Wavelength-adjustable lasing luminescence nanoprobe and preparation method and application thereof
By using Au nanorods, mesoporous silica shells and hyaluronic acid encapsulation layers in the laser luminescent nanoprobe, combined with dye molecules, a narrow band emission and adjustable wavelength laser luminescent nanoprobe was solved The problems of wide spectrum and difficulty in wavelength regulation of traditional fluorescence probes have achieved simultaneous detection of multi-channels in tumor cells and multi-channel imaging in complex biological environments.
Patent Information
- Application Number
- CN202410933796.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
AI Technical Summary
The emission spectrum of traditional fluorescent probes is wide, resulting in spectral overlap and crosstalk problems, limiting the parallel number of multi-channel labeling and imaging, and the wavelength of the laser-emitting nanoprobe is difficult to adjust, hindering super-multi-channel sensing and imaging technology. development.
Au nanorods are used as plasmon resonant cavity, combined with mesoporous silica shell and hyaluronic acid encapsulation layer, and dye molecules are used as gain medium to construct wavelength adjustable laser luminescent nanos with narrowband emission through energy level matching principle Probes enable simultaneous detection of multi-channels in tumor cells.
Overcome the limitation of the spectral line width of the traditional fluorescence probe, achieve a low laser threshold and narrow emission spectrum line width, and can flexibly adjust the wavelength, support a variety of laser wavelengths in the 500nm-900nm wavelength window, solving the spectral crosstalk problem. Simultaneous detection of super multiple channels in tumor cells is achieved.
Smart Images

Figure CN118995194A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of nano materials and biological detection, and in particular to a wavelength-adjustable laser luminescence nano probe and a preparation method and application thereof. Background Art
[0002] In the vast field of modern biological and medical research, the innovation and application of advanced luminescent probes play an indispensable role. However, the common challenge faced by traditional fluorescent probes is their relatively broad emission spectrum (about 30-100nm). This feature causes significant spectral overlap and crosstalk problems in multi-channel labeling and imaging applications, greatly restricting the number of parallel distinguishable color labels and limiting the further development of the technology. Despite years of continuous exploration by scientists, the problem of spectral broadening has never been fundamentally solved due to the physical limitations of spontaneous radiation of fluorescent materials.
[0003] Laser technology stands out with its extremely narrow emission linewidth and becomes an ideal candidate to break through this bottleneck. If the size of the laser can be miniaturized to the nanometer level, the problem of spectral crosstalk will be completely eliminated. However, the traditional optical resonant cavity is limited by the diffraction limit, and its size is difficult to break through the micrometer level, which is too large for labeling and imaging at the cellular and molecular levels. For this reason, the concept of surface plasmon laser (Spaser) came into being. It cleverly uses surface plasmons to replace traditional photon oscillations, successfully compresses the size of the laser to the nanometer level, and opens a new era of nanophotonics. However, the practical application of Spaser technology still faces many challenges, especially how to realize a family of multi-wavelength tunable Spaser nanoprobes, which is crucial to promoting the development of ultra-multi-channel sensing and imaging technology. Since the first successful demonstration of Spaser in 2009, although the Spaser based on nanoparticle resonant cavity has shown the potential for multi-band emission, the flexibility and extensiveness of wavelength adjustment is still a major problem, which urgently needs further exploration and breakthroughs by scientific researchers. Summary of the invention
[0004] Purpose of the invention: The purpose of the present invention is to provide a wavelength-adjustable lasing luminescent nanoprobe and its preparation method and application in order to address the shortcomings of existing fluorescent probes, such as a wide emission spectrum and difficult-to-adjust wavelength of lasing luminescent nanoprobes. The probe not only has a low pump threshold and a narrow emission spectrum linewidth, but also can flexibly adjust the wavelength of the lasing luminescent nanoprobe, thereby realizing simultaneous multi-channel detection in tumor cells and opening up a new path for multi-channel imaging in complex biological environments.
