Method for preparing alkali metal vanadate by mechanochemical reaction method

By using mechanochemical reaction method in the solid-solid-liquid three-phase reaction system, alkali metal vanadate was prepared, and the problems of high cost, high energy consumption and low reaction efficiency in the prior art were solved, and the preparation of a full series of alkali metal vanadate was achieved with an efficient and environmentally friendly preparation.

CN120136168APending Publication Date: 2025-06-13TECHNICAL INST OF PHYSICS & CHEMISTRY - CHINESE ACAD OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510314164.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-17
Publication Date
2025-06-13

AI Technical Summary

Technical Problem

The existing vanadate synthesis technology has problems such as high cost, high energy consumption, low reaction efficiency and difficulty in scale, and lacks methods that can prepare alkali metal vanadate in a full range.

Method used

The alkali metal vanadate was prepared by constructing a solid-solid-liquid three-phase reaction system by initiating a reaction under the action of mechanical force. This method does not require high-temperature calcination and traditional organic solvents, and uses mechanical activation to synergize with water molecules to mass transfer.

Benefits of technology

It has achieved efficient preparation of a full range of alkali metal vanadate at room temperature, which is easy to operate, good reproducibility, low energy consumption, environmentally friendly, high product purity and small particle size, which is suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005315440930000011
    Figure HDA0005315440930000011
  • Figure HDA0005315440930000012
    Figure HDA0005315440930000012
  • Figure HDA0005315440930000021
    Figure HDA0005315440930000021
Patent Text Reader

Abstract

The invention discloses a method for preparing alkali metal vanadate by a mechanochemical reaction method. The method comprises the following steps: mixing a vanadium-containing compound and an alkali metal compound according to the stoichiometric ratio of a target product, adding or not adding a protic solvent, and grinding to induce a mechanochemical reaction among the raw materials, so as to obtain the alkali metal vanadate, wherein the alkali metal vanadate is selected from one of NaVO3, KVO3, RbVO3, CsVO3, Rb3V5O14, Cs2V4O11 and Li3VO4, and the alkali metal vanadate is selected from one of NaVO3, KVO3, RbVO3, CsVO3, Rb3V5O14, Cs2V4O11 and Li3VO4. The preparation method has the advantages of being environmentally friendly, low in energy consumption, high in reaction efficiency and the like, efficient preparation of all series of alkali metal vanadate can be achieved, and the obtained alkali metal vanadate is high in purity, small in particle size and good in dispersity and has potential application value in the fields of lithium ion batteries, photocatalysis, laser crystals and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of inorganic material synthesis. More specifically, it relates to a method for preparing alkali metal vanadate by mechanochemical reaction method. Background Art

[0002] Due to their unique crystal structures, tunable oxidation states, and excellent electrochemical properties, vanadate materials have shown important application values in the fields of energy storage, photocatalysis, biomedicine, environmental treatment, etc. For example, in lithium-ion batteries, Li 3 VO 4 is regarded as a candidate for the next-generation anode material due to its high theoretical capacity (394 mAh / g) and low volume expansion rate; in the field of photocatalysis, vanadate materials such as BiVO 4 can achieve visible light response through energy band regulation and are used for the degradation of organic pollutants.

[0003] However, the existing vanadate synthesis technologies still have the following key problems, restricting their large-scale applications: 1) Traditional vanadate synthesis often has high costs. For example, high-temperature solid-phase method requires calcination at >500 °C, with high energy consumption and easy to cause grain agglomeration. For example, CN103496741A discloses a solid-phase reaction method for preparing Li 3 VO 4 anode material. In this method, vanadium pentoxide and lithium carbonate are used as raw materials, ball-milled for 1 - 3 hours, and then sintered at 400 - 700 °C for 1 - 10 hours; 2) Hydrothermal / solvothermal method: relying on organic solvents (such as ethylene glycol), there are problems such as difficult waste liquid treatment, high energy consumption, low reaction efficiency, and it is difficult to scale up. For example, CN103474641A discloses a Li 3 VO 4 anode material and its preparation method. In this method, lithium carbonate, vanadium pentoxide, and hexamethylenetetramine are first subjected to hydrothermal reaction for 10 - 30 hours, and then sintered at 400 - 700 °C for 1 - 10 hours, which not only has high energy consumption but also takes a long time and has low reaction efficiency; 3) Sol-gel method: The precursor has high cost and complex process. For example, in the article "Study on the Synthesis and Electrochemical Properties of LiCuVO 4 ", using CH 3 COOLi·2H 2 O, Cu(NO 3 ) 2 ·3H 2 O, V 2 O 5 and hydrogen peroxide (30%) as raw materials, LiCuVO 4 precursor was synthesized by sol-gel method and LiCuVO 4, the preparation period is about 20h. In addition, in terms of the universality of the preparation method, the existing methods are generally applicable to the preparation of certain alkali metal vanadates, but not applicable to multiple alkali metal vanadates. Different preparation methods are required for different alkali metal vanadates, which obviously increases the research difficulty. At present, there is no relevant method that can complete the preparation of the full series of alkali metal vanadates. Therefore, developing a method for quickly and greenly preparing vanadates is a task of great significance. Summary of the Invention

