Free-form surface random metal texture manufacturing method
Through ultrasonic cleaning, photoresist film coating and precise laser exposure on the free curved substrate, the deviation problem in multiple scanning and etching of the curved substrate is solved, and high-precision and high-quality metal texture production is achieved. Improves the stability and efficiency of the manufacturing process.
Patent Information
- Application Number
- CN202411175361.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-26
AI Technical Summary
In the fields of micro-nano manufacturing and precision engineering, there are insufficient repetition accuracy and biased position problems during multiple scanning and etching of curved substrates, which affects the high-precision application of laser direct writing technology.
By performing ultrasonic cleaning on a free-surface substrate, photoresist film coating, baking glue solidification, precise laser exposure, development, vacuum evaporation coating and glue dissipation steps, combined with high-precision vision system and pre-programmed space expansion The surface trajectory determines the laser motion trajectory to ensure the laser is accurately exposed and forms a uniform metal texture.
The precise exposure of the free surface substrate and high-quality production of metal textures are achieved, the production accuracy and repeatability are improved, the stability and efficiency of the manufacturing process are enhanced, and the position bias problem in multiple scanning etching is avoided.
Smart Images

Figure CN119002188A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of free-form surface random metal texture production, in particular to a free-form surface random metal texture production method. Background Art
[0002] Currently, in the field of micro-nano manufacturing and precision engineering, laser direct writing technology is widely used to make complex micron- or nano-scale structures due to its high resolution and flexibility. However, for the processing of curved substrates, especially in application scenarios that require multiple scans and etching, this technology faces severe challenges in repeatability. Specifically, at least two scans and etching of the curved surface place particularly stringent requirements on the accuracy and stability of the laser direct writing equipment. During multiple scans, even small mechanical deviations or alignment errors can lead to significant misalignment, which can accumulate and amplify, ultimately affecting the geometric accuracy and functional performance of the product, thereby limiting the scope of application of laser direct writing technology in high-precision curved surface processing. Summary of the invention
[0003] In order to solve the problem of high probability of deviation in multiple scanning and etching of laser direct writing equipment in traditional manufacturing methods, the present application provides a method for manufacturing random metal textures on free-form surfaces.
[0004] A method for producing random metal textures on free-form surfaces, the method comprising: S11, ultrasonic cleaning of water drop-shaped free-form surface substrate, S12, forming a film of photoresist on the water drop-shaped free-form surface substrate after ultrasonic cleaning; S13, baking the water drop-shaped free-form surface substrate after the film coating of the photoresist to solidify the glue; S14, determining prefabricated texture pattern information, obtaining visual image information of the water drop-shaped free-form surface substrate after baking and solidifying the glue according to the prefabricated texture pattern information, analyzing the visual image information and the prefabricated texture pattern information, and determining a laser motion trajectory, wherein the laser motion trajectory is used to control the laser to perform an exposure operation on the water drop-shaped free-form surface substrate after baking and solidifying the glue according to the prefabricated texture pattern information; S15, developing the exposed water drop-shaped free-form surface substrate; S16, performing vacuum evaporation coating on the developed water drop-shaped free-form surface substrate; S17, removing the glue from the water drop-shaped free-form surface substrate after coating; S18, ultrasonic cleaning of the water drop-shaped free-form surface substrate after debonding; S19, transferring the cleaned and debonded water drop-shaped free-form surface substrate to a projection optical imager for texture measurement.
[0005] By adopting the above technical solution, the prefabricated texture pattern information is determined, and combined with the visual image information of the water drop-shaped free-form surface substrate after baking and solidifying, the two are analyzed to determine the movement trajectory of the laser. This step utilizes a high-precision visual system and a pre-programmed spatial expansion surface trajectory to ensure that the laser is accurately exposed according to the prefabricated texture pattern information, thereby reducing the problem of deviation caused by insufficient repeatability. This method achieves accurate exposure of the free-form surface substrate by precisely controlling the movement trajectory of the laser, avoids the deviation that occurs during multiple scanning and etching processes, and improves the production accuracy and repeatability. In addition, through subsequent development, vacuum evaporation coating and degumming steps, this method can form a uniform and precise metal texture on the free-form surface substrate, and finally ensure the texture quality through ultrasonic cleaning and optical imager measurement, realizing high-quality free-form surface random metal texture production; this not only improves the performance and reliability of the product, but also enhances the stability and efficiency of the manufacturing process.
[0006] Preferably, in step S12, a photoresist film is coated on the water drop-shaped free-form surface substrate after ultrasonic cleaning by an ultrasonic coating mechanism, wherein the ultrasonic coating mechanism comprises a control box, a first motion system located on the control box, a contoured heating base and a support frame, wherein the first motion system is provided with an ultrasonic nozzle, and the support frame is provided with a visual system; Step 12 also includes the following steps: Based on the visual system, the motion coordinate system of the water drop-shaped free-form surface base is obtained; Determine a preset three-dimensional trajectory; According to the preset three-dimensional trajectory and the motion coordinate system, the first motion system is controlled to perform a coating operation on the water drop-shaped free-form surface substrate located in the contoured heating base.
[0007] By adopting the above technical solution, the technical effect of using the ultrasonic coating mechanism in step S12 is that, through the assistance of a precise visual system and the control of the first motion system, uniform film coating of the photoresist on the water droplet-shaped free-form surface substrate is achieved, thereby ensuring the quality and accuracy of the subsequent photolithography process. At the same time, the application of a contoured heating base effectively avoids the problem of inconsistent coating thickness caused by the substrate shape or gravity.
[0008] Preferably, the contoured heating base is provided with a controllable heating flexible cloth, and before executing step S12, the following steps are also included: Determining whether the temperature parameter of the controllable heating flexible cloth reaches a preset threshold; If yes, then push a first window for prompting to start the ultrasonic coating mechanism to perform photoresist film coating; If not, a second window is pushed to prompt that the conditions for starting the ultrasonic coating mechanism to perform photoresist film coating are not met, and an audible and visual alarm is issued.
[0009] By adopting the above technical solution, this technology integrates a controllable heating flexible cloth on the contoured heating base and performs preset threshold detection of temperature parameters before coating the photoresist, thereby ensuring that the substrate is coated with photoresist under optimal temperature conditions, thereby improving the film quality and process reliability, while enhancing the controllability and safety of the process through intuitive window prompts and sound and light alarm mechanisms.
[0010] Preferably, the preset threshold is 30±2°C.
[0011] By adopting the above technical solution, by setting the preset threshold value to 30±2°C, this technology ensures the temperature control accuracy of the substrate before photoresist coating, thereby optimizing the film forming effect of the photoresist, improving the uniformity and adhesion of the coating, and reducing process defects caused by temperature fluctuations.
