Rare earth polishing agent for improving easy disc pasting of large polishing pad in TFT (Thin Film Transistor) and ITO (Indium Tin Oxide) glass thinning process

By using rare earth polishing powder, clay, phosphate and maleic acrylic copolymer sodium salt combination additives in the process of TFT and ITO glass thinning, the problem of easy paste of polishing pads on large polishing machines is solved, and high efficiency is achieved The cutting rate is durable and foam-free polishing effect.

CN118995054APending Publication Date: 2024-11-22HUNAN HAOZHI TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095796.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the thinning process of TFT and ITO glass on large polishing machines, the polishing pads tend to paste the disc, resulting in poor cutting rate and durability, affecting the polishing efficiency and flatness.

Method used

Using rare earth polishing powder, clay, phosphate and maleic acrylic copolymer sodium salt combination as additives, the anti-solidation, low viscosity and fluidity optimization of maleic acrylic copolymer sodium salt is combined with phosphoric acid The dispersion effect of salt forms a rare earth polishing agent that is bubble-free and does not easily paste the disk.

Benefits of technology

It realizes the long-term use of large polishing pads during the thinning process of TFT and ITO glass, avoids foam generation, improves the durability of cutting rate, reduces powder adhesion, solves the problem of paste, and improves polishing efficiency. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995054A_ABST
    Figure CN118995054A_ABST
Patent Text Reader

Abstract

The invention discloses a rare earth polishing agent for improving easy disc pasting of a large polishing pad in a TFT (Thin Film Transistor) and ITO (Indium Tin Oxide) glass thinning process, and relates to the technical field of glass polishing material preparation. The rare earth polishing powder comprises the following raw materials in parts by weight: 100 parts of rare earth polishing powder, 1-4 parts of clay, 1-3 parts of phosphate and 1-3 parts of maleic acid-acrylic acid copolymer sodium salt. The polishing machine has the advantages of being free of bubbles, not prone to disc pasting, convenient to use, good in cutting rate durability, suitable for thinning and polishing TFT glass and ITO glass through a large polishing machine table and the like, is suitable for thinning and polishing large optical and panel glass, and is particularly suitable for the field of thinning TFT glass and ITO glass with the large polishing machine table.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass polishing material preparation, in particular to a rare earth polishing agent for improving the easy sticking of large polishing pads in the process of thinning TFT and ITO glass. Background Art

[0002] With the development of electronic products, the demand for glass sheets with high surface quality is increasing, which requires improving the technical requirements for polishing.

[0003] Cerium-based rare earth polishing powder is one of the more important rare earth products. It is known as the "king of polishing powders" because of its advantages such as strong cutting ability, short polishing time and high polishing precision, and has better use effect than other polishing powders (such as Fe2O3 red powder). Cerium-based polishing powder is mainly used in glass polishing and thinning, such as liquid crystal panels, mobile phone covers, optical glass and other fields.

[0004] In the field of glass thinning, rare earth polishing powder is an important raw material, and its quality directly affects the quality and efficiency of glass.

[0005] At present, LCD panel manufacturers mainly use cutting rate, durability, scratches, cleaning, and sticking as the main evaluation indicators in their production process.

[0006] Generally speaking, the cutting rate and scratches are mainly controlled by the burning temperature of the powder and the particle size of the crushing and classification.

[0007] Since rare earth polishing powder has the unique characteristic of strong surface adhesion, it is obviously different from silica sol and the like. In the later glass cleaning and polishing pad cleaning, it needs to be adjusted through additives. Therefore, the formula of its additives will directly affect the cutting rate, durability, cleaning and plate sticking, etc.

[0008] For TFT-LCD customers, the problem of plate sticking will manifest as poor cutting force durability. Therefore, customers need to constantly brush and repair the polishing pad surface, thus affecting the overall polishing efficiency. For ITO customers, after the cutting force durability deteriorates, the flatness index exceeds the standard seriously, and rainbow stripes are easy to appear after coating. Therefore, the general production workshop will clean the polishing pad and tabletop every 8 hours. As long as the plate is not sticky within 8 hours, it can be considered that the polishing pad has a good effect in improving plate sticking.

