Low-internal-resistance lithium ion battery construction method based on graphene-carbon nanotube three-dimensional conductive structure

Through the design of the three-dimensional conductive structure of graphene-carbon nanotubes, the conductive network defects and volume expansion stress problems of traditional lithium-ion batteries are solved, low internal resistance, high energy density and long cycle life are achieved, adapting to extreme environments, and reducing the preparation cost and process complexity.

CN120261726AActive Publication Date: 2025-07-04CHAORONG NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202510418715.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-03
Publication Date
2025-07-04
Estimated Expiration
2045-04-03

AI Technical Summary

Technical Problem

Traditional lithium-ion batteries have problems such as conductive network defects, volume expansion stress, poor adaptability to extreme environments and complexity of the preparation process, resulting in high internal resistance, short cycle life, poor low temperature performance and insufficient high-voltage stability.

Method used

The three-dimensional conductive structure of graphene-carbon nanotubes is adopted, and carbon nanotubes are grown vertically on the graphene surface by chemical vapor deposition. The porous framework is formed by combining high-temperature annealing and nitric acid etching. The electrode structure and electrolyte composition are optimized using iron-manganese oxide catalyst and magnetic field orientation process to form a continuous electron and ion transmission path.

Benefits of technology

Low internal resistance, long cycle life, high energy density and extreme environmental adaptability are achieved. The internal resistance of the battery is reduced to 8mΩ, the capacity attenuation after 2500 cycles is ≤15%, the discharge capacity retention rate at -20℃ is ≥85%, the cost is reduced and the process can be scaled.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120261726A_ABST
    Figure CN120261726A_ABST
Patent Text Reader

Abstract

The invention provides a construction method of a low-internal-resistance lithium ion battery based on a graphene-carbon nanotube three-dimensional conductive structure, which comprises the following steps: step 1, preparation of a three-dimensional conductive composite material: preparing the three-dimensional conductive composite material from graphene oxide (the thickness is 0.8-1.2 nm, and the number of layers is less than or equal to 3), carboxylated carbon nanotubes (the tube diameter is 20-50nm, the thickness is 0.8-1.2 nm, and the number of layers is less than or equal to 3), and the graphene-carbon nanotube three-dimensional conductive composite material is The preparation method comprises the following steps: mixing the raw materials (the length-diameter ratio is greater than or equal to 500) and conductive carbon black (the DBP oil absorption value is greater than or equal to 300cm < 3 > / 100g) according to the mass ratio of (1.5-3): (1-2): (0.5-1), and performing argon protection treatment in a ball mill with the power density being greater than or equal to 200W / L for 2-4 hours to form a premix; the electrochemical performance is improved, the overall internal resistance of the battery is smaller than or equal to 8 m omega (the traditional battery is larger than or equal to 20 m omega), the 5C discharge capacity retention ratio is larger than or equal to 88% (the traditional battery is smaller than or equal to 70%), the mass energy density is larger than or equal to 320 Wh / kg, the volume energy density is larger than or equal to 750 Wh / L, the capacity fading after 2500 times of circulation is smaller than or equal to 15% (the traditional silicon-based battery is smaller than or equal to 500 times), and the 1C discharge capacity at-20 DEG C is larger than or equal to 85% of normal-temperature capacity (the traditional battery is smaller than or equal to 60%). The lithium ion diffusion coefficient is greater than or equal to 1 * 10 <-10 > cm < 2 > / s.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of vehicle-mounted energy systems, and particularly to a method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes. Background Technique

[0002] Traditional lithium-ion batteries face the following key problems:

[0003] Defects in the conductive network: Conventional conductive agents (such as carbon black and carbon fiber) are prone to agglomeration, and the electron / ion transport paths are discontinuous, resulting in a high internal resistance (20 - 25 mΩ) and poor rate performance (5C capacity retention rate ≤ 70%).

[0004] Volume expansion stress: The volume expansion rate of silicon-based anodes during charge and discharge is ≥ 300%, leading to cracking of the electrode sheet and peeling of the active material, and a short cycle life (≤ 500 times).

