Force-induced color-changing material based on optical properties of gold nanoparticles and preparation method of force-induced color-changing material

By assembling the modified spherical gold nanoparticles with elastomer materials, using the plasmon coupling effect, a high sensitivity force-induced colored material was prepared, which solved the problems of low sensitivity and response hysteresis of existing materials, and achieved high sensitivity Force-induced chromic materials with high elastic strength can monitor mechanical stress in real time and provide strain memory.

CN118995192AInactive Publication Date: 2024-11-22SOUTHWEST PETROLEUM UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411084320.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing chromic materials have low sensitivity and hysteresis response, which cannot accurately monitor mechanical loads in real time and reduce the mechanical properties of the materials in applications.

Method used

By assembling the modified spherical gold nanoparticles with elastomer materials, a high-sensitivity force-discolored material is prepared by using the plasmon coupling effect. The assembled gold nanoparticles appear blue and burgundy after disassembly. And there are absorption peaks of different wavelengths in the ultraviolet-visible light region, accompanied by the change in the color of the polyurea film.

Benefits of technology

It realizes a force-induced chromic material with high sensitivity and elastic strength, which can record strain conditions in real time under mechanical stress, and provides strain memory colorimetric sensor function, which significantly improves the response speed and accuracy of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995192A_ABST
    Figure CN118995192A_ABST
Patent Text Reader

Abstract

The invention discloses a mechanochromic material based on optical properties of gold nanoparticles and a preparation method of the mechanochromic material, and relates to the technical field of mechanochromic materials and preparation methods of the mechanochromic materials, and the mechanochromic material is prepared from the following raw materials: assembled gold nanoparticles and a curing agent; the assembled gold nanoparticles are formed by assembling the following raw materials: gold nanoparticles and a cross-linking agent. When the gold nanoparticles are assembled into the nanostructure, the plasmon coupling effect occurs among the nanoparticles close to each other, the assembled gold nanoparticles are blue, the disassembled gold nanoparticles are wine red, and in the assembling and disassembling processes of the gold nanoparticles, the plasmon coupling effect occurs between the nanoparticles close to each other. Absorption peaks with different wavelengths appear in an ultraviolet-visible region, and along with color change of the force-induced color-changing material, the material is high in sensitivity and high in elastic strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of mechanochromic materials and preparation methods thereof, and in particular to a mechanochromic material based on the optical properties of gold nanoparticles and a preparation method thereof. Background Art

[0002] As time goes by, various buildings and large equipment will inevitably break or damage under the stimulation of mechanical loads. If these microcracks are not discovered and handled in time, unpredictable disasters will occur. Therefore, a material that can detect structural damage and damage simply, quickly and visually is urgently needed. Mechanochromic materials have the ability to change their visible color in response to mechanical force, and can monitor uneven stress / strain distribution in real time without the need for expensive power supplies and data processing equipment. Mechanochromic materials are introduced into elastomers by mechanical carriers. Mechanical carriers can produce effective chemical transformations under mechanical loads. In particular, mechanical carriers have the characteristics of showing changes in color or emission wavelength driven by mechanical force, and have been used as sensors for stress, strain and damage detection in polymer materials. Existing widely used mechanical carriers include rhodamine, spiropyran, etc., which have been applied to various polymer elastomers. Common elastomers include polyurethane, polydimethylsiloxane, polyacrylate, etc. However, in existing research, the preparation of materials with high toughness, fast response and high mechanochromic sensitivity is a long-standing challenge. In order for mechanochromic elastomers to play a role in practical applications, they must have properties such as low activation strain and stress, and high toughness. It is reported that there have been relevant studies on the influence of the structure of elastomers on the sensitivity of mechanochromic response and color activation energy. Unfortunately, it is uncommon to develop mechanochromic materials with high sensitivity. The fundamental reason is that high energy dissipation helps to improve the toughness of polymers, while energy dissipation will reduce the elasticity of polymer elastomers and the transmission efficiency of external forces in polymer chains, thereby inevitably reducing the mechanochromic sensitivity. At the same time, some mechanochromic materials with relatively good response to mechanical force stimulation are not fast enough, have a delay, and cannot accurately report the force conditions of the material in real time.

