 50 parts of nitrogen-containing corn starch adhesive in this comparative example, and the rest is the same as Comparative Example 1.
[0096] The performance of the particleboard provided in the above embodiments and comparative examples was tested, and the performance tests included formaldehyde emission, static bending strength, elastic modulus, smoke density rating (SDR) level, and limiting oxygen index (LOI). The specific test methods are as follows:
[0097] Formaldehyde emission: Tested in accordance with the requirements of GB 18580-2017 Limits of formaldehyde emission from artificial boards and their products for interior decoration and renovation materials.
[0098] Static bending strength: Tested in accordance with the requirements of GB / T 4897-2015 Particleboard.
[0099] Elastic modulus: Tested in accordance with the requirements of GB / T 4897-2015 Particleboard.
[0100] Smoke density rating (SDR): Tested in accordance with the requirements of GB / T 8627-2007 Test method for smoke density of burning or decomposition of building materials.
[0101] Limiting oxygen index (LOI): Tested with reference to the requirements of GB / T 2406.2-2009 Plastics - Oxygen index method for combustion behavior - Part 2: Room temperature test.
[0102] The above performance test data is shown in Table 1.
[0103] Table 1 Performance test results
[0104]
[0105] From the above content, it can be seen that the present invention uses biomass materials such as silicon-containing corn stalk shavings, nitrogen-containing corn starch adhesives, and nitrogen-containing corn starch adhesives as raw materials to prepare formaldehyde-free particleboards for furniture production (Examples 1 to 3), which have no detected formaldehyde emission, a static bending strength of 15.1 to 15.4 MPa, an elastic modulus of 1488.6 to 1489.5 MPa, a smoke density rating (SDR) of 36.72 to 36.77, and a limiting oxygen index (LOI) of 40.0 to 40.5.
[0106] Compared with Example 1, if silicon-containing corn straw shavings are not used, the static bending strength and elastic modulus decrease, the flame retardant effect deteriorates, and the smoke density level increases (Example 4); compared with Example 1, if nitrogen-containing corn starch adhesive is not used, the formaldehyde emission increases, the static bending strength and elastic modulus decrease, the flame retardant effect deteriorates, and the smoke density level increases (Example 5); compared with Example 1, if the boron-containing sunflower oil additive is not used, the formaldehyde emission increases, the flame retardant effect deteriorates, and the smoke density level increases (Example 6).
[0107] Comparative Example 1 does not adopt the technical innovation of the present invention, so the performance is poor, and the formaldehyde emission is 0.33 mg / m 3 , the static bending strength is 12.5MPa, the elastic modulus is 1237.3MPa, the smoke density rating (SDR) is 46.14, and the limiting oxygen index (LOI) is 31.4. Compared with comparative example 1, if silicon-containing corn stalk shavings are used, the static bending strength and elastic modulus increase, and the limiting oxygen index is improved (Comparative example 2); compared with comparative example 1, if nitrogen-containing corn starch adhesive is used, the formaldehyde emission is reduced, the static bending strength and elastic modulus increase, and the limiting oxygen index is improved (Comparative example 3).
[0108] In summary, the present invention uses silicon-containing corn straw shavings, nitrogen-containing corn starch adhesive, and nitrogen-containing corn starch adhesive, and the raw materials are all biomass materials, which can effectively reduce the formaldehyde emission of particleboard. At the same time, through the synergistic effect of boron-silicon-nitrogen, the particleboard can achieve high-efficiency flame retardancy and effectively reduce the smoke density level. In addition, the static bending strength and elastic modulus of the particleboard are increased and enhanced through modification treatment.
[0109] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A process for producing formaldehyde-free particleboard for furniture production, characterized in that: The production steps include: Step S1: weighing 60 to 100 parts of wood chips, 30 to 50 parts of nitrogen-containing corn starch adhesive, and 2 to 10 parts of biomass additives; Step S2: placing the wood shavings in an oven for drying to obtain dried wood shavings; Step S3: fully stirring the dried wood chips, nitrogen-containing corn starch adhesive, and biomass additive to obtain a mixture; Step S4: spray 0.2 to 1 part of release agent evenly on the mold; Step S5: spreading the mixture evenly in the mold; Step S6: pre-pressing the mixture together with the mold on a flat vulcanizer to obtain a pre-pressed sample; Step S7: hot-pressing the pre-pressed sample together with the mold on a flat vulcanizer to obtain a hot-pressed sample; Step S8: shaping the hot-pressed sample together with the mold on a flat vulcanizer, releasing the pressure, and keeping the temperature constant at 80-100° C. for 2-5 minutes; Step S9: naturally cool to room temperature, demould the product from the mold, and obtain a formaldehyde-free particleboard for furniture production.