[0004] To solve the above problems, the purpose of the present invention is to provide a method for preparing alkali metal vanadates by mechanochemical reaction. The present invention innovatively adopts a solid-solid-liquid three-phase reaction system. Under the action of mechanical force, a solid-phase reaction is induced to obtain the target product. This method does not require high-temperature calcination and traditional organic solvents, and combines the synergistic effects of mechanical force activation and water molecule mass transfer, breaking through the kinetic limitations of traditional solid-phase reactions.

[0005] To achieve the above purpose, the present invention adopts the following technical solutions:

[0006] The present invention discloses a method for preparing alkali metal vanadates by mechanochemical reaction, including the following steps:

[0007] Mix a vanadium-containing compound and an alkali metal compound according to the stoichiometric ratio of the target product, with or without adding a proton solvent, and grind to induce a mechanochemical reaction between the raw materials to obtain the alkali metal vanadate;

[0008] Among them, the alkali metal vanadate is selected from one of NaVO 3 , KVO 3 , RbVO 3 , CsVO 3 , Rb 3 V 5 O 14 , Cs 2 V 4 O 11 , Li 3 VO 4 .

[0009] The present invention creatively selects vanadium-containing compounds and alkali metal compounds as the initial raw materials, and forms a solid-solid-liquid three-phase reaction system with a proton solvent. Under the action of mechanical force, alkali metal vanadates are obtained. It should be noted here that the selection of the alkali metal source and its combination with the proton solvent are the keys to the reaction. For alkali metals with relatively strong alkalinity (such as Rb and Cs), a small amount of water in the air can meet the reaction requirements, that is, no additional proton solvent needs to be added; on the contrary, if the alkalinity of the alkali metal is weak, such as Na and Li, a proton solvent needs to be added to carry out the reaction. For potassium, some potassium salts (such as potassium carbonate) need to participate in the reaction with the proton solvent, while some potassium salts (such as potassium hydroxide) do not require the participation of the proton solvent. And the selection of the alkali metal source is also very important. If the alkali metal source is selected improperly, the reaction will not be initiated.

[0010] The reaction involved in the present invention is mainly a double decomposition reaction, and its basic principle is that strong acids and strong bases react to form weak acids and weak bases, which belongs to a spontaneous reaction. Therefore, the alkalinity of the alkali metal source plays a decisive role in the occurrence of the reaction (carbonates cannot prepare orthovanadates with stronger alkalinity). The proton solvent (such as water) plays the role of a catalyst and a solvent therein. The principle is that the proton solvent forms vanadic acid with vanadium oxide and releases H + , and at the same time, the alkali metal source ionizes under the action of the solvent and reacts with H + to finally complete the reaction.

[0011] Furthermore, the proton solvent is added to the reaction system as a reaction medium, including but not limited to one or more of H 2 O, HCOOH, CH 3 COOH, CH 3 CH 2 OH, and the volume ratio of CH 3 CH 2 OH in the proton solvent < 70%. It has been found that if the ethanol content in the proton solvent is too high under the reaction system of the present invention, it is not conducive to the formation of the pure-phase target product.

[0012] Furthermore, the proton solvent is H 2 O, and the water is added in an amount of 0-30 wt% based on the total mass of the vanadium-containing compound and the alkali metal compound.

[0013] Furthermore, the grinding method is selected from manual grinding or grinding with the aid of a grinding device. Grinding with the aid of a grinding device generally requires less time. The grinding device is selected from a planetary ball mill, a vibration mill or a sand mill, and its grinding speed is 200-800 rpm.

[0014] Further, the gas atmosphere for the mechanochemical reaction is air, and the grinding time is 10 - 120 min. If the operation is carried out in a glove box, a proton solvent needs to be added regardless of the type of alkali metal.

