Method for densifying fibrous structure by injecting slurry

By using the film reinforcement area with high Young's modulus in the mold to contact the corrugated peaks of the fiber structure and control the injection pressure difference, the problem of increasing smooth surface and thickness during the densification of the fiber structure is solved, and efficient densification is achieved and mechanical strength increase.

CN119013130AActive Publication Date: 2024-11-22SAFRAN CERAMICS SA

Patent Information

Application Number
CN202380033593.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-04
Filing Date
2023-03-28
Publication Date
2024-11-22
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

The prior art is difficult to obtain a smooth surface without increasing thickness when densifying fiber structures, and the manufacturing process is complex, resulting in reduced thermal mechanical resistance and increased cost.

Method used

The film reinforcement zone with Young's modulus greater than 200 GPa is used to contact the corrugated peaks of the pre-densified fiber structure in the mold, and ensure the slurry side by controlling the difference between injection pressure and compression pressure between 0.5x105Pa and 6x105Pa. Injection into the membrane cavity to prevent excessive growth of the matrix and form a smooth surface.

Benefits of technology

The smooth and densification of the fiber structure is achieved, excessive thickness increases, mechanical strength and surface smoothness are improved, while simplifying the manufacturing process and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013130A_ABST
    Figure CN119013130A_ABST
Patent Text Reader

Abstract

The invention relates to a method for densifying a fibrous structure made of a ceramic material for use in an injection apparatus comprising:-a mold cavity defined between a mold and a counter-mold, the mold cavity defining an internal space; and-a membrane comprising a reinforcement zone to be placed between the fibrous structure in the mold cavity and the counter mold, the reinforcement zone of the membrane having a Young's modulus greater than 200 GPa, the method comprising:-placing (110) a pre-densified fibrous structure in the mold cavity, the pre-densified fibrous structure having corrugations on the surface, and placing the membrane on the pre-densified fibrous structure such that the reinforcement regions of the membrane are in contact with the peaks of the corrugations of the pre-densified fibrous structure; closing (120) the injection apparatus by placing a counter mold on the membrane and applying a pressing pressure (Ppressing) to the membrane to maintain the reinforcing regions of the membrane in contact with the peaks of the corrugations of the pre-densified fibrous structure; and densifying (130) the pre-densified fibrous structure by infiltrating a slurry into the pores of the pre-densified fibrous structure, the slurry being injected into the mold cavity laterally with respect to the membrane under an injection pressure (Pinjection) such that the pressure difference between the pressing pressure and the injection pressure is between 0.5 x105 Pa and 6 x105 Pa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the general field of manufacturing components made of ceramic matrix composite (CMC) materials and, more particularly, to a method of densifying a fiber structure made of ceramic material containing a ceramic matrix. Background Art

[0002] Densification of the fiber structure - i.e. forming a ceramic matrix in the fiber structure - comprises a slurry injection step consisting in impregnating the fiber structure with a slurry or a suspension of ceramic particles which penetrates into the pores of the fiber structure and allows obtaining a ceramic matrix in the fiber structure.

[0003] In order to improve the aerodynamic performance of the final component, it is necessary to give the densified fiber structure a smooth surface. Generally speaking, in order to obtain a smooth surface, the surface of the densified fiber structure is smoothed by machining or by adding material (extra thickness). However, this leads to additional costs, reduces the thermomechanical resistance of the material, and most importantly complicates the manufacturing process of the ceramic matrix composite.

[0004] Therefore, it is desirable to provide a new method for densifying a fiber structure so as to obtain a densified fiber preform with a smooth surface without excessive thickness and without requiring additional surface machining steps. Summary of the invention

[0005] The invention relates to a method for densifying a fiber structure made of ceramic material with a ceramic matrix for use in an injection device, the injection device comprising:

[0006] - a cavity defined between the mold and the counter-mold, the cavity defining an interior space; and

[0007] - a membrane comprising a reinforced zone, which membrane is to be placed between the fiber structure present in the mold cavity and the counter-mold, and the Young's modulus of the reinforced zone of the membrane is greater than 200 GPa;

[0008] The method includes:

[0009] - placing a pre-densified fiber structure having corrugations on its surface in the mold cavity, and placing the membrane in such a way that the reinforcement areas of the membrane are in contact with the peaks of the corrugations of the pre-densified fiber structure;

[0010] Placed on a pre-densified fiber structure;

[0011] - closing the injection device and applying a compacting pressure to the membrane by placing a counter-mould on the membrane so as to keep the reinforced areas of the membrane in contact with the peaks of the corrugations of the pre-densified fibrous structure; and

[0012] - densification of the pre-densified fiber structure by infiltrating the slurry into the pores of the pre-densified fiber structure, the slurry being injected into the membrane cavity laterally to the reinforcement zone of the membrane under injection pressure such that the pressure difference between the compaction pressure and the injection pressure is within 0.5 x 10 5 Pa and 6x 10 5 Between Pa.

