Gypsum thermal insulation material and preparation method thereof
The preparation of ettringite through raw materials such as gypsum powder, tricalcium aluminate, modified silica gel and modified expanded graphite has solved the problem of unstable volume in cement by dihydrate gypsum, and achieved efficient and energy-saving gypsum insulation materials and low-carbon applications.
Patent Information
- Application Number
- CN202411115066.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
Smart Images

Figure BDA0004993397550000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of energy-saving building materials, and particularly relates to a gypsum thermal insulation material and a preparation method thereof. Background Art
[0002] At present, gypsum is widely used in the construction field, including as gypsum board for partition walls, suspended ceilings, etc., which has the advantages of light weight, sound insulation, fire resistance, and easy processing; as gypsum blocks, used for walls and partitions, which has the advantages of light weight, heat preservation, sound insulation, heat insulation, and fire resistance; as gypsum mortar, used for leveling, decoration and protection of indoor walls, and can also be used to repair defects such as cracks and holes in the wall.
[0003] Gypsum is mainly divided into natural gypsum and industrial by-product gypsum. Natural gypsum has limited reserves and is a non-renewable resource. However, the emission of industrial by-product gypsum is huge. Scientific utilization of industrial by-product gypsum is an important measure to solve the shortage of natural gypsum and alleviate environmental pollution. Desulfurized gypsum and phosphogypsum account for 90% of the total amount of industrial by-product gypsum. The main component is dihydrate gypsum. The main applications of dihydrate gypsum include: (1) Used as a retarder in the cement industry; (2) Calcination and grinding can obtain β-hemihydrate gypsum (CaSO4·1 / 2H2O), i.e. building gypsum.
[0004] When dihydrate gypsum is used in cement, it is mainly used to form calcium sulfoaluminate AFt (high-sulfur hydrated calcium sulfoaluminate crystals) with tricalcium aluminate during the early hydration process, thereby generating strength, but it will cause volume expansion, and the expansion multiple reaches 120%. Taking advantage of the characteristics of dihydrate gypsum to generate calcium sulfoaluminate, the system of dihydrate gypsum to generate calcium sulfoaluminate is further used as an expansion agent or a measure to compensate for shrinkage. However, since calcium sulfoaluminate will be converted into AFm (monosulfur hydrated calcium sulfoaluminate) after the gypsum is consumed, it will cause volume shrinkage. And when the temperature is high, reaching above 70°C, it will also be converted from AFt to AFm, but it is reversible and will have an adverse effect on volume stability, so it is less used. And dihydrate gypsum cannot be used directly. When dihydrate gypsum is directly used as a cement retarder, it will not only cause bonding and blocking during transportation and storage, but also cause inaccurate metering and unstable production, affecting cement quality. In addition, excessive moisture will also affect the output of the mill. Therefore, before being used as a cement retarder, it is necessary to carry out low-temperature drying to control the moisture content at 3.0% to 5.0%, and the industrial by-product gypsum is made into 5-40 mm small balls or blocks by granulation. When dihydrate gypsum is used as building gypsum, it needs to be calcined and ground to obtain β-type hemihydrate gypsum (CaSO4·1 / 2H2O), which has high strength and gelation. However, the conversion of dihydrate gypsum to hemihydrate gypsum requires high-temperature calcination, which means an increase in energy consumption. Therefore, being able to directly use dihydrate gypsum for the preparation of building materials has become a major research direction. Summary of the invention
[0005] In view of the problems in the prior art, the present invention proposes a gypsum thermal insulation material and a preparation method thereof, which utilizes dihydrate gypsum, the main component of desulfurized gypsum or phosphogypsum, to prepare calcium sulfonate and can avoid the influence of the crystal phase transformation of calcium sulfonate on its volume stability.
[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0007] A gypsum thermal insulation material is mainly made of the following raw materials in parts by mass: 60-80 parts of gypsum powder; 10-20 parts of tricalcium aluminate; 3-5 parts of modified silica gel; 2-4 parts of sodium alginate; 3-5 parts of modified expanded graphite; and 1-3 parts of a foaming agent.
