Lignosulfonate-chitosan gel electrolyte membrane as well as preparation method and application thereof
By preparing the lignin sulfonate-chitosan gel electrolyte membrane, the problems of triple-iodine ion shuttle and zinc negative electrode side reaction in zinc-iodine batteries are solved, and efficient battery circulation performance and environmentally friendly production process are achieved, which is improved. lifespan and coulomb efficiency.
Patent Information
- Application Number
- CN202411198903.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-22
AI Technical Summary
The lifespan of zinc-iodine batteries is limited by uncontrolled shuttle bushing of triiodine ions and zinc negative electrode side reactions, and the production of existing Nafion films is poor stability, high cost and environmental pollution.
Using the preparation method of lignin sulfonate-chitosan gel electrolyte membrane, the lignin sulfonate is dissolved in deionized water and chitosan powder in acetic acid solution to form a transparent solution, and then cast in a mold And soaked in zinc salt solution to prepare a gel electrolyte membrane with high salt resistance and biodegradability.
The gel electrolyte membrane can effectively prevent I3-stop shuttle, inhibit self-discharge and corrosion of zinc negative electrodes, improve the circulation performance of zinc-iodine batteries and the Coulomb efficiency of the battery. At the same time, since the material is extracted from natural biological, it has environmental and economic advantages.
Smart Images

Figure CN119009163A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a lignin sulfonate-chitosan gel electrolyte membrane and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background section is intended to enhance understanding of the overall background of the invention and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Zinc-iodine batteries are considered to be a leading candidate for large-scale energy storage systems due to their large-capacity dissolution-deposition reactions at both electrodes. However, the lifetime of zinc-iodine batteries is limited by the presence of triiodide ions (I 3− ) is severely limited by uncontrolled shuttling and unfavorable side reactions at the Zn anode. During discharge, the primary discharge product I − Anions can quickly coordinate with residual I2 to form soluble I 3− Anions. Dissolved I 3− The migration of ions not only causes I2 loss at the positive electrode, but also causes zinc poisoning at the negative electrode, leading to severe self-discharge, rapid capacity decay, and low Coulombic efficiency. 3− The Nafion membrane has good anion blocking ability and constructs many negatively charged diffusion paths for the specific migration of cations.
[0004] Taking advantage of the Nafion membrane, Li et al. constructed a high energy density zinc-iodine battery in 7.5 M KI + 3.75 M ZnBr2 electrolyte. However, from the perspective of sustainability, the production of membranes using petrochemical products, especially polyfluorinated chemicals, has problems such as poor stability, high cost, and easy environmental pollution. Summary of the invention
[0005] In view of the shortcomings of the prior art, the first object of the present invention is to provide a method for preparing a lignin sulfonate-chitosan gel electrolyte membrane.
[0006] The second object of the present invention is to provide a lignin sulfonate-chitosan gel electrolyte membrane prepared by the above method.
[0007] The third object of the present invention is to provide the application of the above lignin sulfonate-chitosan gel electrolyte membrane.
[0008] To achieve the above object, the present invention adopts the following technical solution: A method for preparing a lignin sulfonate-chitosan gel electrolyte membrane, the preparation method comprising the following steps: (1) dissolving lignin sulfonate in deionized water to obtain a lignin sulfonate aqueous solution with a mass concentration of 0.1-5.0%; (2) Disperse 1-20 g chitosan powder in 1-4% (v / v) acetic acid solution, stir, and fully dissolve to form a transparent solution; (3) mixing the lignin sulfonate aqueous solution obtained in step (1) and the transparent solution obtained in step (2) in a mass ratio of (1-3): (7-9), stirring to obtain a transparent solution; (4) casting the solution obtained in step (3) into a polytetrafluoroethylene mold and leaving it at room temperature to obtain a composite membrane; (5) Soaking the composite membrane obtained in step (4) in a 0.1-10 mol / L zinc salt solution to obtain a gel electrolyte membrane.
[0009] Furthermore, in step (1), the lignin sulfonate is at least one of sodium lignin sulfonate, calcium lignin sulfonate, magnesium lignin sulfonate and ammonium lignin sulfonate.
[0010] Furthermore, in step (1), the stirring temperature is 25-80° C. and the stirring time is 1-4 h.
