Ceramic substrate and preparation method thereof

By alternately stacking of the live porcelain belt and spherical separator layer, combined with isostatic molding and staged sintering, the problem of easy scratching during sintering of ceramic substrates is solved, significantly improving the sintering yield and ensuring product quality.

CN119143483APending Publication Date: 2024-12-17GUANGDONG HUANBO NEW MATERIAL CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410907825.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-12-17

AI Technical Summary

Technical Problem

Existing ceramic substrates are prone to scratches during sintering, resulting in low sintering yield.

Method used

Alternate stacking of raw ceramic tapes and spherical adhesive layers are used, and the particle size of the partition powder is 5-10 μm. The friction between the raw ceramic tapes and the partition powder is avoided by isostatic molding and staged sintering.

Benefits of technology

It effectively improves the sintering yield of ceramic substrates, avoids scratching problems, and ensures high quality of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004932658580000081
    Figure BDA0004932658580000081
  • Figure BDA0004932658580000091
    Figure BDA0004932658580000091
Patent Text Reader

Abstract

The invention discloses a ceramic substrate and a preparation method thereof, and relates to the technical field of electronic packaging materials, the ceramic substrate comprises green tapes and adhesion isolating layers which are alternately stacked, and the green tapes are arranged on the surface layer and the bottom layer of the ceramic substrate; the number of layers of the raw ceramic tapes is 2-6; the adhesion isolation layer is formed by laying adhesion isolation powder, the adhesion isolation powder is spherical, and the particle size of the adhesion isolation powder is 5-10 [mu] m. According to the technical scheme, the anti-sticking powder is spherical in shape, regular in shape and good in fluidity; the particle size of the adhesion-isolating powder is controlled to be 5-10 microns, and the adhesion-isolating powder within the particle size range is low in surface activity and not prone to reacting with a green tape; the number of the layers of the green tapes is 2-6, so that the stress of each layer of the green tapes is basically consistent, and the green tapes positioned below are prevented from being overlarge in stress; according to the technical scheme, when displacement occurs due to sintering shrinkage, friction between the green tape and the adhesion isolating powder can be avoided, and therefore the problem that the green tape is prone to being scratched in the sintering process is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic packaging materials, and in particular to a ceramic substrate and a preparation method thereof. Background Art

[0002] At present, the commonly used electronic packaging materials mainly include plastic substrates, metal substrates, ceramic substrates and composite substrates. Among them, ceramic substrates have excellent electrical insulation properties, high thermal conductivity, excellent soft soldering performance and high adhesion strength, and can be etched with various patterns like PCB boards, and have a large current carrying capacity. Therefore, ceramic substrates are widely used in high-power power semiconductor modules, power control circuits, automotive electronics, aerospace, military electronic components, and solar panel components.

[0003] However, the existing ceramic substrates are easily scratched during sintering, resulting in a low sintering yield of the product. Summary of the invention

[0004] The main purpose of the present invention is to provide a ceramic substrate and a preparation method thereof, aiming to improve the scratch problem of the ceramic substrate during sintering.

[0005] To achieve the above-mentioned purpose, the ceramic substrate proposed in the present invention comprises raw porcelain tapes and insulating layers alternately stacked, and the surface layer and the bottom layer of the ceramic substrate are both raw porcelain tapes; the number of layers of raw porcelain tapes is 2-6; the insulating layer is formed by laying insulating powder, the morphology of the insulating powder is spherical, and the particle size of the insulating powder is 5-10μm.

[0006] In one embodiment, the anti-sticking powder is alumina powder.

[0007] The present invention also provides a method for preparing a ceramic substrate, comprising the following steps:

[0008] Applying isolation powder on the green porcelain tape to form an isolation layer, and then stacking the green porcelain tape and the isolation layer in sequence, controlling the number of stacked layers of the green porcelain tape to be 2-6 layers, and controlling the surface layer to be the green porcelain tape; the morphology of the isolation powder is spherical, and the particle size of the isolation powder is 5-10 μm;

[0009] The stacked green porcelain tapes are evacuated and then isostatically pressed;

[0010] The ceramic substrate can be obtained by sintering the green ceramic tape formed by isostatic pressing.

[0011] In one embodiment, the laying of the isolation powder comprises the following steps: firstly, the isolation powder and the adhesive are mixed into a suspension, and then the suspension is sprayed on the green porcelain tape.