[0008] The modified silicon dioxide gel is prepared by mixing, dispersing, air-drying and grinding nano calcium silicate and hydrophilic silicon dioxide gel.
[0009] The mass ratio of hydrophilic silica gel to nano calcium silicate is (20-30):1.
[0010] The diameter of the nano calcium silicate is ≤40 nm and is smaller than the diameter of the hydrophilic silica gel mesopore.
[0011] The modified expanded graphite is modified by mixing expanded graphite and nano-calcium aluminum phosphate. The expanded graphite and the nano-calcium aluminum phosphate are mixed in a mass ratio of 1:(1-3). The initial expansion temperature of the expanded graphite is 65-70° C., and the diameter of the nano-calcium aluminum phosphate is ≤100nm.
[0012] The gypsum powder is desulfurized gypsum or phosphogypsum powder.
[0013] The specific surface area of tricalcium aluminate is 300 to 500 m 2 / kg.
[0014] The foaming agent is one of sodium dodecyl sulfate (K12), sodium fatty alcohol polyoxyethylene ether sulfate (AES), sodium α-olefin sulfonate, and protein foaming agent.
[0015] A method for preparing a gypsum thermal insulation material, the main steps of which are:
[0016] (1) mixing gypsum powder, tricalcium aluminate, modified silica gel, sodium alginate and modified expanded graphite raw materials uniformly according to parts by mass, and adding water to form a gypsum slurry;
[0017] (2) After the foaming agent is foamed, it is mixed with the gypsum slurry, poured into a mold, and cured to obtain a gypsum thermal insulation material.
[0018] The preparation method of the modified silica gel is as follows: after the hydrophilic silica gel and nano calcium silicate are uniformly mixed, water is added, ultrasonic dispersion is performed, and the mixture is uniformly mixed, and then air-dried, cut into pieces, and ground into pieces with a specific surface area of not less than 500m 2 / kg of micropowder is modified silica gel.
[0019] The modified expanded graphite preparation method comprises the following steps: uniformly mixing expanded graphite and nano-calcium aluminum phosphate at a temperature of 80-120° C., placing the mixture in a constant temperature room at a temperature of 10-20° C. and cooling the mixture to room temperature to obtain the modified expanded graphite.
[0020] The total water consumption in the preparation process of the gypsum thermal insulation material is calculated based on a water-cement ratio of 0.5 to 0.7, wherein step (1) uses 80% to 90% of the total water consumption.
[0021] Beneficial effects:
[0022] (1) The present invention prepares calcium sulfonate based on the reaction of dihydrate gypsum and tricalcium aluminate, which are the main components of desulfurized gypsum or phosphogypsum, and then uses calcium sulfonate to prepare gypsum thermal insulation materials. This method can directly use dihydrate gypsum for reaction without calcining it into hemihydrate gypsum, thus saving resources; at the same time, through the optimization and adjustment of raw materials, the compressive strength, volume stability and thermal insulation performance of the thermal insulation material prepared based on calcium sulfonate under different temperature conditions are achieved, and the dynamic coordination of thermal insulation performance and volume stability is achieved, which is of great significance for the resource utilization of gypsum.
[0023] The gypsum thermal insulation material prepared by the present invention has a compressive strength of 5-5.3 MPa after curing and molding at 30°C, and a thermal conductivity of 0.13-0.14 W / (m·K); after curing and molding at 75°C, the compressive strength is 4.9-5.2 MPa, and the thermal conductivity is 0.13-0.15 W / (m·K), and the volume shrinkage difference is 0.01-0.02 mm / m, and has good compressive strength, volume stability and thermal insulation performance.
[0024] (2) The present invention modifies silica gel, adsorbs nano-calcium silicate in the mesopores of hydrophilic silica gel, utilizes the effect of nano-calcium silicate crystal nuclei, promotes the reaction of hydrophilic silica gel with calcium ions to generate hydrated calcium silicate, promotes the precipitation of calcium ions and calcium sulfate ions in gypsum during the coagulation and hardening process of gypsum slurry, promotes gypsum to participate in the reaction to generate calcium sulfonate, and simultaneously utilizes the self-generated reticular calcium silicate gel to improve the interlocking bonding with the gypsum calcium sulfonate structural system, thereby improving the overall structural stability of the gypsum material. The hydrophilic silica gel itself can improve the elasticity of the gypsum material structural system, enhance the stability of the structural system, reduce the generation of cracks, and has heat preservation effects such as energy absorption and heat storage. The compounding of silica gel and nano-calcium silicate is beneficial to improving compressive strength, volume stability and thermal insulation performance.
