Semi-solid injection-molded high-strength corrosion-resistant magnesium alloy and preparation method thereof

By introducing specific elements and optimized processes, high-strength corrosion-resistant magnesium alloys are prepared, which solves the oxidation and corrosion problems of magnesium alloys in the fields of aerospace and new energy vehicles, and achieves high-strength and high corrosion resistance semi-solid injection molding effect.

CN120330557APending Publication Date: 2025-07-18SHENZHEN RES INST OF SHANGHAI JIAOTONG UNIV +1
View PDF 0 Cites 7 Cited by

Patent Information

Application Number
CN202510666106.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-22
Publication Date
2025-07-18

AI Technical Summary

Technical Problem

The application of existing magnesium alloys in aerospace and new energy vehicles is subject to oxidation and corrosion problems caused by chemical activity, and traditional processes are difficult to take into account high strength and high corrosion resistance, and there are problems of high production costs and many defects.

Method used

By introducing specific proportions of Al, Zn, RE and Ca elements, combined with semi-solid injection molding technology, a high-strength corrosion-resistant magnesium alloy is prepared to form a mesh β-Mg17Al12 phase and dense MgO/CaO composite oxide film, and the heat treatment process is optimized to improve performance.

Benefits of technology

High strength and high corrosion resistance for molding at low temperatures are achieved. The yield strength of semi-solid injection molded castings is ≥180MPa, tensile strength ≥280MPa, elongation ≥8%, and neutral salt spray corrosion rate ≤0.24mm/y, which solves the problems of insufficient strength and poor corrosion resistance in practical applications of traditional magnesium alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120330557A_ABST
    Figure CN120330557A_ABST
Patent Text Reader

Abstract

The invention discloses a semi-solid injection-molded high-strength corrosion-resistant magnesium alloy and a preparation method thereof. The magnesium alloy comprises the following components in percentage by mass: 7%-8.5% of Al, 1%-4% of Zn, 0.1%-0.8% of RE, 0.02%-0.5% of Ca and the balance of Mg and inevitable impurities. Through component design and process optimization, the liquidus temperature of the alloy is lower than 610 DEG C, and the alloy is insensitive to temperature in the solid fraction interval of 20-40% and is suitable for semi-solid injection molding; the Al content is controlled to form a net-shaped Mg17Al12 phase as a corrosion barrier, and Zn and RE / Ca cooperate to achieve heat treatment strengthening and oxidation film densification. The problem that strength and corrosion resistance of a traditional magnesium alloy are difficult to consider at the same time is solved, and the magnesium alloy is suitable for high-performance light-weight components of automobiles, aerospace and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of metal material processing, and particularly relates to a high-strength and corrosion-resistant magnesium alloy for semi-solid injection molding and a preparation method thereof, which are particularly suitable for lightweight and high-performance components such as automotive structural parts and electronic device housings. Background Art

[0002] As a lightweight material, magnesium alloy has irreplaceable application value in fields such as aerospace and new energy vehicles. However, its industrialization process faces multiple technical bottlenecks: First, magnesium alloy has active chemical properties, and the surface oxide film is loose and porous, and it is extremely easy to occur pitting corrosion in humid or saline environments, seriously restricting its large-scale application; Second, there is a contradiction that the corrosion resistance and strength of traditional magnesium alloys are difficult to be improved synergistically. The reason is that most of the second phases that play a strengthening effect in magnesium alloys have a corrosion potential higher than that of the magnesium matrix, which will cause serious micro-galvanic corrosion and make it difficult to form a dense protective film on the alloy surface. In addition, in traditional casting processes (such as die casting), due to the high-speed filling of the melt, gas is easily involved, forming pore defects, and the high temperature of the magnesium melt increases the risk of oxidation and combustion, and it is necessary to rely on inert gas protection to increase production costs.

[0003] The semi-solid injection molding technology realizes near-net shaping by controlling the alloy in the solid-liquid coexistence state. The molding temperature is lower than the liquidus, which can greatly reduce the oxidation and combustion tendency of the magnesium melt. At the same time, laminar filling reduces gas entrapment defects. However, this process puts strict requirements on the alloy system: it also has a certain solidification range (20 °C) at a solid fraction of 20% - 40% to ensure the fluidity of the slurry, and a fine and uniform semi-solid structure to ensure mechanical properties. Existing commercial magnesium alloys (such as AZ and AM series) have a wide solidification range and excellent fluidity, and are ideal materials suitable for semi-solid injection molding, but their mechanical properties and corrosion resistance are usually not satisfactory. Therefore, developing a new semi-solid injection molding magnesium alloy composition system with both high strength and high corrosion resistance has become a major direction to break through the technical barriers of lightweight materials. Summary of the Invention