[0012] In one embodiment, the parameters of isostatic pressing are: temperature 50-80° C., pressure 50-100 MPa, and holding time 5-20 min.

[0013] In one embodiment, the sintering includes a first stage sintering, a second stage sintering and a temperature reduction treatment;

[0014] The parameters of the first stage sintering are: from room temperature to the first sintering temperature, the heating rate is 0.1-0.5°C / min, the holding time is 4-6h, and the first sintering temperature is 400-1000°C; and / or,

[0015] The parameters of the second stage sintering are: from the first sintering temperature to the second sintering temperature, the heating rate is 0.5-1°C / min, the air flow rate is 1-5L / min, the holding time is 2-4h, and the second sintering temperature is 1450-1600°C; and / or,

[0016] The parameters of the cooling treatment are: from the second sintering temperature to room temperature, the cooling rate is 0.5-1°C / min.

[0017] In one embodiment, the method for preparing the ceramic substrate further includes making a green ceramic tape, which specifically includes the following steps:

[0018] Alumina powder and a dispersant are added to a solvent and ground and mixed to obtain slurry I, and then a plasticizer and a binder are added to the slurry I and ground and mixed to obtain slurry II;

[0019] Slurry II was tape cast to form a green tape.

[0020] In one embodiment, the amount of aluminum oxide powder added is 40wt%-60wt%, the amount of dispersant added is 1wt%-3wt%, the amount of plasticizer added is 2wt%-5wt%, the amount of binder added is 5wt%-10wt%, and the balance is solvent.

[0021] In one embodiment, the purity of the aluminum oxide powder is greater than 99%, and the particle size D 50 0.5-1.0 μm; and / or,

[0022] The dispersant is triolein; and / or,

[0023] The plasticizer is selected from at least one of dioctyl phthalate and polyethylene glycol; and / or,

[0024] The binder is polyvinyl butyral; and / or,

[0025] The solvent is a mixture of alcohol and ester, and the mass ratio of the alcohol to the ester is 1-3:7-9.

[0026] In one embodiment, the alcohol is selected from at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol; and / or,

[0027] The ester is selected from at least one of ethyl acetate, methyl acetate, propyl acetate and butyl acetate.

[0028] The technical solution of the present invention alternately stacks the raw porcelain tape and the isolation layer, the isolation layer is formed by applying the isolation powder, and the morphology of the isolation powder is set to be spherical, the spherical isolation powder has a regular morphology and good fluidity; the particle size of the isolation powder is controlled to be 5-10μm, and the isolation powder in this particle size range has low surface activity and is not easy to react with the raw porcelain tape; the number of layers of the raw porcelain tape is set to 2-6 layers, so that the force on each layer of the raw porcelain tape can be ensured to be basically consistent, avoiding excessive pressure on the raw porcelain tape located at the bottom; the above technical solution can avoid friction between the raw porcelain tape and the isolation powder when displacement occurs due to sintering shrinkage, thereby improving the problem of easy scratches during sintering and ensuring the sintering yield of the product. DETAILED DESCRIPTION

[0029] It should be noted that the meaning of "and / or" in the present invention includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. "At least one" in the present invention means one or more, and "more than one" means two or more.

[0030] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.

[0031] "Scope" disclosed in the present invention is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3,4 and 5 are listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present invention, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0032] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0033] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0034] In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0035] In recent years, with the vigorous development of the microelectronics packaging industry, electronic packaging technology has developed in the direction of miniaturization, high density, multi-power and high reliability, and electronic packaging materials have gradually become an important industrial field with high technology content and high economic benefits. Currently, the commonly used electronic packaging materials are mainly divided into four categories: plastic substrates, metal substrates, ceramic substrates and composite substrates. Among them, ceramic substrates have excellent electrical insulation properties, high thermal conductivity, excellent soft soldering performance and high adhesion strength, and can be etched with various patterns like PCB boards, and have great current carrying capacity. Therefore, ceramic substrates are widely used in high-power power semiconductor modules, power control circuits, automotive electronics, aerospace, military electronic components, and solar panel components.

[0036] Existing ceramic substrates use a conventional powder coating and stacking method, specifically, powdered insulation powder is directly spread on the surface of the green porcelain tape. When sintering shrinks, the green porcelain tape and the insulation powder will produce friction, causing scratches on the green porcelain tape, and then scratches on the formed ceramic substrate.