[0009] The reason why the polishing pad sticks is usually because the polishing powder has strong viscosity and is easily embedded in the polishing pad, forming a large amount of white powder prints on the surface of the polishing pad. Therefore, only additives can be used to improve the adhesion. Especially for large-sized polishing machines (polishing pad diameter of more than 800mm), the powder retention time is longer and the degree is deeper, so the polishing pad is particularly prone to sticking.

[0010] A Chinese patent (patent application number 201410757848) discloses "a silicon wafer fine polishing liquid capable of extending the service life of a polishing pad". The polishing liquid of the invention includes silica sol, alkaline compounds, deionized water remainder, polyanionic cellulose, small molecule inorganic non-metallic bridging agent, water-soluble polymer and guanidine compound. The polishing liquid of the invention reduces the wear of the follicles on the surface of the polishing pad and the blockage of the internal pores, significantly extending the service life of the polishing pad during the final polishing of the silicon wafer; at the same time, it improves the surface uniformity of the silicon wafer after the final polishing. However, the scope of application of this patent is only for semiconductor substrate silicon wafers, and is not suitable for TFT and ITO glass thinning polishing.

[0011] Another Chinese patent (patent application number 201310184331.0) discloses "a lanthanum oxide cerium rare earth polishing powder and its preparation method". The additive formula in this invention can enable the abrasive particles to maintain good dispersion and suspension, reduce the hardness of precipitation and solidification, stabilize the production process, and improve the grinding quality and production efficiency.

[0012] There is also a Chinese patent (patent application number 201911356139.9) disclosed "a rare earth polishing liquid for polishing a glass panel and a polishing method using the same", which, in order to solve the existing problem of poor defoaming performance, provides a rare earth polishing liquid for polishing a glass panel, including the following components by mass percentage: rare earth abrasive powder: 40% to 45%, the rare earth abrasive powder contains cerium oxide, lanthanum oxide, praseodymium oxide and fluorine elements, and the weight ratio of cerium oxide: lanthanum oxide: praseodymium oxide: fluorine elements is 66 to 67: 30 to 32: 0.08 to 0.15: 2.5 to 3.0; defoamer: 1.0% to 1.5%; vegetable oil: 1.0% to 1.5%; the balance is water; and the polishing method using the polishing liquid is to polish the glass panel by using the above-mentioned polishing liquid. The invention can achieve high chemical polishing activity and high dispersibility, and achieve effective defoaming ability and long service life.

[0013] There is also a Chinese patent (patent application number 201110228791.X) disclosed in "Lanthanum cerium rare earth fluoride polishing liquid and its preparation method", the lanthanum cerium rare earth fluoride polishing liquid, with water as carrier, contains lanthanum cerium fluoride polishing powder, dispersant and pH value adjuster; the content of dispersant is 0.5-1wt% of the total mass of the polishing liquid, the amount of pH value adjuster is based on the pH value of the polishing liquid reaching 8.5-10.0, the solid content of the polishing liquid is 25-45wt%, cerium accounts for 60-80wt% of the total mass of lanthanum cerium, and the mass fraction of fluorine is 3-5wt% of the total mass of lanthanum cerium fluoride. The invention has the performance characteristics of high suspension stability, fast polishing rate, less scratches and high wear resistance for silica glass, corresponding to the small particle size of rare earth particles, by adding pH value adjuster and organic dispersant, the sedimentation of abrasive in the liquid is delayed, the polishing rate of the polishing liquid on the glass substrate is improved, and the occurrence of scratches is reduced.

[0014] There is also a Chinese patent (patent application number 201410634606.0) that discloses "Rare Earth Polishing Fluid and Its Preparation Method", which includes the following components by weight: 20-50 parts of rare earth polishing powder, 3-15 parts of organic solvent, 1-5 parts of clay, and 30-76 parts of water. This invention solves the problem of suspension and dispersion of polishing powder in water, overcomes the current problem of glue bonding during the preparation and storage of polishing fluids, and the problem of good cleaning during use, and has the characteristics of good suspension and dispersion performance, fast polishing rate, high polishing accuracy, and excellent cleaning performance of polished products. This invention is suitable for surface polishing of precision components in the electronic information industry such as integrated circuits, flat panel displays, and optical glass, meeting the increasingly stringent commercial requirements for polishing materials in terms of accuracy, polishing amount, and easy cleaning.