[0004] In view of the above problems, the present invention provides a high-strength and corrosion-resistant magnesium alloy for semi-solid injection molding and a preparation method thereof through composition design and process innovation to solve the problems existing in the above-mentioned prior art.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention:

[0007] A high-strength and corrosion-resistant magnesium alloy for semi-solid injection molding, by mass percentage, includes: Al: 7% - 8.5%, Zn: 1% - 4%, RE: 0.1% - 0.8%, Ca: 0.02% - 0.5%, and the balance is Mg and unavoidable impurities.

[0008] The present invention introduces elements Al, Zn, RE, and Ca in specific proportions, which can improve the strength of the magnesium alloy while enhancing its corrosion resistance. Specifically, the purpose of controlling the lower limit of the Al content at 7% is to ensure that the second phase can form a continuous network-like β-Mg 17 Al 12 phase to block the corrosion path. The purpose of controlling the upper limit of the Al content at 8.5% is to avoid a sharp drop in plasticity caused by excessive Al; the purpose of the Zn content being greater than 1% is to precipitate the MgZn phase through T6 heat treatment aging to enhance the strength. The reason for the upper limit of the Zn content not exceeding 4% is to ensure that there is still a certain solidification interval (20 °C) at a solid fraction of 20% - 30%, which is suitable for semi-solid injection molding. If the Zn content is too high, it will lead to a too wide solidification interval and easily cause hot cracking; the RE element is controlled at 0.1% - 0.8% to control the ratio of it to Al atoms at 0.25 - 0.5 to form high melting point phases such as Al2RE / Al 11 RE3, effectively refining the grains; adding a trace amount of 0.02% - 0.5% Ca aims to promote the solid solution of Ca in the magnesium matrix during forming, and form a dense MgO / CaO composite oxide film during oxidation.

[0009] The RE is selected from one or more of La, Ce, Y, and Sm.

[0010] The second technical solution of the present invention:

[0011] A preparation method of a semi-solid injection molded high-strength and corrosion-resistant magnesium alloy as described above, comprising the following steps:

[0012] S1. Under a protective atmosphere, the magnesium-based alloy raw materials are subjected to high-temperature melting treatment, refined and purified, and then cast into a mold to obtain a magnesium alloy ingot;

[0013] S2. The magnesium alloy ingot is processed into magnesium alloy particles, and a gradient heating-holding process is implemented to obtain a semi-solid slurry in which a liquid phase and a spherical solid phase are evenly distributed;

[0014] S3. The semi-solid slurry is injected into the mold cavity at high speed, demolded after cooling and solidification, and a T6 solution aging heat treatment process is implemented on the formed part; the semi-solid injection molded high-strength and corrosion-resistant magnesium alloy is obtained.

[0015] In S1, the magnesium-based alloy raw materials include pure Mg, pure Al, pure Zn, Mg-RE master alloy, and Mg-Ca master alloy.

[0016] As an embodiment of the present invention, S1 is specifically as follows: Under an argon atmosphere, pure Mg, pure Al, pure Zn, Mg-RE master alloy, and Mg-Ca master alloy are heated and held at 700 - 760 °C. After complete melting, they are stirred, refined and purified, and then left standing for 20 - 30 minutes before being poured into a mold for cooling to obtain a magnesium alloy ingot.

[0017] S2 is specifically as follows: The above-mentioned magnesium alloy ingot is processed into millimeter-sized magnesium alloy particles with uniform particle size, and then quantitatively transported into the barrel of a metal thixotropic injection machine. Through the spiral shear propulsion of the conveying rod, it is gradually heated and held (the heating temperature and holding time are set according to the properties of the raw materials, aiming to heat and stir the mixture to form a semi-solid state with a certain liquid phase ratio), so that the raw material metal is heated to a semi-solid melt to form a semi-solid slurry with uniform distribution of liquid phase and spherical solid phase.

[0018] S3. Implementing the T6 solution aging heat treatment process for the formed part includes the following steps: In the first stage, it is heated to 375 - 385 °C at a rate of 10 - 15 °C / min and held for 3.5 - 4.5 h. After water quenching in the second stage, it is aged at 190 - 210 °C for 10 - 14 h.

[0019] In S1, the particle size of the magnesium alloy particles is between 1 - 5 mm.

[0020] The speed of the spiral shear propulsion of the conveying rod described in S2 is 150 r / min - 250 r / min.