[0037] To this end, the present invention proposes a ceramic substrate, comprising alternately stacked raw porcelain tapes and insulating layers, and the surface layer and the bottom layer of the ceramic substrate are both raw porcelain tapes; the number of layers of the raw porcelain tapes is 2-6 layers; the insulating layer is formed by laying insulating powder, the morphology of the insulating powder is spherical, and the particle size of the insulating powder is 5-10μm.

[0038] The technical solution of the present invention alternately stacks the raw porcelain tape and the isolation layer, the isolation layer is formed by applying the isolation powder, and the morphology of the isolation powder is set to be spherical, the spherical isolation powder has a regular morphology and good fluidity; the particle size of the isolation powder is controlled to be 5-10μm, and the isolation powder in this particle size range has low surface activity and is not easy to react with the raw porcelain tape; the number of layers of the raw porcelain tape is set to 2-6 layers, so that the force on each layer of the raw porcelain tape can be ensured to be basically consistent, avoiding excessive pressure on the raw porcelain tape located at the bottom; the above technical solution can avoid friction between the raw porcelain tape and the isolation powder when displacement occurs due to sintering shrinkage, thereby improving the problem of easy scratches during sintering and ensuring the sintering yield of the product.

[0039] In an embodiment of the present invention, the anti-sticking powder is aluminum oxide powder.

[0040] The present invention also provides a method for preparing a ceramic substrate, comprising the following steps:

[0041] Applying isolation powder on the green porcelain tape to form an isolation layer, and then stacking the green porcelain tape and the isolation layer in sequence, controlling the number of stacked layers of the green porcelain tape to be 2-6 layers, and controlling the surface layer to be the green porcelain tape; the morphology of the isolation powder is spherical, and the particle size of the isolation powder is 5-10 μm;

[0042] The stacked green porcelain tapes are evacuated and then isostatically pressed;

[0043] The ceramic substrate can be obtained by sintering the green ceramic tape formed by isostatic pressing.

[0044] The preparation method of the present invention adopts all the technical solutions of the above ceramic substrate embodiment, and therefore has at least all the beneficial effects brought by the technical solutions of the above ceramic substrate embodiment, which will not be described one by one here.

[0045] In an embodiment of the present invention, the laying of the isolation powder includes the following steps: firstly, the isolation powder and the adhesive are mixed into a suspension, and then the suspension is sprayed on the green porcelain tape. Compared with directly spreading the isolation powder on the green porcelain tape, spraying the isolation powder suspension can ensure that the isolation powder is evenly distributed.

[0046] Specifically, the adhesive can be selected from polyvinyl alcohol (PVA) or polyvinyl butyral (PVB), and the adhesive powder is added to PVA or PVB to form a suspension. The isolation powder suspension is then atomized by an atomizing spray gun and evenly sprayed on the surface of the green porcelain tape to form an isolation layer, which can further ensure the uniformity of the distribution of the isolation powder.

[0047] In an embodiment of the present invention, the parameters of isostatic pressing are: temperature 50-80° C., pressure 50-100 MPa, and holding time 5-20 min.

[0048] In an embodiment of the present invention, sintering includes first-stage sintering, second-stage sintering and temperature reduction treatment;

[0049] The parameters of the first stage sintering are: from room temperature to the first sintering temperature, the heating rate is 0.1-0.5°C / min, the holding time is 4-6h, and the first sintering temperature is 400-1000°C; and / or,

[0050] The parameters of the second stage sintering are: from the first sintering temperature to the second sintering temperature, the heating rate is 0.5-1°C / min, the air flow rate is 1-5L / min, the holding time is 2-4h, and the second sintering temperature is 1450-1600°C; and / or,

[0051] The parameters of the cooling treatment are: from the second sintering temperature to room temperature, the cooling rate is 0.5-1°C / min.

[0052] The first stage of sintering is pre-sintering, which can ensure that the green porcelain tape is completely degreased on the one hand, and prevent the gas generated by the combustion of residual organic matter from forming voids inside on the other hand; the second stage of sintering is a sintering process, and the appropriate heating and cooling rate can reduce the shrinkage and deformation of the substrate, thereby avoiding friction caused by large shrinkage or deformation displacement.