[0015] Further, the vanadium-containing compound is selected from vanadium oxides (such as vanadium pentoxide), vanadium hydroxides (V 2 O 5 ·xH 2 O), metavanadates of alkali metals (such as NaVO 3 , KVO 3 , etc.), orthovanadates of alkali metals (such as Na 3 VO 4 , K 3 VO 4 ), ammonium metavanadate, or one or more of them, preferably vanadium pentoxide.

[0016] Further, the alkali metal compound is selected from carbonates of alkali metals (such as sodium carbonate, potassium carbonate, etc.), hydroxides of alkali metals (such as sodium hydroxide, potassium hydroxide, etc.), hydrated hydroxides of alkali metals (such as lithium hydroxide monohydrate, etc.), metavanadates of alkali metals (such as NaVO 3、 , KVO 3 , etc.), orthovanadates of alkali metals (such as Na 3 VO 4 , K 3 VO 4 , etc.), or one or more of them.

[0017] Further, when the alkali metal compound is selected from sodium carbonate, potassium carbonate, lithium hydroxide, sodium hydroxide, or lithium hydrated hydroxide, since the alkalinity of the alkali metal is relatively weak, a proton solvent must be introduced during the reaction, and the proton solvent is added in an amount of 5 - 30 wt% based on the total mass of the vanadium-containing compound and the alkali metal compound; exemplarily, the proton solvent is selected from H 2 O, HCOOH, CH 3 COOH, CH 3 CH 2 OH, or one or more of them, and the volume fraction of CH 3 CH 2 OH in the proton solvent < 70%.

[0018] As an example, the preparation processes of various alkali metal vanadates are provided below:

[0019] 1) Preparation of alkali metal vanadate NaVO 3 , and its preparation steps are specifically as follows:

[0020] Mix the vanadium-containing compound and the alkali metal compound according to the stoichiometric ratio of the target product, that is, the molar ratio of sodium element to vanadium element is 1:1. Add a protonic solvent and grind to induce a mechanochemical reaction between the raw materials to obtain the alkali metal vanadate;

[0021] Among them, the alkali metal compound is selected from one or more of sodium carbonate and sodium hydroxide;

[0022] The vanadium-containing compound is selected from one or more of vanadium oxides, vanadium hydroxides, and ammonium metavanadate;

[0023] The protonic solvent is added according to 5-30 wt% of the total mass of the vanadium-containing compound and the alkali metal compound.

[0024] Further, the protonic solvent is selected from one or more of H 2 O, HCOOH, CH 3 COOH, CH 3 CH 2 OH, and the volume fraction of CH 3 CH 2 OH in the protonic solvent < 70%.

[0025] 2) Prepare alkali metal vanadate KVO 3 , and its preparation steps are specifically as follows:

[0026] Mix the vanadium-containing compound and the alkali metal compound according to the stoichiometric ratio of the target product, that is, the molar ratio of potassium element to vanadium element is 1:1. Add a protonic solvent and grind to induce a mechanochemical reaction between the raw materials to obtain the alkali metal vanadate;

[0027] Among them, the alkali metal compound is selected from one or more of potassium carbonates;

[0028] The vanadium-containing compound is selected from one or more of vanadium oxides, vanadium hydroxides, and ammonium metavanadate;

[0029] The protonic solvent is added according to 5-30 wt% of the total mass of the vanadium-containing compound and the alkali metal compound.

[0030] In the present invention, another method for preparing alkali metal vanadate KVO 3 can also be provided, and its preparation steps are specifically as follows:

[0031] Mix the vanadium-containing compound and potassium hydroxide according to the stoichiometric ratio of the target product, that is, the molar ratio of potassium element to vanadium element is 1:1. When potassium hydroxide is used as the raw material, there is no need to add a protonic solvent. Grind to induce a mechanochemical reaction between the raw materials to obtain the alkali metal vanadate, and other conditions are the same as those of the previous method.

[0032] 3) Preparation of alkali metal vanadate RbVO 3 or CsVO 3 , and its preparation steps are specifically as follows:

[0033] Mix the vanadium-containing compound and the alkali metal compound according to the stoichiometric ratio of the target product, that is, the molar ratio of the alkali metal element to the vanadium element is 1:1. Since the alkali metal has strong alkalinity, a proton solvent can be optionally added or not added, and grinding is used to induce the mechanical chemical reaction between the raw materials to obtain the alkali metal vanadate;

[0034] Among them, the alkali metal compound is selected from one or more of the carbonate of the corresponding alkali metal, the hydroxide of the corresponding alkali metal, and the hydrated hydroxide of the corresponding alkali metal;

[0035] The vanadium-containing compound is selected from one or more of vanadium oxides, vanadium hydroxides, and ammonium metavanadate;

[0036] The proton solvent is added in an amount of 0-30 wt% based on the total mass of the vanadium-containing compound and the alkali metal compound.

