Acrylate adhesive, adhesive composition and protective film

By preparing an acrylic adhesive composition with specific viscosity and adhesion, the problem of small molecules remaining in the domestic protective film in the semiconductor process is solved, and the cleanliness of the wafer surface and the continuity of the process are achieved.

CN118956299AInactive Publication Date: 2024-11-15ZHEJIANG DONGROU NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411016338.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-27
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Domestic protective films have small molecule residue problems during the back grinding and chip removal of semiconductor wafers, which contaminates the wafer surface and affects the process quality.

Method used

By using the preparation method of acrylate adhesive, different monomers, thermal initiators and solvents are mixed in a nitrogen atmosphere to form an adhesive composition with specific viscosity and adhesion, and mixed with curing agent, photoinitiator and UV resin. , an adhesive composition is formed, and a protective film is coated on the substrate to ensure that it does not fall off after ultraviolet rays.

Benefits of technology

It effectively avoids small molecules residues, ensures the cleanliness of the wafer surface and the continuity of the process, and ensures the normal progress of the semiconductor front-end grinding, thinning and chip extraction processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956299A_ABST
    Figure CN118956299A_ABST
Patent Text Reader

Abstract

The invention discloses an acrylate adhesive, an adhesive composition and a protective film. The preparation method comprises the following steps: mixing a first monomer, a second monomer and a third monomer in percentage by weight, adding a certain amount of a thermal initiator and a first solvent, copolymerizing in a nitrogen atmosphere, removing nitrogen, adding a certain proportion of a fourth monomer, and continuously reacting for 2 hours to obtain the required adhesive. And mixing the curing agent, the photoinitiator, the UV resin, the second solvent and the acrylate adhesive to form the adhesive composition. The adhesive composition is coated on a base material, and a release film is covered on the adhesive composition to obtain the protective film. The protective film manufactured by the invention can be widely applied to process protection of grinding, thinning and taking processes of the front end of a semiconductor, and ensures that a silicon wafer is not broken or broken in the whole process, and the surface of the wafer is free of small molecule residues and free of pollution to the surface of the wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesive tapes, and in particular relates to an acrylic ester adhesive, an adhesive composition and a protective film. Background Art

[0002] In the front-end process of semiconductor wafer back grinding and wafer removal, the silicon wafer needs to be protected by a film, and then the grinding, wafer thinning, cutting and wafer removal are carried out. In order to protect the silicon wafer from damage, a protective film is usually attached to the silicon wafer before grinding. The protective film usually has a high adhesion to prevent the wafer and the protective film from falling off. After ultraviolet irradiation, the adhesion of the protective film can be rapidly reduced, which can facilitate the pickup of the chip.

[0003] At present, the protective films used by domestic semiconductor manufacturers are mostly provided by foreign manufacturers. Most domestic protective films have the problem of small molecule residues, which will contaminate the wafer surface. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides an acrylate adhesive, an adhesive composition and a protective film made therefrom, which can solve the problem of small molecule residues.

[0005] The technical scheme adopted by the present invention is: a method for preparing an acrylic adhesive, by weight percentage, 60-70% of a first monomer, 10-20% of a second monomer, and 0-5% of a third monomer are mixed, and then a certain amount of a thermal initiator and a first solvent are added, copolymerized under a nitrogen atmosphere, and then the nitrogen is removed, and a certain proportion of a fourth monomer is added, and the reaction is continued for 2 hours to obtain the desired adhesive. The first monomer includes one or more of butyl acrylate, isooctyl acrylate, and ethyl acrylate, the second monomer includes one or more of methyl acrylate, methyl methacrylate, butyl methacrylate, vinyl acetate, and styrene, and the third monomer includes one or more of hydroxyethyl acrylate, hydroxybutyl acrylate, hydroxypropyl acrylate, acrylic acid, and methacrylic acid. The fourth monomer includes one or more of isocyanoethyl methacrylate and isocyanoethyl acrylate. The thermal initiator is an azo or peroxide, and the first solvent is one or more of ethyl acetate, toluene, and butanone.