[0025] (3) Graphite expands at 80-120°C, and calcium aluminum phosphate can be wrapped in the expanded graphite network. After cooling, the expanded graphite forms a mesh structure wrapped on the surface of calcium aluminum phosphate, which has a lubricating effect and promotes the uniform dispersion of calcium aluminum phosphate. When the mass ratio of expanded graphite to nano-calcium aluminum phosphate is 1: (1-3), the expanded graphite can not only form a mesh wrapping effect on calcium aluminum phosphate, but also leave a large number of pores to ensure the free migration of water. At the same time, calcium aluminum phosphate can serve as a catalyst for gypsum reaction, promoting the catalytic reaction of gypsum and tricalcium aluminate near the catalyst, gradually generating a hydration product AFt and gradually enriching it. Modified expanded graphite can control the orderly growth of calcium aluminate and adjust the growth of calcium aluminate along the expansion range of expanded graphite.
[0026] (4) Since sodium alginate is hygroscopic and can easily chelate with calcium ions to form a mesh structure gel, it promotes the decomposition reaction of gypsum and forms a gel containing a large amount of water by chelating calcium ions. As gypsum reacts to form calcium alginate, sodium alginate also loses water and gradually turns into dry gel in the process of transforming into calcium alginate, shrinking in volume, providing a large amount of space for the volume expansion of calcium alginate, avoiding the formation of cracks due to excessive volume expansion. When sodium alginate is lacking, the volume expands rapidly, which has an adverse effect on the structural strength; excessive sodium alginate increases the internal pores, produces shrinkage cracks, and rapidly reduces the compressive strength.
[0027] (5) The gypsum thermal insulation material of the present invention achieves its volume stability and thermal insulation through changes in its own structure and crystal orientation. When the ambient temperature exceeds 70°C, AFt is transformed into AFm, and the entire expansion system disintegrates and shrinks. At this temperature, the expanded graphite absorbs heat and begins to expand rapidly, and the expansion spreads rapidly along the pores formed after AFt is transformed into AFm, thereby improving the stability of the system and maintaining the stability of the entire thermal insulation structure. As the temperature drops, the expanded graphite shrinks, and AFm begins to transform into AFt, refilling the internal void structure. The volume shrinkage under the conditions of crystal phase transformation formed inside the thermal insulation material compensates for each other, greatly improving the structural stability of the thermal insulation material, avoiding the generation of cracks, and improving durability. At the same time, the thermal insulation of the material is improved, that is, in addition to relying on the pore structure for insulation under high temperature conditions, AFt and expanded graphite quickly absorb heat and absorb heat inside their own structure. When the temperature drops, the heat is released quickly to maintain the stability of the temperature inside the building.
[0028] (6) The gypsum thermal insulation material provided by the present application has excellent thermal insulation performance, can effectively reduce the heat transfer inside and outside the building, can significantly reduce the energy consumption of the building in cooling and heating, reduce the heating and cooling load of the building, improve the living comfort rate, improve the energy utilization rate, help reduce the building operation cost, reduce greenhouse gas emissions, promote the development of green buildings and low-carbon buildings, and achieve high efficiency and energy saving of buildings. At the same time, the preparation of the thermal insulation material and its application in construction realize the low-cost and low-energy resource utilization of gypsum waste, and residents have obvious social, environmental and economic benefits. DETAILED DESCRIPTION
[0029] The method of the present invention is described in detail below with reference to specific examples.
[0030] Example 1
[0031] A gypsum thermal insulation material is mainly made of the following raw materials in parts by weight:
[0032] 60 parts of desulfurized gypsum powder;
[0033] 20 parts of tricalcium aluminate;
[0034] 3 parts of modified silica gel;
[0035] 4 parts of sodium alginate;
[0036] 3 parts of modified expanded graphite;
[0037] 3 parts of sodium lauryl sulfate.