[0003] Therefore, current mechanochromic materials have problems such as low sensitivity, reduced mechanical properties of the material after addition, delayed response, and lack of universal applicability. How to solve the above problems has become a research hotspot in this field.

[0004] In view of this, this application is filed. Summary of the invention

[0005] The present invention provides a mechanochromic material based on the optical properties of gold nanoparticles and a preparation method thereof, wherein the assembled mechanochromic material is obtained by assembling gold nanoparticles modified by a BSPP solution with an elastomeric material, so as to solve the problem of low sensitivity of the mechanochromic material in the prior art.

[0006] The present invention is achieved through the following technical solutions:

[0007] The present application proposes a mechanochromic material based on the optical properties of gold nanoparticles, which is prepared from the following raw materials:

[0008] Assembled gold nanoparticles and curing agent;

[0009] The assembled gold nanoparticles are assembled from the following raw materials: gold nanoparticles and a cross-linking agent.

[0010] Preferably, the gold nanoparticles are obtained by modifying gold nanoparticles with a BSPP solution, and the gold nanoparticles are spherical gold nanoparticles.

[0011] Preferably, the crosslinking agent is poly-1,4-butanediol bis(4-aminobenzoate), and the curing agent is carbodiimide-modified diphenylmethane diisocyanate.

[0012] In order to better solve the above problems, an embodiment of the present invention provides a method for preparing a mechanochromic material based on the optical properties of gold nanoparticles, comprising the following steps:

[0013] S1: Preparation of spherical gold nanoparticles;

[0014] S2: Preparation of gold nanoparticles;

[0015] S3: Assembly of gold nanoparticles;

[0016] S4: Synthesis of mechanochromic materials.

[0017] Preferably, the preparation method adopted in S1 is a citric acid reduction method, and includes adding chloroauric acid solution to boiling deionized water, and then adding sodium citrate solution, and continuously stirring under boiling state. When the whole mixed solution turns into wine red, the reaction is completed.

[0018] Preferably, the concentration of the chloroauric acid solution is 0.08-0.12 g / mL; the concentration of the sodium citrate is 0.5-2 wt %.

[0019] Preferably, S2 includes modifying the spherical gold nanoparticles obtained in S1 with a BSPP solution.

[0020] Preferably, the modification preparation process comprises adding BSPP aqueous solution to the spherical gold nanoparticles, stirring the reaction, removing impurities to obtain a concentrated mixed solution, and adding pure water to the concentrated mixed solution for dispersion.

[0021] Preferably, the assembly process in S3 includes taking gold nanoparticles and adding them into anhydrous ethanol for dispersion, then adding a cross-linking agent into dichloromethane for dissolution to obtain a solution, adding the anhydrous ethanol dispersion of gold nanoparticles into the solution for mixed assembly, and when the color turns blue, the assembly is completed.

[0022] Preferably, the S4 synthesis process includes volatilizing the solvent of the assembled gold nanoparticles, and then adding a curing agent to react to obtain a mechanochromic material.

[0023] In the embodiments of the present invention, the gold nanoassembly structure not only has the performance of a single nanoparticle, but also has new properties caused by assembly. For example, when the gold nanoparticles are assembled into a nanostructure, a plasmon coupling effect will occur between the nanoparticles that are close to each other. The assembled gold nanoparticles appear blue, while the disassembled gold nanoparticles appear wine red. During the assembly and disassembly process of the gold nanoparticles, absorption peaks of different wavelengths appear in the ultraviolet-visible light region, accompanied by a change in the color of the polyurea film.

