Method for preparing thin film wafer based on laser lift-off of heterogeneous substrate crystal thin film

The laser peeling technology solves the fragmentation problem caused by the difference in thermal expansion coefficient of heterogeneous material films at high temperatures, and achieves complete peeling of the films, simplifies the process and reduces costs, and is suitable for bonding structures of a variety of heterogeneous material.

CN118969628APending Publication Date: 2024-11-15SHANDONG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410844575.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the preparation process of the existing heterogeneous material lithium niobate/lithium tantalate single crystal thin film, due to the difference in thermal expansion coefficients between the silicon substrate and LiTaO3, the film is easily fragile during high temperature treatment, and when the traditional ion implantation method is peeled off at high temperature There is still a lobe problem.

Method used

The laser peeling technology is adopted to accurately control the laser focal length and act on the ion implantation layer to quickly peel the film, avoiding deformation and lobe problems caused by thermal expansion differences caused by overall heating.

Benefits of technology

The complete peeling of the film is achieved, avoiding the problem of lobes under high temperature treatment, the process is simple and efficient, shortens time and reduces cost, and is suitable for bonding structures of a variety of heterogeneous materials, with high process compatibility and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004915352260000011
    Figure HDA0004915352260000011
  • Figure HDA0004915352260000012
    Figure HDA0004915352260000012
  • Figure HDA0004915352260000021
    Figure HDA0004915352260000021
Patent Text Reader

Abstract

The invention relates to a method for preparing a thin film wafer based on laser lift-off of a heterogeneous substrate crystal thin film, which adopts a laser lift-off method to irradiate and project laser with high energy density on a thin film injection stop layer in an ultra-short time, so that injected ions of the stop layer are quickly heated and gasified, and the lift-off process of the thin film is quickly completed; the heating and cooling speed is high, and the heat aggregation property is high; in the injection ion gasification process, the upper-layer film wafer and the lower-layer substrate wafer are heated slightly, the deformation influence caused by thermal expansion difference of heterogeneous materials is basically avoided, the problem of wafer cracking caused by high-temperature treatment of bonding of the heterogeneous materials is avoided, and the bonding quality of the heterogeneous materials is improved. Complete stripping of thin film sheets bonded by heterogeneous materials is realized by adopting a simple and efficient method, and the method has relatively high process compatibility, can be suitable for thin film structures bonded by various heterogeneous materials, is easy to process, simple in procedure, short in time and low in cost, and provides a new method for crystal thin film processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a thin film wafer based on laser stripping of a heterogeneous substrate crystal film, and belongs to the technical field of integrated optical devices. Background Art

[0002] Heterojunction integrated lithium niobate / lithium tantalate single crystal thin films prepared on silicon substrate have wide applications in acoustic wave devices, optical signal processing, information storage and electronic devices. They can be used to make filters, optical waveguide modulators, optical waveguide switches, spatial light modulators, optical frequency doublers, surface acoustic wave generators, infrared detectors and ferroelectric memories, and have broad application prospects.

[0003] The existing preparation process of heterogeneous material lithium niobate / lithium tantalate single crystal thin film is usually to use ion implantation to obtain a lithium niobate / lithium tantalate single crystal wafer implanted sheet including a thin film layer, a separation layer and a residual layer. After the single crystal wafer implanted sheet is bonded to a silicon substrate, a bonded body is formed. The bonded body is heated and annealed to peel off the residual layer to obtain a lithium niobate / lithium tantalate single crystal thin film. During the annealing process, the implanted ions in the separation layer are heated to form gas, generating bubbles. The bubbles formed in the separation layer are connected to form a piece, so that the residual layer and the film layer are separated as a whole in an instant.

[0004] The thermal mismatch caused by the difference in thermal expansion coefficients of heterogeneous materials is the key issue in preparing single crystal films on a complete and defect-free support substrate. Taking silicon support substrate and LiTaO3 wafer as an example, the thermal expansion coefficient of silicon material is about 2.5K -1 , while the a-axis thermal expansion coefficient of LiTaO3 is about 16K- 1 Such a large thermal expansion coefficient causes the bonding structure of 4-inch silicon and lithium tantalate to break at around 140°C, making high-temperature processing impossible. The peeling temperature of the thin film prepared by ion implantation is usually higher than 140°C.

