Process method for manufacturing quartz filter assembly for semiconductor
By manufacturing quartz filters with specific pore structures, the turbulence problem caused by excessive gas flow rate is solved, the stability and cleanliness of semiconductor products are ensured, and the product quality and applicability are improved.
Patent Information
- Application Number
- CN202510514136.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-22
- Publication Date
- 2025-07-18
AI Technical Summary
In the prior art, inserting the quartz tube directly causes the gas flow rate to be too fast, resulting in turbulence, and affects the stability of product quality in the semiconductor reaction vessel.
High-purity quartz sand is used as the substrate to manufacture quartz filters with specific pore structures through vibration screening sorting, mixing with pure water, mold forming, hydrogen and oxygen flame calcining and other processes, and flow testing and cleaning and packaging are carried out to ensure the gas sustained release function.
It realizes stable and slow release of gas, avoids turbulence, improves the quality stability and yield of semiconductor products, and meets the requirements of semiconductor processes for high cleanliness.
Smart Images

Figure CN120328842A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of quartz filter preparation, and specifically to a process method for manufacturing a quartz filter assembly for semiconductors. Background Art
[0002] In the semiconductor manufacturing process, when injecting gas or breaking the vacuum environment in the reaction vessel, the traditional method is to directly insert a quartz tube into the vessel. However, this method has obvious drawbacks. When the gas flow rate is too fast, turbulence will be generated in the vessel, resulting in unstable product quality in the vessel. To solve this problem, a filter assembly that can slow down the gas release is urgently needed to improve the product quality. Summary of the Invention
[0003] Aiming at the deficiencies of the prior art, the present invention provides a process method for manufacturing a quartz filter assembly for semiconductors, which solves the problem that the existing method of directly inserting a quartz tube easily causes the gas flow rate to be too fast.
[0004] To achieve the above objectives, the present invention is realized through the following technical solutions: A process method for manufacturing a quartz filter assembly for semiconductors, including the following steps:
[0005] S1. Select high-purity quartz sand, and screen the quartz sand by vibration to select it as the base material of the quartz filter;
[0006] S2. Prepare pure water through a pure water equipment;
[0007] S3. Weigh the quartz sand according to the size of the quartz filter, and then mix the quartz sand and pure water in proportion and mix evenly;
[0008] S4. Put the pulped quartz sand into a mold for forming, and place the quartz sand in the mold in an oven for shaping;
[0009] S5. Place the shaped quartz sand in the mold, calcine it with a hydrogen-oxygen flame, and let it cool naturally after calcination. After cooling, complete the sintering of the filter;
[0010] S6. Weld a quartz tube with a pre-calculated length to the quartz filter to form a quartz filter assembly;
[0011] S7. According to the drawing requirements, heat and bend the quartz tube section of the quartz filter assembly to the required angle;
[0012] S8. Use a quartz filter flow rate testing device to test the flow rate of the quartz filter;
[0013] S9. Clean and package the qualified quartz filter assembly.
[0014] Preferably, the specific steps of cleaning and packaging in step S9 are as follows: Place the qualified quartz filter assembly in a 5% - 15% hydrofluoric acid solution and soak it for 15 - 45 minutes, then clean it with pure water, dry it, and perform independent packaging on it in a Class 1000 cleanroom.
[0015] Preferably, the mass concentration of the hydrofluoric acid solution in step S9 is 10%, and the soaking time is 30 minutes.
[0016] Preferably, the oven temperature in step S4 is 80°C, and the shaping time is 50 minutes.
[0017] Preferably, the calcination time in step S5 is 40 minutes.
[0018] Preferably, in step S2, the pure water has particulate matter < 1 particle / ml and the common ion content concentration < 1 ppb.
[0019] Preferably, in step S1, the purity of the high-purity quartz sand is 99.999%, and the vibrating screen is 500 - 600 mesh.
[0020] Preferably, in step S7, the heating and bending adopt an oxy-hydrogen flame heating method, the heating temperature is 1100 - 1200°C, and the bending angle is 30° - 150°.