[0005] Technical solution: To achieve the above purpose, the present invention proposes the following technical solution:
[0006] The present application provides a wavelength-adjustable laser luminescent nanoprobe, which includes an Au nanorod, a dye molecule, a mesoporous silica shell layer and a hyaluronic acid encapsulation layer, wherein the Au nanorod serves as a plasmon resonant cavity of the laser luminescent nanoprobe; the dye molecule serves as a gain medium; the mesoporous silica shell layer serves as a supporting layer to load the dye molecule around the Au nanorod; the hyaluronic acid encapsulation layer covers the surface of the mesoporous silica shell layer to prevent leakage of the dye molecule; the construction of the laser luminescent nanoprobe needs to meet the energy level matching principle.
[0007] The present application also provides a method for preparing the wavelength-tunable laser luminescent nanoprobe, comprising the following steps:
[0008] Step 1: preparing an Au nanorod aqueous solution, using a seed growth mediated method, first reducing chloroauric acid with a strong reducing agent to obtain a gold seed solution, then obtaining a gold growth solution by using a binary surfactant synergistic method, and finally adding silver nitrate, hydrochloric acid and the gold seed solution to the gold growth solution to obtain an Au nanorod aqueous solution;
[0009] Step 2: Prepare an aqueous solution of nanoparticles containing Au nanorods coated with a mesoporous silica shell. Use the Stober method to add a 0.1M sodium hydroxide solution to the Au nanorod aqueous solution prepared in step 1. After stirring for 15 minutes, add a methanol solution containing 20% tetraethyl silicate three times with an interval of 30 minutes. Then stir in a water bath at 28°C-30°C for 24 hours. After centrifugation and washing, obtain an aqueous solution of nanoparticles containing Au nanorods coated with a mesoporous silica shell.
[0010] Step 3: preparing an aqueous solution of nanoparticles doped with dye molecules. According to the principle of energy level matching, the aqueous solution of nanoparticles prepared in step 2 is mixed with the dye molecule solution in the dark for 48 hours to ensure that the dye molecules are fully penetrated and absorbed into the mesoporous silica shell layer. Unloaded dye molecules are removed by centrifugation and redispersion to obtain an aqueous solution of nanoparticles doped with dye molecules.
[0011] Step 4: Prepare a wavelength-tunable laser luminescent nanoprobe, add hyaluronic acid to the aqueous solution of nanoparticles obtained in step 3, stir overnight at room temperature in the dark, and obtain the wavelength-tunable laser luminescent nanoprobe after centrifugation and washing.
[0012] The present application also provides an application of the wavelength-tunable lasing luminescent nanoprobe in multicolor imaging in tumor cells, and uses a laser confocal microscope to test the multicolor imaging of the wavelength-tunable lasing luminescent nanoprobe in tumor cells; during the test, multiple detection channels are set, and the detection range of each channel is set to 10nm, wherein the excitation wavelength of each detection channel is set to the maximum absorption wavelength of the gain medium used by the lasing luminescent nanoprobe, and the excitation light intensity of each detection channel is set higher than the pump threshold to obtain multicolor imaging in tumor cells.
[0013] Beneficial Effects
[0014] The present application uses Au nanorods as plasmon resonant cavities, the resonant frequency of the Au nanorods being affected by their own aspect ratio, and dye molecules as gain media, the energy levels of the dye molecules matching the resonant frequency of the Au nanorods. By regulating the energy transfer between the plasmon resonant cavity and the gain medium, a lasing luminescent nanoprobe with narrow-band emission, low pumping threshold and flexibly adjustable wavelength is constructed.
[0015] Compared with the prior art, the advantages of the present application are: the probe overcomes the limitation of the wide spectral line width of the traditional fluorescent probe, and solves the problem that the wavelength of the laser luminescent nanoprobe is difficult to adjust, and can realize the simultaneous detection of ultra-multi-channels in tumor cells, opening up a new way for multi-channel imaging in complex biological environments;
[0016] The wavelength-tunable lasing nanoprobe of the present invention has a spectral line width of only 3nm to 10nm and a lasing threshold of 0.5mJ / cm 2 , not only has narrow-band emission similar to that of lasers, but can also be excited by commercial confocal microscope systems. By regulating the energy transfer between the plasmon resonant cavity and the gain medium, the emission wavelength of the lasing luminescent nanoprobe can be flexibly adjusted, and a family of nanoprobes including a variety of lasing wavelengths in the 500nm to 900nm wavelength window has been constructed. This probe family successfully solves the impact of spectral crosstalk and realizes simultaneous detection of multiple channels in tumor cells; the preparation method of the above-mentioned wavelength-adjustable lasing luminescent nanoprobe disclosed in this application is safe, efficient, and suitable for large-scale synthesis applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic diagram of the structure of the wavelength-tunable lasing luminescent nanoprobe of the present application.