[0024] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0025] (1) In the embodiment of the present invention, when gold nanoparticles are assembled into a nanostructure, a plasmon coupling effect will occur between the nanoparticles that are close to each other. The assembled gold nanoparticles appear blue, while the disassembled gold nanoparticles appear wine red. During the assembly and disassembly process of the gold nanoparticles, absorption peaks of different wavelengths appear in the ultraviolet-visible light region, accompanied by the color change of the mechanochromic material. The material has strong sensitivity and high elastic strength.

[0026] (2) The deformation of the mechanochromic material provided by the embodiment of the present invention under mechanical stress leads to the disintegration of the embedded AuNP chain and the movement of the plasma band. During the deformation of the mechanochromic material, the uniformly embedded AuNP chain is stretched accordingly, resulting in an increase in the distance between particles, a weakening of the plasmon coupling, and a change in the color of the mechanochromic material. Then, the maximum absorption peak in the ultraviolet-visible region of the film can be recorded and associated with the degree of deformation, thereby producing a strain memory colorimetric sensor.

[0027] (3) In the embodiment of the present invention, BSPP-AuNPs were directly assembled in the matrix material P1000 (poly-1,4-butanediol bis(4-aminobenzoate)), and a highly sensitive, mechanochromic polyurea film was prepared by volatilizing the solvent, removing water, and then adding a carbodiimide-modified diphenylmethane diisocyanate (CD-MDI) curing agent. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0029] Figure 1 This is a schematic diagram of the color change of the BSPP-AuNPs-polyurea film prepared in Example 1 upon stretching;

[0030] Figure 2 This is a color schematic diagram of BSPP-AuNPs before assembly in Example 1 of the present invention;

[0031] Figure 3 This is a color schematic diagram of BSPP-AuNPs after assembly in Example 1 of the present invention;

[0032] Figure 4 Schematic diagram of ultraviolet detection of BSPP-AuNPs before assembly in Example 1 of the present invention;

[0033] Figure 5 Schematic diagram of ultraviolet detection during the BSPP-AuNPs assembly process in Example 1 of the present invention;

[0034] Figure 6 This is a picture of BSPP-AuNPs-P1000 after water removal in Example 1 of the present invention;

[0035] Figure 7 This is a schematic diagram of the BSPP-AuNPs-polyurea film prepared in Example 1 of the present invention;

[0036] Figure 8 This is the color image of the BSPP-AuNPs-polyurea film prepared in Example 1 of the present invention before stretching;

[0037] Fig. 9 This is a color diagram of the BSPP-AuNPs-polyurea film after stretching prepared in Example 1 of the present invention;

[0038] Fig.10This is the UV absorption graph of the BSPP-AuNPs-polyurea film prepared in Example 1 of the present invention during the stretching process;

[0039] Fig.11 This is a graph showing the strain and ultraviolet absorption peak change rate of the BSPP-AuNPs-polyurea film prepared in Example 1 of the present invention;

[0040] Fig.12 for Fig.11 A partial enlarged view of

[0041] Fig.13 This is the influence curve of the strain gradient of the BSPP-AuNPs-polyurea film prepared in Example 1 of the present invention on the RGB value of the red channel;

[0042] Fig.14 for Fig.13 A partial enlarged view of . DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0044] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0046] Gold nanoparticles have been the focus of intensive research, mainly because they have strong size- and shape-dependent properties. The formation of nanoparticle assemblies through collective effects such as interparticle coupling and structural ordering may produce new properties that cannot be achieved by individual nanoparticles. An important feature of this secondary structure is that the properties of nanoparticle assemblies can be dynamically controlled by manipulating assembly and disassembly behaviors. Colloidal nanoparticles of plasmonic noble metals (such as gold and silver) exhibit localized surface plasmon resonances (LSPRs), resulting in significant scattering and absorption in the visible spectrum. The LSPR effect occurs when there are a large number of free electrons on the surface of gold nanoparticles, and light irradiates the surface of the particles, causing the electrons to oscillate collectively under the action of light waves. When the frequency of the incident light matches the vibration frequency of the surface free electrons, a resonance effect occurs. The LSPR resonance frequency of gold nanoparticles is mainly concentrated in the visible to near-infrared region, which is manifested as the appearance of maximum absorption peaks of different wavelengths in the ultraviolet-visible region, making the gold nanoparticles in solution appear in different colors.