[0011] Furthermore, in step (2), the viscosity of the chitosan powder is 100-400 mPa·s.
[0012] Furthermore, in step (3), the stirring time is 1-24 h.
[0013] Furthermore, in step (4), the time of standing at room temperature is 3 days.
[0014] Furthermore, in step (5), the zinc salt is at least one of ZnCl2, ZnSO4·7H2O, Zn(CH3COO)2·2H2O, Zn(NO3)2·6H2O, Zn(BF4)2·6H2O and Zn(CF3SO3)2.
[0015] Furthermore, in step (5), the soaking time is 12-48 h.
[0016] A lignin sulfonate-chitosan gel electrolyte membrane prepared by the above method.
[0017] The application of the above lignin sulfonate-chitosan gel electrolyte membrane can be used in the field of zinc-iodine batteries.
[0018] Beneficial effects: (1) The large number of polar oxygen-containing groups such as hydroxyl, phenolic hydroxyl, and sulfonic acid groups on the lignin sulfonate chain and chitosan chain not only have high salt tolerance and water retention capacity, but also provide Zn2+ The induced gelation provides abundant bridging sites; (2) due to the high electrolyte absorption and rich hydroxyl, sulfonic acid, amino and other groups, this gel electrolyte membrane can easily transport Zn 2+ cations, ensuring uniform Zn 2+ flux, and effectively blocks I 3− (3) The design of the gel electrolyte membrane can reduce the corrosion of the zinc negative electrode by limiting most of the free water away from the electrolyte / negative electrode interface; (4) Since lignin sulfonate and chitosan are green chemical products extracted from natural organisms, they have the advantages of being cheap, easily available and biodegradable. Therefore, the gel electrolyte membrane obtained by the present invention has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention, and the exemplary embodiments of the present invention and their descriptions are used to explain the present invention, and do not constitute an improper limitation of the present invention. Detailed description of the embodiments of the present invention will be given below in conjunction with the accompanying drawings.
[0020] Figure 1 is the tensile stress-strain curve of the gel electrolyte membrane obtained in Example 1; Figure 2 The electrochemical impedance diagram of a stainless steel blocking cell assembled with the gel electrolyte membrane obtained in Example 1; Figure 3 The cycle performance of the zinc-iodine battery assembled with the gel electrolyte membrane obtained in Example 1; Figure 4 is the tensile stress-strain curve of the gel electrolyte membrane obtained in Example 2; Figure 5 The electrochemical impedance diagram of a stainless steel blocking cell assembled with the gel electrolyte membrane obtained in Example 2; Figure 6 The cycle performance of the zinc-iodine battery assembled with the gel electrolyte membrane obtained in Example 2; Figure 7 is the tensile stress-strain curve of the gel electrolyte membrane obtained in Example 3; Figure 8 The electrochemical impedance diagram of a stainless steel blocking cell assembled with the gel electrolyte membrane obtained in Example 3; Fig. 9 The cycle performance of the zinc-iodine battery assembled with the gel electrolyte membrane obtained in Example 3; Fig.10 is the tensile stress-strain curve of the gel electrolyte membrane obtained in Comparative Example 1; Fig.11The electrochemical impedance diagram of a stainless steel blocked cell assembled with the gel electrolyte membrane obtained in Comparative Example 1; Fig.12 The cycle performance of the zinc-iodine battery assembled with the gel electrolyte membrane obtained in Comparative Example 1; Fig.13 is the tensile stress-strain curve of the electrolyte membrane obtained in Comparative Example 2; Fig.14 The electrochemical impedance diagram of the stainless steel blocked cell assembled with the electrolyte membrane obtained in Comparative Example 2; Fig.15 The cycle performance of the zinc-iodine battery assembled using the electrolyte membrane obtained in Comparative Example 2. DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0022] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. If not otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in the present invention are for demonstration purposes only. The present invention is further described according to the accompanying drawings and specific embodiments of the specification.