[0038] The specific surface area of the tricalcium aluminate is 300 m 2 / kg.
[0039] The preparation method of the modified silica gel is as follows: after the hydrophilic silica gel and the nano calcium silicate with a diameter of 20 nm (mass ratio of 20:1) are mixed evenly, an appropriate amount of water is added, the mixture is dispersed evenly by ultrasonication, and then air-dried, cut into pieces, and ground into pieces with a specific surface area of 600 m 2 / kg of micropowder is modified silica gel.
[0040] The modified expanded graphite preparation method comprises: at a temperature of 80° C., evenly mixing expanded graphite with an initial expansion temperature of 65 to 70° C. and nano-calcium aluminum phosphate with a diameter of 80 nm in a mass ratio of 1:3, placing the mixture in a constant temperature room at 10° C. and cooling the mixture to room temperature to obtain the modified expanded graphite.
[0041] Preparation method of gypsum thermal insulation material: (1) After uniformly mixing the above raw materials except the foaming agent sodium dodecyl sulfate, the total water consumption is calculated according to the water-cement ratio of 0.5, and 90% of the total water consumption is mixed with the above raw materials to form gypsum slurry. (2) After uniformly mixing the remaining water with the foaming agent, the foaming agent is beaten into rich and fine foam by a foaming machine, mixed with the gypsum slurry, poured into a mold, and cured and formed to obtain the gypsum thermal insulation material.
[0042] Example 2
[0043] A gypsum thermal insulation material is mainly made of the following raw materials in parts by weight:
[0044] 80 parts of phosphogypsum powder;
[0045] 10 parts of tricalcium aluminate;
[0046] 5 parts of modified silica gel;
[0047] 2 parts of sodium alginate;
[0048] 5 parts of modified expanded graphite;
[0049] 1 part of sodium α-olefin sulfonate.
[0050] The specific surface area of the tricalcium aluminate is 500 m 2 / kg.
[0051] The preparation method of the modified silica gel is as follows: after the hydrophilic silica gel and the nano calcium silicate with a diameter of 40nm (mass ratio of 30:1) are mixed evenly, an appropriate amount of water is added, the mixture is dispersed evenly by ultrasonication, and then air-dried, cut into pieces, and ground into pieces with a specific surface area of 500m 2 / kg of micropowder is modified silica gel.
[0052] The modified expanded graphite preparation method comprises: at 120° C., evenly mixing expanded graphite with an initial expansion temperature of 65-70° C. and nano-calcium aluminum phosphate with a diameter of 100 nm in a mass ratio of 1:1, placing the mixture in a constant temperature room at 10° C. and cooling the mixture to room temperature to obtain the modified expanded graphite.
[0053] Preparation method of gypsum thermal insulation material: (1) After uniformly mixing the above raw materials except the foaming agent sodium α-olefin sulfonate, the total water consumption is calculated according to the water-cement ratio of 0.7, and 80% of the total water consumption is mixed with the above raw materials to form a gypsum slurry. (2) The remaining water of the total water consumption is mixed with the foaming agent, and the foaming agent is beaten into rich and fine foam by a foaming machine, and mixed with the gypsum slurry, poured into a mold, and cured and formed to obtain a gypsum thermal insulation material.
[0054] Example 3
[0055] A gypsum thermal insulation material is mainly made of the following raw materials in parts by weight:
[0056] 70 parts of desulfurized gypsum powder;
[0057] 15 parts of tricalcium aluminate;
[0058] 4 parts of modified silica gel;
[0059] 3 parts of sodium alginate;
[0060] 4 parts of modified expanded graphite;
[0061] 2 parts of egg white foaming agent.
[0062] The specific surface area of the tricalcium aluminate is 500 m 2 / kg.
[0063] The preparation method of the modified silica gel is as follows: after the hydrophilic silica gel and the nano calcium silicate with a diameter of 28 nm (mass ratio of 25:1) are mixed evenly, an appropriate amount of water is added, the mixture is dispersed evenly by ultrasonication, and then air-dried, cut into pieces, and ground into pieces with a specific surface area of 580 m 2 / kg of micropowder is modified silica gel.