[0012] Preferably, in step S14, the texture pattern corresponding to the prefabricated texture pattern information is spread all over the surface of the water drop-shaped free-form surface substrate by the laser system and the second motion system to complete the exposure operation; The laser system determines the prefabricated texture micro-units through a DMD spatial light modulator and a beam shaping lens group, and projects a small light curtain of the prefabricated texture micro-units onto a water drop-shaped free-form surface substrate.
[0013] By adopting the above technical solution, the technology adopted in step S14 achieves high-resolution and high-precision texture pattern exposure by precisely controlling the collaborative operation of the laser system and the second motion system, combined with the DMD spatial light modulator and the beam shaping lens group, ensuring that the prefabricated texture micro-units can be evenly and accurately projected and covered on the entire droplet-shaped free-form surface substrate surface, thereby giving it a predetermined functional texture pattern while maintaining the original characteristics of the surface.
[0014] Preferably, the wavelength of the laser light source in the laser system is 375±10 nm.
[0015] By adopting the above technical solution and selecting a laser light source with a wavelength of 375±10nm, this technology achieves precise absorption and processing of specific materials, while minimizing the heat-affected zone, effectively avoiding unnecessary damage to the droplet-shaped free-form surface substrate, and ensuring the fineness of micro-nano structure processing and the integrity of the substrate material.
[0016] Preferably, in step S15, the debonding liquid is sprayed onto the surface of the water droplet-shaped free-form surface substrate for development, wherein the thickness of the micron thin film coating formed after the solvent in the photoresist evaporates will also be different in different time periods of the development process, and the development operation time is defined by determining different photoresist materials and the thickness difference of the micron thin film coating; In step 17, the debonding liquid is sprayed onto the surface of the water droplet-shaped free-form surface substrate for debonding. The thickness of the micron thin film coating formed after the solvent in the photoresist evaporates will also be different in different time periods of the debonding process. The debonding operation time is defined by determining different photoresist materials and the thickness difference of the micron thin film coating.
[0017] By adopting the above technical solution, by precisely controlling the spraying of the degumming liquid during the development and degumming process, combined with real-time monitoring of different photoresist materials and micron film coating thickness, this technology achieves the precise definition of the development and degumming operation time, ensuring the uniform removal of the photoresist coating and the accurate transfer of the micron-level pattern, thereby optimizing the accuracy and repeatability of the entire lithography process.
[0018] Preferably, in step S16, the following steps are included: Clamping the developed water drop-shaped free-form surface substrate in a self-rotating fixture; The RF ion source is used to bombard and clean the water drop-shaped free-form surface substrate clamped in the rotating fixture according to the preset operation time; A layer of chromium film, a layer of copper film, another layer of chromium film, another layer of copper film and a final layer of chromium film are sequentially deposited on the surface of the water drop-shaped free-form surface substrate.
[0019] By adopting the above technical solution, the technology used in step S16 fixes the developed water drop-shaped free-form surface substrate in a rotating fixture, uses an RF ion source to perform surface bombardment cleaning, and then accurately evaporates multiple layers of alternating chromium and copper films, thereby achieving a uniform and high-quality electromagnetic shielding layer deposition, while ensuring the precise alignment and cleanliness of the substrate, thereby improving the performance and reliability of the final product.
[0020] A method for producing a random metal texture on a free-form surface, the method comprising: S21, ultrasonic cleaning of water drop-shaped free-form surface substrate, S22, performing vacuum evaporation coating on the water drop-shaped free-form surface substrate after ultrasonic cleaning; S23, forming a film and coating a photoresist on the water drop-shaped free-form surface substrate after coating; S24, baking the drop-shaped free-form surface substrate after the film coating of the photoresist to solidify the glue; S25, determining prefabricated texture pattern information, obtaining visual image information of the water drop-shaped free-form surface substrate after baking and solidifying the glue according to the prefabricated texture pattern information, analyzing the visual image information and the prefabricated texture pattern information, and determining a laser motion trajectory, wherein the laser motion trajectory is used to control the laser to perform an exposure operation on the water drop-shaped free-form surface substrate after baking and solidifying the glue according to the prefabricated texture pattern information; S26, developing the exposed water drop-shaped free-form surface substrate; S27, etching the developed water drop-shaped free-form surface substrate; S28, debonding the etched water drop-shaped free-form surface substrate S29, ultrasonic cleaning of the water drop-shaped free-form surface substrate after debonding; S210, transferring the cleaned and debonded water drop-shaped free-form surface substrate to a projection optical imager for texture measurement.
[0021] By adopting the above technical scheme, the technical effect of the method for producing random metal textures on free-form surfaces is that, through a series of finely controlled steps such as ultrasonic cleaning, vacuum evaporation coating, photoresist coating and baking, precise laser exposure, development and etching, debonding and ultrasonic cleaning, a uniform and precise random metal texture with predetermined electromagnetic shielding properties is produced on a water drop-shaped free-form surface substrate, while ensuring the integrity and optical properties of the substrate, and finally the texture is measured by an optical imager to verify the product quality.
[0022] Preferably, step S26 includes: Spraying an etching liquid onto the developed water drop-shaped free-form surface substrate, wherein the etching liquid is used for simultaneously etching chromium and copper; The drop-shaped free-form surface substrate after etching is dried.
[0023] By adopting the above technical solution, the technical effect in step S26 is that the chromium and copper layers on the developed droplet-shaped free-form surface substrate are simultaneously removed by spraying etching liquid, thereby achieving accurate metal layer pattern transfer, and the subsequent drying treatment ensures the cleanliness of the substrate and the smooth progress of subsequent processes, thereby giving the substrate the required functional texture while maintaining the surface characteristics.