[0021] The liquid phase ratio in the semi-solid slurry described in S2 is controlled between 60 - 80%.

[0022] The injection speed of the semi-solid slurry by the injection machine in S3 is 4 m / s - 8 m / s, and the mold temperature is 250 - 350 °C.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention provides a high-strength and corrosion-resistant magnesium alloy with a liquidus temperature lower than 610 °C, and also has a solidification range of ~20 °C at a solid phase ratio of 20% - 40%, which is suitable for forming by semi-solid injection molding technology, avoiding the problems of insufficient strength and poor corrosion resistance brought by traditional casting methods. The semi-solid formed casting prepared has a yield strength ≥180 MPa, a tensile strength ≥280 MPa, an elongation ≥8%, and a neutral salt spray corrosion rate ≤0.24 mm / y after T6 heat treatment, providing an effective solution to the problems of insufficient strength and poor corrosion resistance encountered by traditional magnesium alloys in practical applications. Description of the Drawings

[0025] Other features, objects, and advantages of the present invention will become more apparent from the following detailed description of non - limiting embodiments read in conjunction with the accompanying drawings:

[0026] Figure 1 Schematic diagram of the microstructure of the alloy in Example 1;

[0027] Figure 2 Schematic diagram of the microstructure of the alloy in Example 2;

[0028] Figure 3 Schematic diagram of the microstructure of the alloy in Comparative Example 1;

[0029] Figure 4 Schematic diagram of the microstructure of the alloy in Comparative Example 2;

[0030] Figure 5 Schematic diagram of the microstructure of the alloy in Comparative Example 3. Detailed implementation manners

[0031] The present invention will be described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but do not limit the present invention in any form. It should be noted that for those of ordinary skill in the art, without departing from the concept of the present invention, several adjustments and improvements can still be made. These all fall within the protection scope of the present invention.

[0032] In the following embodiments and comparative examples:

[0033] A BOLE MTX3000 metal thixotropic injection molding machine is used.

[0034] Mechanical property test method: After heat treatment, the specimens are subjected to room - temperature mechanical property testing on a universal testing machine (Zwick / Roell Z100) equipped with a contact extensometer at a strain rate of 1 mm / min to obtain the yield strength, tensile strength, and elongation of the material.

[0035] Corrosion rate test method: The specimens after heat treatment are wire - cut into specimens with dimensions of 40×40×3 mm. After the surface is polished to be bright, they are placed in a salt - spray corrosion chamber (AOTSI - 90H) for a 7 - day corrosion experiment under neutral 5 wt.% NaCl salt - spray conditions to measure the corrosion rate of the material.

[0036] Example 1

[0037] This example provides a high - strength and corrosion - resistant semi - solid injection - molded magnesium alloy, which includes the following components in mass percentages: Al: 7%, Zn: 1%, RE (0.2% La + 0.2% Y + 0.1% Sm): 0.5%, Ca: 0.2%, and the balance is Mg and unavoidable impurities; its preparation method is as follows:

[0038] S1. Under the protection of argon gas, pure Mg, pure Al, pure Zn, Mg-RE master alloy, and Mg-Ca master alloy are heated and held at 760 °C. After complete melting and sufficient stirring, they are refined and purified. After standing for 20 minutes, they are quickly poured into a metal mold for air cooling to obtain a magnesium alloy ingot;

[0039] S2. The above magnesium alloy ingot is processed into 5-mm magnesium alloy particles with uniform particle size, and then quantitatively conveyed into the barrel of a metal thixotropic injection machine. Through the spiral shearing and propulsion of the conveying rod, the speed of the spiral shearing and propulsion of the conveying rod is 200 r / min, and step-by-step heating and holding are carried out to heat the raw metal to a semi-solid melt, forming a semi-solid slurry with uniform distribution of liquid phase and spherical solid phase, and the liquid fraction is 70%;

[0040] S3. The semi-solid slurry is ejected at a high speed of 5 m / s through an injection machine, the mold temperature is 250 °C, and after molding and cooling in the mold, the mold is opened to take out the part.

[0041] S4. The taken-out casting is subjected to T6 heat treatment. The specific process parameters are as follows: in the first stage, it is heated to 370 °C at a rate of 10 °C / min and held for 4 h. After water quenching in the second stage, it is aged at 200 °C for 12 h.

[0042] Measure the mechanical properties and corrosion rate in the T6 heat treatment state. The corresponding metallographic structure is shown in Figure 1 . The yield strength of the T6 heat treatment state sample is 182 MPa, the tensile strength is 295 MPa, the elongation is 8.1%, and the corrosion rate is 0.19 mm / y.