[0018] Figure 2 is the transmission electron microscope image and ultraviolet absorption spectrum of the present application, wherein, Figure 2 A to E in the middle are schematic diagrams of probe transmission electron microscopy; Figure 2 F in the figure is the UV absorption spectra of Au nanorods with different aspect ratios.
[0019] Figure 3 This is a graph of the laser luminescence spectrum as a function of pump energy involved in this application. Figure 3 A is the original lasing spectrum as the pump energy increases from 0.1mJ / cm 2 -0.5mJ / cm 2 The change process diagram, Figure 3 B is the lasing spectrum after deducting the baseline as the pump energy increases from 0.5 mJ / cm 2 -1.0mJ / cm 2 Graph of the change process.
[0020] Figure 4 This is the curve of the laser luminescence spectrum varying with the pump energy involved in the present application.
[0021] Figure 5 These are all the lasing luminescence spectra of this application.
[0022] Figure 6 It is the multicolor imaging diagram of cells involved in this application. Among them, Figure 6 A in the middle is a bright field image of cells. Figure 6 Middle B is the separate imaging of four laser luminescence probes with different wavelengths in the same cell. Figure 6 Center C shows the simultaneous imaging of four lasing luminescence probes with different wavelengths in the same cell. DETAILED DESCRIPTION
[0023] The preferred embodiments of the present application will be described in detail below in conjunction with the examples. It should be understood that the following examples are provided only for the purpose of illustration and are not intended to limit the scope of the present application. Those skilled in the art may make various modifications and substitutions to the present application without departing from the purpose and spirit of the present application.
[0024] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0025] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0026] Sources of reagents used in the following examples:
[0027] Tetrachloroauric acid trihydrate, hexadecyltrimethylammonium bromide, sodium borohydride, sodium oleate, silver nitrate, ascorbic acid, sodium hydroxide, tetraethyl silicate, dimethyl sulfoxide and hyaluronic acid were purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.; Oregon green 488 and Alexa Fluor series dyes were purchased from Thermo Fisher Scientific (China) Co., Ltd.; LDS821 and IR140 dyes were purchased from Zhiyun Optoelectronics (Shanghai) Co., Ltd.
[0028] An embodiment of the present application provides a wavelength-tunable lasing luminescent nanoprobe, which includes an Au nanorod, a dye molecule, a mesoporous silica shell layer and a hyaluronic acid encapsulation layer, wherein the Au nanorod serves as a plasmon resonant cavity of the lasing luminescent nanoprobe; the dye molecule serves as a gain medium; the mesoporous silica shell layer serves as a supporting layer to load the dye molecule around the Au nanorod; the hyaluronic acid encapsulation layer covers the surface of the mesoporous silica shell layer to prevent leakage of the dye molecule; the construction of the lasing luminescent nanoprobe needs to meet the energy level matching principle.
[0029] In one embodiment, the aspect ratio of the Au nanorods is in the range of 1.0 to 5.0. The resonant frequency of the Au nanorods is affected by their aspect ratio.
[0030] In one embodiment, the dye molecules include Oregon green 488, Alexa Fluor 568, Alexa Fluor 594, Alexa Fluor 660, Alexa Fluor 680, Alexa Fluor 700, Alexa Fluor 790, LDS821 and IR140.
[0031] In one embodiment, the energy level matching principle is that the resonance absorption curve of the Au nanorods and the spontaneous emission curve of the dye molecules overlap in spectral form.
[0032] In one embodiment, the wavelength-tunable lasing luminescent nanoprobe includes different lasing wavelengths, and the lasing wavelength range of the wavelength-tunable lasing luminescent nanoprobe is 500nm to 900nm.
[0033] In one embodiment, the lasing wavelength of the wavelength-tunable lasing luminescent nanoprobe can be flexibly adjusted within a wavelength window of 500 to 900 nm.
[0034] In one embodiment, the pump threshold of the wavelength-tunable lasing nanoprobe is 0.5 mJ / cm2, and the lasing spectrum line width is 3 nm to 10 nm.