[0024] In summary, the present application includes at least one of the following beneficial technical effects: 1. By determining the prefabricated texture pattern information and combining it with the visual image information of the water drop-shaped free-form surface substrate after baking and solidifying the glue, the two are analyzed to determine the movement trajectory of the laser. This step utilizes a high-precision visual system and a pre-programmed spatial expansion surface trajectory to ensure that the laser is accurately exposed according to the prefabricated texture pattern information, thereby reducing the problem of deviation caused by insufficient repeatability. This method achieves precise exposure of the free-form surface substrate by precisely controlling the movement trajectory of the laser, avoids deviations that occur during multiple scanning and etching processes, and improves manufacturing accuracy and repeatability. In addition, through subsequent development, vacuum evaporation coating, and degumming steps, this method can form a uniform and precise metal texture on the free-form surface substrate, and finally ensures the texture quality through ultrasonic cleaning and optical imager measurement, thereby achieving high-quality free-form surface random metal texture production; this not only improves the performance and reliability of the product, but also enhances the stability and efficiency of the manufacturing process; 2. Through the coordinated operation of the laser system and the second motion system, the laser exposure process is precisely controlled, and the spraying of the degumming liquid is precisely controlled in the development and degumming steps, which can reduce the damage caused by the laser energy to the substrate. In particular, by using a DMD spatial light modulator and a beam shaping lens group to determine the prefabricated texture micro-unit and accurately project it onto the substrate, the efficient use of laser energy can be ensured and unnecessary high energy input can be avoided. In addition, selecting a suitable laser light source wavelength (such as the 375±10nm wavelength mentioned in step S16) can reduce the thermal effect of the laser on the substrate material, thereby reducing thermal stress and surface damage. Through these measures, the integrity of the substrate can be protected, its imaging quality and structural strength can be maintained, and the problem that the curved electromagnetic shielding substrate is transparent to laser, and the laser will be transmitted to the other side of the curved surface while removing the curved metal coating, and the transmitted laser will damage the grid on the other side and the high-energy laser etching will cause irreparable surface damage to the curved substrate and changes in the internal stress of the substrate, affecting the imaging quality of the curved surface and the strength of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the three-dimensional structure of the ultrasonic coating mechanism in one embodiment of the present application.
[0026] Description of Reference Numerals 1. Control box; 2. First motion system; 3. Contour heating base; 4. Support frame; 5. Ultrasonic nozzle; 6. Camera; 7. Telecentric lens; 8. Array light source; 9. Water drop-shaped free-form surface base. DETAILED DESCRIPTION
[0027] The present application is further described in detail below in conjunction with the accompanying drawings.
[0028] Embodiment 1: A method for producing random metal textures on free-form surfaces, the method comprising: S11, ultrasonic cleaning of the water drop-shaped free-form surface substrate 9, S12, forming a film of photoresist on the water drop-shaped free-form surface substrate 9 after ultrasonic cleaning; S13, baking the water drop-shaped free-form surface substrate 9 after the photoresist is coated on the film to solidify the glue; S14, determining the prefabricated texture pattern information, obtaining the visual image information of the water drop-shaped free-form surface substrate 9 after the glue is baked and solidified according to the prefabricated texture pattern information, analyzing the visual image information and the prefabricated texture pattern information, and determining the laser motion trajectory, wherein the laser motion trajectory is used to control the laser to perform an exposure operation on the water drop-shaped free-form surface substrate 9 after the glue is baked and solidified according to the prefabricated texture pattern information; S15, developing the exposed water drop-shaped free-form surface substrate 9; S16, performing vacuum evaporation coating on the developed water drop-shaped free-form surface substrate 9; S17, removing the glue from the water drop-shaped free-form surface substrate 9 after coating; S18, ultrasonically cleaning the water drop-shaped free-form surface substrate 9 after the glue is removed; S19, transferring the cleaned and debonded water drop-shaped free-form surface substrate 9 to a projection optical imager for texture measurement.
[0029] In this embodiment, in step S11 , the water drop-shaped free-form surface substrate 9 is ultrasonically cleaned.
[0030] In step S12, the visual manipulator holds an ultrasonic spray gun to coat the water drop-shaped free-form surface substrate 9 with photoresist film. The vision uses a 2000W camera 6 and a telecentric lens 7. The water drop-shaped free-form surface substrate 9 is fixed on a contoured base, and the base is covered with high-precision temperature-uniform controllable heating flexible cloth. Before the coating process, the temperature control heating function is turned on and the film coating is started after the temperature digital display is stable. This base can greatly reduce the problem of inconsistent photoresist thickness in various regions of the water drop-shaped free-form surface substrate 9 due to gravity and low viscosity of the photoresist water. The manipulator obtains the accurate coordinate system of the water drop-shaped free-form surface substrate 9 through vision and then moves according to a pre-programmed 3D trajectory to perform the coating operation. The operating parameters are as follows: robot movement speed 10mm / s, contour base temperature 30℃, spray gun normal distance from the droplet-shaped free-form surface 45mm, photoresist viscosity 1~2cps, ultrasonic frequency 5000kHz, liquid supply flow 1.8L / h, and use a tiny air flow of ≤0.15MPA to guide the photoresist evenly onto the substrate to be sprayed, and a micron thin film coating is formed after the solvent evaporates.
[0031] In step S13, the water drop-shaped free-form surface substrate 9 after the photoresist film is formed is transferred into a clean constant temperature oven for baking and solidifying.
[0032] In step S14, the laser direct writing lithography equipment adopts a combination of A-axis and C-axis dual-axis cradle-type turntable plus X-axis, Y-axis and Z-axis three linear axes. The laser direct writing head is fixed on the X-axis Z-axis cross module, and the A-axis and C-axis dual-axis cradle-type turntable is fixed on the Y-axis. At the same time, a 2000w pixel camera 6 plus a telecentric lens 7 is fixed on the Z-axis. After the accurate coordinate system of the water droplet-shaped free-form surface substrate 9 is obtained by vision, the five axes can move according to the pre-programmed spatial expansion surface trajectory. The laser light source adopts a wavelength of 375±10nm. The laser system projects a small light curtain of the prefabricated texture micro-unit to the water droplet-shaped free-form surface substrate 9 through a DMD spatial light modulator and a special beam shaping lens group. The prefabricated texture pattern is spread all over the surface of the water droplet-shaped free-form surface substrate 9 through the collaborative operation of the laser system and the motion system, and the exposure is completed.
[0033] In step S15, the exposed product is fixedly placed on a developing device with a contoured vacuum adsorption rotating shaft. The rotating shaft speed of the device is turned on and adjusted to 30rpm~40rpm, and the developer is sprayed onto the surface of the water drop-shaped free-form surface substrate 9 for development. The development time will vary due to different photoresist materials and micron film thickness differences. The development operation time can be customized on the device. After the development is completed, the spray is automatically turned off, and the rotating shaft speed jumps to 200rpm~300rpm for spin drying. The whole process is controlled by a microcomputer program, and different production formulas can be transferred to different products.
[0034] In step S16, the developed product is clamped on a specific tooling fixture for self-rotation to produce an electromagnetic shielding metal layer. The vacuum evaporation coating method is adopted, and the surface is bombarded and cleaned with an RF ion source for 10 minutes, and 15nm chromium film, 100nm copper film, 15nm chromium film, 100nm copper film, and 15nm chromium film are evaporated in sequence. The process parameters are vacuum degree of vacuum chamber 3.0×103Pa, vacuum chamber temperature 200°C, industrial rotation 20r / min, vacuum insulation time 30min, normal temperature stress release after plating, and placement time 1H.