[0005] High voltage and low temperature bottlenecks:

[0006] At high voltages (≥ 4.35 V), the structure of the cathode material is unstable, and the oxidation and decomposition of the electrolyte are serious (gas production ≥ 0.2 mL / Ah);

[0007] At low temperatures (-20 °C), the ion mobility drops sharply, and the capacity loss is ≥ 40%.

[0008] Process complexity: The preparation of traditional three-dimensional conductive structures relies on noble metal catalysts (such as cobalt) and complex template methods, with high costs and difficulty in large-scale production.

[0009] Therefore, a method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes is proposed. Summary of the Invention

[0010] The present invention aims to solve the problems raised in the background technique, and provides a method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes.

[0011] The specific technical solution is as follows:

[0012] A method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes, comprising the following steps:

[0013] Step 1. Preparation of a three-dimensional conductive composite material:

[0014] Graphene oxide with a thickness of 0.8 - 1.2 nm and ≤ 3 layers, carboxylated carbon nanotubes with a tube diameter of 20 - 50 nm and an aspect ratio of ≥ 500, and a DBP oil absorption value of ≥ 300 cm 3The conductive carbon black per 100 g is mixed in a mass ratio of (1.5 - 3):(1 - 2):(0.5 - 1), and treated in a ball mill with a power density ≥ 200 W / L for 2 - 4 hours under argon protection to form a premix;

[0015] The premix is placed in a tubular furnace. Using acetylene as the carbon source, under the action of an iron-manganese oxide catalyst with a molar ratio of Fe3O4 / MnO2 of 2:1, carbon nanotubes are vertically grown on the surface of graphene by chemical vapor deposition CVD. The reaction temperature is controlled at 650 - 750 °C, the gas flow rate is 50 - 80 sccm, and the growth time is 20 - 40 minutes to form a three-dimensional porous network with a carbon nanotube spacing ≤ 100 nm;

[0016] The product is annealed in an argon atmosphere by heating to 800 - 1200 °C at a rate of 5 - 10 °C / min for 1 - 3 hours, and then immersed in a 30 - 50 wt% nitric acid solution for etching for 30 - 60 minutes to obtain a self-supporting skeleton with a porosity of 85 - 92% and a specific surface area of 1600 - 2000 m 2 / g.

[0017] The above method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure, wherein, it further includes step two, coating of electrode slurry and current collector:

[0018] The 6 - 9 wt% three-dimensional conductive composite material obtained in step one, SiOx@C, where x = 0.8 - 1.2, with a particle size of 80 - 150 nm, 85 - 90 wt% of the silicon-carbon composite negative electrode active material, and a molecular weight ≥ 1×10 6 , 5 - 10 wt% of polyvinylidene fluoride and N-methylpyrrolidone NMP are mixed, and the solid content of the slurry is adjusted to 40 - 50% and the viscosity at 25 °C is 50 - 200 Cp, and homogenized by a three-roll mill;

[0019] The slurry is coated on the surface of a copper foil current collector with a thickness of 8 - 12 μm by a microgravure coating process, and pressed by a double-roll calender under a pressure of 5 - 10 MPa and a temperature of 80 - 100 °C and a magnetic field of 0.5 - 1 T is applied to form a conductive coating with a thickness of 200 - 300 nm and a carbon nanotube orientation degree ≥ 70%.

[0020] The above method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure, wherein, it further includes step three, battery assembly and performance optimization:

[0021] The coated positive and negative electrode sheets and an Al2O3-coated PE separator (thickness 12 μm, porosity 45%) are assembled into ≥ 50 layers by a sandwich laminating process;

[0022] Inject an EC / DMC / EMC electrolyte containing 1 M LiPF6, and add 1.5 wt% FEC, 0.3 wt% LiDFOB, 0.2 wt% BP, and 0.1 wt% TMSP;

[0023] After encapsulation, press it by isostatic pressing at 1.2 MPa for 5 minutes. Finally, the internal resistance of the battery is ≤8 mΩ, and the mass energy density is ≥320 Wh / kg;

[0024] Among them: The positive active material of the positive and negative electrode plates is a gradient doping material of LiNi 0.8 Co 0.1 Mn 0.1 O2 and LiCoO2, with a mass ratio of 6:4; the volume ratio of EC / DMC / EMC is 3:4:3.