[0064] The modified expanded graphite preparation method comprises: at a temperature of 100° C., uniformly mixing expanded graphite and nano-calcium aluminum phosphate with a diameter of 90 nm in a mass ratio of 1:2, placing the mixture in a constant temperature room at 10° C. and cooling the mixture to room temperature to obtain the modified expanded graphite.
[0065] Preparation method of gypsum thermal insulation material: (1) After uniformly mixing the above raw materials except the protein foaming agent, the total water consumption is calculated according to the water-cement ratio of 0.6, and 85% of the water is mixed with the above raw materials to form a gypsum slurry. (2) After uniformly mixing the remaining water with the foaming agent, the foaming agent is beaten into rich and fine foam by a foaming machine, mixed with the gypsum slurry, poured into a mold, and cured and formed to obtain a gypsum thermal insulation material.
[0066] Comparative Example 1
[0067] The difference from Example 3 is that no modified silica gel is added.
[0068] Comparative Example 2-1
[0069] The difference from Example 3 is that the hydrophilic silica gel and nano calcium silicate are added separately, and the hydrophilic silica gel is not modified in advance.
[0070] Comparative Example 2-2
[0071] The difference from Example 3 is that no nano calcium silicate is added, and only hydrophilic silica gel is added.
[0072] Comparative Examples 2-3
[0073] The difference from Example 3 is that no hydrophilic silica gel is added, and only nano calcium silicate is added.
[0074] Comparative Example 3
[0075] The difference from Example 3 is that the mass ratio of graphite to calcium aluminum phosphate is 1:0.5.
[0076] Comparative Example 4
[0077] The difference from Example 3 is that the mass ratio of graphite to calcium aluminum phosphate is 1:5.
[0078] Comparative Example 5
[0079] The difference from Example 3 is that the diameter of calcium aluminum phosphate is 1 μm.
[0080] Comparative Example 6
[0081] The difference from Example 3 is that the content of tricalcium aluminate is 30 parts.
[0082] Comparative Example 7
[0083] The difference from Example 3 is that the content of tricalcium aluminate is 5 parts.
[0084] Comparative Example 8
[0085] The difference from Example 3 is that sodium alginate is not added.
[0086] Comparative Example 9
[0087] The difference from Example 3 is that 6 parts of sodium alginate are added.
[0088] Comparative Example 10
[0089] The difference from Example 3 is that no modified expanded graphite is added.
[0090] Benchmark Group
[0091] The difference from Example 3 is that no modified silica gel, sodium alginate and modified expanded graphite are added.
[0092] The gypsum insulation materials prepared in the above embodiments and comparative examples were tested for compressive strength and thermal conductivity according to JC / T 1062-2022 "Test Method for Foam Concrete Blocks"; the volume shrinkage difference was tested with reference to the test method for drying shrinkage in GB / T 11969-2020 "Test Method for Performance of Autoclaved Aerated Concrete". After curing for 28 days, the length of the specimen at 30°C was directly sampled and tested, and then the test block was stored at 75°C. The length of the specimen under the temperature condition was tested, and the difference between the two was the volume shrinkage value. The smaller the volume shrinkage difference, the better the volume stability at different temperatures, and the larger the volume shrinkage difference, the worse the volume stability. The results are shown in Table 1 (30°C means that the molding is cured for 28 days and then stored at 30°C for 8 hours and then tested immediately, and 75°C means that the molding is cured for 28 days and then stored at 75°C for 8 hours and then tested immediately).
[0093] Table 1 Performance indexes of gypsum insulation materials
[0094]
[0095] It can be seen from the data in Table 1 that in Examples 1-3, the compressive strength of the gypsum thermal insulation material after curing and molding at 30°C is 5-5.3 MPa, and the thermal conductivity can reach 0.13-0.14 W / (m·K); the compressive strength after curing and molding at 75°C is 4.9-5.2 MPa, and the thermal conductivity can reach 0.13-0.15 W / (m·K); the volume shrinkage difference is 0.01-0.02 mm / m, and it has good compressive strength, volume stability and thermal insulation performance.