[0015] In order to improve the cutting rate, scratching, cleaning and other problems of the rare earth polishing powder / liquid mentioned above, the problems are simply solved from the suspension and dispersibility of the slurry or powder. For polishing machines with small-sized polishing pads (polishing pad diameter less than 800mm), the effect of polishing pad sticking can be ignored.

[0016] However, when thinning and polishing TFT and ITO glass are performed using large polishing machines (polishing pad diameter is more than 800 mm, and the polishing pad is polyurethane), the problem of poor cutting rate sustainability caused by the polishing pad sticking is particularly prominent. The rare earth polishing powder / liquid in the above-mentioned patents is not involved, and there is no report in the relevant public literature.

[0017] Therefore, in view of the above technical problems, it is necessary to develop a polishing agent specifically for solving the problem of polishing pad sticking in large-scale polishing machines for TFT and ITO glass. Summary of the invention

[0018] The technical problem to be solved by the present invention is to provide a rare earth polishing agent which is free of bubbles, not easy to stick to the plate, easy to use, has a good cutting rate and is suitable for thinning and polishing on large polishing machines (i.e., polishing pads with a diameter of more than 800 mm) for TFT and ITO glass.

[0019] In order to solve the above technical problems, the technical solution adopted by the present invention is to invent a rare earth polishing agent for improving the easy sticking of large polishing pads in the process of thinning TFT and ITO glass, which comprises the following raw materials in parts by weight:

[0020] Rare earth polishing powder 100 Clay 1-4

[0021] Phosphate 1-3 Maleic acid acrylic acid copolymer sodium salt 1-3;

[0022] The clay is one or more of kaolin, bentonite and montmorillonite, with a particle size D50 of 1-3 μm, a D100 of less than 13.54 μm, and a large particle content of less than 800 ppm (large particles are those on the sieve of a sieve with an aperture of more than 15 μm). When there are two or three types of clay, the proportion of each component is equal in weight; cosmetic grade bentonite is preferred;

[0023] The particle size was tested using a Malvern particle size analyzer 2000;

[0024] The phosphate is one or both of sodium orthophosphate and sodium tripolyphosphate. When there are two, the proportion of each component is equal by weight; preferably food grade sodium tripolyphosphate;

[0025] The average molecular weight of the sodium salt of maleic acid acrylic acid copolymer is 20000-30000;

[0026] The rare earth polishing powder complies with the "GB / T20165-2012" standard, and its particle size D50 is 0.8-2.0 μm.

[0027] The large particle detection method is as follows: take a 1L beaker, add 400ml of water, then add 20g of 10% weight concentration sodium hexametaphosphate solution, turn on magnetic stirring, slowly add 10g of clay while stirring, stir for 30min until it is completely dispersed, and finally crush it with an ultrasonic crusher for 5min to obtain slurry; then, filter the slurry on a 15μm sieve until it is completely filtered, wash the sieve with pure water 3 times, and finally dry the sieve in an oven at 105°C to obtain large particles.

[0028] The first optimized technical solution comprises the following raw materials in parts by weight:

[0029] Rare earth polishing powder 100 Clay 1

[0030] Phosphate 1 Maleic acid acrylic acid copolymer sodium salt 1.

[0031] The second optimized technical solution includes the following raw materials in parts by weight:

[0032] Rare earth polishing powder 100 Clay 2

[0033] Phosphate 1 Maleic acid acrylic acid copolymer sodium salt 1.

[0034] The optimized technical solution three includes the following raw materials in parts by weight:

[0035] Rare earth polishing powder 100 Clay 2

[0036] Phosphate 1.5 Maleic acid acrylic acid copolymer sodium salt 1.5.

[0037] The fourth optimized technical solution includes the following raw materials in parts by weight:

[0038] Rare earth polishing powder 100 Clay 1

[0039] Phosphate 3 Maleic acid acrylic acid copolymer sodium salt 3.