[0021] Beneficial effects
[0022] The present invention provides a process method for manufacturing a quartz filter assembly for semiconductors, having the following
[0023] Beneficial effects:
[0024] By selecting high-purity quartz sand and manufacturing a quartz filter with a specific pore structure through a series of processes, when gas passes through the filter, the pores can slow down the release of the gas, avoiding the formation of turbulence due to too fast gas flow rate. This stable gas flow state can create a uniform and stable reaction environment in the reaction vessel, improving the quality stability and consistency of semiconductor products;
[0025] Using high-purity quartz sand with a purity of up to 99.999% as the base material of the quartz filter, and using pure water (particulate matter < 1 particle / ml, common ion content concentration < 1 ppb) for pulping during the preparation process, impurities are avoided from the source, which ensures that in the semiconductor process, the product will not be contaminated by the impurities of the filter itself, effectively improving the yield rate of semiconductor products;
[0026] Through processes such as die forming and oxy-hydrogen flame calcination, the shape and size of the quartz filter can be precisely controlled. Meanwhile, after welding the quartz tube and the quartz filter to form an assembly, the quartz tube section can be heated and bent to an accurate angle according to the requirements of the drawing. This precise structural forming enables the filter assembly to better adapt to different semiconductor equipment and process requirements, improving the versatility and practicality of the assembly.
[0027] Use a quartz filter flow test device to conduct a flow test on the quartz filter to ensure that the gas release performance of each filter assembly meets the requirements, guaranteeing the consistency and reliability of product performance. After passing the test, soak the quartz filter assembly in hydrofluoric acid solution, then wash it with pure water, dry it, and perform independent packaging in a thousand-class clean room, which can remove impurities and contaminants on the surface of the filter, ensure the cleanliness of the product, and further improve the applicability of the product in semiconductor processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic flow chart of the steps of the present invention.
[0029] Figure 2 It is a schematic structural diagram of the quartz filter assembly of the present invention.
[0030] In the figure, 1. Quartz filter; 2. Quartz tube. DETAILED DESCRIPTION OF THE EMBODIMENTS
[0031] Next, the technical solutions in the embodiments of the present invention will be clearly and completely described in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative efforts shall fall within the protection scope of the present invention.
[0032] Please refer to Figure 1-2 , the present invention provides a technical solution: a process method for manufacturing a quartz filter assembly for semiconductors, including the following steps:
[0033] S1. Select high-purity quartz sand and screen the quartz sand by vibration to serve as the base material of the quartz filter;
[0034] S2. Prepare pure water through a pure water equipment;
[0035] S3. Weigh the quartz sand according to the size of the quartz filter, and then mix the quartz sand and pure water in proportion and mix them evenly;
[0036] S4. Put the pulped quartz sand into a mold for forming and place it in an oven to shape the quartz sand in the mold;
[0037] S5. Place the shaped quartz sand in a mold and calcine it with a hydrogen-oxygen flame. After calcination, let it cool naturally. After cooling, complete the sintering of the filter.
[0038] S6. Weld a quartz tube with a pre-calculated length to the quartz filter to form a quartz filter assembly.
[0039] S7. According to the requirements of the drawing, heat and bend the quartz tube section of the quartz filter assembly to the required angle.
[0040] S8. Use a quartz filter flow rate testing device to test the flow rate of the quartz filter.
[0041] S9. Clean and package the qualified quartz filter assembly after testing.
[0042] By adopting the above technical solution, a complete manufacturing process method for quartz filter components used in semiconductors is constructed, covering all aspects from raw material preparation to final product packaging, ensuring that the filter components can achieve the function of slow gas release, providing reliable technical support for improving the quality of semiconductor products. The filter components manufactured by this process can effectively avoid the turbulence problem caused by too fast gas flow rate in the traditional method, creating a stable reaction environment for semiconductor processes.