2. The process for producing formaldehyde-free particleboard for furniture production according to claim 1, characterized in that: The wood shavings in step S1 are silicon-containing corn stalk shavings.
3. The process for producing formaldehyde-free particleboard for furniture production according to claim 2, characterized in that: The preparation method of the silicon-containing corn straw shavings is as follows: 50 parts of corn straw shavings, 30 parts of sodium silicate and 100 parts of deionized water are weighed and added into an impregnation tank, and the mixture is evenly stirred and then vacuumed to -0.1 MPa, and the pressure is maintained for 1 hour; 5 parts of polyethylene glycol are added into 100 parts of deionized water, and the mixture is stirred and dissolved to obtain a polyethylene glycol solution, and the above-mentioned impregnation tank is depressurized and then 20 parts of the polyethylene glycol solution are added, and the mixture is vacuumed to -0.1 MPa, and the pressure is maintained for 2 hours; after the decompression, the impregnated material is taken out, and the impregnated material is rinsed with deionized water for 3 times, and the impregnated material is put into a drying oven and the temperature is set to 90° C., and the silicon-containing corn straw shavings are obtained after the treatment for 24 hours.
4. The process for producing formaldehyde-free particleboard for furniture production according to claim 1, characterized in that: The preparation method of the nitrogen-containing corn starch adhesive in step S1 is as follows: 30 parts of corn starch are added to 300 parts of deionized water, and stirred evenly at a temperature of 65° C., then the pH is adjusted to 5, and 4 parts of sodium periodate are added to react for 1 hour; after the reaction is completed, the pH is adjusted to 2.5 to precipitate, and the precipitate is repeatedly centrifuged and washed with deionized water, and vacuum dried to obtain oxidized corn starch; 10 parts of oxidized corn starch, 1 part of sodium hydroxide and 160 parts of deionized water are mixed, stirred evenly, 10 parts of polyethyleneimine are added to react for 48 hours, and then the pH is adjusted to 2, centrifuged, washed, and dried to obtain the nitrogen-containing corn starch adhesive.
5. The process for producing formaldehyde-free particleboard for furniture production according to claim 1, characterized in that: The biomass additive is a boron-containing sunflower oil additive.
6. A process for producing formaldehyde-free particleboard for furniture production according to claim 5, characterized in that: The preparation method of the boron-containing sunflower oil additive is as follows: 100 parts of sunflower oil and 50 parts of diethanolamine are mixed evenly, the temperature is set to 160° C., and the mixture is stirred for reaction for 4 hours; then 10 parts of boric acid powder and 50 parts of solvent benzene are added, the temperature is set to 75° C. under a nitrogen atmosphere, and the mixture is reacted for 4 hours; after the reaction is completed, the solvent benzene is evaporated by reduced pressure distillation to obtain the boron-containing sunflower oil additive.
7. The process for producing formaldehyde-free particleboard for furniture production according to claim 1, characterized in that: The drying temperature in step S2 is 80-120° C., the drying time is 5-10 hours, and the moisture content of the wood chips after drying is 5-8%.
8. The process for producing formaldehyde-free particleboard for furniture production according to claim 1, characterized in that: The release agent in step S4 is dimethyl silicone oil.
9. The process for producing formaldehyde-free particleboard for furniture production according to claim 1, characterized in that: The pre-pressing temperature in step S6 is 80-100° C., the pressure is 1-2 MPa, and the time is 2-5 min.
10. The process for producing formaldehyde-free particleboard for furniture production according to claim 1, characterized in that: The hot pressing temperature in step S7 is 110-170° C., the pressure is 10-20 MPa, and the time is 30-50 min.
Citation Information
Patent Citations
Modified boric acid ester interface activating agent and preparation method thereof
CN102000527A
Production method of light particle board
CN107671979A
Preparation method for formaldehyde-free high-strength moisture-proof shaving board
CN108162120A
High water-resistant wood adhesive material
CN110499135A
Aldehyde-free environment-friendly shaving board and preparation method thereof
CN116674049A
Cited By
Lysimachia barystachys fiber board and preparation method thereof
CN121105158A
Flame-retardant biological base material without formaldehyde release and preparation method thereof
CN122034105A
A non-formaldehyde-releasing flame-retardant bio-based material and a method for preparing the same
CN122034105B