[0043] Example 2

[0044] This example provides a high-strength and corrosion-resistant semi-solid injection-molded magnesium alloy, which includes the following components in weight percentages: Al: 8.5%, Zn: 4%, RE(0.2% Y + 0.1% Sm): 0.3%, Ca: 0.3%, and the balance is Mg and unavoidable impurities; its preparation method is as follows:

[0045] S1. Under the protection of argon gas, pure Mg, pure Al, pure Zn, Mg-RE master alloy, and Mg-Ca master alloy are heated and held at 740 °C. After complete melting and sufficient stirring, they are refined and purified. After standing for 30 minutes, they are quickly poured into a metal mold for air cooling to obtain a magnesium alloy ingot;

[0046] S2. Process the above magnesium alloy ingot into 5-mm magnesium alloy particles with uniform particle size, and then quantitatively convey them into the barrel of a metal thixotropic injection machine. Through the spiral shearing and propulsion of a conveying rod at a speed of 250 r / min, gradually heat and keep warm to heat the raw metal to a semi-solid melt, forming a semi-solid slurry with a uniform distribution of liquid phase and spherical solid phase, and the liquid fraction is 75%.

[0047] S3. High-speed inject the semi-solid slurry through an injection machine at a speed of 6 m / s, with the mold temperature at 300 °C. After molding and cooling in the mold, open the mold to take out the part.

[0048] S4. Perform T6 heat treatment on the taken-out casting. The specific process parameters are as follows: in the first stage, heat up to 370 °C at a rate of 10 °C / min and keep warm for 4 h. After water quenching in the second stage, age at 200 °C for 12 h. The corresponding metallographic structure is shown in Figure 2

[0049] Measure the mechanical properties and corrosion rate in the T6 heat-treated state. The yield strength is 195 MPa, the tensile strength is 309 MPa, the elongation is 8%, and the corrosion rate is 0.23 mm / y.

[0050] Comparative Example 1

[0051] This comparative example provides a high-strength and corrosion-resistant semi-solid injection molding magnesium alloy, including the following components in weight percentages: Al: 7%, Zn: 0.2%, RE (0.2% La + 0.2% Y + 0.1% Sm): 0.5%, Ca: 0.2%, and the balance is Mg and inevitable impurities; its preparation method is the same as that of Example 1. The corresponding metallographic structure is shown in Figure 3 。

[0052] Measure the mechanical properties and corrosion rate in the T6 heat-treated state. The yield strength is 175 MPa, the tensile strength is 282 MPa, the elongation is 5.8%, and the corrosion rate is 0.21 mm / y. Compared with Example 1 and Example 2, the yield strength of Comparative Example 1 is significantly reduced because the Zn content is too low and no MgZn phase precipitates during the aging process; the elongation is significantly reduced because the Al content is too high, forming a large amount of Mg 17 Al 12 phase, which deteriorates the plasticity.

[0053] Comparative Example 2

[0054] This comparative example provides a high-strength and corrosion-resistant semi-solid injection molding magnesium alloy, including the following components in weight percentages: Al: 9%, Zn: 4%, RE (0.2% La + 0.2% Y + 0.1% Sm): 0.5%, Ca: 0.2%, and the balance is Mg and inevitable impurities; its preparation method is the same as that of Example 1. The corresponding metallographic structure is shown in Figure 4 。

[0055] Measure the mechanical properties and corrosion rate of the T6 heat-treated state. The yield strength is 168 MPa, the tensile strength is 276 MPa, the elongation is 6.1%, and the corrosion rate is 0.22 mm / y. Compared with Example 1, the yield strength of Comparative Example 3 is significantly reduced because too high Al content forms a large amount of Mg 17 Al 12 phase, which deteriorates plasticity.

[0056] Comparative Example 3

[0057] This comparative example provides a high-strength and corrosion-resistant semi-solid injection molding magnesium alloy, including the following components by weight percentage: Al: 8.5%, Zn: 4%, RE(0.2% Y + 0.1% Sm): 0.3%, Ca: 0.01%, and the balance is Mg and unavoidable impurities; its preparation method is the same as that of Example 1. The corresponding metallographic structure is shown in Figure 5 .

[0058] Measure the mechanical properties and corrosion rate of the T6 heat-treated state. The yield strength is 184 MPa, the tensile strength is 300 MPa, the elongation is 8%, and the corrosion rate is 0.36 mm / y. Compared with Example 1 and Example 2, the corrosion rate of Comparative Example 2 is significantly increased because the Ca content is too low to form a dense MgO / CaO composite oxide film.