[0025] The above method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure, wherein the loading method of the iron-manganese oxide catalyst is:

[0026] Prepare a 0.05-0.1 mol / L precursor solution by mixing Fe(NO3)3·9H2O and Mn(CH3COO)2·4H2O in a molar ratio of Fe:Mn = 2:1;

[0027] Load it onto the surface of graphene by ultrasonic-assisted impregnation method, and form a Fe3O4 / MnO2 composite catalyst with a particle size of 5-10 nm after calcination at 400-500 °C, and the density is (1.5-2.5)×10 4 pieces / μm 2 ;

[0028] Among them: The process parameters of the ultrasonic-assisted impregnation method are: pH = 3-4, ultrasonic frequency 40 kHz, impregnation time ≥2 hours.

[0029] The above method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure, wherein the conductive coating is treated by plasma, and carboxylic acid groups are grafted on the surface of the carbon nanotubes, the contact angle with the electrolyte is ≤25°, and the electron mobility is ≥1200 cm 2 / (V·s);

[0030] Among them, the parameters of the plasma treatment process are: Ar / O2 = 4:1, power 200-300 W, time 5-10 minutes, and the density of -COOH in the carboxylic acid groups is ≥3×10 14 cm -2 .

[0031] The above method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes, wherein, in the silicon-carbon composite negative electrode, the three-dimensional conductive network absorbs ≥80% of the silicon volume expansion stress through the graphene wrinkled structure, so that the capacity retention rate is ≥90% after 200 cycles at 1C;

[0032] Among them, the wrinkling height of the graphene wrinkled structure is 20-50 nm.

[0033] The above method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes, wherein the Co concentration on the surface of the positive electrode gradient doping material is 10-15% higher than that inside, and the combination with the three-dimensional conductive network inhibits the crack propagation of the positive electrode under 4.4V high-voltage cycling, and the capacity decay is ≤3% after 50 cycles.

[0034] The above method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes, wherein the synergistic effect of FEC and LiDFOB in the electrolyte reduces the SEI film impedance by 40%, and the combination of BP and TMSP makes the gas generation amount during 4.45V overcharge ≤0.05 mL / Ah.

[0035] The above method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes, wherein the 1C discharge capacity of the battery at -20°C is ≥85% of the room temperature capacity, and the lithium ion diffusion coefficient is ≥1×10 -10 cm 2 / s.

[0036] The above method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes, wherein the battery cycle life is ≥2500 times, the capacity decay is ≤15%, and the 5C discharge capacity retention rate is ≥88%.

[0037] The present invention has the following beneficial effects:

[0038] The method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes provided by the present invention has the following technical effects:

[0039] 1. Improvement of electrochemical performance:

[0040] Low internal resistance: The overall internal resistance of the battery is ≤8 mΩ (≥20 mΩ for traditional batteries), and the 5C discharge capacity retention rate is ≥88% (≤70% for traditional ones).

[0041] High energy density: The mass energy density is ≥320 Wh / kg, and the volume energy density is ≥750 Wh / L.

[0042] Long cycle life: The capacity decay is ≤15% after 2500 cycles (≤500 cycles for traditional silicon-based batteries).

[0043] 2. Extreme environmental adaptability:

[0044] Low-temperature performance: The discharge capacity at 1C at -20°C is ≥ 85% of the normal-temperature capacity (for traditional batteries ≤ 60%), and the lithium-ion diffusion coefficient is ≥ 1×10-10 cm 2 / s.

[0045] High-voltage stability: After 50 cycles at 4.4V, the capacity attenuation is ≤ 3% (for traditional cathodes ≥ 10%).

[0046] 3. Process and cost advantages:

[0047] Environmentally friendly catalyst: Iron-manganese oxide replaces cobalt-based catalyst, significantly reducing costs;

[0048] Scalability compatibility: Microgravure coating + magnetic field orientation process can achieve continuous production with a high yield rate. Description of the drawings

[0049] Figure 1 It is a flowchart of a method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure provided by an embodiment of the present invention. Detailed implementation manners

[0050] The technical solution of the present invention will be further described below with reference to the drawings and through specific implementation manners.