[0035] In step S17, the prepared electromagnetic shielding water drop-shaped free-form surface is placed on a degumming device with a contoured vacuum adsorption rotating shaft. The rotating shaft speed of the equipment is turned on and adjusted to 30rpm~40rpm, and the degumming liquid is sprayed on the surface of the water drop-shaped free-form surface substrate 9 to degumming. The degumming time will vary due to different photoresist materials and differences in the thickness of the micron film layer. The degumming operation time can be customized on the device. After the degumming is completed, the spraying rotation shaft speed is automatically turned off and jumped to 200rpm~300rpm for spin drying. The whole process is controlled by a microcomputer program, and different production formulas can be adjusted for different products.
[0036] In step S18, the debonded product is placed in an ultrasonic cleaning tank to clean the remaining debonding liquid. At this point, the processing of the drop-shaped free-form optical cover with electromagnetic shielding function and extremely low diffraction is completed.
[0037] In step S19, the texture is measured under a projection optical imager. The line width of the texture is 5um, and the texture has no defects such as deformation, broken lines, and missing corners in overall appearance.
[0038] In summary, by determining the prefabricated texture pattern information and combining it with the visual image information of the water drop-shaped free-form surface substrate 9 after baking and solidifying the glue, the two are analyzed to determine the movement trajectory of the laser. This step utilizes a high-precision visual system and a pre-programmed spatial expansion surface trajectory to ensure that the laser is accurately exposed according to the prefabricated texture pattern information, thereby reducing the problem of deviation caused by insufficient repeatability. This method achieves accurate exposure of the free-form surface substrate by precisely controlling the movement trajectory of the laser, avoids the deviation that occurs during multiple scanning and etching processes, and improves the manufacturing accuracy and repeatability. In addition, through subsequent development, vacuum evaporation coating and degumming steps, this method can form a uniform and precise metal texture on the free-form surface substrate, and finally ensure the texture quality through ultrasonic cleaning and optical imager measurement, thereby achieving high-quality free-form surface random metal texture production; this not only improves the performance and reliability of the product, but also enhances the stability and efficiency of the manufacturing process.
[0039] Further, in step S12, a photoresist film is coated on the water drop-shaped free-form surface substrate 9 after ultrasonic cleaning by an ultrasonic coating mechanism, wherein the ultrasonic coating mechanism comprises a control box 1, a first motion system 2, a contour heating base 3 and a support frame 4 located on the control box 1, an ultrasonic nozzle 5 is provided on the first motion system 2, and a visual system corresponding to the contour heating base 3 and a planar array light source 8 corresponding to the contour heating base 3 are provided on the support frame 4, wherein the visual system comprises a camera 6 and a telecentric lens 7 located on the camera 6; Step 12 also includes the following steps: Based on the visual system, a motion coordinate system of the water drop-shaped free-form surface base 9 is obtained; Determine a preset three-dimensional trajectory; According to the preset three-dimensional trajectory and the motion coordinate system, the first motion system 2 is controlled to perform a coating operation on the water drop-shaped free-form surface substrate 9 located in the contoured heating base 3 .
[0040] To sum up, the technical effect of using the ultrasonic coating mechanism in step S12 is that, through the assistance of a precise visual system and the control of the first motion system 2, uniform film coating of the photoresist on the teardrop-shaped free-form surface substrate 9 is achieved, thereby ensuring the quality and accuracy of the subsequent photolithography process. At the same time, the application of the contoured heating base 3 effectively avoids the problem of inconsistent coating thickness caused by the substrate shape or gravity.
[0041] Furthermore, the contoured heating base 3 is provided with a controllable heating flexible cloth, and before executing step S12, the following steps are also included: Determining whether the temperature parameter of the controllable heating flexible cloth reaches a preset threshold; If yes, then push a first window for prompting to start the ultrasonic coating mechanism to perform photoresist film coating; If not, a second window is pushed to prompt that the conditions for starting the ultrasonic coating mechanism to perform photoresist film coating are not met, and an audible and visual alarm is issued.
[0042] In summary, this technology ensures that the substrate is coated with photoresist under optimal temperature conditions by integrating a controllable heating flexible cloth on the contoured heating base 3 and performing preset threshold detection of temperature parameters before coating the photoresist, thereby improving the film quality and process reliability, while enhancing the controllability and safety of the process through intuitive window prompts and sound and light alarm mechanisms.
[0043] Furthermore, the preset threshold is 30±2°C.
[0044] In summary, by setting the preset threshold at 30±2°C, this technology ensures the temperature control accuracy of the substrate before photoresist coating, thereby optimizing the film formation effect of the photoresist, improving the uniformity and adhesion of the coating, and reducing process defects caused by temperature fluctuations.
[0045] Further, in step S14, the texture pattern corresponding to the prefabricated texture pattern information is spread all over the surface of the water drop-shaped free-form surface substrate 9 by the laser system and the second motion system to complete the exposure operation; The laser system determines the prefabricated texture micro-units through the DMD spatial light modulator and the beam shaping lens group, and projects the prefabricated texture micro-units into a small light curtain onto the water drop-shaped free-form surface substrate 9.
[0046] In this embodiment, this description is an explanation of a high-precision laser direct writing lithography device and its working process. This device is composed of multiple precision mechanical axes and advanced optical systems, and can achieve precise processing of complex curved surfaces. The specific analysis is as follows: 1) Five-axis linkage system: The equipment has A-axis and C-axis (two-axis cradle turntable), as well as X-axis, Y-axis and Z-axis (three linear axes), which can realize complex spatial motion trajectories.
[0047] 2) Laser direct writing head: fixed on the cross module of X-axis and Z-axis, responsible for emitting laser.
[0048] 3) Vision system: A 20-megapixel camera 6 and a telecentric lens 7 are mounted on the Z-axis to capture and identify the exact position and shape of the substrate.
[0049] 4) Spatial light modulator (DMD): used to control the shape and direction of the laser beam to meet different processing requirements.
[0050] 5) Beam shaping lens group: further adjusts the laser beam to ensure that it is accurately projected onto the substrate.
[0051] 6) Prefabricated texture micro-units: The designed texture pattern is projected onto the substrate through a laser system.
[0052] 7) Exposure process: The laser system and the motion system work together to completely transfer the prefabricated texture pattern to the entire water drop-shaped free-form surface substrate 9.