[0005] Patent document CN112259678A discloses a method and thin film material for improving the cracking of a thin film layer, comprising: injecting ions into the thin film wafer from the ion implantation surface of the thin film wafer to form a thin film layer, a separation layer and a residual layer in the thin film wafer corresponding to the ion implantation area; bonding the ion implantation surface of the thin film wafer to the bonding surface of the base layer to obtain a first bonding body; heat treating the first bonding body to obtain a second bonding body; grinding and polishing the remaining thin film wafer corresponding to the non-ion implantation area in the second bonding body, and the thin film layer to a target thickness. By retaining a circle of non-ion implantation area outside the ion implantation area, after ion injection, a thin film layer and a separation layer are formed only in the thin film wafer corresponding to the ion implantation area. Therefore, during bonding and separation, due to the existence of the remaining thin film wafer corresponding to the non-ion implantation area, the thin film layer will not instantly recover to a flat state from a warped state, thereby solving the problem of thin film layer bursting. This method still needs to complete the film peeling under high temperature conditions. For the crystal thin film of a heterogeneous substrate, there is still a problem of cracking. The non-implanted area and the implanted area are made of the same material, and there is still an obvious difference in thermal expansion coefficient with the substrate material. Therefore, the bonded body will produce severe warping deformation due to the difference in thermal expansion coefficient under high temperature conditions, and in severe cases, cracking will occur. Summary of the invention

[0006] In view of the defects and shortcomings of the prior art, the present invention provides a method for preparing a thin film wafer based on laser stripping of a heterogeneous substrate crystal film.

[0007] The present invention adopts a laser annealing method to adjust the laser focal length and accurately control the laser action depth to the ion implantation layer, so that the implantation layer is quickly heated to achieve peeling, while the thin film wafer and substrate material far away from the implantation layer are heated slowly, which simply and efficiently solves the fragmentation problem caused by the overall heating of the bonded wafer, and completely peels the thin film when the thermal expansion coefficients of the substrate and the thin film are inconsistent.

[0008] Injection stop layer: Plasma carries a certain amount of charge, and the positive ions can be accelerated by the electric field, and the direction of their movement can be changed by the magnetic field. In this way, the ions can be controlled to enter the wafer with a certain energy. After the ions are injected into the wafer, they will collide with the atoms and nuclei of the wafer and lose energy. When the energy is exhausted, the ions will stop at a certain depth in the wafer, which is the injection stop layer.

[0009] To achieve the above object, the present invention is implemented through a technical solution.

[0010] The method for preparing a thin film wafer based on laser stripping of a heterogeneous substrate crystal film comprises the following steps:

[0011] 1) providing a substrate wafer, and after cleaning, preparing a layer of silicon dioxide as an isolation layer on the substrate wafer;

[0012] 2) Provide a thin film wafer, clean it, and then use ion implantation to inject helium ions (He + ) is injected into the thin film wafer;

[0013] 3) bonding the thin film layer of the thin film wafer implanted with ions in step 2) to the silicon dioxide layer of the substrate wafer in step 1) to obtain a bonded body;

[0014] 4) The lithium niobate surface of the bonded body is irradiated with laser. When the bonded body is scanned with laser, the laser focus position is focused on the injection stop layer of the lithium niobate thin film to realize the stripping of the lithium niobate injection layer.

[0015] Preferably according to the present invention, in step 1), the substrate wafer is selected from silicon, silicon carbide, sapphire, quartz, fused quartz, has a size of 3 to 12 inches, and a thickness of 0.2 to 1 mm.

[0016] Further preferably, in step 1), the substrate wafer is a silicon wafer having a size of 4 inches.

[0017] Preferably according to the present invention, in step 1), the smooth surface of the substrate wafer is cleaned, and after cleaning, a silicon dioxide layer is prepared on the substrate wafer by thermal oxidation, PECVD, LPCVD or CVD, and the thickness of the silicon dioxide layer is 50nm to 5μm.

[0018] Further preferably, in step 1), the deposited silicon dioxide layer is annealed to eliminate impurity ions in the deposited silicon dioxide layer to reduce absorption loss.

[0019] Further preferably, in step 1), the roughness of the silicon dioxide layer is less than 0.5 nm.

[0020] Preferably according to the present invention, in step 2), the thin film wafer is lithium niobate, lithium tantalate or silicon carbide, with a size of 3 to 12 inches and a thickness of 0.2 to 1 mm.

[0021] Preferably according to the present invention, in step 2), the thin film wafer is a thin film wafer having good transmittance to laser.

[0022] According to the preferred embodiment of the present invention, in step 2), the helium ion implantation energy is 30KeV to 5MeV, and the dose is 1×10 15 ions / cm 2 ~1×10 17 ions / cm 2 .

[0023] Further preferably, in step 2), the helium ion implantation energy is 400 KeV and the dose is 5×10 16 ions / cm 2 .

[0024] Preferably, according to the present invention, in step 3), bonding is performed by plasma bonding, and the bonding body structure is, from top to bottom, a lithium niobate thin film sheet, a silicon dioxide isolation layer, and a silicon substrate sheet.