[0096] From the comparison between Comparative Example 1 and Example 3, it can be seen that without adding modified silica gel, the compressive strength decreases, the volume shrinkage difference becomes larger, the volume stability becomes worse, the thermal conductivity increases, and the thermal insulation performance becomes worse.
[0097] From the comparison between comparative example 2-1 and example 3, it can be seen that the strength of silica gel and nano calcium silicate added separately is reduced, the volume stability is reduced, and the thermal conductivity is increased compared to adding after modification. This is because modifying the silica gel in advance can constrain the nano calcium silicate in the silica gel, so that when it is used as the crystal nucleus to form a hydrated calcium silicate gel, it can form a good bond with the silica gel, thereby enhancing the toughness of the hydration product structure. When added separately, the two cannot play a good synergistic role, and the improvement effect is not obvious.
[0098] Further comparison of Comparative Example 2-1 with Comparative Example 1 shows that the addition of silica gel and nano-calcium silicate alone does not significantly improve its strength, but slightly decreases it, but the volume stability and thermal insulation performance have a certain improvement. Further, it can be seen from Comparative Example 2-2 and Comparative Example 1 that although the addition of silica gel alone will cause a decrease in strength, it is beneficial to volume stability. Further, it can be seen from Comparative Example 2-3 and Comparative Example 1 that although the volume stability is not significantly improved by the addition of nano-calcium silicate alone, it is beneficial to improve strength. When both are added as in Comparative Example 2-1, compared with Comparative Example 2-2 and Comparative Example 2-3, the strength is in the middle, but the volume stability is improved and the thermal insulation performance is improved. If both are modified and then added as in Example 3, the strength is significantly improved, the volume stability is further improved, and the thermal insulation performance is further improved. This shows that the synergistic modification of the two has a significant improvement effect that is not available when added alone.
[0099] From the comparison of Comparative Examples 3 and 4 with Example 3, it can be seen that if the expanded graphite content is too high, it plays a hydrophobic role, and calcium aluminum phosphate cannot play a catalytic role, participates in the gypsum reaction, and causes the compressive strength to decrease. If the expanded graphite content is too low, the effect is not obvious in the later structure filling pores, causing the volume shrinkage difference to increase and the volume stability to decrease. Therefore, selecting an appropriate amount of expanded graphite can both improve the compressive strength and enhance the volume stability.
[0100] From the comparison between Comparative Example 5 and Example 3, it can be seen that when the diameter of calcium aluminum phosphate is too large, the packaging is not good, the later structural filling effect is not obvious, the volume shrinkage difference is increased, and the volume stability is reduced; at the same time, the catalytic gypsum reaction effect is not obvious, and the compressive strength is reduced. Therefore, the diameter of calcium aluminum phosphate should not be too large, otherwise it will reduce the volume stability and compressive strength.
[0101] From the comparison of Comparative Examples 6 and 7 with Example 3, it can be seen that if the content of tricalcium aluminate is too high, the strength decreases and shrinkage occurs. This is because excessive tricalcium aluminate will cause AFt to be converted into AFm in advance, the volume stability decreases, the ettringite loses its mechanical properties, and the compressive strength decreases. If the content of tricalcium aluminate is too low, the compressive strength decreases, because a small amount of tricalcium aluminate is not enough to form enough ettringite with dihydrate gypsum, resulting in a weak structural system. Therefore, controlling the content of tricalcium aluminate is crucial to compressive strength.
[0102] From the comparison of comparative examples 8 and 9 with Example 3, it can be seen that without adding sodium alginate, the compressive strength is significantly reduced. When sodium alginate is lacking, the volume expands rapidly, and the structural strength is negatively affected. Sodium alginate has water absorption, and is easy to form a mesh structure gel by calcium ion chelation. While promoting the decomposition reaction of gypsum, a gel containing a large amount of water is formed by chelating calcium ions. As gypsum reacts to generate calcium aluminate, sodium alginate is gradually converted into calcium alginate dehydration and gradually converted into dry gel, volume shrinkage, providing a large amount of space for the volume expansion of calcium aluminate, avoiding the generation of excessive volume expansion cracks. If excessive sodium alginate is added, the internal pores are increased, shrinkage cracks are generated, and the compressive strength is rapidly reduced. Therefore, the sodium alginate selected in an appropriate amount can improve the compressive strength.