[0013] The Young's modulus of the reinforcement zone is greater than 200 GPa, which makes the reinforcement zone rigid enough so as not to deform during the compaction pressure applied to the membrane and the densification of the fiber structure.

[0014] Thanks to the method of the invention, and in particular by placing the reinforcement zone of the membrane at the peaks of the corrugations of the fiber structure and making the Young's modulus of the reinforcement zone greater than 200 GPa, it is possible to smooth the surface of the fiber structure during its densification while avoiding the generation of excessive thickness (the excess thickness generated by the growth of the matrix is ​​very limited, reaching at most 0.05 mm). In fact, the growth of the matrix - that is to say the densification of the fiber structure - stops at the reinforcement zone of the membrane, which avoids the formation of excessive thickness on the surface of the fiber structure. Therefore, the volume of the matrix thus formed is limited to the highest corrugations of the pre-densified fiber structure.

[0015] Furthermore, the pressure difference between the compaction pressure and the injection pressure is set between 0.5 bar and 6 bar (i.e., between 0.5 x 10 5 Pa and 6x 10 5 Pa), which allows the reinforcement zone of the membrane to remain in contact only with the peaks of the corrugations of the fiber structure. Therefore, this reinforcement zone does not match the contour of the structure and does not deform during the growth of the matrix in the pores of the fiber structure. This difference in pressure range allows to obtain a fiber preform with a smooth surface, that is, a densified fiber structure.

[0016] Furthermore, the fiber structure is pre-densified when it is placed in the mold cavity so that it can no longer deform. In other words, the fiber structure is consolidated before being introduced into the mold cavity. This increases its mechanical strength to prevent it from deforming. This also extends the compaction pressure range and provides a compaction pressure between 0.5 bar and 6 bar, which is not possible for deformable reinforcements.

[0017] The slurry can be injected into the mold cavity laterally to the reinforcement area of ​​the membrane and into the pores of the pre-densified fiber structure at an applied flow rate or at an applied pressure, so that the pressure difference between the compaction pressure and the injection pressure remains constant throughout the injection process. When injecting at the applied flow rate, the pressure distribution can be monitored, especially during the growth of the matrix, the pressure rises with the increase of the flow resistance to prove that the pressure difference between the compaction pressure and the injection pressure remains constant.

[0018] According to a particular feature of the invention, the reinforcement zone of the membrane is formed by a metal foil placed on the surface of the membrane opposite to the fiber structure.

[0019] According to another particular feature of the invention, the metal foil is made of molybdenum or Made.

[0020] According to another particular feature of the invention, the metal foil comprises an anti-stick coating on the surface facing the fibrous structure.

[0021] According to another particular feature of the invention, the method also comprises, before placing the metal foil, treating the metal foil with an anti-adhesive coating in the form of a spray or a self-adhesive film.

[0022] The anti-stick coating is, for example, a polytetrafluoroethylene (PTFE) film.

[0023] The presence of a release coating on the metal foil helps limit tearing of the material.

[0024] According to another particular feature of the invention, the reinforcement zone of the membrane is formed by a fabric or a metal insert inside the membrane. In other words, there is a metal insert or a fabric between the inner and outer surfaces of the membrane. The fabric is, for example, a consolidated fabric formed by woven fibers, for example a fine two-dimensional fabric made of carbon or glass, which can be formed integrally during the casting of the membrane. The metal insert is, for example, a Inserts made of molybdenum or steel.

[0025] According to another particular feature of the present invention, the pressure difference between the compaction pressure and the injection pressure is within 0.5 x 10 5 Pa and 1.5x 10 5 Pa (i.e. between 0.5 bar and 1.5 bar).

[0026] This allows to improve the smoothness of the surface of the fiber structure after densification.

[0027] According to another particular feature of the invention, the thickness of the reinforced zone of the membrane is between 50 μm and 100 μm.