[0006] As a preferred embodiment of the above technical solution, the thermal initiator is one or more of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, dibenzoyl peroxide, and lipid peroxide.

[0007] As a preferred embodiment of the above technical solution, different proportions of the first monomer, the second monomer, the third monomer, the thermal initiator, and the first solvent are weighed and put into a container, heated in a water bath and stirred, and then nitrogen is passed into the container for 30 minutes. Under the protection of nitrogen, the water bath is heated to react for about 2-4 hours, and then the nitrogen is removed, and the fourth monomer is added thereto, and the reaction is continued for 2 hours to obtain the acrylic adhesive.

[0008] The acrylic adhesive is prepared by the above preparation method.

[0009] The adhesive composition is formed by mixing a curing agent, a photoinitiator, a UV resin, a second solvent and the above-mentioned acrylate adhesive. The adhesive composition includes 50-60 parts of acrylate adhesive, 0.01-0.1 parts of curing agent, 0.1-0.5 parts of photoinitiator, 5-10 parts of UV resin, and 40-60 parts of solvent by weight. Different monomer combinations and different molecular weights and molecular weight distributions can make PSA have different viscosity, holding force and adhesion. The curing agent is an isocyanate curing agent, and the photoinitiator is one or more of benzoin, isopropyl benzoin ether, isobutyl benzoin ether, benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, and 2-hydroxy-2-methyl-1-phenylacetone-1-ketone. The purpose of the curing agent is to cross-link with PSA to form a network structure to improve properties such as cohesion and heat resistance. The main function of the photoinitiator is to generate photo free radicals under ultraviolet light, and the photo free radicals open the carbon-carbon double bonds in the PSA, causing the molecular weight to rise sharply, thereby achieving the purpose of reducing viscosity. The UV resin is a polyurethane acrylate oligomer, and the urethane acrylate oligomer is obtained by reacting a polyester-type or polyether-type polyol compound with a polyvalent isocyanate compound such as a (methyl) acrylate having a hydroxyl group and a polyvalent isocyanate to obtain a urethane prepolymer. The role of the UV resin is that the carbon-carbon double bonds of the low molecular weight UV resin itself can further reduce the peeling force after UV, and the specific carbon-carbon double bond functionality is difunctional, tetrafunctional, hexafunctional, decafunctional, etc. The second solvent includes one or more of ethyl acetate, toluene, butanone, and butyl acetate. The main function of the second solvent is to dilute the PSA mixture, which is conducive to coating.

[0010] As a preferred embodiment of the above technical solution, the curing agent is one or more of 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate.

[0011] The protective film comprises a substrate, the substrate is coated with the above adhesive composition, and the adhesive composition is covered with a release film.

[0012] As a preferred embodiment of the above technical solution, the substrate is one or more of ethylene terephthalate film, polyethylene film, polyvinyl chloride film, polypropylene film, and PO film.

[0013] As a preferred embodiment of the above technical solution, the thickness of the substrate is one or more of 10um, 20um, 50um, 80um, 100um, 140um, preferably 100um or 140um. The coating thickness of the adhesive composition on the substrate is 5um, 10um, 15um, 20um or 40um, preferably 20um or 40um. The thickness of the release film is 38um, 50um, 75um, 100um or 150um, preferably 38um or 50um.