[0047] Based on this, an embodiment of the present invention provides a method for preparing a mechanochromic material based on the optical properties of gold nanoparticles, comprising the following steps:

[0048] S1: Preparation of spherical gold nanoparticles, which is a citric acid reduction method, and includes adding chloroauric acid solution to boiling deionized water, and then adding sodium citrate solution, and continuously stirring under boiling state. When the whole mixed solution turns into wine red, the reaction is completed, wherein the concentration of the chloroauric acid solution is 0.08-0.12 g / mL; the concentration of the sodium citrate is 0.5-2wt%.

[0049] S2: Preparation of gold nanoparticles, the preparation process includes adding BSPP aqueous solution to spherical gold nanoparticles, stirring the reaction and removing impurities to obtain a concentrated mixed solution, and adding pure water to the concentrated mixed solution for dispersion.

[0050] S3: Assembly of gold nanoparticles; the assembly process includes taking gold nanoparticles and adding them into anhydrous ethanol for dispersion, then adding a cross-linking agent into dichloromethane for dissolution to obtain a solution, adding the anhydrous ethanol dispersion of gold nanoparticles into the solution for mixed assembly, and when the color turns blue, the assembly is completed.

[0051] S4: Synthesis of mechanochromic materials, the synthesis process includes volatilizing the solvent of the assembled gold nanoparticles, and then adding a curing agent to react to obtain the mechanochromic material.

[0052] Wherein, the volume ratio of anhydrous ethanol to dichloromethane is 1-5:1-5, and the preferred volume ratio is 1:1.

[0053] Example 1

[0054] Provided is a method for preparing a mechanochromic material based on the optical properties of gold nanoparticles, comprising the following steps:

[0055] S1, preparation of spherical gold nanoparticles: Spherical gold nanoparticles were synthesized by the classic citric acid reduction method. Specifically, 200 μL of 0.1 g / mL chloroauric acid was added to 95 mL of boiling pure water, and then 5 mL of 1 wt% sodium citrate solution was quickly added. The heating temperature was adjusted to keep the solution in a boiling and stirring state. When the solution color turned into wine red (such as Figure 2 As shown in the figure, it indicates that gold nanosphere particles have been generated in the solution and the reaction is complete. The solution is cooled to room temperature to obtain a mixed solution product of spherical gold nanospheres.

[0056] S2. Preparation of gold nanoparticles: BSPP-modified gold nanoparticles (BSPP-AuNPs) were synthesized based on spherical gold nanoparticles. Specifically, 0.5 mL (40 mg / mL) of BSPP aqueous solution was added to the mixed liquid product of spherical gold nanoparticles. After stirring at 800 r / min for 4 h, the condensed liquid was centrifuged to remove impurities, and pure water was added to redisperse to 10 mL, and stored for later use.

[0057] S3, assembly of gold nanoparticles: assembly of BSPP-AuNPs in anhydrous ethanol, dichloromethane and P1000. Specifically, 1.5 ml of the gold nanoparticle liquid prepared in S2 was taken in a 2 mL centrifuge tube, and it was centrifuged to remove water. The supernatant was poured out, and the gold nanoparticles at the bottom were placed in a new centrifuge tube, and 3 ml of anhydrous ethanol was added to redisperse. At the same time, 0.912 g of poly-1,4-butanediol bis(4-aminobenzoate) was taken in a 20 ml small glass bottle, and 3 ml of dichloromethane was added to dissolve P1000. The anhydrous ethanol solution was transferred to the P1000 solution, the small glass bottle was sealed and shaken thoroughly, and it was heated in an oil bath for co-assembly, and the assembly liquid turned blue (such as Figure 3 The BSPP-AuNPs before assembly and the BSPP-AuNPs during assembly were tested using a UV-visible spectrophotometer. The test results were as follows: Figure 4 and Figure 5 As shown, Figure 5 The start of oil bath heating was taken as the starting time, wherein the oil bath heating temperature was 40°C, and the reaction times of 10 min, 40 min, 70 min, 130 min, 190 min, 250 min and 310 min were tested respectively.