[0025] According to the preferred embodiment of the present invention, in step 4), the laser irradiation uses a laser wavelength of 694 nm, a pulse width of 30 to 50 ns, and an energy density of 1.5 to 1.7 J / cm 2 A high-power ruby ​​laser is used, and the scanning speed is maintained at 25 mm / s, scanning in a zigzag pattern from the edge of the wafer until the film is completely peeled off.

[0026] Preferably, according to the present invention, in step 4), the laser focus position is focused on the implant stop layer of the lithium niobate thin film so that the instantaneous temperature of the lithium niobate implant stop layer reaches 400°C to 600°C.

[0027] Preferably, according to the present invention, the method further comprises a step of polishing the peeled lithium niobate film, wherein the surface roughness of the film layer after polishing is less than 1 nm.

[0028] The beneficial effects of the present invention are as follows:

[0029] 1. The present invention adopts the laser stripping method to irradiate high energy density laser (several J / cm 2 ) is projected onto the injection stop layer of the thin film, so that the injected ions in the stop layer are quickly heated and vaporized, so as to quickly complete the film peeling process; the heating and cooling speeds are fast and the heat concentration is high; due to its highly focused energy, during the injection ion vaporization process, the upper film wafer and the lower substrate wafer are both less heated, and basically will not cause deformation caused by the difference in thermal expansion of heterogeneous materials. Therefore, the cracking problem of high-temperature treatment of heterogeneous material bonding is avoided, and a simple and efficient method is used to achieve complete peeling of heterogeneous material bonded thin film sheets. It has high process compatibility and can be applied to a variety of heterogeneous material bonded thin film structures. It is easy to process, with a simple process, short time and low cost, and provides a new method for crystal thin film processing.

[0030] 2. The present invention adopts the laser lift-off method. Due to the highly focused energy, the ion implantation stop layer can be quickly heated to above 400°C. The laser scanning of the entire 4-inch wafer can be completed in a few minutes. Compared with the traditional thermal annealing treatment (generally 24h to 72h), it has the characteristics of simple process, short time and low cost, and can be greatly shortened.

[0031] 3. The present invention adopts a laser stripping method, and its local focused heating feature has the effect of repairing damage to the ion implanted layer of the thin film. It can quickly repair the implantation damage to the thin film layer caused by ion implantation without the need for additional annealing of the stripped film to repair the implantation damage, thus greatly shortening the process flow.

[0032] 4. The method of the present invention can be used to prepare a composite thin film with a complete heterogeneous substrate, wherein a laser peeling scheme is adopted. The quartz low dielectric layer possessed by the laser has a smaller dielectric constant and very little impurity content, and can have better high-frequency response characteristics. In addition, the microwave and light wave speed adaptation problem caused by the slow-wave effect caused by the T-type electrode structure of the lithium niobate thin film modulator is solved. The electro-optic modulator prepared using this thin film product can have both ultra-high modulation bandwidth and ultra-low half-wave voltage. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 A flow chart for preparing thin film wafers based on laser lift-off of crystalline thin films on foreign substrates;

[0034] Figure 2 Schematic diagram of the laser focusing on the implantation stop layer of the lithium niobate thin film;

[0035] Figure 3 This is a schematic diagram of the film peeling structure by laser irradiation;

[0036] Among them, 1. Laser, 2. LN wafer, 3. LN film, 4. Silicon dioxide layer, 5. Substrate DETAILED DESCRIPTION

[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. The specific details set forth in the following description are for a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.

[0038] Example 1

[0039] A method for preparing a thin film wafer based on laser stripping of a crystal film on a heterogeneous substrate, the preparation process is as follows Figure 1 As shown, the steps are as follows:

[0040] 1) Providing a silicon substrate wafer with a smooth surface, a size of 4 inches and a thickness of 0.5 mm;

[0041] 2) Cleaning the smooth surface of the silicon substrate wafer, and preparing a layer of silicon dioxide as an isolation layer thereon by thermal oxidation; the thickness of the silicon dioxide layer is 500 nm, and the deposited silicon dioxide is annealed to eliminate impurity ions in the deposited silicon dioxide layer to reduce absorption loss, and the roughness of the silicon dioxide layer is less than 0.5 nm;

[0042] 3) Providing a lithium niobate thin film wafer with a smooth surface, a size of 4 inches and a thickness of 0.5 mm;

[0043] 4) Clean the smooth surface of the lithium niobate thin film wafer and use ion implantation to inject helium ions (He + ) is implanted into the lithium niobate thin film wafer, the helium ion implantation energy is 400 KeV (corresponding to the thickness of the implantation stop layer in the lithium niobate crystal is about 1100 nm), and the dose is 5×10 16 ions / cm 2 ; A thin film wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer is formed.