[0051] Among them, the drawings are only for illustrative purposes, showing only schematic diagrams, not physical diagrams, and cannot be understood as a limitation of this patent; in order to better illustrate the embodiments of the present invention, some components in the drawings will be omitted, enlarged or reduced, and do not represent the size of the actual product; for those skilled in the art, it is understandable that some well-known structures and their descriptions in the drawings may be omitted.

[0052] In the drawings of the embodiments of the present invention, the same or similar reference numerals correspond to the same or similar components; in the description of the present invention, it should be understood that if terms such as "upper", "lower", "left", "right", "inner", "outer", etc. are used to indicate the orientation or positional relationship, it is based on the orientation or positional relationship shown in the drawings, and is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, the terms used to describe the positional relationship in the drawings are only for illustrative purposes and cannot be understood as a limitation of this patent. For those of ordinary skill in the art, the specific meanings of the above terms can be understood according to specific circumstances.

[0053] In the description of the present invention, unless otherwise clearly specified and defined, if terms such as "connection" are used to indicate the connection relationship between components, such terms should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium, and it can be the communication inside two components or the interaction relationship between two components. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0054] Example 1

[0055] The method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure provided in this embodiment is as Figure 1 shown, and includes the following steps:

[0056] Step 1: Preparation of three-dimensional conductive composite material:

[0057] Mix graphene oxide (thickness 0.8 - 1.2 nm, number of layers ≤ 3), carboxylated carbon nanotubes (diameter 20 - 50 nm, length-to-diameter ratio ≥ 500), and conductive carbon black (DBP oil absorption value ≥ 300 cm 3 / 100 g) in a mass ratio of (1.5 - 3):(1 - 2):(0.5 - 1), and treat in a ball mill with a power density ≥ 200 W / L for 2 - 4 hours under argon protection to form a premix;

[0058] Place the premix in a tubular furnace, use acetylene as the carbon source, and under the action of an iron-manganese oxide catalyst (Fe3O4 / MnO2 molar ratio 2:1), vertically grow carbon nanotubes on the surface of graphene through chemical vapor deposition (CVD), control the reaction temperature at 650 - 750 °C, the gas flow rate at 50 - 80 sccm, and the growth time at 20 - 40 minutes to form a three-dimensional porous network with a carbon nanotube spacing ≤ 100 nm;

[0059] Heat the product to 800 - 1200 °C at a rate of 5 - 10 °C / min in an argon atmosphere and anneal for 1 - 3 hours, and then immerse it in a 30 - 50 wt% nitric acid solution for etching for 30 - 60 minutes to obtain a self-supporting skeleton with a porosity of 85 - 92% and a specific surface area of 1600 - 2000 m 2 / g;

[0060] Step 2: Coating of electrode slurry and current collector:

[0061] Mix the three-dimensional conductive composite material (6 - 9 wt%) obtained in Step 1, the silicon-carbon composite negative electrode active material (SiOx@C, x = 0.8 - 1.2, particle size 80 - 150 nm, 85 - 90 wt%), and polyvinylidene fluoride (PVDF, molecular weight ≥ 1 × 10 6, it is mixed with N-methylpyrrolidone (NMP), the solid content of the slurry is adjusted to 40-50%, and the viscosity is adjusted to 50-200 Cp (25 °C), and it is homogenized by a three-roll mill;

[0062] The slurry is coated on the surface of a copper foil current collector (thickness 8-12 μm) by a microgravure coating process, pressed by a two-roll calender (pressure 5-10 MPa, temperature 80-100 °C), and a magnetic field of 0.5-1 T is applied to form a conductive coating with a thickness of 200-300 nm and a carbon nanotube orientation degree ≥70%;

[0063] Step 3: Battery assembly and performance optimization:

[0064] The coated positive and negative electrode plates (the positive electrode active material is LiNi 0.8 Co 0.1 Mn 0.1 O2 and LiCoO2 gradient doping material, mass ratio 6:4) and an Al2O3-coated PE separator (thickness 12 μm, porosity 45%) are assembled into ≥50 layers according to the sandwich lamination process;

[0065] An electrolyte containing 1 M LiPF6 in EC / DMC / EMC (volume ratio 3:4:3) is injected, and 1.5 wt% FEC, 0.3 wt% LiDFOB, 0.2 wt% BP, and 0.1 wt% TMSP are added;

[0066] After encapsulation, it is pressed by isostatic pressing at 1.2 MPa for 5 minutes. Finally, the internal resistance of the battery ≤8 mΩ, and the mass energy density ≥320 Wh / kg.