[0058] S4, synthesis of mechanochromic materials: under the same oil bath conditions, the anhydrous ethanol and dichloromethane solvents were evaporated. After completing the above steps, the small glass bottle was placed in a vacuum oven to further remove water. Figure 6Figure 1 is the BSPP-AuNPs-P1000 after water removal. Weigh 0.23g of carbodiimide-modified diphenylmethane diisocyanate (CD-MDI) and dissolve it in dichloromethane. Add the CD-MDI solution to the assembled gold nanoparticles and use a rubber-tipped dropper to absorb and sonicate at the same time. Spread the solution evenly on a glass slide, evaporate the solvent dichloromethane in the air, transfer it to a drying dish and place it overnight for preliminary curing, and finally put it in a vacuum oven for curing to obtain a blue film of assembled gold nanoparticles. The specific BSPP-AuNPs-polyurea film is shown in Figure 1. Figure 7 shown.

[0059] The BSPP-AuNPs-polyurea film prepared in the embodiment of the present invention was tested. Fig.10 (UV absorption diagram during film stretching), Fig.11 (Correspondence diagram of strain and ultraviolet absorption peak change rate) and Fig.12 ( Fig.11 ). During the deformation of the film, the assembled BSPP-AuNPs are stretched accordingly, the distance between the particles increases (i.e., a disassembly process of the gold nanoparticles), and the plasmon decoupling leads to a change in the overall color of the film, accompanied by a blue shift of the ultraviolet absorption peak. The mechanochromic material can achieve a significant shift in the ultraviolet absorption peak within 10% strain, and a significant color change within 100% film strain, which is difficult to achieve for most mechanochromic materials. During the strain of the matrix material, due to changes in the assembly mode and structure of the gold nanoparticles, the RGB value of the red channel of the film spline changes during the stretching process, with a strain gradient of 1% (such as 1%-40%). Fig.14 As shown), the strain gradient after 40% strain is 20% (as shown Fig.13 shown).

[0060] This will affect the properties and wavelength of LSPR. Compared with the current research in related fields, the mechanochromic material reduces the color activation strain. Fig.11 Hehe Fig.12 It can be seen that during the spline stretching process, the strain gradient between 0-60% is 1%, and the strain gradient after 60% is 20%. Fig.11 and Fig.12 The ordinate is the ratio of the highest absorption peak before and after stretching to the ordinate corresponding to the abscissa. Figure 8 Schematic diagram of the color of BSPP-AuNPs-polyurea film before stretching. Fig. 9 Schematic diagram of the color of BSPP-AuNPs-polyurea film after stretching. Figure 1 Schematic diagram of the color change of BSPP-AuNPs-polyurea film upon stretching.

[0061] In general, the gold nanoassembly structure not only has the performance of a single nanoparticle, but also has new properties caused by assembly. When gold nanoparticles are assembled into a nanostructure, plasmon coupling effect will occur between nanoparticles close to each other. The assembled gold nanoparticles appear blue, while the disassembled gold nanoparticles appear wine red. During the assembly and disassembly process of the gold nanoparticles, absorption peaks of different wavelengths appear in the ultraviolet-visible region, accompanied by the color change of the polyurea film. The embodiment of the present invention uses the self-assembly of BSPP-AuNPs in a mixed solvent of anhydrous ethanol and dichloromethane and the optical properties of the plasmon resonance of gold nanoparticles to prepare a highly sensitive mechanochromic material.