[0059] The specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various deformations or modifications within the scope of the claims, which does not affect the essence of the present invention.

Claims

1. A semi-solid injection molding high-strength and corrosion-resistant magnesium alloy, characterized in that The magnesium alloy by mass percentage includes: Al: 7% - 8.5%, Zn: 1% - 4%, RE: 0.1% - 0.8%, Ca: 0.02% - 0.5%, and the balance is Mg and inevitable impurities.

2. The semi-solid injection molded high-strength and corrosion-resistant magnesium alloy according to claim 1, wherein The RE is selected from one or more of La, Ce, Y, and Sm.

3. A preparation method of a semi-solid injection molding high-strength and corrosion-resistant magnesium alloy as described in claim 1, characterized in that, It includes the following steps: S1. Under a protective atmosphere, the magnesium-based alloy raw materials are subjected to high-temperature melting treatment, refined and purified, and then cast into shape to obtain a magnesium alloy ingot. S2. The magnesium alloy ingot is processed into magnesium alloy particles, and a gradient heating-holding process is implemented to obtain a semi-solid slurry with a uniform distribution of liquid phase and spherical solid phase. S3. The semi-solid slurry is injected into the mold cavity at high speed, demolded after cooling and solidification, and the formed part is subjected to a T6 solution aging heat treatment process to obtain the semi-solid injection-molded high-strength and corrosion-resistant magnesium alloy.

4. The preparation method of the semi-solid injection molding high-strength and corrosion-resistant magnesium alloy according to claim 3, characterized in that, In S1, the magnesium-based alloy raw materials include pure Mg, pure Al, pure Zn, Mg-RE master alloy, and Mg-Ca master alloy.

5. The preparation method of the semi-solid injection molding high-strength and corrosion-resistant magnesium alloy according to claim 3, characterized in that, S1 is specifically: Under an argon atmosphere, pure Mg, pure Al, pure Zn, Mg-RE master alloy, and Mg-Ca master alloy are heated and held at 700 - 760 °C. After complete melting, they are stirred, refined and purified, and left standing for 20 - 30 minutes, and then poured into a mold for cooling to obtain a magnesium alloy ingot.

6. The preparation method of the semi-solid injection molded high-strength and corrosion-resistant magnesium alloy according to claim 3, wherein, S2 is specifically: The above-mentioned magnesium alloy ingot is processed into millimeter-sized magnesium alloy particles with uniform particle size, and then transported to the barrel of a metal thixotropic injection machine. Through the spiral shearing and propulsion of the conveying rod, heating and holding are carried out to heat the raw metal to a semi-solid melt, forming a semi-solid slurry with a uniform distribution of liquid phase and spherical solid phase.

7. The preparation method of the semi-solid injection molded high-strength and corrosion-resistant magnesium alloy according to claim 3, characterized in that, In S3, implementing the T6 solution aging heat treatment process for the formed part includes the following steps: In the first stage, it is heated to 375 - 385 °C at a rate of 10 - 15 °C / min and held for 3.5 - 4.5 h. After water quenching in the second stage, it is aged at 190 - 210 °C for 10 - 14 h.

8. The preparation method of the semi-solid injection molded high-strength and corrosion-resistant magnesium alloy according to claim 3, characterized in that, The particle size of the magnesium alloy particles is between 1 and 5 mm.

9. The preparation method of the semi-solid injection molding high-strength and corrosion-resistant magnesium alloy according to claim 6, characterized in that, The speed of the spiral shearing and propulsion of the conveying rod is 150 r / min - 250 r / min.

10. The preparation method of the semi-solid injection molding high-strength and corrosion-resistant magnesium alloy according to claim 6, wherein, The injection speed of the semi-solid slurry by the injection machine is 4 m / s - 8 m / s, and the mold temperature is 250 - 350 °C.

Citation Information

Cited By

  • Magnesium alloy automobile front end upper cross beam and manufacturing method

    CN120922246A

  • Magnesium alloy large component semi-solid injection molding microstructure control method and application

    CN121892645A

  • Magnesium alloy large component semi-solid injection molding microstructure control method and application

    CN121892645B

  • Injection-casting high-Zn magnesium alloy based on two-stage corrosion-resistant barrier and preparation method of injection-casting high-Zn magnesium alloy

    CN121951276A

  • High-zn magnesium alloy based on two-stage corrosion-resistant barrier and preparation method thereof

    CN121951276B