[0040] The fifth optimized technical solution includes the following raw materials in parts by weight:

[0041] Rare earth polishing powder 100 Clay 3

[0042] Phosphate 2 Maleic acid acrylic acid copolymer sodium salt 2.

[0043] The sixth optimized technical solution includes the following raw materials in parts by weight:

[0044] Rare earth polishing powder 100 Clay 4

[0045] Phosphate 3 Maleic acid acrylic acid copolymer sodium salt 3.

[0046] Optimally, the average molecular weight of the sodium salt of maleic acid acrylic acid copolymer is 22,000-28,000.

[0047] Further optimized, the average molecular weight of the sodium salt of maleic acid acrylic acid copolymer is 25,000.

[0048] The preparation method thereof is as follows: directly mixing the raw materials uniformly.

[0049] The rare earth polishing agent of the present invention improves the easy sticking of large polishing pads in the thinning process of TFT and ITO glass, and adopts a combination of clay, phosphate and sodium salt of maleic acid acrylic acid copolymer as an auxiliary agent. The clay itself has no dispersibility, and its main function in the rare earth polishing agent is to help clean the glass; the applicant has found through repeated experiments that sodium salt of maleic acid acrylic acid copolymer (which has not been reported in the use of previous rare earth polishing powder / agents) has the effect of preventing slurry from hardening, low viscosity, and good fluidity in polishing powder / agents, although its slurry suspension durability is general, and it has poor adhesion to glass and is easy to rinse; although phosphate is not ideal for glass cleaning and reducing powder adhesion, it has a good dispersion effect on rare earth polishing powder and clay. Therefore, after the three are combined, it brings unexpected technical effects, and the beneficial technical effects brought are as follows:

[0050] First, no defoaming agent or foaming ingredients are added, which eliminates the generation of foam from the source, and there is no need to add defoaming agent for treatment. Therefore, it will not affect the cutting rate during the production process (that is, the reduction in the cutting rate from the initial 1h cutting rate to the cutting rate when the disc is pasted is relatively small), and no broken pieces will be generated.

[0051] The second is to make the finished product into powder. When using it, just add it directly into pure water and stir it evenly. Therefore, it is extremely convenient to use and meets the needs of existing customers.

[0052] Thirdly, it eliminates the generation of foam from the source, and the use of sodium maleic acid acrylic acid copolymer itself has the effect of reducing the adhesion of powders. After combining with clay and phosphate, it can better reduce the adhesion of powders on the polishing pad. Therefore, it not only solves the problem of easy sticking to the client, but also improves the durability of the client's cutting force. Therefore, it is suitable for thinning and polishing of TFT and ITO glass on large polishing machines (i.e.: polishing pad diameter of more than 800mm). BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 is a photograph of the polishing pad after grinding for 1 hour in Example 1;

[0054] Figure 2 is a photograph of the polishing pad after 4 hours of grinding in Example 1;

[0055] Figure 3 is a photograph of the polishing pad after grinding for 8 hours in Example 1;

[0056] Figure 4 is a photograph of the polishing pad after grinding for 1 hour in Example 2;

[0057] Figure 5 is a photograph of the polishing pad after 4 hours of grinding in Example 2;

[0058] Figure 6 is a photograph of the polishing pad after grinding for 8 hours in Example 2;

[0059] Figure 7 is a photograph of the polishing pad after grinding for 1 hour in Example 3;

[0060] Figure 8 is a photograph of the polishing pad after 4 hours of grinding in Example 3;

[0061] Fig. 9 is a photograph of the polishing pad after grinding for 8 hours in Example 3;

[0062] Fig.10 is a photograph of the polishing pad after grinding for 1 hour in Example 4;

[0063] Fig.11 is a photograph of the polishing pad of Example 4 after 4 hours of grinding;

[0064] Fig.12 is a photograph of the polishing pad after grinding for 8 hours in Example 4;

[0065] Fig.13 is a photograph of the polishing pad after grinding for 1 hour in Example 5;

[0066] Fig.14 is a photograph of the polishing pad after 4 hours of grinding in Example 5;

[0067] Fig.15 is a photograph of the polishing pad of Example 5 after grinding for 8 hours;