[0035] An embodiment of the present application provides a method for preparing the wavelength-tunable laser luminescence nanoprobe, comprising the following steps:
[0036] Step 1: preparing an Au nanorod aqueous solution, using a seed growth mediated method, first reducing chloroauric acid with a strong reducing agent to obtain a gold seed solution, then obtaining a gold growth solution by using a binary surfactant synergistic method, and finally adding silver nitrate, hydrochloric acid and the gold seed solution to the gold growth solution to obtain an Au nanorod aqueous solution;
[0037] Step 2: Prepare an aqueous solution of nanoparticles containing Au nanorods coated with a mesoporous silica shell. Use the Stober method to add a 0.1M sodium hydroxide solution to the Au nanorod aqueous solution prepared in step 1. After stirring for 15 minutes, add a methanol solution containing 20% tetraethyl silicate three times with an interval of 30 minutes. Then stir in a water bath at 28°C-30°C for 24 hours. After centrifugation and washing, obtain an aqueous solution of nanoparticles containing Au nanorods coated with a mesoporous silica shell.
[0038] Step 3: preparing an aqueous solution of nanoparticles doped with dye molecules. According to the principle of energy level matching, the aqueous solution of nanoparticles prepared in step 2 is mixed with the dye molecule solution in the dark for 48 hours to ensure that the dye molecules are fully penetrated and absorbed into the mesoporous silica shell layer. Unloaded dye molecules are removed by centrifugation and redispersion to obtain an aqueous solution of nanoparticles doped with dye molecules.
[0039] Step 4: Prepare a wavelength-tunable laser luminescent nanoprobe, add hyaluronic acid to the aqueous solution of nanoparticles obtained in step 3, stir overnight at room temperature in the dark, and obtain the wavelength-tunable laser luminescent nanoprobe after centrifugation and washing.
[0040] In one embodiment, in step 1, the strong reducing agent is sodium borohydride, and the binary surfactant includes hexadecyl ammonium bromide and sodium oleate.
[0041] In one embodiment, in step 2, the volume ratio of the Au nanorod solution, the sodium hydroxide solution and the methanol solution containing 20% tetraethyl silicate is 100:1:1.
[0042] In one embodiment, in step 3, the molar ratio of the Au nanorod particles to the dye molecules is 1:10. 4 Magnitude.
[0043] In one embodiment, in step 4, the molecular weight of the hyaluronic acid is 5000 Da.
[0044] An embodiment of the present application provides an application of the wavelength-tunable lasing luminescent nanoprobe in multi-color imaging in tumor cells, and a laser confocal microscope is used to test the multi-color imaging of the wavelength-tunable lasing luminescent nanoprobe in tumor cells. During the test, multiple detection channels are set, and the detection range of each channel is set to 10nm, wherein the excitation wavelength of each detection channel is set to the maximum absorption wavelength of the gain medium used by the lasing luminescent nanoprobe, and the excitation light intensity of each detection channel is set higher than the pump threshold to obtain multi-color imaging in tumor cells.
[0045] Example 1
[0046] like Figure 1As shown, this embodiment provides a wavelength-tunable laser luminescent nanoprobe, which includes Au nanorods 1, dye molecules 2, mesoporous silica shells 3 and hyaluronic acid encapsulation layers 4. The preparation method of the wavelength-tunable laser luminescent nanoprobe is as follows:
[0047] (1) Preparation of Au nanorods (Au NRs) aqueous solution:
[0048] First, 2.5 mL of 0.5 mM chloroauric acid and an equal volume of 0.2 M hexadecyl trimethyl ammonium bromide solution were mixed in a beaker. Under vigorous stirring, 300 μL of 0.01 M sodium borohydride ice water solution was added, stirred for 2 min, and aged at room temperature for 1 h to obtain a gold seed solution; then, 0.7 g hexadecyl trimethyl ammonium bromide and 0.1234 g sodium oleate were dissolved in 25 mL of warm water, cooled to 30 ° C, and 25 mL of 1 mM chloroauric acid solution was added, stirred until the solution became colorless, 125 μL of 0.064 M ascorbic acid was added to the above mixed solution, and the gold growth solution was obtained after vigorous stirring for 30 s; finally, 40 μL of gold seed solution was added to the gold growth solution, stirred for 30 s, and then allowed to stand at room temperature for 12 h to obtain an aqueous solution of Au nanorods (Au NRs (1.0)) with an aspect ratio of 1.0.