[0014] The beneficial effect of the present invention is that the protective film manufactured by the present invention can be widely used in process protection of semiconductor front-end grinding, thinning, and wafer removal processes, ensuring that the silicon wafer is not fragmented or broken during the entire process, and there is no small molecule residue on the wafer surface, and there is no pollution to the wafer surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a structural schematic diagram of the present invention. DETAILED DESCRIPTION

[0016] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] Example 1

[0018] Acrylate adhesive: 20 g butyl acrylate, 60 g isooctyl acrylate, 10 g butyl methacrylate, 8 g hydroxyethyl acrylate, 2 g acrylic acid, 0.05 g thermal initiator (azobisisobutyronitrile), and 150 g solvent (ethyl acetate) were weighed and added into a 500 ml three-necked flask in sequence. 2 Under protection, the temperature was raised to 80°C for reaction for 6 hours, then N2 was removed, 2 g of isocyanoethyl methacrylate was added to the three-necked flask, and the reaction was continued for 2 hours to obtain adhesive 1;

[0019] Acrylate adhesive composition: 110 g of adhesive, 0.05 g of isocyanate curing agent TDI, 10.1 g of photoinitiator 651, 0.5 g of UV resin (polyurethane acrylate oligomer), and 5 g of solvent (ethyl acetate) were weighed and stirred to obtain PSA composition 1;

[0020] The protective film comprises a release film layer of 38 μm, a PSA composition of 140 μm, and a PO substrate of 140 μm. The PSA composition 1 is coated on the release film, dried in an oven at 100° C. for 3 min, and then transferred and pasted on the PO film substrate to obtain the desired UV protective film 1 (such as Figure 1 shown);

[0021] Example 2 (Compared with Example 1, the amount of isocyanoethyl methacrylate in the acrylic adhesive formulation is increased from 2g to 4g)

[0022] Acrylate adhesive: 20 g butyl acrylate, 60 g isooctyl acrylate, 10 g butyl methacrylate, 8 g hydroxyethyl acrylate, 2 g acrylic acid, 0.05 g thermal initiator (azobisisobutyronitrile), and 150 g solvent (ethyl acetate) were weighed and added into a 500 ml three-necked flask in sequence. 2 Under protection, the temperature was raised to 80°C for reaction for 6 hours, then N2 was removed, 4 g of isocyanoethyl methacrylate was added to the three-necked flask, and the reaction was continued for 2 hours to obtain adhesive 2;

[0023] Acrylate adhesive composition: 210 g of adhesive, 0.05 g of isocyanate curing agent TDI, 0.1 g of photoinitiator 651, 0.5 g of UV resin (polyurethane acrylate oligomer), and 5 g of solvent (ethyl acetate) were weighed and stirred to obtain PSA composition 2;

[0024] The protective film comprises a release film layer of 38 μm, a PSA composition of 240 μm, and a PO substrate of 140 μm. The PSA composition 2 is coated on the release film, dried in an oven at 100° C. for 3 min, and then transferred and pasted on the PO film substrate to obtain the desired protective film 2 (such as Figure 1 shown);

[0025] Example 3 (Compared with Example 2, the amount of isocyanoethyl methacrylate in the acrylic adhesive formulation is increased from 4g to 7.5g)

[0026] Acrylate adhesive: 20 g butyl acrylate, 60 g isooctyl acrylate, 10 g butyl methacrylate, 8 g hydroxyethyl acrylate, 2 g acrylic acid, 0.05 g thermal initiator (azobisisobutyronitrile), and 150 g solvent (ethyl acetate) were weighed and added into a 500 ml three-necked flask in sequence. 2 Under protection, the temperature was raised to 80°C for reaction for 6 hours, then N2 was removed, 7.5 g of isocyanoethyl methacrylate was added to the three-necked flask, and the reaction was continued for 2 hours to obtain adhesive 3;

[0027] Acrylate adhesive composition: 310 g of adhesive, 0.05 g of isocyanate curing agent TDI, 0.1 g of photoinitiator 651, 0.5 g of UV resin (polyurethane acrylate oligomer), and 5 g of solvent (ethyl acetate) were weighed and stirred to obtain PSA composition 3;

[0028] A protective film, comprising a release film layer of 38 μm, a PSA composition of 340 μm, and a PO substrate of 140 μm, wherein the PSA composition 3 is coated on the release film, dried in an oven at 100° C. for 3 min, and then transferred and pasted on the PO film substrate to obtain the desired protective film 3 (such as Figure 1 shown);