[0103] From the comparison between comparative example 10 and example 3, it can be seen that without adding modified expanded graphite, the compressive strength at 75°C is significantly reduced; the volume shrinkage difference is significantly increased, the volume stability is reduced, and the thermal conductivity at 75°C is significantly increased, that is, the thermal insulation performance is also significantly reduced. After experiencing 75°C once, cracks appeared in the foam insulation board and the compressive strength decreased rapidly. Therefore, adding modified expanded graphite can improve the compressive strength, volume stability and thermal insulation performance of the thermal insulation material.
[0104] From the comparison between the reference group and Example 3, it can be seen that the reference group has obvious volume changes at different temperatures. When it experiences 75°C, the volume shrinkage of the foamed insulation board increases significantly, and the compressive strength decreases rapidly. This shows that the gypsum material prepared under the conditions of gypsum, tricalcium aluminate and foaming agent has poor performance. By adding modified silica gel, sodium alginate and modified expanded graphite, the compressive strength, volume stability and thermal insulation performance of the material can be improved, and a product with superior performance can be prepared.
Claims
1. A gypsum thermal insulation material, characterized in that: It is mainly made of the following raw materials by weight: 60-80 parts of gypsum powder; 10-20 parts of tricalcium aluminate; 3-5 parts of modified silica gel; 2-4 parts of sodium alginate; 3-5 parts of modified expanded graphite; 1 to 3 parts of foaming agent.
2. The gypsum thermal insulation material according to claim 1, characterized in that: The modified silicon dioxide gel is prepared by mixing, dispersing, air-drying and grinding nano calcium silicate and hydrophilic silicon dioxide gel.
3. The gypsum thermal insulation material according to claim 2, characterized in that: The diameter of the nano calcium silicate is ≤40 nm and is smaller than the diameter of the hydrophilic silica gel mesopore.
4. The gypsum thermal insulation material according to claim 1, characterized in that: The modified expanded graphite is formed by mixing and modifying expanded graphite and nano-calcium aluminum phosphate.
5. The gypsum thermal insulation material according to claim 4, characterized in that: The expanded graphite and nano-calcium aluminum phosphate are mixed in a mass ratio of 1:(1-3); the diameter of the nano-calcium aluminum phosphate is ≤100nm.
6. The gypsum thermal insulation material according to claim 1, characterized in that: The gypsum powder is desulfurized gypsum or phosphogypsum powder.
7. The gypsum thermal insulation material according to claim 1, characterized in that: The specific surface area of tricalcium aluminate is 300 to 500 m 2 / kg.
8. A method for preparing the gypsum thermal insulation material according to any one of claims 1 to 7, characterized in that: The main steps are: (1) mixing gypsum powder, tricalcium aluminate, modified silica gel, sodium alginate and modified expanded graphite raw materials uniformly according to parts by mass, and adding water to form a gypsum slurry; (2) After the foaming agent is foamed, it is mixed with the gypsum slurry, poured into a mold, and cured to obtain a gypsum thermal insulation material.
9. The method for preparing a gypsum thermal insulation material according to claim 8, characterized in that: The preparation method of the modified silica gel is as follows: after the hydrophilic silica gel and nano calcium silicate are uniformly mixed, water is added, ultrasonic dispersion is performed, and the mixture is uniformly mixed, and then air-dried, cut into pieces, and ground into pieces with a specific surface area of not less than 500m 2 / kg of micropowder is modified silica gel.
10. The method for preparing a gypsum thermal insulation material according to claim 8, characterized in that: The modified expanded graphite preparation method comprises the following steps: uniformly mixing expanded graphite and nano-calcium aluminum phosphate at a temperature of 80-120° C., and then cooling the mixture to room temperature to obtain the modified expanded graphite.