[0049] (2) Preparation of aqueous solution of Au nanorods coated with mesoporous silica shell (Au NRs@SiO2):
[0050] Take 20mL of the Au NRs (1.0) aqueous solution prepared in step (1), wash it by centrifugation, and then redisperse it in 10ml of 1mM hexadecyltrimethylammonium bromide solution. Subsequently, add 100μL of 0.1M sodium hydroxide solution and stir for 15min. Then, under gentle stirring, add a total of 100μL of a methanol solution containing 20% tetraethyl silicate in 3 times, with an interval of 30min. Finally, stir the reaction at 28-30°C for 24h. After the obtained product is washed by centrifugation, it is dispersed in 5mL of ultrapure water to finally obtain an Au NRs (1.0) @ SiO2 aqueous solution. Its transmission electron microscopy image is shown as follows Figure 2 As shown in A, the UV absorption spectrum is Figure 2 As shown in curve a in FIG.
[0051] (3) Preparation of dye-doped Au NRs@SiO2 nanoparticle aqueous solution:
[0052] The aqueous solution of nanoparticles prepared in step (2) was added with Oregongreen 488 (OG488) dye solution matching its energy level under slight stirring, and mixed for 48 hours to ensure that the dye molecules were fully penetrated and absorbed into the mesoporous silica shell layer. The unloaded dye molecules were removed by centrifugation and redispersion to obtain an OG488-Au NRs (1.0) @ SiO2 aqueous solution.
[0053] (4) Preparation of hyaluronic acid encapsulated Dye-Au NRs@SiO2 (Dye-Au NRs@SiO2-HA) nanoparticle aqueous solution:
[0054] 5 mg of hyaluronic acid was added to the aqueous solution of nanoparticles prepared in step (3), stirred overnight at room temperature in the dark, and centrifuged and washed to obtain a lasing luminescent nanoprobe.
[0055] Example 2
[0056] The preparation method of the wavelength-tunable laser luminescence nanoprobe is as follows:
[0057] (1) Preparation of Au nanorods (Au NRs) aqueous solution:
[0058] First, take 2.5mL of 0.5mM chloroauric acid and an equal volume of 0.2M hexadecyltrimethylammonium bromide solution and mix them in a beaker. Under vigorous stirring, add 300μL of 0.01M sodium borohydride ice water solution, stir for 2min, and age at room temperature for 1h to obtain a gold seed solution; then, dissolve 0.7g of hexadecyltrimethylammonium bromide and 0.1234g of sodium oleate in 25mL of warm water. Then, add 1.2mL and 2.4mL of silver nitrate solution respectively, let stand for 15min, add 25mL of 1mM chloroauric acid solution, and stir until the solution becomes colorless. Subsequently, 210 μL and 150 μL of hydrochloric acid solution were introduced respectively, and after stirring for 15 min, 125 μL of 0.064 M ascorbic acid was added to the mixed solution, and the gold growth solution was obtained after vigorous stirring for 30 s. Finally, 80 μL and 20 μL of gold seed solution were added to the gold growth solution respectively, and after stirring for 30 s, the mixture was allowed to stand at room temperature for 12 h to obtain Au nanorod aqueous solutions with aspect ratios of 1.9 and 2.7, respectively (Au NRs (1.9) and Au NRs (2.7)).
[0059] (2) Preparation of aqueous solution of Au nanorods coated with mesoporous silica shell (Au NRs@SiO2):
[0060] Take 20mL of the Au NRs (1.9) and Au NRs (2.7) aqueous solutions prepared in step (1) respectively, wash them by centrifugation, and then redisperse them in 10ml of 1mM hexadecyltrimethylammonium bromide solution. Subsequently, add 100μL of 0.1M sodium hydroxide solution and stir for 15min. Then, under gentle stirring, add 100μL of a methanol solution containing 20% tetraethyl silicate in 3 times, with an interval of 30min. Finally, stir the reaction at 28-30°C for 24h. After the obtained product is washed by centrifugation, it is dispersed in 5mL of ultrapure water to finally obtain Au NRs (1.9) @SiO2 and Au NRs (2.7) @SiO2 aqueous solutions. The transmission electron microscope image is as shown below Figure 2 As shown in B and C in 2, the UV absorption spectrum is Figure 2 As shown in curve b and curve c of F.