[0062] For Example 1, the entire mechanochromic film production process is to assemble BSPP-AuNPs directly in the matrix material P1000, and then add carbodiimide modified diphenylmethane diisocyanate (CD-MDI) curing agent after evaporating the solvent and removing water to prepare a highly sensitive, mechanochromic polyurea film. The prepared BSPP-AuNPs-polyurea film exhibits a colorimetric response to mechanical force and can "remember" the strain and stress it has experienced. The deformation of the polymer material under mechanical stress leads to the disintegration of the embedded AuNP chain and the movement of the plasma band. During the deformation of the polyurea film, the uniformly embedded AuNP chain is stretched accordingly, resulting in an increase in the distance between particles, a weakening of the plasmon coupling, and a change in the overall color of the film. Then, the maximum absorption peak in the ultraviolet-visible region of the film can be recorded in association with the degree of deformation, thereby producing a strain memory colorimetric sensor.

[0063] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A mechanochromic material based on the optical properties of gold nanoparticles, characterized in that: The invention is prepared from the following raw materials: Assembled gold nanoparticles and curing agent; The assembled gold nanoparticles are assembled from the following raw materials: gold nanoparticles and a cross-linking agent.

2. A mechanochromic material based on the optical properties of gold nanoparticles according to claim 1, characterized in that: The gold nanoparticles are obtained by modifying gold nanoparticles with a BSPP solution, and the gold nanoparticles are spherical gold nanoparticles.

3. The mechanochromic material based on the optical properties of gold nanoparticles according to claim 1, characterized in that: The crosslinking agent is poly-1,4-butanediol bis(4-aminobenzoate), and the curing agent is carbodiimide-modified diphenylmethane diisocyanate.

4. A method for preparing a mechanochromic material based on the optical properties of gold nanoparticles according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: Preparation of spherical gold nanoparticles; S2: Preparation of gold nanoparticles; S3: Assembly of gold nanoparticles; S4: Synthesis of mechanochromic materials.

5. The method for preparing a mechanochromic material based on the optical properties of gold nanoparticles according to claim 4, characterized in that: The preparation method adopted in S1 is a citric acid reduction method, and includes adding chloroauric acid solution to boiling deionized water, and then adding sodium citrate solution, and continuously stirring under boiling state. When the whole mixed solution turns into wine red, the reaction is completed.

6. The method for preparing a mechanochromic material based on the optical properties of gold nanoparticles according to claim 5, characterized in that: The concentration of the chloroauric acid solution is 0.08-0.12 g / mL; the concentration of the sodium citrate is 0.5-2 wt %.

7. The method for preparing a mechanochromic material based on the optical properties of gold nanoparticles according to claim 4, characterized in that: S2 includes modifying and preparing the spherical gold nanoparticles obtained in S1 with a BSPP solution.

8. The method for preparing a mechanochromic material based on the optical properties of gold nanoparticles according to claim 7, characterized in that: The modification preparation process comprises adding BSPP aqueous solution into spherical gold nanoparticles, stirring for reaction, removing impurities to obtain a concentrated mixed solution, and adding pure water into the concentrated mixed solution for dispersion.

9. The method for preparing a mechanochromic material based on the optical properties of gold nanoparticles according to claim 4, characterized in that: The assembly process in S3 includes taking gold nanoparticles and adding them into anhydrous ethanol for dispersion, then adding a cross-linking agent into dichloromethane for dissolution to obtain a solution, adding the anhydrous ethanol dispersion of gold nanoparticles into the solution for mixed assembly, and when the color turns blue, the assembly is completed.

10. The method for preparing a mechanochromic material based on the optical properties of gold nanoparticles according to claim 4, characterized in that: The S4 synthesis process includes evaporating the solvent of the assembled gold nanoparticles and then adding a curing agent to react to obtain a mechanochromic material.

Citation Information

Patent Citations

  • Plasmonic nanoparticle-based colorimetric stress memory sensor

    CN106415196A

  • Nanofiller with high force-induced discoloration sensitivity and preparation method thereof

    CN117659257A

  • Airflow control method for air flotation cyclone operation of low-pressure heat treatment device

    KR1020250011584A

  • Plasmonic nanoparticle-based colorimetric stress memory sensor

    US20170176272A1