[0067] This method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes vertically grows carbon nanotubes and graphene composites by CVD method to form a three-level conductive network (graphene-carbon nanotubes-carbon black), greatly shortening the electron conduction path and significantly increasing the conductivity of the composite conductive agent; high-temperature annealing combined with nitric acid etching optimizes the pore structure of the framework, significantly increasing the pore penetration rate and greatly enhancing the ion diffusion rate; magnetic field-induced carbon nanotube oriented coating reduces the interface contact resistance, and the overall internal resistance of the battery ≤8 mΩ.

[0068] Among them, the loading method of the iron-manganese oxide catalyst is:

[0069] Fe(NO3)3·9H2O and Mn(CH3COO)2·4H2O are prepared into a precursor solution with a molar ratio of Fe:Mn = 2:1 and a concentration of 0.05-0.1 mol / L;

[0070] Loaded on the surface of graphene by ultrasonic-assisted impregnation method (pH = 3 - 4, ultrasonic frequency 40 kHz, impregnation time ≥ 2 h), and calcined at 400 - 500 °C to form Fe3O4 / MnO2 composite catalyst with a particle size of 5 - 10 nm, density (1.5 - 2.5)×10 4 pieces / μm 2 .

[0071] The Fe3O4 / MnO2 composite catalyst is uniformly loaded by ultrasonic-assisted impregnation (density ≥ 1.5×10 4 pieces / μm 2 ), enabling a relatively high yield of vertically grown carbon nanotubes and avoiding the breakage of the conductive network caused by the agglomeration of traditional catalysts; the calcination temperature control (400 - 500 °C) makes the catalyst particle size ≤ 10 nm, resulting in a deviation angle of the carbon nanotube growth direction ≤ 5°, greatly improving the three-dimensional network regularity.

[0072] Among them, the conductive coating is treated by plasma (Ar / O2 = 4:1, power 200 - 300 W, time 5 - 10 min), and carboxylic acid groups (-COOH density ≥ 3×10 14 cm -2 ) are grafted on the surface of the carbon nanotubes, the contact angle with the electrolyte ≤ 25°, the electron mobility ≥ 1200 cm 2 / (V·s). The plasma grafting of carboxylic acid groups enhances the surface polarity of the carbon nanotubes, shortening the electrolyte infiltration time to ≤ 10 s (traditional coating ≥ 30 s); the electron mobility ≥ 1200 cm 2 / (V·s), and the interfacial charge transfer impedance is reduced to 0.5 Ω·cm 2 , improving the battery rate performance.

[0073] Among them, in the silicon-carbon composite anode, the three-dimensional conductive network absorbs ≥ 80% of the silicon volume expansion stress through the graphene wrinkled structure (wrinkle height 20 - 50 nm), enabling the capacity retention rate to be ≥ 90% after 200 cycles at 1C. The graphene wrinkled structure (height 20 - 50 nm) absorbs the silicon particle volume expansion stress through elastic deformation, and the crack propagation rate of the electrode sheet ≤ 5% (traditional silicon-carbon anode ≥ 20%); the three-dimensional network provides a continuous electron conduction channel, and the specific capacity of the anode remains ≥ 550 mAh / g after 200 cycles at 1C.

[0074] Among them, the Co concentration on the surface of the positive electrode gradient doping material is 10-15% higher than that inside, combined with the three-dimensional conductive network to inhibit the crack propagation of the positive electrode under 4.4V high-voltage cycling, the capacity attenuation after 50 cycles ≤ 3%, and the high Co concentration on the surface (inside +10-15%) inhibits the phase transition of LiCoO2 under 4.4V high voltage, improving the structural stability of the positive electrode; the three-dimensional conductive network penetrates the gaps between the positive electrode particles, effectively dispersing the charge and discharge stress, and the crack length of the positive electrode particles after 50 high-voltage cycles ≤ 1μm (compared with the non-network structure ≥ 5μm).