[0061] (3) Preparation of dye-doped Au NRs@SiO2 nanoparticle aqueous solution:
[0062] The aqueous solution of nanoparticles prepared in step (2) was added with Alexa Fluor 568 (AF568), Alexa Fluor 594 (AF594) (matched with Au NRs (1.9) @ SiO2), Alexa Fluor 660 (AF660), Alexa Fluor 680 (AF680) and Alexa Fluor 700 (AF700) (matched with Au NRs (2.7) @ SiO2) dye solutions with energy levels matching the nanoparticles under slight stirring, and mixed for 48 hours to ensure that the dye molecules fully penetrate and absorb into the mesoporous silica shell layer, and the unloaded dye molecules were removed by centrifugation and redispersion to obtain AF568-Au NRs (1.9) @ SiO2, AF594-AuNRs (1.9) @ SiO2, AF660-Au NRs (2.7) @ SiO2, AF680-Au NRs(2.7)@SiO2 and AF700-Au NRs(2.7)@SiO2 aqueous solutions.
[0063] (4) Preparation of hyaluronic acid encapsulated Dye-Au NRs@SiO2 (Dye-Au NRs@SiO2-HA) nanoparticle aqueous solution:
[0064] 5 mg of hyaluronic acid was added to the aqueous solution of nanoparticles obtained in step (3), stirred overnight at room temperature in the dark, and centrifuged and washed to obtain lasing luminescent nanoprobes.
[0065] Example 3
[0066] The preparation method of the wavelength-tunable laser luminescence nanoprobe is as follows:
[0067] (1) Preparation of Au nanorods (Au NRs) aqueous solution:
[0068] First, take 2.5mL of 0.5mM chloroauric acid and mix it with an equal volume of 0.2M hexadecyltrimethylammonium bromide solution in a beaker. Under vigorous stirring, add 300μL of 0.01M sodium borohydride ice water solution, stir for 2min, and age at room temperature for 1h to obtain a gold seed solution; then, dissolve 0.7g of hexadecyltrimethylammonium bromide and 0.1234g of sodium oleate in 25mL of warm water. Then, add 2.4mL and 1.8mL of silver nitrate solution respectively, let it stand for 15min, then add 25mL of 1mM chloroauric acid solution and stir until the solution becomes colorless. Subsequently, 300 μL and 210 μL of hydrochloric acid solution were introduced respectively, and after stirring for 15 min, 125 μL of 0.064 M ascorbic acid was added to the mixed solution, and the gold growth solution was obtained after vigorous stirring for 30 s. Finally, 20 μL and 80 μL of gold seed solution were added to the gold growth solution respectively, and after stirring for 30 s, the mixture was allowed to stand at room temperature for 12 h to obtain Au nanorod aqueous solutions with aspect ratios of 4.1 and 5.0, respectively (Au NRs (4.1) and Au NRs (5.0)).
[0069] (2) Preparation of aqueous solution of Au nanorods coated with mesoporous silica shell (Au NRs@SiO2):
[0070] Take 20mL of the Au NRs (4.1) and Au NRs (5.0) nanoparticle aqueous solutions prepared in step (1), wash them by centrifugation, and then redisperse them in 10ml of 1mM hexadecyltrimethylammonium bromide solution. Subsequently, add 100μL of 0.1M sodium hydroxide solution and stir for 15min. Then, under gentle stirring, add 100μL of a methanol solution containing 20% tetraethyl silicate in 3 times, with an interval of 30min. Finally, stir the reaction at 28-30°C for 24h. After the obtained product is washed by centrifugation, it is dispersed in 5mL of ultrapure water to finally obtain Au NRs (4.1) @SiO2 and Au NRs (5.0) @SiO2 aqueous solutions. The transmission electron microscopy images are shown as follows Figure 2 As shown in D and E in 2, the UV absorption spectrum is Figure 2 As shown in curve d and curve e in FIG.