[0028] According to another specific feature of the invention, the thickness of the reinforcement zone of the membrane is greater than 50 μm, for example between 0.05 mm and 0.5 mm, in particular between 0.05 mm and 0.1 mm. This is especially true in the densification process of a fiber structure with a flat surface. These thickness ranges and / or these materials for the reinforcement zone allow to have a region that is rigid enough so that it does not deform when pressed against the fiber structure and when the matrix grows in the fiber structure, and is flexible enough so that it can match the geometric singularity of the component and maintain contact with the peaks of the corrugations of the fiber structure at all points.

[0029] According to another particular feature of the invention, outside its reinforced zone, the membrane has a thickness between 1.5 and 4 mm and a hardness between 30 and 60 Shore A.

[0030] This makes it possible to have a membrane in which the compaction pressure is applied evenly over its reinforced areas without hindering the injection of the slurry.

[0031] According to another particular feature of the invention, the method also comprises drying the densified fibrous structure and demoulding the densified fibrous structure after densification.

[0032] According to another particular feature of the invention, drying is carried out in the mould before demoulding or outside the mould after demoulding in an oven, in a climate chamber or by freeze drying.

[0033] For example, the temperature of drying in the oven or climate chamber is between 40° C. and 80° C. Furthermore, the oven or climate chamber preferably has a relative humidity between 40% and 90% in order to limit cracking.

[0034] According to another specific feature of the present invention, the slurry includes ceramic filler, binder and plasticizer, the volume ratio of the ceramic filler is 5% to 50%, for example, the volume ratio is 15% to 25%, the mass ratio of the binder is 0% to 20%, and the mass ratio of the plasticizer is 0%-20%.

[0035] For example, the ceramic filler includes silicon carbide SiC particles with a d50 of less than 2 μm. The binder is, for example, polyvinyl alcohol (PVA), polyethylene glycol (PEG) or glycerol. The plasticizer is, for example, polyethylene glycol 200 (PEG 200). BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Other characteristics and advantages of the invention will emerge from the description given below, with reference to the accompanying drawings, which show exemplary embodiments of the invention without any limiting character.

[0037] Figure 1 A method for densifying a fiber structure made of ceramic material and having a ceramic matrix according to one embodiment of the invention is schematically shown.

[0038] Figure 2A An exploded view of an injection device for carrying out a densification method according to one embodiment of the invention is shown schematically and partially.

[0039] Figure 2B Schematically and partially shown Figure 2A Part of an injection device.

[0040] Figure 3Schematically and partially shown is a metal foil in contact with the peaks of the corrugations of a pre-densified fiber structure present in an injection device for implementing the invention. DETAILED DESCRIPTION

[0041] Figure 1 A method 100 for densifying a fiber structure made of a ceramic material and having a ceramic matrix according to one embodiment of the present invention is schematically shown.

[0042] Figure 2A , Figure 2B and Figure 3 Schematically and partially shows a method for implementing Figure 1 The method 100 is shown as including an injection device 260 for the fiber structure 210 .

[0043] The injection device 260 includes a mold cavity 263 defined between a mold 261 and a counter mold 262. Therefore, the mold cavity 263 defines an internal space. The injection device 260 also includes a film 240, which is intended to be placed between the fiber structure 210 present in the mold cavity 263 and the counter mold 262. The film 240 includes a reinforcement area 220. In this exemplary embodiment, the reinforcement area 220 is formed by a metal foil present on the surface of the film 240 facing the fiber structure 210. Therefore, in the remaining description of these figures, the reinforcement area 220 of the film 240 will be referred to as "metal foil" for short.

[0044] The thickness of the film 240 may be between 1.5 mm and 4 mm, except for the area comprising the metal foil 220. Its hardness may be between 30 Shore A and 60 Shore A. The film 240 has, for example, a hardness of 50 Shore A and a thickness of 4 mm, so as to facilitate good management of the seal between the counter-mold 262 / mold 261 and the film 240.

[0045] The device 260 also includes two ports 251 for injecting the slurry into the mold cavity 263 and an outlet port 252 configured to eliminate the liquid phase from the injected slurry. It can also include an injection wedge 250 that allows the film 240 and the fiber structure 210 to be wedged so as not to hinder the injection of the slurry and its impregnation into the structure 210.

[0046] The injection device 260 also includes a filter element 230 present in the mold cavity 263 below the fiber structure 210. The filter element 230 is configured to filter the liquid phase of the slurry injected into the mold cavity 263. The liquid phase filtered by the filter element 230 can be discharged through the outlet port 252.