[0029] Example 4 (Compared with Example 3, butyl acrylate is removed from the acrylic adhesive formulation, and butyl methacrylate is replaced with methyl methacrylate)

[0030] Acrylate adhesive: weigh 70 g of isooctyl acrylate, 20 g of methyl methacrylate, 8 g of hydroxyethyl acrylate, 2 g of acrylic acid, 0.05 g of thermal initiator (azobisisobutyronitrile), and 150 g of solvent (ethyl acetate), and add them into a 500 ml three-necked flask in sequence. 2 Under protection, the temperature was raised to 80°C for reaction for 6 hours, then N2 was removed, 7.5 g of isocyanoethyl methacrylate was added to the three-necked flask, and the reaction was continued for 2 hours to obtain adhesive 4;

[0031] Acrylate adhesive composition: 410 g of adhesive, 0.05 g of isocyanate curing agent TDI, 10.1 g of photoinitiator 65, 0.5 g of UV resin (polyurethane acrylate oligomer), and 5 g of solvent (ethyl acetate) were weighed and stirred to obtain PSA composition 4;

[0032] The protective film comprises a release film layer of 38 μm, a PSA composition of 440 μm, and a PO substrate of 140 μm. The PSA composition 4 is coated on the release film, dried in an oven at 100° C. for 3 min, and then transferred and pasted on the PO film substrate to obtain the desired protective film 4 (such as Figure 1 shown);

[0033] Example 5 (Compared with Example 4, the amount of isooctyl acrylate in the acrylic adhesive formulation is reduced, and the amounts of methyl methacrylate, hydroxyethyl acrylate, and isocyanoethyl methacrylate are increased, and acrylic acid is removed)

[0034] Acrylate adhesive: weigh 55 g of isooctyl acrylate, 25 g of methyl methacrylate, 20 g of hydroxyethyl acrylate, 0.05 g of thermal initiator (azobisisobutyronitrile), and 150 g of solvent (ethyl acetate), and add them into a 500 ml three-necked flask in sequence. 2Under protection, the temperature was raised to 80°C for reaction for 6 hours, then N2 was removed, 15 g of isocyanoethyl methacrylate was added to the three-necked flask, and the reaction was continued for 2 hours to obtain adhesive 5;

[0035] Acrylate adhesive composition: 510 g of adhesive, 0.05 g of isocyanate curing agent TDI, 6510.1 g of photoinitiator, 0.5 g of UV resin (polyurethane acrylate oligomer), and 5 g of solvent (ethyl acetate) were weighed and stirred to obtain PSA composition 5;

[0036] The protective film comprises a release film layer of 38 μm, a PSA composition of 540 μm, and a PO substrate of 140 μm. The PSA composition 5 is coated on the release film, dried in an oven at 100° C. for 3 min, and then transferred and pasted on the PO film substrate to obtain the desired protective film 5 (such as Figure 1 shown);

[0037] Example 6 (Compared with Example 5, isooctyl acrylate in the acrylate adhesive formula is replaced with butyl acrylate, and the amounts of isocyanoethyl methacrylate and hydroxyethyl acrylate are increased)

[0038] Acrylate adhesive: weigh 50 g butyl acrylate, 20 g methyl methacrylate, 30 g hydroxyethyl acrylate, 0.05 g thermal initiator (azobisisobutyronitrile), and 150 g solvent (ethyl acetate), and add them into a 500 ml three-necked flask in sequence. 2 Under protection, the temperature was raised to 80°C for reaction for 6 hours, then N2 was removed, 27 g of isocyanoethyl methacrylate was added to the three-necked flask, and the reaction was continued for 2 hours to obtain adhesive 6;

[0039] Acrylate adhesive composition: 610 g of adhesive, 0.05 g of isocyanate curing agent TDI, 6510.1 g of photoinitiator, 0.5 g of UV resin (polyurethane acrylate oligomer), and 5 g of solvent (ethyl acetate) were weighed and stirred to obtain PSA composition 6;