[0043] This embodiment is further set as follows. The specific steps of cleaning and packaging in step S9 are: place the qualified quartz filter assembly after testing in a 5% - 15% hydrofluoric acid solution and soak it for 15 - 45 minutes, then wash it with pure water, dry it, and perform independent packaging on it in a thousand-class clean room.
[0044] By adopting the above technical solution, soaking in the hydrofluoric acid solution can remove impurities and contaminants on the surface of the filter, further ensuring surface cleanliness by washing with pure water, and preventing secondary contamination by packaging in a thousand-class clean room, ensuring the cleanliness of the filter components and enabling them to meet the requirements of high cleanliness in semiconductor processes.
[0045] This embodiment is further set as follows. The mass concentration of the hydrofluoric acid solution in step S9 is 10%, and the soaking time is 30 minutes.
[0046] By adopting the above technical solution, the preferred hydrofluoric acid concentration and soaking time can effectively remove impurities on the surface of the filter while avoiding damage to the filter structure caused by excessive etching, balancing the cleaning effect and the protection of the filter, and further improving the product quality and stability.
[0047] This embodiment is further set as follows. The oven temperature in step S4 is 80°C, and the shaping time is 50 minutes.
[0048] By adopting the above technical solution, the setting of the temperature and time can enable the quartz sand to be fully shaped in the mold, initially forming the required shape and providing a stable basis for the subsequent calcination process.
[0049] In this embodiment, it is further set that the calcination time in step S5 is 40 min.
[0050] In this embodiment, it is further set that in step S2, the pure water particulate matter < 1 particle / ml, and the common ion content concentration < 1 ppb.
[0051] By adopting the above technical solution, high-purity pure water can avoid introducing impurities during the pulping process, ensuring that the quartz sand is not contaminated during the pulping and subsequent process.
[0052] In this embodiment, it is further set that in step S1, the purity of the high-purity quartz sand is 99.999%, and the vibrating screen is 500 - 600 mesh.
[0053] By adopting the above technical solution, the high-purity quartz sand ensures the purity of the filter from the source, avoiding the contamination of semiconductor products by impurities. The particle size range of 500 - 600 mesh enables the quartz sand to form a uniform pore structure after sintering, which is beneficial to realizing the slow-release function of gas and improving the performance and quality of the filter component.
[0054] In this embodiment, it is further set that in step S7, the heating and bending adopt the oxy-hydrogen flame heating method, the heating temperature is 1100 - 1200 °C, and the bending angle is 30° - 150°.
[0055] Those skilled in the art should connect the components in this case in sequence. For the specific connection and operation sequence, reference should be made to the following working principle. The detailed connection means are well-known techniques in this field. The following mainly introduces the working principle and process.
[0056] Embodiment: A process method for manufacturing a quartz filter component for semiconductors includes the following steps:
[0057] Screening quartz sand: Select high-purity quartz sand with a purity of 99.999%. Use a vibrating screen to separate quartz sand with a particle size of 500 - 600 mesh as the base material of the quartz filter. The quartz sand with a particle size of 500 - 600 mesh can ensure that the pores of the quartz filter meet the requirements for slow-releasing gas after sintering.
[0058] Preparation of pure water: Through a pure water equipment, the prepared pure water has particulate matter < 1 particle / ml (particle size ≥ 0.22 μm) and common ion content concentration < 1 ppb. Using plasma water can ensure the purity of the quartz filter after the quartz sand is pulped and formed.
[0059] Pulping: Weigh the quartz sand according to the size of the quartz filter, and then mix the quartz sand and pure water in proportion and mix them evenly.
[0060] Forming: Put the pulped quartz sand into a mold for forming and place it in an 80°C oven for 50 minutes. Shape the quartz sand in the mold.
[0061] Sintering: Place the shaped quartz sand taken out in a mold and calcine it with a hydrogen-oxygen flame for 40 minutes. After calcination, let it cool naturally. After cooling, complete the sintering of the filter.
[0062] Butt welding: Weld a quartz tube with a pre-calculated length to the quartz filter to form a quartz filter assembly.
[0063] Bending of the filter assembly: Heat the quartz tube according to the drawing requirements and bend the quartz filter assembly to the required angle.