[0047] The densification method 100 includes placing 110 a pre-densified fiber structure 210 in a mold cavity 263 of an injection device 260, and placing a film 240 on the pre-densified fiber structure 210. The pre-densified fiber structure 210 has corrugations 211, 212 (e.g., Figure 3 ). For example, there is a difference of up to 0.3 mm between the peaks of the corrugations 211, 212 and the lowest point of the corrugations. The metal foil 220 of the membrane 240 is placed on the fiber structure 210 so that it is in contact with the peaks of the corrugations 211, 212 of the fiber structure 210. The metal foil 220 is in contact only with the peaks of the corrugations and not with the lowest point located, for example, 0.3 mm from the peaks.

[0048] The metal foil 220 is made of, for example, molybdenum, steel or Its Young's modulus is greater than 200 GPa, and its thickness may be between 50 μm and 100 μm, for example 100 μm. The metal foil 220 may further include an anti-stick coating on its surface facing the fiber structure 210 .

[0049] The method 100 then comprises closing 120 the injection device 260 by placing a counter-mold 262 on the film. 压紧 Applied onto the film 240 , the metal foil 220 is held in contact with the peaks of the corrugations 211 , 212 of the pre-densified fiber structure 210 .

[0050] The compaction pressure P is applied to the membrane 240, for example, by air pressure or pressure from another fluid such as, for example, silicone oil. 压紧 Applied to the metal foil 220.

[0051] Finally, the method 100 includes densifying 130 the pre-densified fiber structure 210 by infiltrating the slurry into the pores of the pre-densified fiber structure 210. 注射 Under the present invention, the slurry is injected into the mold cavity 263 through the injection port 251 of the injection device 260 laterally to the film 240, in particular laterally to the metal foil 220. Therefore, the densified fiber structure forms a fiber preform containing a matrix.

[0052] Injection pressure P 注射 and the pressing pressure P 压紧 The value of is defined as the pressure difference ΔP (ΔP = P 压紧 –P 注射 ) between 0.5 bar and 6 bar (that is, in Pascals, between 0.5 x 10 5 Pa and 6x10 5 The pressure difference ΔP is, for example, between 0.5 bar and 1.5 bar, for example, 1 bar.

[0053] Injection pressure P 注射 For example, it may be between 3 bar and 20 bar.

[0054] Compressing pressure P 压紧 For example, it may be between 0.5 bar and 6 bar.

[0055] During the injection 130 of the slurry, the compaction pressure P 压紧 and injection pressure P 注射 The value of may vary, so the method 100 may include monitoring the pressure difference ΔP throughout the injection 130 to maintain the pressure difference ΔP within the range of 0.5 bar to 6 bar, or within a more limited range, such as between 0.5 bar and 1.5 bar.

[0056] The method 100 may also include drying the densified fiber structure 210 and demolding it. Drying can be performed before or after demolding the densified fiber structure. For example, drying is performed in the mold before demolding, or outside the mold after demolding. When drying is performed outside the mold, it can be performed in a climate chamber, an oven, or by freeze drying.

[0057] The method 100 may further include treating the metal foil 220 with a release coating prior to placing 110 the film 240 on the fiber structure 210. Treating the foil 220 with the release coating may be accomplished by spraying the release coating onto the foil 220 or by bonding a self-adhesive film to the foil 220.

[0058] Pre-densified or consolidated fiber structures include, for example, silicon carbide fibers. The fiber structure can be produced by superimposing layers or plies obtained by two-dimensional weaving. The structure can also be produced directly as a whole by three-dimensional weaving. Two-dimensional weaving here refers to the traditional weaving method in which each weft thread passes from one side of the line of a single warp thread layer to the other side or vice versa. Three-dimensional weaving here refers to the weaving of warp threads passing through several weft thread layers, or weft threads passing through several warp thread layers.

[0059] The fiber structure can also be realized by unidirectional fiber sheets, which can be obtained by automated fiber placement or fiber winding.

[0060] The fiber structure can be pre-densified or consolidated by chemical vapor infiltration (CVI) by depositing a boron nitride or pyrolytic carbon interfacial phase and then depositing a layer of silicon carbide or silicon nitride or a mixture of the two (vapor phase consolidation). Densification with silicon carbide can also be performed on the outside of the molded part to protect the structure during the melt infiltration step.

[0061] The slurry injected during the densification step 130 may include a ceramic filler in a volume ratio of between 10% and 50%, for example, a volume ratio of between 15% and 25%, a binder in a mass ratio of between 0% and 20%, and a plasticizer in a mass ratio of between 0% and 20%. The ceramic filler is, for example, silicon carbide powder with a size d50 less than 2 μm. The binder is, for example, polyvinyl alcohol (PVA), polyethylene glycol (PEG), or glycerol. The plasticizer is, for example, polyethylene glycol 200 (PEG 200). The slurry may also include a dispersant, which may be electrostatic (such as tetraethylammonium hydroxide (TEAH)), or electrostatic steric hindrance (such as polyetherimide (PEI)), or steric hindrance (such as polyvinyl pyrrolidone (PvP)). It may also include a wetting agent.