[0037] 4) Preparation of alkali metal vanadate Li 3 VO 4 , and its preparation steps are specifically as follows:

[0038] Mix the vanadium-containing compound and the alkali metal compound according to the stoichiometric ratio of the target product, that is, the molar ratio of the Li element to the vanadium element is 1:1, add a proton solvent, and grind to induce the mechanical chemical reaction between the raw materials to obtain the alkali metal vanadate;

[0039] Among them, the alkali metal compound is selected from Li hydroxide and / or Li hydrated hydroxide;

[0040] The vanadium-containing compound is selected from one or more of vanadium oxides, vanadium hydroxides, and ammonium metavanadate;

[0041] The proton solvent is added in an amount of 0-30 wt% based on the total mass of the vanadium-containing compound and the alkali metal compound.

[0042] 5) Preparation of alkali metal vanadate Rb 3 V 5 O 14 or Cs 2 V 4 O 11 , and its preparation steps are specifically as follows:

[0043] Mix the vanadium-containing compound and the alkali metal compound according to the stoichiometric ratio of the target product, that is, the molar ratio of Rb element to vanadium element is 3:5, and the molar ratio of Cs element to vanadium element is 2:4. Optionally, a proton solvent can be added or not added, and mechanical grinding can induce a mechanical chemical reaction between the raw materials to obtain the alkali metal vanadate;

[0044] Among them, the alkali metal compound is selected from one or more of the carbonate of the corresponding alkali metal, the hydroxide of the corresponding alkali metal, the hydrous hydroxide of the corresponding alkali metal, the metavanadate of the corresponding alkali metal, and the orthovanadate of the corresponding alkali metal; if the metavanadate of the corresponding alkali metal or the orthovanadate of the corresponding alkali metal is selected as the initial raw material for preparation, it is only necessary to pay attention to the preparation of the vanadium-containing compound and the alkali metal compound according to the stoichiometric ratio of the target product;

[0045] The vanadium-containing compound is selected from one or more of vanadium oxides, vanadium hydroxides, metavanadates of corresponding alkali metals, orthovanadates of corresponding alkali metals, and ammonium metavanadate;

[0046] The proton solvent is added according to 0-30 wt% of the total mass of the vanadium-containing compound and the alkali metal compound.

[0047] According to whether a proton solvent is introduced or not, the above preparation method can arbitrarily choose to use drying or natural air drying after the reaction to completely volatilize the proton solvent.

[0048] The beneficial effects of the present invention are as follows:

[0049] The present invention provides a method for preparing alkali metal vanadate by mechanical chemical reaction at room temperature. In this method, through the constructed solid-solid-liquid three-phase reaction system (including alkali metal compound + vanadium-containing compound + trace water or moisture in the air), the efficient preparation of the full series of alkali metal vanadates (Li / Na / K / Rb / Cs) is successfully realized by means of mechanical force. Its creativity breaks through the traditional solid-phase reaction kinetic limit through the synergistic effect of mechanical force activation and water molecule mass transfer. The whole preparation method is simple to operate, has good reproducibility, does not require high temperature and a large amount of organic solvents (water can be used as the proton solvent uniformly), has the advantages of environmental friendliness and low energy consumption, and the prepared alkali metal vanadate has a high purity (above 99%), small particle size, and good dispersion, and has good prospects in practical applications. Description of the Drawings

[0050] The following further details the specific embodiments of the present invention with reference to the drawings.

[0051] Figure 1 Shows the XRD pattern of NaVO prepared in Example 1 3 of.

[0052] Figure 2XRD patterns of KVO prepared in Example 2 3 are shown.

[0053] Figure 3 XRD patterns of RbVO prepared in Example 3 3 are shown.

[0054] Figure 4 XRD patterns of CsVO prepared in Example 4 3 are shown.

[0055] Figure 5 XRD patterns of Rb 3 V 5 O 14 prepared in Example 5 are shown.

[0056] Figure 6 XRD patterns of Cs 2 V 4 O 11 prepared in Example 6 are shown.