[0075] Among them, the synergistic effect of FEC and LiDFOB in the electrolyte reduces the SEI film impedance by 40%, the combination of BP and TMSP makes the gas generation amount during 4.45V overcharge ≤ 0.05mL / Ah, and the synergistic effect of FEC and LiDFOB forms a double-layer SEI film (the inner layer is rich in LiF and the outer layer contains borate), increasing the lithium ion transference number to 0.75 (conventional electrolyte ≤ 0.5); BP and TMSP form a dense CEI film on the surface of the positive electrode, reducing the electrolyte oxidation decomposition rate by 80% during 4.45V overcharge.

[0076] Among them, the 1C discharge capacity of the battery at -20℃ ≥ 85% of the normal temperature capacity, and the lithium ion diffusion coefficient ≥ 1×10 - 10 cm 2 / s. The high porosity penetration (≥ 95%) of the three-dimensional network reduces the ion transport activation energy at low temperature, and the -20℃ discharge efficiency ≥ 85%; the carboxylated carbon nanotube surface provides lithium ion adsorption sites, and the low-temperature lithium deposition overpotential ≤ 50mV (conventional battery ≥ 100mV).

[0077] Among them, the battery cycle life ≥ 2500 times (capacity attenuation ≤ 15%), the 5C discharge capacity retention rate ≥ 88%, the three-dimensional conductive network inhibits the side reaction between the active material and the electrolyte, and the negative electrode lithium inventory loss after 2500 cycles ≤ 8%; the gradient positive electrode and the directional conductive coating work together, and the ear temperature rise ≤ 5℃ during high-rate (5C) cycling (traditional battery ≥ 15℃).

[0078] Experimental data

[0079]

[0080]

[0081] In summary, through the design of the graphene-carbon nanotube three-dimensional conductive structure and multi-dimensional collaborative optimization, this solution achieves a breakthrough in battery performance:

[0082] 1. Construction of three-dimensional conductive network:

[0083] Vertically grown carbon nanotubes: Carbon nanotubes are directionally grown on the surface of graphene by CVD method to form a hierarchical conductive network of "graphene (in-plane conductivity) + carbon nanotubes (vertical conduction) + carbon black (filling micropores)", shortening the electron transport path (conductivity ≥ 500 S / cm).

[0084] Self-supporting porous framework: By combining high-temperature annealing and nitric acid etching, a framework structure with a porosity of 85 - 92% and a through-rate ≥ 95% is formed, providing a fast ion diffusion channel and significantly enhancing the ionic conductivity.

[0085] 2. Interface and structure optimization:

[0086] Magnetic field-induced orientation coating: Apply a magnetic field of 0.5 - 1 T during the coating process to make the carbon nanotubes distributed in a chain-like manner (orientation degree ≥ 70%), effectively reducing the interfacial contact resistance.

[0087] Plasma grafting modification: Introduce carboxylic acid groups (-COOH density ≥ 3×10 14 cm -2 ) on the surface of carbon nanotubes to enhance the electrolyte wettability (contact angle ≤ 25°).

[0088] 3. Material and electrolyte synergy:

[0089] Silicon anode buffer design: The graphene wrinkled structure (height 20 - 50 nm) elastically absorbs the volume expansion stress of silicon, and the crack rate of the electrode sheet is ≤ 5% after 200 cycles.

[0090] High-voltage cathode protection: Gradient-doped cathode material (surface Co concentration +10 - 15%) combined with an electrolyte of FEC + LiDFOB + BP + TMSP multi-additives inhibits the phase change of the cathode and the decomposition of the electrolyte under high voltage (4.4 V) (gas production ≤ 0.05 mL / Ah).

[0091] Technical effects

[0092] 1. Improvement of electrochemical performance:

[0093] Low internal resistance: The overall internal resistance of the battery ≤ 8 mΩ (traditional battery ≥ 20 mΩ), and the capacity retention rate at 5C discharge ≥ 88% (traditional ≤ 70%).