[0068] Fig.16 is a photograph of the polishing pad after grinding for 1 hour in Example 6;

[0069] Fig.17 is a photograph of the polishing pad after 4 hours of grinding in Example 6;

[0070] Fig.18 is a photograph of the polishing pad of Example 6 after grinding for 8 hours;

[0071] Fig.19 This is a photo of the polishing pad of control group 1 after 1 hour of grinding;

[0072] Fig. 20 This is a photo of the polishing pad of control group 1 after 2 hours of grinding;

[0073] Fig.21 This is a photo of the polishing pad of control group 2 after 1 hour of grinding;

[0074] Fig. 22 This is a photo of the polishing pad of control group 2 after 4 hours of grinding;

[0075] Fig.23 This is a photo of the polishing pad of control group 2 after 8 hours of grinding;

[0076] Fig.24 This is a photo of the polishing pad of control group 3 after 1 hour of grinding;

[0077] Fig.25 This is a photo of the polishing pad of control group 3 after 4 hours of grinding;

[0078] Fig.26 This is a photo of the polishing pad of control group 3 after 8 hours of grinding;

[0079] Fig. 27 This is a photo of the polishing pad of control group 4 after 1 hour of grinding;

[0080] Fig.28 This is a photo of the polishing pad of control group 4 after 2 hours of grinding;

[0081] Fig.29 is a photograph of the polishing pad of control group 5 after 1 hour of grinding;

[0082] Fig.30 This is a photo of the polishing pad of control group 5 after 4 hours of grinding;

[0083] Fig.31 is a photograph of the polishing pad of control group 6 after 1 hour of grinding;

[0084] Fig.32 This is a photograph of the polishing pad of Control Group 6 after 2 hours of polishing.

[0085] in: Fig.13 The bright white part in the middle is the reflection when taking the photo, not the white formed by the paste plate. DETAILED DESCRIPTION

[0086] The present invention is further described below in conjunction with the embodiments. The following description is by way of example, but the protection scope of the present invention should not be limited thereto.

[0087] The cutting force test and the plate sticking phenomenon test used in the following embodiments and control groups were performed using the following equipment and methods:

[0088] Cutting force test: Use ITO single-sided ring polishing machine (model: P-PM-7 ITO polishing machine, polishing pad diameter 800mm, the same below) and ITO glass (size 360×300×0.7mm, can hold two or four pieces of ITO glass, the same below), grind for 1h, the weight before grinding minus the weight after grinding divided by the grinding time is the cutting force.

[0089] The sticking phenomenon test: Use ITO single-sided ring polishing machine and ITO glass (size 360×300×0.7mm), polish continuously for 1 hour, observe the powder print on the polishing pad after stopping, then grind for another 1 hour, observe the powder print on the polishing pad, and so on. The sticking state of the disc can be judged by the appearance time and thickness of the powder print.

[0090] From the attached drawings, we can see that wherever there is a white part in the picture, it is a phenomenon of plate sticking, and the brighter and larger the white part is, the more serious the phenomenon of plate sticking is.

[0091] The rare earth polishing powder used in the following Examples 1-6 and Control Groups 4-6 is a rare earth polishing powder that complies with the "GB / T20165-2012" standard and has a particle size D50 of 0.8-2.0 μm, specifically a rare earth polishing powder produced by the CN103450814A method. Other rare earth polishing powders that comply with the "GB / T20165-2012" standard may also be used.

[0092] The rare earth polishing powder used in the control groups 1-3 is the rare earth polishing powder provided by the corresponding manufacturers and complies with the "GB / T20165-2012" standard.

[0093] Embodiment 1:

[0094] The rare earth polishing agent of this embodiment for improving the easy sticking of the polishing pad during the glass thinning process is prepared and tested as follows:

[0095] First, 20g of bentonite, 20g of sodium salt of maleic acid acrylic acid copolymer (average molecular weight of 25000, the same below), 20g of sodium tripolyphosphate, and 2kg of rare earth polishing powder were mixed evenly to prepare a rare earth polishing agent (i.e., a rare earth polishing agent for improving the easy sticking of the polishing pad during glass thinning, the same below). Finally, the mixed rare earth polishing agent was poured into 18kg of pure water, stirred for 30min, and then a grinding test was performed. By grinding at different time intervals, the sticking phenomenon of the polishing pad was observed. The observation results are detailed in the attached table and attached table below. Figure 1-3 .