[0040] The protective film comprises a release film layer of 38 μm, a PSA composition of 640 μm, and a PO substrate of 140 μm. The PSA composition 6 is coated on the release film, dried in an oven at 100° C. for 3 min, and then transferred and pasted on the PO film substrate to obtain the desired protective film 6 (such as Figure 1 shown);

[0041] Comparative Example 1 (Compared with Example 1, isocyanoethyl methacrylate in the acrylic adhesive formula is removed)

[0042] Acrylate adhesive: 20 g butyl acrylate, 60 g isooctyl acrylate, 10 g butyl methacrylate, 8 g hydroxyethyl acrylate, 2 g acrylic acid, 0.05 g thermal initiator (azobisisobutyronitrile), and 150 g solvent (ethyl acetate) were weighed and added into a 500 ml three-necked flask in sequence. 2 Under protection, the temperature was raised to 80°C for reaction for 6 hours to obtain adhesive 7;

[0043] Acrylate adhesive composition: 710 g of adhesive, 0.05 g of isocyanate curing agent TDI, 6510.1 g of photoinitiator, 0.5 g of UV resin (polyurethane acrylate oligomer), and 5 g of solvent (ethyl acetate) were weighed and stirred to obtain PSA composition 7;

[0044] The protective film comprises a release film layer of 38 μm, a PSA composition of 140 μm, and a PO substrate of 140 μm. The PSA composition 7 is coated on the release film, dried in an oven at 100° C. for 3 min, and then transferred and pasted on the PO film substrate to obtain the desired protective film 7 (such as Figure 1 shown);

[0045] Comparative Example 2 (Compared with Example 6, the amount of isocyanoethyl methacrylate in the acrylic adhesive formula was increased)

[0046] Acrylate adhesive: 50 g butyl acrylate, 20 g methyl methacrylate, 30 g hydroxyethyl acrylate, 0.05 g thermal initiator (azobisisobutyronitrile), and 150 g solvent (ethyl acetate) were weighed and added into a 500 ml three-necked flask in sequence. 2 Under protection, the temperature was raised to 80°C for reaction for 4 hours, then the nitrogen was removed, 35 g of isocyanoethyl methacrylate was added, and the reaction was continued for 2 hours to obtain adhesive 8;

[0047] Acrylate adhesive composition: 810 g of adhesive, 0.05 g of isocyanate curing agent TDI, 6510.1 g of photoinitiator, 0.5 g of UV resin (polyurethane acrylate oligomer), and 5 g of solvent (ethyl acetate) were weighed and stirred to obtain PSA composition 8;

[0048] The protective film comprises a release film layer of 38 μm, a PSA composition of 840 μm, and a PO substrate of 140 μm. The PSA composition 8 is coated on the release film, dried in an oven at 100° C. for 3 min, and then transferred and pasted on the PO film substrate to obtain the desired protective film 8 (such as Figure 1 shown);

[0049] The product obtained in the above embodiment was subjected to a performance test experiment, and the specific experimental data are as follows:

[0050]

[0051] From the above test results, it can be seen that in Example 1, Example 2, and Example 3, as the number of MOI grafting increases, the more double bonds grafted, the smaller the post-UV peeling force, and the less small molecule residues. In Example 3 and Example 4, the types and proportions of monomers are changed, and the same MOI grafting ratio is used, which has no effect on the small molecule residues and post-UV peeling force. In Example 5 and Example 6, in order to improve the initial adhesion performance of the glue, the proportion of short-chain monomers and monomers with stronger polarity is increased, and MOI grafting is used, and finally the small molecule residues and UV peeling force are very good. In Example 3 and Comparative Example 1, it is found that if there is no MOI grafting, the small molecule residues are more serious. In Example 6 and Comparative Example 2, the MOI grafting ratio is too high. Although there is no small molecule residue, too much remaining MOI will harden the glue, affecting the initial adhesion and peeling force of the glue.

[0052] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in this field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in this technical field through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the existing technology should be within the scope of protection determined by the claims.