[0057] Figure 7 XRD patterns of Li 3 VO 4 prepared in Example 7 are shown.

[0058] Figure 8 EDS surface scans of NaVO prepared in Example 1 3 are shown.

[0059] Figure 9 EDS surface scans of KVO prepared in Example 2 3 are shown.

[0060] Figure 10 EDS surface scans of RbVO prepared in Example 3 3 are shown.

[0061] Figure 11 EDS surface scans of CsVO prepared in Example 4 3 are shown.

[0062] Figure 12 EDS surface scans of Rb 3 V 5 O 14 prepared in Example 5 are shown.

[0063] Figure 13 EDS surface scans of Cs 2 V 4 O 11 prepared in Example 6 are shown.

[0064] Figure 14 EDS surface scans of Li prepared in Example 73 VO 4 EDS surface scan of

[0065] Figure 15 showing Rb prepared in Example 5 3 V 5 O 14 Powder second harmonic generation pattern, with the comparative sample being AgGaS@2090nm with a particle size of 20 - 50μm, Rb 3 V 5 O 14 The second harmonic generation effect is about 0.37 times that of the comparative sample.

[0066] Figure 16 showing Cs prepared in Example 6 2 V 4 O 11 Powder second harmonic generation pattern, with the comparative sample being KH₂PO₄@1064nm with a particle size of 50 - 100μm, Cs 2 V 4 O 11 The second harmonic generation effect is about 0.95 times that of the comparative sample. Detailed implementation manners

[0067] To more clearly illustrate the present invention, the present invention will be further described below in conjunction with preferred embodiments and the accompanying drawings. Those skilled in the art should understand that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the protection scope of the present invention.

[0068] Example 1

[0069] This example provides a preparation method of an alkali metal vanadate NaVO 3 The preparation method includes the following steps:

[0070] Manually grind using a mortar. Weigh 1.527 g of sodium hydroxide and 3.473 g of vanadium pentoxide according to the molar ratio of sodium element to vanadium element of 1:1, place them in the mortar, add 1 mL of deionized water, and grind at room temperature in an air atmosphere for 10 min until the reactants completely turn white. After drying at 60°C for 4 h, NaVO 3 powder is obtained. The purity of the product is more than 99% as characterized by XRD (see Figure 1 ).

[0071] Figure 8 Showing the EDS surface scan of NaVO prepared in Example 1 3 The obtained material is irregular particles, with uniform element distribution and no segregation phenomenon.

[0072] Example 2

[0073] This example provides an alkali metal vanadate KVO3 Preparation method, and the preparation method includes the following steps:

[0074] Manually grind using a mortar. Weigh 2.159 g of potassium carbonate and 2.841 g of vanadium pentoxide according to the molar ratio of potassium element to vanadium element being 1:1, place them in the mortar, add 1 mL of deionized water, and grind at room temperature in an air atmosphere for 10 min until the reactants completely turn white. After drying at 60 °C for 4 h, KVO 3 powder is obtained. The purity of the product is over 99% by XRD characterization test (see Figure 2 ).

[0075] Figure 9 Fig. shows the EDS surface scan of KVO prepared in Example 2 3 The obtained material is irregular particles with uniform element distribution and no segregation phenomenon.

[0076] Example 3

[0077] This example provides a preparation method of an alkali metal vanadate RbVO 3 The preparation method includes the following steps:

[0078] Manually grind using a mortar. Weigh 2.797 g of rubidium carbonate and 2.203 g of vanadium pentoxide according to the molar ratio of rubidium element to vanadium element being 1:1, place them in the mortar, add 1 mL of deionized water, and grind at room temperature in an air atmosphere for 10 min until the reactants completely turn white. After drying at 60 °C for 4 h, RbVO 3 powder is obtained. The purity of the product is over 99% by XRD characterization test (see Figure 3 ).

[0079] Figure 10 Fig. shows the EDS surface scan of RbVO prepared in Example 3 3 The obtained material is irregular particles with uniform element distribution and no segregation phenomenon.

[0080] Example 4

[0081] This example provides a preparation method of an alkali metal vanadate CsVO 3 The preparation method includes the following steps:

[0082] Manually grind using a mortar. Weigh 3.209 g of cesium carbonate and 1.791 g of vanadium pentoxide according to the molar ratio of cesium element to vanadium element being 1:1, place them in the mortar, add 1 mL of deionized water, and grind at room temperature in an air atmosphere for 10 min until the reactants completely turn white. After drying at 60 °C for 4 h, CsVO 3 powder is obtained. The purity of the product is over 99% by XRD characterization test (see Figure 4 ).