[0044] 5) using a plasma bonding method, bonding the thin film layer of the ion-implanted thin film wafer to the silicon dioxide layer of the silicon substrate wafer obtained in step 2) to obtain a bonded body, wherein the structure of the bonded body is, from top to bottom, a lithium niobate thin film sheet, a silicon dioxide isolation layer, and a silicon substrate sheet;

[0045] 6) Then place the bonded body on the workbench with the lithium niobate facing upwards, and use a laser wavelength of 694nm, a pulse width of 30ns, and an energy density of 1.5J / cm 2 A high-power ruby ​​laser is used to irradiate the lithium niobate surface by scanning from the edge of the wafer in a zigzag pattern at a scanning speed of 25 mm / s until the film is completely peeled off ( Figure 3 ); When the laser is used to scan the bonded body, the laser focus position is focused on the injection stop layer of the lithium niobate thin film ( Figure 2 ) so that the instantaneous temperature of the lithium niobate injection stop layer reaches 400°C to 600°C to achieve the stripping of the lithium niobate injection layer.

[0046] Example 2

[0047] The method for preparing a thin film wafer based on laser lift-off of a heterogeneous substrate crystal film described in Example 1 is different in that:

[0048] In step 6), the laser wavelength is 694 nm, the pulse width is 50 ns, and the energy density is 1.7 J / cm 2 A high-power ruby ​​laser is used, and the scanning speed is maintained at 25 mm / s, scanning in a zigzag pattern from the edge of the wafer until the film is completely peeled off.

Claims

1. A method for preparing a thin film wafer based on laser stripping of a heterogeneous substrate crystal film, comprising the following steps: 1) providing a substrate wafer, and after cleaning, preparing a layer of silicon dioxide as an isolation layer on the substrate wafer; 2) Provide a thin film wafer, clean it, and then use ion implantation to inject helium ions (He + ) is injected into the thin film wafer; 3) bonding the thin film layer of the thin film wafer implanted with ions in step 2) to the silicon dioxide layer of the substrate wafer in step 1) to obtain a bonded body; 4) The lithium niobate surface of the bonded body is irradiated with laser. When the bonded body is scanned with laser, the laser focus position is focused on the injection stop layer of the lithium niobate thin film to realize the stripping of the lithium niobate injection layer.

2. The method according to claim 1, characterized in that In step 1), the substrate wafer is selected from silicon, silicon carbide, sapphire, quartz, and fused quartz, with a size of 3 to 12 inches and a thickness of 0.2 to 1 mm.

3. The method according to claim 1, characterized in that In step 1), the smooth surface of the substrate wafer is cleaned, and after cleaning, a silicon dioxide layer is prepared on the substrate wafer by thermal oxidation, PECVD, LPCVD or CVD. The thickness of the silicon dioxide layer is 50nm to 5μm, and the roughness of the silicon dioxide layer is less than 0.5nm.

4. The method according to claim 1, characterized in that: In step 2), the thin film wafer is lithium niobate, lithium tantalate or silicon carbide, with a size of 3 to 12 inches and a thickness of 0.2 to 1 mm.

5. The method according to claim 1, characterized in that In step 2), the helium ion implantation energy is 30 KeV to 5 MeV, and the dose is 1×10 15 ions / cm 2 ~1×10 17 ions / cm 2 .

6. The method according to claim 1, characterized in that In step 3), bonding is performed by plasma bonding, and the bonding body structure is, from top to bottom, a lithium niobate thin film sheet, a silicon dioxide isolation layer, and a silicon substrate sheet.

7. The method according to claim 1, characterized in that In step 4), the laser irradiation uses a laser wavelength of 694nm, a pulse width of 30-50ns, and an energy density of 1.5-1.7J / cm 2 A high-power ruby ​​laser is used, and the scanning speed is maintained at 25 mm / s, scanning in a zigzag pattern from the edge of the wafer until the film is completely peeled off.

8. The method according to claim 1, characterized in that In step 4), the laser focus position is focused on the injection stop layer of the lithium niobate thin film so that the instantaneous temperature of the lithium niobate injection stop layer reaches 400°C to 600°C.

9. The method according to claim 1, characterized in that: The method also includes a step of polishing the stripped lithium niobate film, wherein the surface roughness of the film layer after polishing is less than 1 nm.

Citation Information

Cited By

  • Method for improving SiC crystal ingot laser slicing surface roughness through laser annealing

    CN119566564A

  • Laser-assisted heterogeneous bonding stripping method, heterogeneous bonding structure and optical element

    CN121925047A