Claims

1. A method for preparing an acrylic adhesive, characterized in that: Calculated by weight percentage, 60-70% of the first monomer, 10-20% of the second monomer, and 0-5% of the third monomer are mixed, and then a certain amount of thermal initiator and a first solvent are added, and copolymerization is carried out under a nitrogen atmosphere. Then the nitrogen is removed, and a certain proportion of the fourth monomer is added, and the reaction is continued for 2 hours to obtain the desired adhesive, wherein the first monomer includes one or more of butyl acrylate, isooctyl acrylate, and ethyl acrylate, the second monomer includes one or more of methyl acrylate, methyl methacrylate, butyl methacrylate, vinyl acetate, and styrene, the third monomer includes one or more of hydroxyethyl acrylate, hydroxybutyl acrylate, hydroxypropyl acrylate, acrylic acid, and methacrylic acid, the fourth monomer includes one or more of isocyanoethyl methacrylate and isocyanoethyl acrylate, the thermal initiator is an azo or peroxide, and the first solvent is one or more of ethyl acetate, toluene, and butanone.

2. The method for preparing an acrylic adhesive according to claim 1, wherein: The thermal initiator is one or more of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, dibenzoyl peroxide, and lipid peroxide.

3. The method for preparing the acrylic adhesive according to claim 1, wherein: The weighed first monomer, second monomer, third monomer, thermal initiator and first solvent are put into a container, heated in a water bath and stirred, and then nitrogen is passed into the container for 30 minutes. Under the protection of nitrogen, the water bath is heated to react for about 2-4 hours, and then the nitrogen is removed, and the fourth monomer is added thereto, and the reaction is continued for 2 hours to obtain the acrylic adhesive.

4. Acrylic adhesive, characterized in that: Prepared by the preparation method according to any one of claims 1 to 3.

5. An adhesive composition, characterized in that: A certain amount of curing agent, photoinitiator, UV resin, second solvent and the acrylate adhesive as claimed in claim 4 are mixed to form an adhesive composition, wherein the adhesive composition includes 50-60 parts of acrylate adhesive, 0.01-0.1 parts of curing agent, 0.1-0.5 parts of photoinitiator, 5-10 parts of UV resin and 40-60 parts of solvent by weight, wherein the curing agent is an isocyanate curing agent, the photoinitiator is one or more of benzoin, isopropyl benzoin ether, isobutyl benzoin ether, benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone and 2-hydroxy-2-methyl-1-phenylacetone-1-one, and the second solvent includes one or more of ethyl acetate, toluene, butanone and butyl acetate.

6. The adhesive composition according to claim 5, characterized in that The curing agent is one or more of 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate.

7. A protective film comprising a substrate, characterized in that: The substrate is coated with the adhesive composition as claimed in claim 5 or 6, and the adhesive composition is covered with a release film.

8. The protective film according to claim 7, characterized in that The substrate is one or more of ethylene terephthalate film, polyethylene film, polyvinyl chloride film, polypropylene film and PO film.

9. The protective film according to claim 8, characterized in that The thickness of the substrate is one or more of 10um, 20um, 50um, 80um, 100um, 140um, preferably 100um or 140um. The coating thickness of the adhesive composition on the substrate is 5um, 10um, 15um, 20um or 40um, preferably 20um or 40um. The thickness of the release film is 38um, 50um, 75um, 100um or 150um, preferably 38um or 50um.

Citation Information

Patent Citations

  • OCA resin composition, OCA adhesive tape and preparation method thereof

    CN109096441A

  • UV visbreaking adhesive and preparation method thereof

    CN116042140A

  • Surface protection film

    KR101205509B1

  • Ultraviolet-curable adhesive resin composition and adhesive tape for dicing or surface-protection comprising the same

    KR1020110131772A

Cited By

  • Protruding ball-mounting wafer thinning adhesive tape, preparation method thereof and wafer thinning machine

    CN121160243A