[0053] The present invention limits the air intake flow rate of the second stage sintering. If the air intake flow rate is too large, the airflow will impact the product and affect the product quality; if the air intake volume is too small, the binder will evaporate too slowly, resulting in incomplete volatilization of the binder. When the temperature is raised to the second sintering temperature (high temperature sintering), the un-volatilized binder will form an instantaneous airflow and impact the substrate, thereby affecting the quality of the substrate.

[0054] It should be noted that air or nitrogen is introduced during both the first-stage sintering and the second-stage sintering.

[0055] In an embodiment of the present invention, the method for preparing a ceramic substrate further includes making a green ceramic tape, which specifically includes the following steps:

[0056] Alumina powder and a dispersant are added to a solvent and ground and mixed to obtain slurry I, and then a plasticizer and a binder are added to the slurry I and ground and mixed to obtain slurry II;

[0057] The slurry II is cast to form a green porcelain tape. The thickness of the green porcelain tape can be set to 30-60 μm, which is not specifically limited in the embodiment of the present invention and can be adjusted according to actual needs.

[0058] In an embodiment of the present invention, the addition amount of alumina powder is 40wt%-60wt%, the addition amount of dispersant is 1wt%-3wt%, the addition amount of plasticizer is 2wt%-5wt%, the addition amount of binder is 5wt%-10wt%, and the balance is solvent.

[0059] In the embodiment of the present invention, the purity of the aluminum oxide powder is greater than 99%, and the particle size D 50 is 0.5-1.0 μm; and / or, the dispersant is triolein; and / or, the plasticizer is selected from at least one of dioctyl phthalate and polyethylene glycol; and / or, the binder is polyvinyl butyral; and / or, the solvent is a mixture of alcohol and ester, and the mass ratio of alcohol to ester is 1-3:7-9.

[0060] It should be noted that the particle size D 50 The median diameter or median particle size refers to the particle size corresponding to when the cumulative particle size distribution percentage of the sample reaches 50%. Taking the embodiment of the present invention as an example, in the alumina powder, the particles with a particle size greater than 0.5-1.0 μm account for 50%, and the particles with a particle size less than 0.5-1.0 μm also account for 50%.

[0061] The alumina powder in the embodiment of the present invention is of submicron grade, so that after sintering, the dielectric properties of the ceramic substrate can be improved and defects such as gray spots and white spots on the appearance of the ceramic substrate can be ensured.

[0062] In an embodiment of the present invention, the alcohol is selected from at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol; and / or the ester is selected from at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate.

[0063] The following describes the invention in conjunction with specific embodiments.

[0064] Example 1

[0065] The method for preparing a ceramic substrate comprises the following steps:

[0066] (1) Weigh 1000 g of alumina powder (purity 99.98%, particle size D 50 0.6 μm), 20 g of triolein, 80 g of dioctyl phthalate, 100 g of polyvinyl butyral, and 800 g of solvent (including 240 g of ethanol and 560 g of ethyl acetate);

[0067] (2) adding the weighed alumina powder to the solvent, and then adding triolein, grinding and mixing by a ball mill for 24 hours to obtain slurry I; then adding dioctyl phthalate and polyvinyl butyral to slurry I, grinding and mixing by a ball mill for 24 hours to obtain slurry II;

[0068] (3) Casting slurry II into a 60 μm thick green porcelain tape;

[0069] (4) adding an isolating powder to PVA to prepare a suspension, and then spraying the suspension on the green porcelain tape through an atomizing spray gun to form an isolating layer, wherein the isolating powder is spherical alumina powder with a particle size of 5 μm, and then sequentially stacking the green porcelain tape and the isolating layer, wherein the number of layers of the green porcelain tape is 2, and the surface layer is the green porcelain tape;

[0070] (5) evacuating the laminated green porcelain tape, and placing it in an isostatic press for isostatic pressing after evacuating the vacuum, wherein the isostatic pressing parameters are: temperature 80° C., pressure 80 MPa, and holding time 10 min;

[0071] (6) First stage sintering: heating from room temperature to 500 °C, heating rate 0.2 °C / min, holding time 2 h;

[0072] (7) Second stage sintering: heating from 500°C to 1530°C, air flow rate of 5 L / min, heating rate of 1°C / min, and holding time of 4 h;

[0073] (8) Cooling treatment: cooling from 1530 °C to room temperature, cooling rate 1 °C / min;

[0074] (9) After sintering, the ceramic substrate can be obtained.