[0071] (3) Preparation of dye-doped Au NRs@SiO2 nanoparticle aqueous solution:
[0072] The aqueous solution of nanoparticles prepared in step (2) was added with Alexa Fluor 700 (AF700), Alexa Fluor 790 (AF790), LDS821 (compatible with Au NRs (4.1) @SiO2) and IR140 (compatible with Au NRs (5.0) @SiO2) dye solutions with matching energy levels under slight stirring, and mixed for 48 hours to ensure that the dye molecules were fully penetrated and absorbed into the mesoporous silica shell layer. The unloaded dye molecules were removed by centrifugation and redispersion to obtain aqueous solutions of AF700-Au NRs (4.1) @SiO2, AF790-Au NRs (4.1) @SiO2, LDS821-Au NRs (4.1) @SiO2 and IR140-Au NRs (5.0) @SiO2.
[0073] (4) Preparation of hyaluronic acid encapsulated Dye-Au NRs@SiO2 (Dye-Au NRs@SiO2-HA) nanoparticle aqueous solution:
[0074] 5 mg of hyaluronic acid was added to the aqueous solution of nanoparticles prepared in step (3), stirred overnight at room temperature in the dark, and centrifuged and washed to obtain lasing luminescent nanoprobes.
[0075] Example 4
[0076] Detection of the luminescence properties of wavelength-tunable laser-luminescent nanoprobes:
[0077] The luminescence performance of the laser luminescent nanoprobes prepared in Examples 1 to 3 was measured using a self-built spectrometer system. The self-built spectrometer system uses a pulsed laser (20 Hz, Quanta-Ray INDI, spectra-physis, USA) as a pump source and a compact fiber spectrometer (CCS200, Thorlabs Inc., USA) to collect the emission spectrum. Taking the prepared AF700-Au NRs(2.7)@SiO2-HA as an example, the relationship between the luminescence intensity of the laser luminescent nanoprobe and the pump energy is shown in the figure. Figure 3 and Figure 4 As shown, the pump threshold is about 0.5mJ / cm 2 .like Figure 5 As shown, by regulating the energy transfer between the gain medium and the plasmon resonant cavity, the wavelength of the lasing luminescent nanoprobe is flexibly adjustable. At the same time, a nanoprobe family with 9 lasing wavelengths in the wavelength window of 500 to 900 nm is constructed, and the lasing spectrum linewidth is between 3 and 10 nm.
[0078] Example 5
[0079] Wavelength-tunable lasing nanoprobes for multicolor imaging in tumor cells:
[0080] A laser confocal microscope system was used to measure the application of the lasing luminescent nanoprobes prepared in Examples 1 to 3 for multicolor imaging in tumor cells. Taking four of the prepared lasing luminescent nanoprobes as an example, Hela cells were first cultured on a confocal dish for 18 hours, and then four luminescent nanoprobe solutions with the same concentration (50 μg / mL) and different lasing wavelengths were added to the confocal dish in turn and incubated at 37°C for 6 hours. Before the test, the confocal dish was washed three times with a PBS solution with a pH of 7.4 to remove excess nanoparticles. During the test, four detection channels were set, the detection range of each channel was set to 10 nm, the excitation wavelength of each channel was set to the maximum absorption wavelength of the gain medium used, and the excitation light intensity of each detection channel was set to be higher than the pump threshold. Figure 6 As shown, Figure 6 A in the middle is a bright field image of cells. Figure 6 Middle B is the separate imaging of four laser luminescence probes with different wavelengths in the same cell. Figure 6 Figure C shows the simultaneous imaging of four laser luminescence probes with different wavelengths in the same cell. This wavelength-tunable laser luminescence nanoprobe achieves four-color simultaneous imaging in tumor cells.
[0081] The above are only preferred implementations of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.
Claims
1. A wavelength-tunable lasing nanoprobe, characterized in that: The probe includes Au nanorods, dye molecules, a mesoporous silica shell and a hyaluronic acid encapsulation layer, wherein the Au nanorods serve as the plasmon resonant cavity of the laser luminescent nanoprobe; the dye molecules serve as the gain medium; the mesoporous silica shell serves as a supporting layer to load the dye molecules around the Au nanorods; the hyaluronic acid encapsulation layer covers the surface of the mesoporous silica shell to prevent leakage of the dye molecules; the construction of the laser luminescent nanoprobe needs to meet the energy level matching principle.