[0053] It's like engraving a detailed map on a spherical glass. This device is like an advanced paintbrush that can accurately draw every detail on the spherical surface. First, the "eyes" (visual system) on the device will carefully observe the spherical glass to determine its shape and position. Then, the "arm" (five-axis linkage system) on the device will move accurately to the correct position based on this information. At the same time, the "brush" (laser direct writing head) will adjust the laser beam through a series of lenses and reflectors (beam shaping lens group and DMD) to adapt to the curvature of the sphere, and then draw every detail of the map on the sphere. The whole process is like precise painting in a three-dimensional space, and finally a complete map pattern is formed on the glass ball.
[0054] Preferably, during the manufacturing process, there is a close relationship between the "prefabricated texture micro-units" and the "prefabricated texture patterns", which together define the surface characteristics of the final product. The following is the relationship and function between them: 1) Texture micro-unit: This usually refers to the basic graphic elements or units that make up the texture pattern. Each micro-unit contains a specific line, shape or structure, which is the basis for more complex patterns.
[0055] 2) Texture pattern: This refers to a complete pattern composed of multiple texture micro-units arranged and combined according to certain rules. The texture pattern defines the final appearance and characteristics of the product surface.
[0056] 3) Relevance: Texture micro-units are the "building blocks" for constructing texture patterns. Their size, shape and arrangement determine the final effect of the texture pattern. The texture pattern is achieved by replicating and arranging these micro-units, involving different arrangements and combinations such as repetition, rotation, and mirroring. The design and selection of micro-units will affect the functionality of the texture pattern, such as electromagnetic shielding effect, optical properties or mechanical properties.
[0057] 4) Manufacturing process: During the manufacturing process, the geometry and size of the texture micro-units are first designed and determined. Then, these micro-units are combined into texture patterns in a specific arrangement according to the desired application and performance requirements. Finally, these prefabricated texture patterns are transferred to the product substrate using technologies such as laser direct writing lithography.
[0058] For example, if you want to make a complex pattern composed of many small dots on a piece of glass, each small dot is a texture micro-unit, and the entire pattern is a texture pattern composed of these small dots arranged and combined according to certain rules.
[0059] Among them, DMD (digital micromirror device) spatial light modulator and beam shaping lens group are usually used in laser direct writing lithography system to control and adjust the characteristics of laser beam to achieve precise pattern transfer. Their role is directly related to determining the prefabricated texture micro-units, but their main functions are to achieve the following aspects: 1) Beam modulation: The DMD spatial light modulator modulates the incident laser beam by controlling the micromirror array, which can turn on or off specific micromirrors to control the path of the beam. This can be used to selectively form or block the beam to form the desired micro-unit pattern.
[0060] 2) Pattern generation: DMD can quickly switch the state of the micromirrors to generate complex patterns on the path of the light beam. These patterns can be texture patterns composed of multiple microunits.
[0061] 3) Beam shaping: The beam shaping lens set is used to adjust the shape and size of the laser beam, ensuring that the beam is projected onto the substrate in the desired shape and size. This helps to accurately transfer the micro-unit pattern onto the substrate.
[0062] 4) Precision alignment: In complex manufacturing processes, these devices can also help to precisely align patterns, ensuring that they are placed exactly at specific locations on the substrate as designed.
[0063] 5) Dynamic adjustment: DMD and beam shaping lens group can be dynamically adjusted to adapt to different pattern design and manufacturing requirements, providing high flexibility.
[0064] Therefore, it can be said that the DMD spatial light modulator and the beam shaping lens group are used to achieve the precise transfer and positioning of the prefabricated texture micro-units. They are key components to ensure the pattern accuracy and quality during laser direct writing lithography. Through these devices, the designed texture micro-units can be accurately projected and transferred to the substrate according to the prefabricated texture pattern to achieve the desired surface features.
[0065] In summary, the technology used in step S14 achieves high-resolution and high-precision texture pattern exposure by precisely controlling the collaborative operation of the laser system and the second motion system, combined with the DMD spatial light modulator and the beam shaping lens group, ensuring that the prefabricated texture micro-units can be evenly and accurately projected and covered on the entire surface of the droplet-shaped free-form surface substrate 9, thereby giving it a predetermined functional texture pattern while maintaining the original characteristics of the surface.
[0066] Furthermore, the wavelength of the laser light source in the laser system is 375±10 nm.
[0067] In summary, by selecting a laser light source with a wavelength of 375±10nm, this technology achieves precise absorption and processing of specific materials, while minimizing the heat-affected zone, effectively avoiding unnecessary damage to the droplet-shaped free-form surface substrate 9, and ensuring the fineness of micro-nanostructure processing and the integrity of the substrate material.
[0068] Further, in step S15, the debonding liquid is sprayed onto the surface of the water drop-shaped free-form surface substrate 9 for development, wherein the thickness of the micron thin film coating formed after the solvent in the photoresist evaporates will also be different in different time periods of the development process, and the development operation time is defined by determining different photoresist materials and the thickness difference of the micron thin film coating; In step 17, the debonding liquid is sprayed onto the surface of the water droplet-shaped free-form surface substrate 9 for debonding. The thickness of the micron thin film coating formed after the solvent in the photoresist evaporates will also be different in different time periods of the debonding process. The debonding operation time is defined by determining different photoresist materials and the thickness difference of the micron thin film coating.
[0069] In summary, by precisely controlling the spraying of the photoresist solution during the development and stripping process, combined with real-time monitoring of different photoresist materials and micron film coating thickness, this technology achieves precise definition of the development and stripping operation time, ensuring uniform removal of the photoresist coating and accurate transfer of micron-level patterns, thereby optimizing the accuracy and repeatability of the entire lithography process.
[0070] Furthermore, in step S16, the following steps are included: The developed water drop-shaped free-form surface substrate 9 is clamped in a self-rotating fixture; The surface of the water drop-shaped free-form surface substrate 9 clamped in the self-rotating fixture is bombarded and cleaned by using an RF ion source according to a preset operation time; A layer of chromium film, a layer of copper film, another layer of chromium film, another layer of copper film and a final layer of chromium film are sequentially deposited on the surface of the water drop-shaped free-form surface substrate 9 .
[0071] In summary, the technology used in step S16 achieves the deposition of a uniform and high-quality electromagnetic shielding layer by fixing the developed drop-shaped free-form surface substrate 9 in a rotating fixture, performing surface bombardment cleaning using an RF ion source, and then precisely evaporating multiple layers of alternating chromium and copper films, while ensuring the precise alignment and cleanliness of the substrate, thereby improving the performance and reliability of the final product.