[0062] According to another embodiment, the reinforced zone of the membrane may be formed by a metal insert or a fabric present between the two outer surfaces of the membrane.

[0063] For example, the metal insert can be made of Made of molybdenum or steel.

[0064] The fabric may be, for example, a consolidated fabric, such as a two-dimensional fabric. The fabric may be made of carbon or glass fibers and may include an epoxy resin matrix.

[0065] The expression "between... and..." should be understood as including the endpoint values.

Claims

1. A method (100) of densifying a fiber structure made of a ceramic material having a ceramic matrix for use in an injection device (260), the injection device comprising: - a mold cavity (263) defined between the mold (261) and the counter-mold (262), the mold cavity defining an internal space, and a membrane (240) comprising a reinforced zone (220) to be placed between the fiber structure (210) present in the mold cavity and a counter mold, and wherein the reinforced zone of the membrane has a Young's modulus greater than 200 GPa, The method comprises: - placing (110) a pre-densified fiber structure in the mold cavity, the pre-densified fiber structure having corrugations (211, 212) on the surface, and placing the reinforcement area of ​​the membrane on the pre-densified fiber structure in such a way that the reinforcement area of ​​the membrane is in contact with the peaks of the corrugations of the pre-densified fiber structure; - closing (120) the injection device by placing the counter-mold on the film and applying a compacting pressure (P 压紧 ) to maintain the reinforced areas of the membrane in contact with the peaks of the corrugations of the pre-densified fibrous structure; and - densifying (130) the pre-densified fiber structure by infiltrating a slurry into the pores of the pre-densified fiber structure, the slurry being injected at an injection pressure (P 注射 ) is injected into the mold cavity toward the reinforcement area of ​​the film, so that the pressure difference (ΔP) between the pressing pressure and the injection pressure is within 0.5 x 10 5 Pa and 6x 10 5 Between Pa.

2. The densification method according to claim 1, wherein: The pressure difference between the compaction pressure and the injection pressure is within 0.5 x 10 5 Pa and 1.5x 10 5 Between Pa.

3. The densification method according to claim 1 or 2, wherein: The thickness of the reinforced zone of the membrane is between 50 μm and 100 μm.

4. The densification method according to any one of claims 1 to 3, wherein: The reinforcement zone of the membrane is formed by a metal foil arranged on the surface of the membrane opposite to the fiber structure.

5. The densification method according to claim 4, wherein: The metal foil is made of molybdenum or Made.

6. The densification method according to claim 4 or 5, wherein: The metal foil comprises a non-stick coating on the surface facing the fiber structure.

7. Densification method according to any one of claims 4 to 6, further comprising treating the metal foil with a release coating in the form of a spray or a self-adhesive film.

8. The densification method according to any one of claims 1 to 3, wherein: The reinforced areas of the membrane are formed by fabric or metal inserts within the membrane.

9. The densification method according to any one of claims 1 to 8, wherein: Outside the reinforced area of ​​the membrane, the membrane has a thickness between 1.5 mm and 4 mm and a hardness between 30 Shore A and 60 Shore A.

10. The densification method according to any one of claims 1 to 9, further comprising drying and demoulding the densified fiber structure after densification.

11. The densification method according to claim 10, wherein: The drying of the fiber structure takes place in the mold before demoulding or outside the mold after demoulding in an oven, a climate chamber or by freeze drying.

12. The densification method according to any one of claims 1 to 11, wherein: The slurry comprises a ceramic filler in a volume ratio of between 10% and 50%, a binder in a mass ratio of between 0% and 20%, and a plasticizer in a mass ratio of between 0% and 20%.

Citation Information

Patent Citations

  • Method for manufacturing a fibrous preform filled with refractive ceramic particles

    CN107206624A

  • Method for producing a part made from a composite material by means of the injection of a laden ceramic slurry into a fibrous structure

    CN111971263A

  • Method for producing a part from composite material by injecting a filled slip into a fibrous texture

    CN114080311A

  • Method and special mold for preparing unfired ceramic element sheet

    CN1370759A

  • Pressure slip casting and pressure demoulding ceramic blank forming device

    CN200984780Y

Cited By

  • Slurry infiltration process

    WO2026161691A1