[0075] Example 2

[0076] The difference from Example 1 is that the number of layers of the green porcelain tape in this example is 3, and the remaining steps are the same as those in Example 1.

[0077] Example 3

[0078] The difference from Example 1 is that the number of layers of the green porcelain tape in this example is 6, and the remaining steps are the same as those in Example 1.

[0079] Example 4

[0080] The difference from Example 1 is that the particle size of the anti-sticking powder in this example is 10 μm, and the remaining steps are the same as those in Example 1.

[0081] Example 5

[0082] Different from Example 1, the particle size of the insulating and adhesive powder in this example is 10 μm, the number of layers of the green porcelain tape is 3, and the remaining steps are the same as those in Example 1.

[0083] Example 6

[0084] Different from Example 1, the particle size of the insulating and adhesive powder in this example is 10 μm, the number of layers of the green porcelain tape is 6, and the remaining steps are the same as those in Example 1.

[0085] Comparative Example 1

[0086] Different from Example 1, the number of layers of the green porcelain tape in this comparative example is 7, and the remaining steps are the same as those in Example 1.

[0087] Comparative Example 2

[0088] Different from Example 1, the particle size of the septum adhesive powder in this comparative example is 15 μm, the number of layers of the green porcelain tape is 3, and the remaining steps are the same as those in Example 1.

[0089] Comparative Example 3

[0090] Different from Example 1, the particle size of the septum adhesive powder in this comparative example is 15 μm, the number of layers of the green porcelain tape is 6, and the remaining steps are the same as those in Example 1.

[0091] Comparative Example 4

[0092] Different from Example 1, the particle size of the septum adhesive powder in this comparative example is 15 μm, the number of layers of the green porcelain tape is 7, and the remaining steps are the same as those in Example 1.

[0093] Comparative Example 5

[0094] The difference from Example 1 is that the septum adhesive powder in this comparative example is flaky aluminum oxide powder, and the remaining steps are the same as those in Example 1.

[0095] Comparative Example 6

[0096] Different from Example 1, the insulating powder in this comparative example is flaky aluminum oxide powder, the particle size of the insulating powder is 15 μm, the number of layers of the green porcelain tape is 7, and the remaining steps are the same as in Example 1.

[0097] The appearance of the ceramic substrates prepared in the above Examples 1-6 and Comparative Examples 1-6 was evaluated. Specifically, 360 ceramic substrates were prepared in the same batch under various experimental conditions. The appearance of the ceramic substrates was then visually inspected under strong light conditions. The scratch ratio was calculated to determine the proportion of scratched ceramic substrates to the total number of ceramic substrates. The specific results are shown in the following table.

[0098] Table 1 Experimental parameters and results in Examples 1-6 and Comparative Examples 1-6

[0099]

[0100]

[0101] It can be seen from the above table that when spherical alumina is used as the isolating powder, and the particle size of the isolating powder and the number of layers of the green ceramic tape are within the specified range of the present invention, the prepared ceramic substrate has no scratches and the sintering yield reaches 100%.

[0102] By comparing Example 1 and Comparative Example 1, it can be seen that, under the condition that other conditions remain unchanged, when the number of layers of the green porcelain tape is greater than the range specified by the present invention, the ceramic substrate will be scratched. This is because when the number of layers of the green porcelain tape is greater, the pressure on the green porcelain tape located in the lower layer is greater, and when the sintering shrinkage moves, it will produce friction with the isolation powder and cause scratches on the substrate.

[0103] By comparing Examples 1 and 4 with Comparative Example 2, it can be seen that, when other conditions remain unchanged, when the particle size of the isolation powder is larger than the range specified in the present invention, the ceramic substrate will be scratched. This is because when the particle size of the isolation powder is too large, the surface activity of the isolation powder is relatively high, and it is easy to react with the green ceramic tape. When the sintering shrinkage moves, it is easy to produce friction with the isolation powder and cause scratches on the substrate.

[0104] By comparing Example 1 and Comparative Example 5, it can be seen that, when other conditions remain unchanged, when the morphology of the isolation powder changes from spherical to flaky, the ceramic substrate will be scratched. This is because the flaky isolation powder has an irregular morphology and poor fluidity. When the green ceramic tape moves during sintering shrinkage, it is easy to rub against the isolation powder and cause scratches on the substrate.