[0072] In summary, this manufacturing method is used to make a teardrop-shaped free-form optical cover with electromagnetic shielding function and extremely low diffraction characteristics. Through these technical means, the manufacturing process can: reduce laser damage to the back of the substrate because precise laser control and beam shaping technology are used. Through the precise operation of the visual system and the manipulator, the deviation problem caused by multiple scanning etching is reduced. Through the steps of baking, developing and drying, the damage caused by high-energy laser etching to the substrate is reduced. Through vacuum evaporation coating and ion source cleaning, the quality and uniformity of the electromagnetic shielding layer are improved, and the impact on the substrate is reduced.
[0073] Embodiment 2: A method for producing a random metal texture on a free-form surface, the method comprising: S21, ultrasonic cleaning of the water drop-shaped free-form surface substrate 9, S22, performing vacuum evaporation coating on the water drop-shaped free-form surface substrate 9 after ultrasonic cleaning; S23, forming a film of photoresist on the water drop-shaped free-form surface substrate 9 after coating; S24, baking the water drop-shaped free-form surface substrate 9 after the film coating of the photoresist to solidify the glue; S25, determining the prefabricated texture pattern information, obtaining the visual image information of the water drop-shaped free-form surface substrate 9 after the glue is baked and solidified according to the prefabricated texture pattern information, analyzing the visual image information and the prefabricated texture pattern information, and determining the laser motion trajectory, wherein the laser motion trajectory is used to control the laser to perform an exposure operation on the water drop-shaped free-form surface substrate 9 after the glue is baked and solidified according to the prefabricated texture pattern information; S26, etching the developed water drop-shaped free-form surface substrate 9; S27, removing the glue from the etched water drop-shaped free-form surface substrate 9 S28, ultrasonically cleaning the water drop-shaped free-form surface substrate 9 after the glue is removed; S29, transferring the cleaned and debonded water drop-shaped free-form surface substrate 9 to a projection optical imager for texture measurement.
[0074] In this embodiment, the water drop-shaped free-form surface substrate 9 is ultrasonically cleaned in step S21.
[0075] In step S22, the cleaned product is clamped on a specific tooling fixture for self-rotation to produce an electromagnetic shielding metal layer. The vacuum evaporation coating method is adopted, and the surface is bombarded and cleaned with an RF ion source for 10 minutes, and 15nm chromium film, 100nm copper film, 15nm chromium film, 100nm copper film, and 15nm chromium film are evaporated in sequence. The process parameters are vacuum degree of vacuum chamber 3.0×103Pa, vacuum chamber temperature 200°C, working speed 20r / min, vacuum insulation time 30min, normal temperature stress release after plating, and placement time 1H. In step S23, the visual manipulator holds an ultrasonic spray gun to perform photoresist film coating on the water drop-shaped free-form surface workpiece that has been plated with an electromagnetic shielding metal layer. The vision adopts a 2000W camera 6 and a telecentric lens 7. The water drop-shaped free-form surface substrate 9 is fixed on a contour base, and the base is covered with high-precision temperature-uniform controllable heating flexible cloth. Before the coating process, the temperature control heating function is turned on and the film coating is started after the temperature digital display is stable. This base can greatly reduce the problem of inconsistent photoresist thickness in various regions of the water drop-shaped free-form surface substrate 9 due to gravity and low viscosity of photoresist water. The manipulator obtains the accurate coordinate system of the water drop-shaped free-form surface substrate 9 through vision and then moves according to a pre-programmed 3D trajectory to perform the coating operation. The operating parameters are as follows: robot movement speed 10mm / s, contour base temperature 30℃, spray gun normal distance from the droplet-shaped free-form surface 45mm, photoresist viscosity 1~2cps, ultrasonic frequency 5000kHz, liquid supply flow 1.8L / h, and use a tiny air flow of ≤0.15MPA to guide the photoresist evenly onto the substrate to be sprayed, and a micron thin film coating is formed after the solvent evaporates.
[0076] In step S24, the water drop-shaped free-form surface substrate 9 after the photoresist film is formed is transferred into a clean constant temperature oven for baking and curing.
[0077] In step S25, the laser direct writing lithography equipment adopts a combination of A-axis and C-axis dual-axis cradle-type turntable plus X-axis, Y-axis and Z-axis three linear axes. The laser direct writing head is fixed on the X-axis Z-axis cross module, and the A-axis and C-axis dual-axis cradle-type turntable is fixed on the Y-axis. At the same time, a 2000w pixel camera 6 plus a telecentric lens 7 is fixed on the Z-axis. After the accurate coordinate system of the water droplet-shaped free-form surface substrate 9 is obtained by vision, the five axes can move according to the pre-programmed spatial expansion surface trajectory. The laser light source adopts a wavelength of 375±10nm. The laser system projects a small light curtain of the prefabricated texture micro-unit to the water droplet-shaped free-form surface substrate 9 through a DMD spatial light modulator and a special beam shaping lens group. The prefabricated texture pattern is spread all over the surface of the water droplet-shaped free-form surface metal layer through the collaborative operation of the laser system and the motion system, and the exposure is completed.
[0078] In step S26, the exposed product is fixedly placed on a developing device with a contoured vacuum adsorption rotating shaft. The rotating shaft speed of the device is turned on and adjusted to 30rpm~40rpm, and the developer is sprayed synchronously to the surface of the droplet-shaped free-form metal layer for development. The development time will vary due to different photoresist materials and micron film thickness differences. The development operation time can be customized on the device. After the development is completed, the spray is automatically turned off, and the rotating shaft speed jumps to 200rpm~300rpm for spin drying. The whole process is controlled by a microcomputer program, and different production formulas can be transferred to different products.
[0079] In step S27, the developed product is fixedly placed on an etching device with a contoured vacuum adsorption rotating shaft. The rotating shaft speed of the device is turned on and adjusted to 30rpm~40rpm, and the special etching liquid is sprayed on the surface of the water drop-shaped free-form surface substrate 9 for etching. The special etching liquid can etch chromium and copper metals simultaneously. After etching is completed, the spray is automatically turned off, and the rotating shaft speed jumps to 200rpm~300rpm for drying. The whole process is controlled by a microcomputer program, and different production formulas can be adjusted for different products.
[0080] In step S28, the etched electromagnetic shielding water drop-shaped free-form surface is placed on a degumming device with a contoured vacuum adsorption rotating shaft. The rotating shaft speed of the equipment is turned on and adjusted to 30rpm~40rpm, and the degumming liquid is sprayed on the surface of the water drop-shaped free-form surface for degumming. The degumming time is about 2~4 minutes. After the degumming is completed, the spraying is automatically turned off and the rotating shaft speed jumps to 200rpm~300rpm for spin drying. The whole process is controlled by a microcomputer program, and different production formulas can be adjusted for different products.