[0064] Testing: Use a quartz filter flow test device to test the flow rate of the quartz filter.
[0065] Cleaning and packaging: Immerse the qualified quartz filter assembly in a 10% hydrofluoric acid solution for 30 minutes, then clean it with pure water, dry it, and independently package it in a thousand-class dust-free room.
[0066] It should be noted that in this article, relational terms such as first and second are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the term "comprising", "including" or any other variant thereof is intended to cover non-exclusive inclusion, so that a process, method, article or device comprising a series of elements not only includes those elements, but also includes other elements not expressly listed, or also includes elements inherent to such process, method, article or device. Without further limitation. An element defined by the statement "comprising a..." does not exclude the existence of additional identical elements in the process, method, article or device comprising the element.
[0067] Although the embodiments of the present invention have been shown and described, for those of ordinary skill in the art, it can be understood that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention. The scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A process method for manufacturing a quartz filter component for semiconductors, characterized in that, It includes the following steps: S1. Select high-purity quartz sand, and screen the quartz sand through vibration to select it as the base material of the quartz filter; S2. Prepare pure water through a pure water equipment; S3. Weigh the quartz sand according to the size of the quartz filter, and then mix the quartz sand and pure water in proportion and mix them evenly; S4. Put the pulped quartz sand into a mold for forming, and place the quartz sand in the mold in an oven for shaping; S5. Place the shaped quartz sand in the mold, calcine it with a hydrogen-oxygen flame, naturally cool it after calcination is completed, and complete the sintering of the filter after cooling; S6. Weld a quartz tube with a pre-calculated length to the quartz filter to form a quartz filter assembly; S7. According to the requirements of the drawing, heat and bend the quartz tube section of the quartz filter assembly to the required angle; S8. Use a quartz filter flow rate test device to test the flow rate of the quartz filter; S9. Carry out cleaning and packaging treatment on the qualified quartz filter assembly after testing.
2. The manufacturing process method of a quartz filter component for semiconductor use according to claim 1, characterized in that, The specific steps of cleaning and packaging in step S9 are: place the qualified quartz filter assembly after testing in a 5% - 15% hydrofluoric acid solution and soak it for 15 - 45 minutes, then clean it with pure water, dry it, and perform independent packaging on it in a thousand-class dust-free room.
3. A manufacturing process method for a quartz filter assembly for semiconductors according to claim 2, characterized in that, In step S9, the mass concentration of the hydrofluoric acid solution is 10%, and the soaking time is 30 minutes.
4. A manufacturing process method for a quartz filter assembly for semiconductors according to claim 3, characterized in that, In step S4, the oven temperature is 80°C, and the shaping time is 50 minutes.
5. A manufacturing process method of a quartz filter assembly for semiconductors according to claim 1, characterized in that, In step S5, the calcination time is 40 minutes.
6. A process method for manufacturing a quartz filter assembly for semiconductors according to claim 1, characterized in that, In step S2, the pure water has particle matter < 1 particle / ml, and the concentration of common ion content < 1 ppb.
7. A manufacturing process method for a quartz filter assembly for semiconductors according to claim 1, characterized in that, In step S1, the purity of the high-purity quartz sand is 99.999%, and the vibrating screen is 500 - 600 mesh.
8. A manufacturing process method for a quartz filter assembly for semiconductors according to claim 1, characterized in that, In step S7, the heat bending adopts a hydrogen-oxygen flame heating method, the heating temperature is 1100 - 1200°C, and the bending angle is 30° - 150°.
Citation Information
Patent Citations
Water permeable material and preparation method thereof
CN107349686A
Quartz filter sheet and preparation method thereof
CN108101573A
Manufacturing method of polishing grindstone and polishing grindstone
CN113830997A
Cordierite-based diesel particulate filter and preparation method thereof
CN118637898A
Air cleaning method and high purity silicon filter
JP1993057136A
Cited By
A method for manufacturing a gas dispersion nozzle for a semiconductor process chamber
CN122502091B