[0083] Figure 11 The EDS surface scan of CsVO prepared in Example 4 is shown 3 . The obtained material is irregular particles with uniform element distribution and no segregation phenomenon.

[0084] Example 5

[0085] This example provides a preparation method of an alkali metal vanadate Rb 3 V 5 O 14 . The preparation method includes the following steps:

[0086] Manually grind using a mortar. Weigh 2.162 g of rubidium carbonate and 2.838 g of vanadium pentoxide according to the molar ratio of rubidium element to vanadium element of 3:5 and place them in the mortar. Add 1 mL of deionized water and grind at room temperature in an air atmosphere for 10 min until the reactants completely turn red. After drying at 60 °C for 4 h, Rb 3 V 5 O 14 powder is obtained. The purity of the product is more than 99% by XRD characterization test (see Figure 5 ).

[0087] Figure 12 The EDS surface scan of Rb 3 V 5 O 14 prepared in Example 5 is shown. The obtained material is irregular particles with uniform element distribution and no segregation phenomenon.

[0088] Example 6

[0089] This example provides a preparation method of an alkali metal vanadate Cs 2 V 4 O 11 . The preparation method includes the following steps:

[0090] Manually grind using a mortar. Weigh 2.362 g of cesium carbonate and 2.638 g of vanadium pentoxide according to the molar ratio of cesium element to vanadium element of 2:4 and place them in the mortar. Add 1 mL of deionized water and grind at room temperature in an air atmosphere for 10 min until the reactants completely turn yellow. After drying at 60 °C for 4 h, Cs 2 V 4 O 11 powder is obtained. The purity of the product is more than 99% by XRD characterization test (see Figure 6 ).

[0091] Figure 13 The EDS surface scan of Cs 2 V 4 O 11The EDS surface scan image shows that the obtained material is irregular particles with uniform element distribution and no segregation phenomenon.

[0092] Example 7

[0093] This example provides a preparation method of an alkali metal vanadate Li 3 VO 4 , and the preparation method includes the following steps:

[0094] Manually grind using a mortar. Weigh 2.903 g of lithium hydroxide monohydrate and 2.097 g of vanadium pentoxide according to the molar ratio of lithium element to vanadium element of 3:1, place them in the mortar, add 1 mL of deionized water, and grind at room temperature in an air atmosphere for 10 min until the reactants completely turn white. After drying at 60 °C for 4 h, Li 3 VO 4 powder is obtained. The purity of the product characterized by XRD is more than 99% (see Figure 7 ).

[0095] Figure 14 Figure 1 shows the EDS surface scan image of Li 3 VO 4 prepared in Example 7. The obtained material is irregular particles with uniform element distribution. Since the mass of the Li element is relatively light, it cannot be scanned.

[0096] Example 8

[0097] This example provides a preparation method of an alkali metal vanadate KVO 3 , and the preparation method includes the following steps:

[0098] Manually grind using a mortar. Weigh 1.179 g of potassium hydroxide and 3.821 g of vanadium pentoxide according to the molar ratio of potassium element to vanadium element of 1:1 in the mortar, and grind at room temperature in an air atmosphere for 20 min until the reactants completely turn white to obtain KVO 3 powder. The purity of the product characterized by XRD is more than 99%.

[0099] Example 9

[0100] This example provides a preparation method of an alkali metal vanadate RbVO 3 , and the preparation method includes the following steps:

[0101] Manually grind using a mortar. Weigh 2.797 g of rubidium carbonate and 2.203 g of vanadium pentoxide according to the molar ratio of rubidium element to vanadium element of 1:1, place them in the mortar, and grind at room temperature in an air atmosphere for 20 min until the reactants completely turn white to obtain RbVO 3 powder. When no water is added, the grinding time is slightly longer and the reaction can also be complete. The purity of the product characterized by XRD is also more than 99%.

[0102] Example 10

[0103] This example provides a preparation method of alkali metal vanadate CsVO 3 , and its preparation method includes the following steps:

[0104] Manually grind using a mortar. Weigh 3.209 g of cesium carbonate and 1.791 g of vanadium pentoxide according to the molar ratio of cesium element to vanadium element of 1:1, place them in the mortar, and grind at room temperature in an air atmosphere for 20 min to obtain white CsVO 3 powder. The purity of the product characterized by XRD is above 99%.