[0081] In step S29, the debonded product is placed in an ultrasonic cleaning tank to clean the remaining debonding liquid. At this point, the processing of the drop-shaped free-form optical cover with electromagnetic shielding function and extremely low diffraction is completed.
[0082] In step S210, the texture is measured under a projection optical imager. The line width of the texture is 5um, and the texture has no defects such as deformation, broken lines, and missing corners in overall appearance.
[0083] To sum up, the technical effect of the method for producing random metal textures on free-form surfaces is that, through a series of finely controlled steps such as ultrasonic cleaning, vacuum evaporation coating, photoresist coating and baking, precise laser exposure, development and etching, debonding and ultrasonic cleaning, a uniform and precise random metal texture with predetermined electromagnetic shielding properties is produced on a droplet-shaped free-form surface substrate 9, while ensuring the integrity and optical properties of the substrate, and finally the texture is measured by an optical imager to verify the product quality.
[0084] Preferably, the difference between the two embodiments is that the second method has higher requirements for the uniformity and integrity of the plated layer during the photoresist curing and exposure process because the film is plated first, so as to avoid affecting the accuracy of the final pattern. If the coating material has specific requirements for the adhesion of the photoresist or the baking process, this will affect the choice of the manufacturing process. The first method is suitable for the case where the substrate needs to undergo certain surface treatments first or needs to form a specific pattern before coating. The second method is suitable for the case where a pattern needs to be formed on a specific material and then subjected to subsequent processing.
[0085] Furthermore, step S26 includes: Spraying etching liquid onto the developed water drop-shaped free-form surface substrate 9, wherein the etching liquid is used for simultaneously etching chromium and copper; The water drop-shaped free-form surface base 9 after etching is dried.
[0086] In summary, the technical effect of step S26 is that the chromium and copper layers on the developed droplet-shaped free-form surface substrate 9 are simultaneously removed by spraying etching liquid, thereby achieving accurate metal layer pattern transfer, and the subsequent drying treatment ensures the cleanliness of the substrate and the smooth progress of subsequent processes, thereby giving the substrate the required functional texture while maintaining the surface characteristics.
[0087] In summary, this manufacturing method is used to make a teardrop-shaped free-form optical cover with electromagnetic shielding function and extremely low diffraction characteristics. Through these technical means, the manufacturing process can: reduce laser damage to the back of the substrate because precise laser control and beam shaping technology are used. Through the precise operation of the visual system and the manipulator, the deviation problem caused by multiple scanning etching is reduced. Through the steps of baking, developing, etching and degumming, the damage caused by high-energy laser etching to the substrate is reduced. Through vacuum evaporation coating and ion source cleaning, the quality and uniformity of the electromagnetic shielding layer are improved, and the impact on the substrate is reduced.
[0088] Preferably, in these two embodiments, the feature of "water drop shape" refers to the shape of the substrate, which is a specific technical feature, but is not necessarily required for manufacturing a free-form optical cover with electromagnetic shielding function and extremely low diffraction. The water drop shape design is based on the following considerations: Optical properties: The drop shape contributes to specific optical properties, such as reducing reflection or scattering of light and improving optical imaging quality.
[0089] Electromagnetic shielding effect: The specific shape helps to optimize the electromagnetic shielding effect, and the performance of the shielding layer can be enhanced or adjusted through shape design.
[0090] Structural Strength: The teardrop shape provides better structural strength, making it more suitable for withstanding mechanical stress or environmental factors.
[0091] Aesthetic or design requirements: In some applications, the teardrop shape is a design choice to meet specific aesthetic or brand identity needs.
[0092] Adaptability of manufacturing process: The teardrop-shaped surface requires specific manufacturing processes to achieve, such as photoresist coating and laser direct writing lithography mentioned in the article. These processes are particularly suitable for processing curved surface shapes.
[0093] However, whether the "water drop shape" is a necessary technical feature depends on the specific application and performance requirements of the final product. In some cases, other shapes of substrates also meet the technical requirements as long as they can achieve the required functions and performance. Therefore, the "water drop shape" can be regarded as a design choice rather than an absolutely necessary technical feature.
[0094] For reference, the existing technical production process is: Step 1: Clean the curved surface; Step 2: Use vacuum coating technology to coat metal titanium film and copper film; Step 3: Use 515nm femtosecond laser to remove through multiple laser processing; Step 4: Ultrasonic cleaning; Step 5: Use an imager to perform appearance inspection; Disadvantages and shortcomings of existing invention technology: The curved electromagnetic shielding substrate is all laser transparent. When removing the metal coating on the curved surface, the laser will be transmitted to the other side of the curved surface, and the transmitted laser will destroy the grid on the other side.
[0095] The repeated accuracy of the laser direct writing equipment is particularly strict when the curved surface is scanned and etched at least twice. There is a high probability of deviation in multiple scans and etchings.
[0096] High-energy laser etching can cause irreparable surface damage to the curved substrate and change the internal stress of the substrate, affecting the imaging quality of the curved surface and the strength of the substrate.
[0097] The present application can produce a uniform photoresist film on a teardrop-shaped free-form surface. This technology can produce non-standard grids on complex teardrop-shaped free-form surfaces. The designed texture pattern can be formed with one exposure. There is no displacement deviation caused by repeated positioning. The teardrop-shaped free-form surface substrate is not damaged during the production process, and the original strength and optical properties of the substrate can be guaranteed. The texture of the teardrop-shaped free-form surface in the straight direction will not be damaged due to laser transmission, and a complete irregular grid can be produced. The technology of using a laser to project a small light curtain is many times more efficient than the existing technology.
[0098] More importantly, it avoids damage caused by laser transmission: the new process avoids damage to the other side of the free-form surface by the laser during the production process. Forming a texture pattern with one exposure: compared with the existing technology, the new method can complete the designed texture pattern with one exposure, eliminating the displacement deviation caused by repeated positioning. Damage-free substrate processing: the teardrop-shaped free-form surface substrate is not damaged during the production process, and the original strength and optical properties of the substrate are maintained. Production of complete irregular grids: the new technology can produce complete irregular grids that are not damaged by laser transmission. Improved production efficiency: the use of laser projection small light curtain technology significantly improves production efficiency compared to existing technologies. Combination of optical performance and electromagnetic shielding: the free-form random metal grid can achieve excellent optical performance while maintaining electromagnetic shielding performance, without optical diffraction problems.
[0099] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.