[0094] High energy density: Mass energy density ≥ 320 Wh / kg, volume energy density ≥ 750 Wh / L.

[0095] Long cycle life: The capacity decay is ≤ 15% after 2500 cycles (traditional silicon-based battery ≤ 500 cycles).

[0096] 2. Adaptability to extreme environments:

[0097] Low-temperature performance: The discharge capacity at 1C at -20°C ≥ 85% of the room-temperature capacity (for traditional batteries ≤ 60%), and the lithium-ion diffusion coefficient ≥ 1×10 -10 cm 2 / s.

[0098] High-voltage stability: After 50 cycles at 4.4V, the capacity fade ≤ 3% (for traditional cathodes ≥ 10%).

[0099] 3. Process and cost advantages:

[0100] Environmentally friendly catalyst: Iron-manganese oxides replace cobalt-based catalysts, significantly reducing costs;

[0101] Scalability compatibility: The microgravure coating + magnetic field orientation process can achieve continuous production with a high yield rate.

[0102] The above are only the preferred embodiments of the present invention, and thus do not limit the implementation manners and protection scope of the present invention. For those skilled in the art, it should be realized that any equivalent replacements and obvious changes made by using the description and illustrations of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for constructing a low internal resistance lithium-ion battery based on a three-dimensional conductive structure of graphene-carbon nanotubes, characterized in that, It includes the following steps: Step 1. Preparation of three-dimensional conductive composite material: Graphene oxide with a thickness of 0.8 - 1.2 nm and a number of layers ≤ 3, carboxylated carbon nanotubes with a tube diameter of 20 - 50 nm and a length-to-diameter ratio ≥ 500, and conductive carbon black with a DBP absorption value ≥ 300 cm 3 / 100 g are mixed at a mass ratio of (1.5 - 3):(1 - 2):(0.5 - 1), and processed in a ball mill with a power density ≥ 200 W / L under argon protection for 2 - 4 hours to form a premix; Place the premix in a tubular furnace. Using acetylene as the carbon source, under the action of an iron-manganese oxide catalyst with a molar ratio of Fe3O4 / MnO2 of 2:1, vertically grow carbon nanotubes on the surface of graphene through chemical vapor deposition (CVD). Control the reaction temperature at 650 - 750 °C, the gas flow rate at 50 - 80 sccm, and the growth time at 20 - 40 minutes to form a three-dimensional porous network with a carbon nanotube spacing ≤ 100 nm; The product was annealed at 800 - 1200 °C for 1 - 3 hours with a heating rate of 5 - 10 °C / min in an argon atmosphere, and then immersed in a 30 - 50 wt% nitric acid solution for etching for 30 - 60 minutes to obtain a self-supporting skeleton with a porosity of 85 - 92% and a specific surface area of 1600 - 2000 m 2 / g.

2. The method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure according to claim 1, wherein It also includes Step 2. Coating of electrode paste and current collector: The 6-9 wt% three-dimensional conductive composite material obtained in the first step, SiOx@C, where x = 0.8-1.2 and the particle size is 80-150 nm, 85-90 wt% of the silicon-carbon composite anode active material, and a molecular weight ≥ 1×10 6 , 5-10 wt% of polyvinylidene fluoride and N-methylpyrrolidone NMP are mixed, the solid content of the slurry is adjusted to 40-50%, and the viscosity at 25°C is 50-200 Cp, and homogenization treatment is carried out by a three-roll mill; Use the microgravure coating process to coat the paste on the surface of a copper foil current collector with a thickness of 8 - 12 μm, press it with a double-roll calender under a pressure of 5 - 10 MPa and a temperature of 80 - 100 °C, and apply a magnetic field of 0.5 - 1 T to form a conductive coating with a thickness of 200 - 300 nm and a carbon nanotube orientation degree ≥ 70%; 3. The method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure according to claim 2, wherein It also includes Step 3. Battery assembly and performance optimization: Assemble ≥ 50 layers of the coated positive and negative electrode plates and an Al2O3-coated PE separator (thickness 12 μm, porosity 45%) according to the sandwich lamination process; Inject an electrolyte containing 1 M LiPF6 in EC / DMC / EMC, and add 1.5 wt% FEC, 0.3 wt% LiDFOB, 0.2 wt% BP, and 0.1 wt% TMSP; After encapsulation, press it with an isostatic pressure of 1.2 MPa for 5 minutes. Finally, the internal resistance of the battery ≤ 8 mΩ, and the mass energy density ≥ 320 Wh / kg; Among them: the positive active material of the positive and negative electrode plates is LiNi 0.8 Co 0.1 Mn 0.1 O2 and LiCoO2 gradient doping material, with a mass ratio of 6:4; the volume ratio of EC / DMC / EMC is 3:4:

3.

4. The method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure according to claim 3, wherein The loading method of the iron-manganese oxide catalyst is as follows: Prepare a precursor solution with a concentration of 0.05 - 0.1 mol / L by mixing Fe(NO3)3·9H2O and Mn(CH3COO)2·4H2O in a molar ratio of Fe:Mn = 2:1; Loaded on the surface of graphene by ultrasonic-assisted impregnation method, and after calcination at 400 - 500 °C, a Fe3O4 / MnO2 composite catalyst with a particle size of 5 - 10 nm is formed, with a density of (1.5 - 2.5)×10 4 particles / μm 2 ; Among them: the process parameters of the ultrasonic-assisted impregnation method are: pH = 3 - 4, ultrasonic frequency 40 kHz, and impregnation time ≥ 2 hours.

5. The method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure according to claim 3, wherein The conductive coating is treated by plasma, and carboxylic acid groups are grafted on the surface of carbon nanotubes. The contact angle with the electrolyte is ≤25°, and the electron mobility is ≥1200 cm 2 / (V·s); Among them, the parameters of the plasma treatment process are: Ar / O2 = 4:1, power 200 - 300 W, time 5 - 10 minutes, and the density of -COOH in the carboxylic acid group ≥ 3×10 14 cm -2 .

6. The method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure according to claim 3, characterized in that In the silicon-carbon composite negative electrode, the three-dimensional conductive network absorbs ≥ 80% of the silicon volume expansion stress through the graphene wrinkled structure, so that the capacity retention rate ≥ 90% after 200 cycles at 1C; Among them, the wrinkled height of the graphene wrinkled structure is 20 - 50 nm.

7. The method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure according to claim 3, wherein The Co concentration on the surface of the positive electrode gradient doping material is 10 - 15% higher than that inside, and combined with the three-dimensional conductive network, it inhibits the crack propagation of the positive electrode under a 4.4 V high-voltage cycle, and the capacity decay ≤ 3% after 50 cycles.

8. The method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure according to claim 3, wherein The synergistic effect of FEC and LiDFOB in the electrolyte reduces the SEI film impedance by 40%, and the combination of BP and TMSP makes the gas generation amount during 4.45 V overcharge ≤ 0.05 mL / Ah.

9. The method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure according to claim 3, wherein The battery has a 1C discharge capacity at -20°C ≥ 85% of the room temperature capacity, and a lithium ion diffusion coefficient ≥ 1×10 -10 cm 2 / s.

10. The method for constructing a low internal resistance lithium-ion battery based on a graphene-carbon nanotube three-dimensional conductive structure according to claim 3, wherein, The battery cycle life ≥ 2500 times, the capacity decay ≤ 15%, and the 5C discharge capacity retention rate ≥ 88%.

Citation Information

Patent Citations

  • Composite conductive paste as well as preparation method and application thereof

    CN112331380A

  • Preparation method of graphene composite conductive slurry

    CN113036143A

  • Preparation method and application of graphene-carbon nanotube composite material

    CN116332168A

  • Three-dimensional conductive graphene and carbon nano conductive agent capable of reducing internal resistance of lithium battery

    CN119400862A

  • An odorous air pollutant removing device using both an activated carbon adsorption bed and electric decomposition

    KR1020220168755A

Cited By

  • Preparation method of composite material with carbon nanotubes growing on graphene surface