[0096] Embodiment 2:

[0097] The rare earth polishing agent of this embodiment for improving the easy sticking of the polishing pad during the glass thinning process is prepared and tested as follows:

[0098] First, 40g of bentonite, 20g of sodium salt of maleic acid acrylic acid copolymer, 20g of sodium tripolyphosphate, and 2kg of rare earth polishing powder were mixed evenly to prepare a rare earth polishing agent. Finally, the mixed rare earth polishing agent was poured into 18kg of pure water, stirred for 30min, and then a grinding test was performed. The phenomenon of the polishing pad sticking to the plate was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached table below. Figure 4-6 .

[0099] Embodiment 3:

[0100] The rare earth polishing agent of this embodiment for improving the easy sticking of the polishing pad during the glass thinning process is prepared and tested as follows:

[0101] First, 40g of bentonite, 30g of sodium salt of maleic acid acrylic acid copolymer, 30g of sodium tripolyphosphate, and 2kg of rare earth polishing powder were mixed evenly to prepare a rare earth polishing agent. Finally, the mixed rare earth polishing agent was poured into 18kg of pure water, stirred for 30min, and then a grinding test was performed. The phenomenon of the polishing pad sticking to the plate was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached Figure 7-9 .

[0102] Embodiment 4:

[0103] The rare earth polishing agent of this embodiment for improving the easy sticking of the polishing pad during glass thinning is prepared and tested as follows:

[0104] First, 20g of bentonite, 60g of sodium salt of maleic acid acrylic acid copolymer, 60g of sodium tripolyphosphate, and 2kg of rare earth polishing powder were mixed evenly to prepare a rare earth polishing agent. Finally, the mixed rare earth polishing agent was poured into 18kg of pure water, stirred for 30min, and then a grinding test was performed. The phenomenon of the polishing pad sticking to the plate was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached Figure 10-12 .

[0105] Embodiment 5:

[0106] The rare earth polishing agent of this embodiment for improving the easy sticking of the polishing pad during the glass thinning process is prepared and tested as follows:

[0107] First, 60g of bentonite, 40g of sodium salt of maleic acid acrylic acid copolymer, 40g of sodium tripolyphosphate, and 2kg of rare earth polishing powder were mixed evenly to prepare a rare earth polishing agent. Finally, the mixed rare earth polishing agent was poured into 18kg of pure water, stirred for 30min, and then a grinding test was performed. The phenomenon of the polishing pad sticking to the plate was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached Figure 13-15 .

[0108] Embodiment 6:

[0109] The rare earth polishing agent of this embodiment for improving the easy sticking of the polishing pad during glass thinning is prepared and tested as follows:

[0110] First, 80g of bentonite, 60g of sodium salt of maleic acid acrylic acid copolymer, 60g of sodium tripolyphosphate, and 2kg of rare earth polishing powder were mixed evenly to prepare a rare earth polishing agent. Finally, the mixed rare earth polishing agent was poured into 18kg of pure water, stirred for 30min, and then a grinding test was performed. The phenomenon of polishing pad sticking was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached Figure 16-18 .

[0111] Control group 1:

[0112] Sodium hexametaphosphate, which is commonly used in the field of optics and mobile phone covers, was used as a dispersant. Its addition amount was 0.4% of the rare earth polishing powder. Grinding tests and polishing pad sticking comparisons were carried out. The polishing pad sticking phenomenon was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached Figure 19-20 .

[0113] Control group 2:

[0114] The polishing pad sticking and cutting force test was carried out using the product of a polishing powder factory in Shanghai (D50 about 1.1μm, CeO2 / REO about 65%). The product of this factory is relatively excellent, mainly able to solve the problem of polishing pad sticking, with a high market share and good reputation. The polishing pad sticking phenomenon was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached Figure 21-23 .