[0105] Example 11

[0106] This example provides a preparation method of alkali metal vanadate Rb 3 V 5 O 14 , and its preparation method includes the following steps:

[0107] Manually grind using a mortar. Weigh 3.763 g of rubidium metavanadate and 1.237 g of vanadium pentoxide according to the molar ratio of rubidium element to vanadium element of 3:5, place them in the mortar, add 1 mL of deionized water, and grind at room temperature in an air atmosphere for 10 min until the reactants completely turn red. After drying at 60 °C for 4 h, Rb 3 V 5 O 14 powder is obtained. The purity of the product characterized by XRD is above 99%.

[0108] Example 12

[0109] This example provides a preparation method of alkali metal vanadate Cs 2 V 4 O 11 , and its preparation method includes the following steps:

[0110] Manually grind using a mortar. Weigh 3.591 g of cesium metavanadate and 1.409 g of vanadium pentoxide according to the molar ratio of cesium element to vanadium element of 2:4, place them in the mortar, add 1 mL of deionized water, and grind at room temperature in an air atmosphere for 10 min until the reactants completely turn yellow. After drying at 60 °C for 4 h, Cs 2 V 4 O 11 powder is obtained. The purity of the product characterized by XRD is above 99%.

[0111] Comparative Example 1

[0112] This example provides a preparation method of alkali metal vanadate NaVO 3 , and its preparation method includes the following steps:

[0113] Manual grinding was carried out using a mortar. 1.841 g of sodium carbonate and 3.159 g of vanadium pentoxide were weighed according to the molar ratio of sodium element to vanadium element of 1:1 and placed in the mortar. They were ground at room temperature in an air atmosphere for 20 min. No obvious color change was observed, and it was judged that no reaction occurred.

[0114] Comparative Example 2

[0115] This example provides a preparation method of an alkali metal vanadate NaVO 3 The preparation method includes the following steps:

[0116] Manual grinding was carried out using a mortar. 1.527 g of sodium hydroxide and 3.473 g of vanadium pentoxide were weighed according to the molar ratio of sodium element to vanadium element of 1:1 in the mortar. They were ground at room temperature in a glove box (anhydrous and oxygen-free environment) for 20 min. No obvious color change was observed, and it was judged that no reaction occurred.

[0117] Comparative Example 3

[0118] This example provides a preparation method of an alkali metal vanadate KVO 3 The preparation method includes the following steps:

[0119] Manual grinding was carried out using a mortar. 2.159 g of potassium carbonate and 2.841 g of vanadium pentoxide were weighed according to the molar ratio of potassium element to vanadium element of 1:1 in the mortar. They were ground at room temperature in an air atmosphere for 20 min. No obvious color change was observed, and it was judged that no reaction occurred.

[0120] Comparative Example 4

[0121] This example provides a preparation method of an alkali metal vanadate KVO 3 The preparation method includes the following steps:

[0122] Manual grinding was carried out using a mortar. 1.179 g of potassium hydroxide and 3.821 g of vanadium pentoxide were weighed according to the molar ratio of potassium element to vanadium element of 1:1 in the mortar. They were ground at room temperature in a glove box (anhydrous and oxygen-free environment) for 20 min. No obvious color change was observed, and it was judged that no reaction occurred.

[0123] Comparative Example 5

[0124] This example provides a preparation method of an alkali metal vanadate RbVO 3 The preparation method includes the following steps:

[0125] Manual grinding was carried out using a mortar. 2.797 g of rubidium carbonate and 2.203 g of vanadium pentoxide were weighed according to the molar ratio of rubidium element to vanadium element of 1:1 and placed in the mortar. They were ground at room temperature in a glove box (anhydrous and anaerobic environment) for 20 min. No obvious color change was observed, indicating that no reaction occurred.

[0126] Comparative Example 6

[0127] This example provides a preparation method of an alkali metal vanadate CsVO 3 The preparation method includes the following steps:

[0128] Manual grinding was carried out using a mortar. 3.209 g of cesium carbonate and 1.791 g of vanadium pentoxide were weighed according to the molar ratio of cesium element to vanadium element of 1:1 and placed in the mortar. They were ground at room temperature in a glove box (anhydrous and anaerobic environment) for 20 min. No obvious color change was observed, indicating that no reaction occurred.