[0023] Example 1 (1) stirring and dissolving sodium lignin sulfonate in deionized water to obtain a sodium lignin sulfonate solution with a mass concentration of 2%; (2) Disperse 10 g of chitosan powder (200-400 mPa·s) in 2% (v / v) acetic acid solution and stir at 60 °C for 1 h to form a transparent chitosan solution after it is fully dissolved. (3) mixing the sodium lignin sulfonate solution obtained in step (1) and the chitosan solution obtained in step (2) at a mass ratio of 1:9, and stirring for 12 h to obtain a mixed solution; (4) casting the mixed solution obtained in step (3) into a polytetrafluoroethylene mold and placing it at room temperature for 3 days to obtain a composite membrane; (5) The composite membrane obtained in step (4) was immersed in a 2 mol / L ZnSO4 aqueous solution for 24 h to obtain a gel electrolyte membrane.
[0024] Example 2 (1) stirring and dissolving sodium lignin sulfonate in deionized water to obtain a sodium lignin sulfonate solution with a mass concentration of 2%; (2) Disperse 10 g of chitosan powder (200-400 mPa·s) in 2% (v / v) acetic acid solution and stir at 60 °C for 1 h to form a transparent chitosan solution after it is fully dissolved. (3) mixing the sodium lignin sulfonate solution obtained in step (1) and the chitosan solution obtained in step (2) at a mass ratio of 2:8, and stirring for 12 h to obtain a mixed solution; (4) casting the mixed solution obtained in step (3) into a polytetrafluoroethylene mold and leaving it at room temperature for 3 days to obtain a composite membrane; (5) The composite membrane obtained in step (4) was immersed in a 2 mol / L ZnSO4 aqueous solution for 24 h to obtain a gel electrolyte membrane.
[0025] Example 3 (1) stirring and dissolving sodium lignin sulfonate in deionized water to obtain a sodium lignin sulfonate solution with a mass concentration of 2%; (2) Disperse 10 g of chitosan powder (200-400 mPa·s) in 2% (v / v) acetic acid solution and stir at 60 °C for 1 h to form a transparent chitosan solution after it is fully dissolved. (3) mixing the sodium lignin sulfonate solution obtained in step (1) and the chitosan solution obtained in step (2) at a mass ratio of 3:7, and stirring for 12 h to obtain a mixed solution; (4) casting the mixed solution obtained in step (3) into a polytetrafluoroethylene mold and placing it at room temperature for 3 days to obtain a composite membrane; (5) The composite membrane obtained in step (4) was immersed in a 2 mol / L ZnSO4 aqueous solution for 24 h to obtain a gel electrolyte membrane.
[0026] Comparative Example 1 (1) Disperse 10 g of chitosan powder (200-400 mPa·s) in 2% (v / v) acetic acid solution and stir at 60°C for 1 h to form a transparent chitosan solution after it is fully dissolved. (2) casting the chitosan solution obtained in step (1) into a polytetrafluoroethylene mold and leaving it at room temperature for 3 days to obtain a chitosan film; (3) The chitosan membrane obtained in step (2) was immersed in a 2 mol / L ZnSO4 aqueous solution for 24 h to obtain a chitosan gel electrolyte membrane.
[0027] Comparative Example 2 The glass fiber separator (Whatman, 1823-090) was immersed in a 2 mol / L ZnSO4 aqueous solution for 24 h to obtain a glass fiber electrolyte membrane.
[0028] Performance Testing (1) Assembly and testing of chitosan gel electrolyte membrane zinc iodine battery: iodine powder and activated carbon powder were ground and mixed, placed in the bottom of a reactor, sealed and heated to 120°C, and kept warm for 6 hours to obtain iodine / activated carbon powder; the obtained powder, conductive carbon black and polyvinylidene fluoride were dispersed in N-methylpyrrolidone at a mass ratio of 7:2:1, and ground into a uniform slurry; the slurry was evenly coated on a stainless steel mesh and dried at 40°C to obtain an iodine positive electrode sheet; with a zinc sheet as the negative electrode, the gel electrolyte membrane obtained in Example 1, the gel electrolyte membrane obtained in Example 2, the gel electrolyte membrane obtained in Example 3 and the chitosan gel electrolyte membrane obtained in Comparative Example 1 were placed between the positive and negative electrodes, respectively, to assemble a CR2032 type zinc iodine battery; a constant current charge and discharge test was performed using a CT4008 test device, with a voltage range of 0.6-1.6 V; (2) Assembly and testing of glass fiber electrolyte membrane zinc-iodine battery: Grind and mix iodine powder and activated carbon powder, put them into the bottom of a reactor, seal them, heat them to 120°C, and keep them warm for 6 hours to obtain iodine / activated carbon powder; disperse the obtained powder, conductive carbon black and polyvinylidene fluoride in N-methylpyrrolidone at a mass ratio of 7:2:1, and grind them into a uniform slurry; evenly apply the slurry on a stainless steel mesh and dry it at 40°C to obtain an iodine positive electrode sheet; use a zinc sheet as the negative electrode, place the electrolyte membrane prepared in Comparative Example 2 between the positive and negative electrodes, and assemble them into a CR2032 zinc-iodine battery; use a CT4008 test device to perform constant current charge and discharge tests with a voltage range of 0.6-1.6 V.