[0115] Control group 3:

[0116] The polishing pad sticking and cutting force test was conducted using the polishing powder product of a Jiangsu polishing powder factory (D50 about 1.1μm, CeO2 / REO about 65%). The company's products are mainly able to solve the problem of polishing pad sticking in the field of TFT thinning, and have a certain high market share. The polishing pad sticking phenomenon was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached Figure 24-26 .

[0117] Control group 4:

[0118] First, 40g of bentonite, 40g of sodium tripolyphosphate, and 2kg of rare earth polishing powder were mixed evenly to prepare rare earth polishing agent. Finally, the mixed rare earth polishing agent was poured into 18kg of pure water and stirred for 30min before grinding test. The polishing pad sticking phenomenon was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached table below. Figure 27-28 .

[0119] Control group 5:

[0120] First, 40g of bentonite, 40g of sodium salt of maleic acid acrylic acid copolymer, and 2kg of rare earth polishing powder were mixed evenly to prepare rare earth polishing agent. Finally, the mixed rare earth polishing agent was poured into 18kg of pure water, stirred for 30min, and then the grinding test was carried out. The phenomenon of polishing pad sticking was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached Figure 29-30 .

[0121] Control group 6:

[0122] First, 40g of sodium tripolyphosphate, 40g of sodium salt of maleic acid acrylic acid copolymer, and 2kg of rare earth polishing powder were mixed evenly to prepare a rare earth polishing agent. Finally, the mixed rare earth polishing agent was poured into 18kg of pure water and stirred for 30 minutes before grinding test. The polishing pad sticking phenomenon was observed by grinding at different time intervals. The observation results are detailed in the attached table and attached table below. Figure 31-32 .

[0123] Attached table: Summary table of test results of each embodiment and each control group:

[0124]

[0125] Note: The cutting rate during the pasting of the plate in control group 1 is the cutting rate of 2h.

[0126] It can be seen from the above test result summary table that, except for Example 1 and Example 4 which showed slight sticking after 8 hours of grinding, the other examples (i.e., Example 2, Example 3, Example 5 and Example 6) did not show sticking after 8 hours of grinding. Compared with the control group 1 which showed obvious sticking after 2 hours of grinding and the control group 3 which showed obvious sticking after 4 hours of grinding, the effects of improving sticking in the examples of the present invention (i.e., Examples 1-6) were better than those in the control group 1 and the control group 3, and even the relatively poor improvement effects of Example 1 and Example 4 were equal to the improvement effects of the control group 2. At the same time, the reduction degree of the cutting rate of Examples 1-6 from the initial 1h cutting rate to the sticking cutting rate was relatively small, and was less than the reduction degree of the cutting rate of Control Groups 1-3 from the initial 1h cutting rate to the sticking cutting rate, which shows that the cutting rate durability of Examples 1-6 is better than that of Control Groups 1-3.

[0127] Control groups 4-6 use any two of the three raw materials of bentonite, sodium salt of maleic acid acrylic acid copolymer and sodium tripolyphosphate as auxiliary agents, wherein: control group 4 uses bentonite and sodium tripolyphosphate as auxiliary agents, control group 5 uses bentonite and sodium salt of maleic acid acrylic acid copolymer as auxiliary agents, and control group 6 uses sodium salt of maleic acid acrylic acid copolymer and sodium tripolyphosphate as auxiliary agents. It can be seen from the test result summary table that control group 4 and control group 6 have obvious disc sticking after grinding for 2 hours, and control group 5 also has obvious disc sticking after grinding for 4 hours. This shows that using any two of the three raw materials of bentonite, sodium salt of maleic acid acrylic acid copolymer and sodium tripolyphosphate as auxiliary agents, the effect of improving disc sticking is inferior to the cutting rate durability of Examples 1-6 using bentonite, sodium salt of maleic acid acrylic acid copolymer and sodium tripolyphosphate as auxiliary agents. At the same time, the degree of reduction in the cutting rate of the control group 4-6 from the initial 1 hour cutting rate to the cutting rate when the plate is stuck is also higher than the degree of reduction in the cutting rate of the embodiment 1-6 from the initial 1 hour cutting rate to the cutting rate when the plate is stuck, which indicates that the cutting rate durability of the embodiment 1-6 is also better than that of the control group 4-6.