[0105] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the technical concept of the present invention, or direct / indirect application in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A ceramic substrate, It is characterized in that The ceramic substrate comprises raw ceramic tapes and adhesive-isolating layers stacked alternately, and both the surface layer and the bottom layer of the ceramic substrate are raw ceramic tapes; The number of layers of the green porcelain tape is 2-6; The isolation layer is formed by laying isolation powder, the isolation powder is spherical in shape, and the particle size of the isolation powder is 5-10 μm.

2. The ceramic substrate according to claim 1, It is characterized in that The anti-sticking powder is aluminum oxide powder.

3. A method for preparing a ceramic substrate, It is characterized in that The following steps are involved: Applying isolation powder on the green porcelain tape to form an isolation layer, and then stacking the green porcelain tape and the isolation layer in sequence, controlling the number of stacked layers of the green porcelain tape to be 2-6 layers, and controlling the surface layer to be the green porcelain tape, the morphology of the isolation powder is spherical, and the particle size of the isolation powder is 5-10 μm; The stacked green porcelain tapes are evacuated and then isostatically pressed; The ceramic substrate can be obtained by sintering the green ceramic tape formed by isostatic pressing.

4. The method for preparing a ceramic substrate according to claim 3, It is characterized in that The laying of the isolation powder comprises the following steps: firstly, the isolation powder and the adhesive are mixed into a suspension, and then the suspension is sprayed on the green porcelain tape.

5. The method for preparing a ceramic substrate according to claim 3, It is characterized in that The parameters of the isostatic pressing are: temperature 50-80° C., pressure 50-100 MPa, and holding time 5-20 min.

6. The method for preparing a ceramic substrate according to claim 3, It is characterized in that The sintering includes a first stage sintering, a second stage sintering and a temperature reduction treatment; The parameters of the first stage sintering are: from room temperature to the first sintering temperature, the heating rate is 0.1-0.5°C / min, the holding time is 4-6h, and the first sintering temperature is 400-1000°C; and / or, The parameters of the second stage sintering are: from the first sintering temperature to the second sintering temperature, the heating rate is 0.5-1°C / min, the air flow rate is 1-5L / min, the holding time is 2-4h, and the second sintering temperature is 1450-1600°C; and / or, The parameters of the cooling treatment are: from the second sintering temperature to room temperature, the cooling rate is 0.5-1°C / min.

7. The method for preparing a ceramic substrate according to claim 3, It is characterized in that The method for preparing the ceramic substrate also includes the production of a green ceramic tape, which specifically includes the following steps: Alumina powder and a dispersant are added to a solvent and ground and mixed to obtain slurry I, and then a plasticizer and a binder are added to the slurry I and ground and mixed to obtain slurry II; The slurry II was tape cast to form a green tape.

8. The method for preparing a ceramic substrate according to claim 7, It is characterized in that The addition amount of the alumina powder is 40wt%-60wt%, the addition amount of the dispersant is 1wt%-3wt%, the addition amount of the plasticizer is 2wt%-5wt%, the addition amount of the binder is 5wt%-10wt%, and the balance is solvent.

9. The method for preparing a ceramic substrate according to claim 7 or 8, It is characterized in that The purity of the aluminum oxide powder is greater than 99%, and the particle size D 50 0.5-1.0 μm; and / or, The dispersant is triolein; and / or, The plasticizer is selected from at least one of dioctyl phthalate and polyethylene glycol; and / or, The binder is polyvinyl butyral; and / or, The solvent is a mixture of alcohol and ester, and the mass ratio of the alcohol to the ester is 1-3:7-9.

10. The method for preparing a ceramic substrate according to claim 9, It is characterized in that The alcohol is selected from at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol and isobutanol; and / or, The ester is selected from at least one of ethyl acetate, methyl acetate, propyl acetate and butyl acetate.

Citation Information

Patent Citations

  • Powder laying technology and system for ceramic substrate blank body

    CN108058264A

  • Batch sintering method of high-performance silicon nitride ceramic substrate

    CN112811912A

  • High-purity ultrathin high-strength aluminum oxide ceramic substrate as well as preparation method and application thereof

    CN114538900A