[0029] Figure 1 2 is the tensile stress-strain curve of the gel electrolyte membrane obtained in Example 1. It can be seen that the tensile strength is as high as 5.1 MPa, which is significantly higher than the chitosan gel electrolyte membrane in Comparative Example 1 (4.14 MPa) and the glass fiber electrolyte membrane in Comparative Example 2 (0.13 MPa).
[0030] Figure 2 The electrochemical impedance diagram of the stainless steel blocked cell assembled with the gel electrolyte membrane obtained in Example 1 shows that the ionic conductivity of the gel electrolyte membrane obtained in Example 1 is 4.99 mS / cm, which is significantly higher than the chitosan gel electrolyte membrane in Comparative Example 1 (4.47 mS / cm).
[0031] Figure 3The cycling performance of the zinc-iodine battery assembled with the gel electrolyte membrane obtained in Example 1 was studied. The results showed that the residual discharge specific capacity of the battery was 159.2 mAh / g after 1000 cycles at a current density of 2 C, which were better than the zinc-iodine batteries prepared using the gel electrolyte membrane of Comparative Example 1 and the glass fiber electrolyte membrane of Comparative Example 2.
[0032] Figure 4 The tensile stress-strain curve of the gel electrolyte membrane obtained in Example 2 shows that the tensile strength is as high as 5.29 MPa, which is significantly higher than the chitosan gel electrolyte membrane in Comparative Example 1 (4.14 MPa) and the glass fiber electrolyte membrane in Comparative Example 2 (0.13 MPa).
[0033] Figure 5 This is an electrochemical impedance diagram of a stainless steel blocked battery assembled with the gel electrolyte membrane obtained in Example 2. The results show that the ionic conductivity of the gel electrolyte membrane obtained in Example 2 is 5.44 mS / cm, which is significantly higher than the ionic conductivity of the battery assembled with the chitosan gel electrolyte membrane in Comparative Example 1 (4.47 mS / cm) and the ionic conductivity of the battery assembled with the glass fiber electrolyte membrane in Comparative Example 2 (5.11 mS / cm).
[0034] Figure 6 This is a cycle performance diagram of a zinc-iodine battery assembled with the gel electrolyte membrane obtained in Example 2. The results show that the residual discharge specific capacity of the battery is 161.2 mAh / g after 1000 cycles at a current density of 2C, which are better than the battery assembled with the chitosan gel electrolyte membrane of Comparative Example 1 and the zinc-iodine battery assembled with the glass fiber electrolyte membrane of Comparative Example 2.
[0035] Figure 7 The tensile stress-strain curve of the gel electrolyte membrane obtained in Example 3 shows that the tensile strength is as high as 5.25 MPa, which is significantly higher than the chitosan gel electrolyte membrane in Comparative Example 1 (4.14 MPa) and the glass fiber electrolyte membrane in Comparative Example 2 (0.13 MPa).
[0036] Figure 8 The electrochemical impedance diagram of the stainless steel blocked cell assembled with the gel electrolyte membrane obtained in Example 3 shows that the ionic conductivity of the gel electrolyte membrane obtained in Example 3 is 6.02 mS / cm, which is significantly higher than the chitosan gel electrolyte membrane in Comparative Example 1 (4.47 mS / cm) and the glass fiber electrolyte membrane in Comparative Example 2 (5.11 mS / cm).
[0037] Fig. 9The cycling performance of the zinc-iodine battery assembled with the gel electrolyte membrane obtained in Example 3 was studied. The results showed that the residual discharge specific capacity of the battery was 166.8 mAh / g after 1000 cycles at a current density of 2C, which was better than the zinc-iodine batteries assembled with the gel electrolyte membrane of Comparative Example 1 and the glass fiber electrolyte membrane of Comparative Example 2.