[0129] Comparative Example 7

[0130] This example provides a preparation method of an alkali metal vanadate Li 3 VO 4 The preparation method includes the following steps:

[0131] Manual grinding was carried out using a mortar. 1.444 g of lithium carbonate and 3.556 g of vanadium pentoxide were weighed according to the molar ratio of lithium element to vanadium element of 3:1 and placed in the mortar. 1 mL of water was added, and they were ground at room temperature in an air atmosphere for 20 min. No obvious color change was observed, indicating that no reaction occurred.

[0132] The performance of the above-prepared samples was tested as follows by way of example.

[0133] Test Example 1

[0134] The Rb 3 V 5 O 14 prepared in Example 5 was subjected to the following powder frequency doubling test:

[0135] The sample was subjected to a powder frequency doubling test using a Q-switched laser with a wavelength of 2090 nm. The AGS crystal was selected as a reference, and the SHG signal was collected using a photomultiplier tube and recorded on a digital oscilloscope. The results are shown in Figure 15 It can be found that the frequency doubling effect of the Rb 3 V 5 O 14 prepared in the present invention is about 0.37 times that of the AGS crystal.

[0136] Test Example 2

[0137] The Cs 2 V4 O 11 The following powder frequency doubling test is carried out:

[0138] The Q-switched laser with a wavelength of 1064 nm is used to conduct the powder frequency doubling test on the sample. The KDP crystal is selected as the reference. The photomultiplier tube is used to collect the SHG signal and record it on the digital oscilloscope. The results are shown in Figure 16 . It can be found that the Cs 2 V 4 O 11 prepared by the present invention has a frequency doubling effect about 0.95 times that of the KDP crystal.

[0139] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, rather than limitations on the implementation manners of the present invention. For those of ordinary skill in the art, other different forms of changes or variations can be made based on the above description. It is impossible to list all the implementation manners here. Any obvious changes or variations derived from the technical solutions of the present invention still fall within the protection scope of the present invention.

Claims

1. A method for preparing alkali metal vanadate by a mechanochemical reaction method, characterized in that: The steps include: The vanadium-containing compound and the alkali metal compound are mixed according to the stoichiometric ratio of the target product, a protic solvent is added or not added, and the mixture is ground to induce a mechanochemical reaction between the raw materials to obtain the alkali metal vanadate; Wherein, the alkali metal vanadate is selected from NaVO3, KVO3, RbVO3, CsVO3, Rb3V5O 14 , Cs2V4O 11 , one of Li3VO4.

2. The method according to claim 1, characterized in that The protic solvent is selected from one or more of H2O, HCOOH, CH3COOH, and CH3CH2OH, and the volume proportion of CH3CH2OH in the protic solvent is less than 70%.

3. The method according to claim 1, characterized in that The protic solvent is H2O, wherein water is added in an amount of 0-30 wt % of the total mass of the vanadium-containing compound and the alkali metal compound.

4. The method according to claim 1, characterized in that: The grinding method is selected from manual grinding or grinding with the aid of a grinding device, wherein the grinding device is selected from a planetary ball mill, a vibration mill or a sand mill, and the grinding speed is 200-800 rpm.

5. The method according to claim 1, characterized in that: The gas atmosphere for the mechanochemical reaction is air, and the grinding time is 10-120 min.

6. The method according to claim 1, characterized in that The vanadium-containing compound is selected from one or more of vanadium-containing oxides, vanadium-containing hydroxides, alkali metal metavanadates, alkali metal orthovanadates, and ammonium metavanadate.

7. The method according to claim 1, characterized in that The vanadium-containing compound is selected from vanadium pentoxide.

8. The method according to claim 1, characterized in that The alkali metal compound is selected from one or more of alkali metal carbonates, alkali metal hydroxides, alkali metal hydrated hydroxides, alkali metal metavanadates, and alkali metal orthovanadates.

9. The method according to claim 8, characterized in that The alkali metal compound is selected from sodium carbonate, potassium carbonate, lithium hydroxide, sodium hydroxide or lithium hydroxide hydrate, and the protic solvent is added at 5-30wt% of the total mass of the vanadium-containing compound and the alkali metal compound.

10. The method according to claim 8, characterized in that The alkali metal compound is selected from rubidium carbonate, cesium carbonate, potassium hydroxide, rubidium hydroxide or cesium hydroxide, and the protic solvent is added according to 0-30wt% of the total mass of the vanadium-containing compound and the alkali metal compound.

Citation Information

Patent Citations

  • Lithium ion battery anode material Li3VO4 and preparation method thereof

    CN103474641A

  • Li3VO4 negative electrode material prepared by solid-phase reaction method

    CN103496741A