2. The wavelength-tunable lasing nanoprobe according to claim 1, characterized in that: The aspect ratio of the Au nanorods is in the range of 1.0 to 5.
0.
3. The wavelength-tunable lasing nanoprobe according to claim 1, characterized in that: The dye molecules include Oregon green 488, Alexa Fluor 568, Alexa Fluor 594, Alexa Fluor 660, Alexa Fluor 680, Alexa Fluor 700, Alexa Fluor 790, LDS821 and IR140.
4. The wavelength-tunable lasing nanoprobe according to claim 1, characterized in that: The energy level matching principle is that the resonance absorption curve of the Au nanorods and the spontaneous emission curve of the dye molecules overlap in spectral form.
5. The wavelength-tunable lasing nanoprobe according to claim 1, characterized in that: The lasing wavelength range of the wavelength-adjustable lasing luminescent nanoprobe is 500nm-900nm.
6. The wavelength-tunable lasing nanoprobe according to claim 1, characterized in that: The pumping threshold of the wavelength-tunable lasing nanoprobe is 0.5 mJ / cm 2 The lasing spectrum line width is 3nm~10nm.
7. A method for preparing a wavelength-tunable lasing nanoprobe according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: preparing an Au nanorod aqueous solution, firstly reducing chloroauric acid with a strong reducing agent to obtain a gold seed solution, then obtaining a gold growth solution by using a binary surfactant synergistic method, and finally adding silver nitrate, hydrochloric acid and the gold seed solution to the gold growth solution to obtain an Au nanorod aqueous solution; Step 2: Prepare an aqueous solution of nanoparticles containing Au nanorods coated with a mesoporous silica shell, add a 0.1M sodium hydroxide solution to the Au nanorod aqueous solution prepared in step 1, stir for 15 minutes, add a methanol solution containing 20% tetraethyl silicate three times, with an interval of 30 minutes, and then stir for 24 hours in a water bath at 28°C-30°C, centrifuge and wash with water to obtain an aqueous solution of nanoparticles containing Au nanorods coated with a mesoporous silica shell; Step 3: preparing an aqueous solution of nanoparticles doped with dye molecules. According to the principle of energy level matching, the aqueous solution of nanoparticles prepared in step 2 is mixed with the dye molecule solution in the dark for 48 hours, and unloaded dye molecules are removed by centrifugation and redispersion to obtain an aqueous solution of nanoparticles doped with dye molecules. Step 4: Prepare a wavelength-tunable laser luminescent nanoprobe, add hyaluronic acid to the aqueous solution of nanoparticles obtained in step 3, stir overnight at room temperature in the dark, and obtain the wavelength-tunable laser luminescent nanoprobe after centrifugation and washing.
8. The method for preparing the wavelength-tunable laser luminescence nanoprobe according to claim 7, characterized in that: In step 1, the strong reducing agent is sodium borohydride, and the binary surfactant includes hexadecyl ammonium bromide and sodium oleate; in step 2, the volume ratio of the Au nanorod solution, the sodium hydroxide solution and the methanol solution containing 20% tetraethyl silicate is 100:1:
1.
9. The method for preparing the wavelength-tunable laser luminescence nanoprobe according to claim 7, characterized in that: In step 3, the molar ratio of the Au nanorod particles to the dye molecules is 1:10 4 Magnitude; in step 4, the molecular weight of the hyaluronic acid is 5000Da.
10. An application of the wavelength-tunable lasing luminescent nanoprobe according to any one of claims 1 to 6 in multicolor imaging in tumor cells, characterized in that: A laser confocal microscope is used to test the multi-color imaging of the wavelength-adjustable lasing luminescent nanoprobe in tumor cells. During the test, multiple detection channels are set, and the detection range of each channel is set to 10 nm, wherein the excitation wavelength of each detection channel is set to the maximum absorption wavelength of the gain medium used by the lasing luminescent nanoprobe, and the excitation light intensity of each detection channel is set higher than the pumping threshold to obtain multi-color imaging in tumor cells.
Citation Information
Cited By
Lasing light-emitting nano recognition probe as well as preparation method and application thereof
CN122609227A
Wavelength-adjustable stimulated-emission nanoprobe, preparation method therefor and use thereof
WO2026011714A1