[0128] Therefore, the rare earth polishing agent for improving the easy sticking of large polishing pads during the thinning process of TFT and ITO glass of the present invention has a strong advantage in improving the easy sticking of large polishing pads during the thinning process of TFT and ITO glass.

[0129] The rare earth polishing agent for improving the easy sticking of large polishing pads in the process of TFT and ITO glass thinning is suitable for thinning and polishing of large optical and panel glass, especially in the field of TFT and ITO glass thinning using large polishing machines.

Claims

1. A rare earth polishing agent for improving the problem of large polishing pads being easily stuck during TFT and ITO glass thinning, characterized in that: The invention comprises the following raw materials in parts by weight: Rare earth polishing powder 100 clay 1-4 Phosphate 1-3 maleic acid acrylic acid copolymer sodium salt 1-3; The clay is one or more of kaolin, bentonite and montmorillonite, with a particle size D50 of 1-3 μm, a D100 of less than 13.54 μm, and a large particle size of less than 800 ppm. When there are two or three types of clay, the proportion of each component is equal by weight; cosmetic grade bentonite is preferred; The phosphate is one or both of sodium orthophosphate and sodium tripolyphosphate. When there are two, the proportion of each component is equal by weight; preferably food grade sodium tripolyphosphate; The average molecular weight of the sodium salt of maleic acid acrylic acid copolymer is 20000-30000; The rare earth polishing powder complies with the "GB / T20165-2012" standard, and its particle size D50 is 0.8-2.0 μm.

2. The rare earth polishing agent for improving the problem of large polishing pads being easily stuck during TFT and ITO glass thinning process according to claim 1, characterized in that: The large particle detection method is as follows: take a 1L beaker, add 400ml of water, then add 20g of 10% weight concentration sodium hexametaphosphate solution, turn on magnetic stirring, slowly add 10g of clay while stirring, stir for 30min until it is completely dispersed, and finally crush it with an ultrasonic crusher for 5min to obtain slurry; then, filter the slurry on a 15μm sieve until it is completely filtered, wash the sieve with pure water 3 times, and finally dry the sieve in an oven at 105°C to obtain large particles.

3. The rare earth polishing agent for improving the easy sticking of large polishing pads in the thinning process of TFT and ITO glass according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: Rare earth polishing powder 100 clay 1 Phosphate 1 maleic acid acrylic acid copolymer sodium salt 1.

4. The rare earth polishing agent for improving the problem of easy sticking of large polishing pads in the thinning process of TFT and ITO glass according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: Rare earth polishing powder 100 clay 2 Phosphate 1 maleic acid acrylic acid copolymer sodium salt 1.

5. The rare earth polishing agent for improving the problem of large polishing pads being easily stuck during TFT and ITO glass thinning process according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: Rare earth polishing powder 100 clay 2 Phosphate 1.5 Maleic Acid Acrylic Acid Copolymer Sodium Salt 1.

5.

6. The rare earth polishing agent for improving the easy sticking of large polishing pads in the thinning process of TFT and ITO glass according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: Rare earth polishing powder 100 clay 1 Phosphate 3 maleic acid acrylic acid copolymer sodium salt 3.

7. The rare earth polishing agent for improving the problem of large polishing pads being easily stuck during TFT and ITO glass thinning process according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: Rare earth polishing powder 100 clay 3 Phosphate 2 Maleic Acid Acrylic Acid Copolymer Sodium Salt 2.

8. The rare earth polishing agent for improving the problem of large polishing pads being easily stuck during TFT and ITO glass thinning process according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: Rare earth polishing powder 100 clay 4 Phosphate 3 maleic acid acrylic acid copolymer sodium salt 3.

9. The rare earth polishing agent for improving the problem of large polishing pads being easily stuck during the thinning process of TFT and ITO glass according to any one of claims 1 to 8, characterized in that: The average molecular weight of the sodium salt of maleic acid acrylic acid copolymer is 22000-28000.

10. The rare earth polishing agent for improving the problem of large polishing pads being easily stuck during TFT and ITO glass thinning process according to claim 9, characterized in that: The average molecular weight of the sodium salt of maleic acid acrylic acid copolymer is 25,000.