[0038] Fig.10 This is the tensile stress-strain curve of the gel electrolyte membrane obtained in Comparative Example 1. The results show that the tensile strength is 4.14 MPa.
[0039] Fig.11 The electrochemical impedance diagram of a stainless steel blocked cell assembled with the gel electrolyte membrane obtained in Comparative Example 1 shows that the ionic conductivity of the gel electrolyte membrane obtained in Comparative Example 1 is 4.47 mS / cm.
[0040] Fig.12 The cycle performance of the zinc-iodine battery assembled with the gel electrolyte membrane obtained in Comparative Example 1 is shown. The results show that the residual discharge capacity of the battery is 143.2 mAh / g after 1000 cycles at a current density of 2C.
[0041] Fig.13 This is the tensile stress-strain curve of the glass fiber electrolyte membrane of comparative example 2. The results show that the tensile strength is only 0.13 MPa.
[0042] Fig.14 This is the electrochemical impedance diagram of a stainless steel blocked cell assembled with the glass fiber electrolyte membrane of Comparative Example 2. The results show that the ionic conductivity of the glass fiber electrolyte membrane of Comparative Example 2 is 5.11 mS / cm.
[0043] Fig.15 The cycling performance of the zinc-iodine battery assembled with the glass fiber electrolyte membrane of Comparative Example 2 was studied. The results showed that the residual discharge capacity of the battery was 147.5 mAh / g after 336 cycles at a current density of 2C.
[0044] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A method for preparing a lignin sulfonate-chitosan gel electrolyte membrane, characterized in that: The preparation method comprises the following steps: (1) dissolving lignin sulfonate in deionized water to obtain a lignin sulfonate aqueous solution with a mass concentration of 0.1-5.0%; (2) Disperse 1-20 g chitosan powder in 1-4% (v / v) acetic acid solution, stir, and fully dissolve to form a transparent solution; (3) mixing the lignin sulfonate aqueous solution obtained in step (1) and the transparent solution obtained in step (2) in a mass ratio of (1-3): (7-9), stirring to obtain a transparent solution; (4) casting the solution obtained in step (3) into a polytetrafluoroethylene mold and leaving it at room temperature to obtain a composite membrane; (5) Soaking the composite membrane obtained in step (4) in a 0.1-10 mol / L zinc salt solution to obtain a gel electrolyte membrane.
2. The preparation method according to claim 1, characterized in that: In step (1), the lignin sulfonate is at least one of sodium lignin sulfonate, calcium lignin sulfonate, magnesium lignin sulfonate and ammonium lignin sulfonate.
3. The preparation method according to claim 1, characterized in that: In step (1), the stirring temperature is 25-80°C and the stirring time is 1-4 h.
4. The preparation method according to claim 1, characterized in that: In step (2), the viscosity of the chitosan powder is 100-400 mPa·s.
5. The preparation method according to claim 1, characterized in that: In step (3), the stirring time is 1-24h.
6. The preparation method according to claim 1, characterized in that: In step (4), the time of standing at room temperature is 3 days.
7. The preparation method according to claim 1, characterized in that: In step (5), the zinc salt is at least one of ZnCl2, ZnSO4·7H2O, Zn(CH3COO)2·2H2O, Zn(NO3)2·6H2O, Zn(BF4)2·6H2O and Zn(CF3SO3)2.
8. The preparation method according to claim 1, characterized in that: In step (5), the soaking time is 12-48 hours.
9. A lignin sulfonate-chitosan gel electrolyte membrane prepared by the method according to any one of claims 1 to 8.
10. Use of the lignin sulfonate-chitosan gel electrolyte membrane prepared by the method according to claim 1 and / or the lignin sulfonate-chitosan gel electrolyte membrane according to claim 9, characterized in that: The lignin sulfonate-chitosan gel electrolyte membrane is used in the field of zinc-iodine batteries.
Citation Information
Cited By
Zinc-iodine battery positive electrode binder, zinc-iodine battery positive electrode plate based on binder and preparation method and application of zinc-iodine battery positive electrode plate
CN119812334A