Claims
1. A method for producing random metal textures on free-form surfaces, characterized in that: The method for producing a random metal texture on a free-form surface comprises: S11, ultrasonic cleaning of water drop-shaped free-form surface substrate, S12, forming a film of photoresist on the water drop-shaped free-form surface substrate after ultrasonic cleaning; S13, baking the water drop-shaped free-form surface substrate after the film coating of the photoresist to solidify the glue; S14, determining prefabricated texture pattern information, obtaining visual image information of the water drop-shaped free-form surface substrate after baking and solidifying the glue according to the prefabricated texture pattern information, analyzing the visual image information and the prefabricated texture pattern information, and determining a laser motion trajectory, wherein the laser motion trajectory is used to control the laser to perform an exposure operation on the water drop-shaped free-form surface substrate after baking and solidifying the glue according to the prefabricated texture pattern information; S15, developing the exposed water drop-shaped free-form surface substrate; S16, performing vacuum evaporation coating on the developed water drop-shaped free-form surface substrate; S17, removing the glue from the water drop-shaped free-form surface substrate after coating; S18, ultrasonic cleaning of the water drop-shaped free-form surface substrate after debonding; S19, transferring the cleaned and debonded water drop-shaped free-form surface substrate to a projection optical imager for texture measurement.
2. The method for producing a free-form surface random metal texture according to claim 1, characterized in that: In step S12, a photoresist film is coated on the water droplet-shaped free-form surface substrate after ultrasonic cleaning by an ultrasonic coating mechanism, wherein the ultrasonic coating mechanism comprises a control box (1), a first motion system (2) located on the control box (1), a contoured heating base (3) and a support frame (4), the first motion system (2) being provided with an ultrasonic nozzle (5), and the support frame (4) being provided with a visual system; Step 12 also includes the following steps: Based on the visual system, the motion coordinate system of the water drop-shaped free-form surface base is obtained; Determine a preset three-dimensional trajectory; According to the preset three-dimensional trajectory and the motion coordinate system, the first motion system (2) is controlled to perform a coating operation on the water droplet-shaped free-form surface substrate located in the contoured heating base (3).
3. The method for producing a free-form surface random metal texture according to claim 2, characterized in that: The contoured heating base (3) is provided with a controllable heating flexible cloth, and before executing step S12, the following steps are also included: Determining whether the temperature parameter of the controllable heating flexible cloth reaches a preset threshold; If yes, then push a first window for prompting to start the ultrasonic coating mechanism to perform photoresist film coating; If not, a second window is pushed to prompt that the conditions for starting the ultrasonic coating mechanism to perform photoresist film coating are not met, and an audible and visual alarm is issued.
4. The method for producing a free-form surface random metal texture according to claim 3, characterized in that: The preset threshold is 30±2°C.
5. The method for producing a free-form surface random metal texture according to claim 1, characterized in that: In step S14, the texture pattern corresponding to the prefabricated texture pattern information is spread all over the surface of the water drop-shaped free-form surface substrate through the laser system and the second motion system to complete the exposure operation; The laser system determines the prefabricated texture micro-units through a DMD spatial light modulator and a beam shaping lens group, and projects a small light curtain of the prefabricated texture micro-units onto a water drop-shaped free-form surface substrate.
6. The method for producing a free-form surface random metal texture according to claim 1, characterized in that: The wavelength of the laser light source in the laser system is 375±10 nm.
7. The method for producing a free-form surface random metal texture according to claim 1, characterized in that: In step S15, the debonding liquid is sprayed onto the surface of the water droplet-shaped free-form surface substrate for development, wherein the thickness of the micron thin film coating formed after the solvent in the photoresist evaporates will also be different in different time periods of the development process. The development operation time is defined by determining different photoresist materials and the thickness difference of the micron thin film coating; In step 17, the debonding liquid is sprayed onto the surface of the water droplet-shaped free-form surface substrate for debonding. The thickness of the micron thin film coating formed after the solvent in the photoresist evaporates will also be different in different time periods of the debonding process. The debonding operation time is defined by determining different photoresist materials and the thickness difference of the micron thin film coating.
8. The method for producing a free-form surface random metal texture according to claim 1, characterized in that: In step S16, the following steps are included: Clamping the developed water drop-shaped free-form surface substrate in a self-rotating fixture; The RF ion source is used to bombard and clean the water drop-shaped free-form surface substrate clamped in the rotating fixture according to the preset operation time; A layer of chromium film, a layer of copper film, another layer of chromium film, another layer of copper film and a final layer of chromium film are sequentially deposited on the surface of the water drop-shaped free-form surface substrate.
9. A method for producing a random metal texture on a free-form surface, characterized in that: The production method comprises: S21, ultrasonic cleaning of water drop-shaped free-form surface substrate, S22, performing vacuum evaporation coating on the water drop-shaped free-form surface substrate after ultrasonic cleaning; S23, forming a film and coating a photoresist on the water drop-shaped free-form surface substrate after coating; S24, baking the drop-shaped free-form surface substrate after the film coating of the photoresist to solidify the glue; S25, determining prefabricated texture pattern information, obtaining visual image information of the water drop-shaped free-form surface substrate after baking and solidifying the glue according to the prefabricated texture pattern information, analyzing the visual image information and the prefabricated texture pattern information, and determining a laser motion trajectory, wherein the laser motion trajectory is used to control the laser to perform an exposure operation on the water drop-shaped free-form surface substrate after baking and solidifying the glue according to the prefabricated texture pattern information; S26, developing the exposed water drop-shaped free-form surface substrate; S27, etching the developed water drop-shaped free-form surface substrate; S28, debonding the etched water drop-shaped free-form surface substrate S29, ultrasonic cleaning of the water drop-shaped free-form surface substrate after debonding; S210, transferring the cleaned and debonded water drop-shaped free-form surface substrate to a projection optical imager for texture measurement.
10. The method for producing a free-form surface random metal texture according to claim 9, characterized in that: Step S26 includes: Spraying an etching liquid onto the developed water drop-shaped free-form surface substrate, wherein the etching liquid is used for simultaneously etching chromium and copper; The drop-shaped free-form surface substrate after etching is dried.
Citation Information
Patent Citations
Method for projection-type laser etching on free curved surface
CN101786200A
Manufacturing method of free-form surface optical micro lens array
CN102902156A
Curved surface film circuit manufacture method based on laser projection technology
CN105448799A
Novel semi-additive 3D fine circuit manufacturing process
CN108513445A
Layered control method for laser marking textures
CN114578761A
Cited By
Film coating equipment and flexible film coating method for surface patterning of complex curved surface part