Optimized electrode interface area for alkaline batteries

By optimizing the relationship between interface area and membrane thickness in alkaline battery packs, the difficulty of performance optimization of alkaline battery packs in high- and low-speed applications is solved, and the efficient use of the battery under different loads is achieved.

CN120500778APending Publication Date: 2025-08-15ENERGIZER BRANDS LLC
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202480008232.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-01-18
Filing Date
2024-01-12
Publication Date
2025-08-15

AI Technical Summary

Technical Problem

Alkaline battery packs are difficult to balance performance optimization in high- and low-ratio applications. Existing designs reduce low-ratio performance when increasing the interface area to improve high-ratio performance, and thinner diaphragms can cause structural integrity issues.

Method used

By optimizing the relationship between the interface area and the separator thickness between the anode and the cathode, it is defined within a specific range to achieve a balance between high and low magnification performance of the electrochemical cell. The specific relationship includes a combination of the membrane thickness between 0.1 mil and 18 mils and the interface area within different ranges.

Benefits of technology

The performance optimization of electrochemical batteries in high- and low-magnification applications is achieved, and the average ANSI performance is within 8% of the maximum theoretical performance, improving the overall use efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120500778A_ABST
    Figure CN120500778A_ABST
Patent Text Reader

Abstract

An electrochemical cell is provided. An exemplary electrochemical cell may include a container; an electrolyte; an anode; a cathode; a current collector; and a separator disposed between the anode and the cathode. In some embodiments, the anode and the cathode may define an interfacial area y, and the separator may define a thickness x, where a relationship between the interfacial area y and the separator thickness x is defined between # imgabs0 #.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-reference to related applications

[0002] This application claims priority to U.S. non-provisional patent application No. 18 / 156,178, filed on January 18, 2023, entitled “Optimized Electrode Interface Area for Alkaline Batteries,” the contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] The present disclosure relates generally to alkaline batteries and, more particularly, to optimizing the interfacial area between electrodes in alkaline batteries.

[0004] background

[0005] Alkaline battery performance (e.g., runtime) varies depending on whether the battery is used for low-rate (e.g., low current draw) or high-rate (e.g., high current draw) applications. For low-rate applications, the active materials within the anode and cathode of alkaline batteries have been observed to have a relatively high depth of discharge (i.e., a significant amount of active material is discharged even at a relatively large distance from the interface region between the anode and cathode). However, the runtime of alkaline batteries used for high-rate discharge applications depends on the interfacial area between the anode and cathode within the electrochemical cell. Furthermore, the anode and cathode within an alkaline electrochemical cell must be electrically separated by a separator of non-negligible thickness to avoid short circuits. Therefore, increasing the interfacial area between the anode and cathode proportionally increases the volume of the separator within the electrochemical cell. Because alkaline electrochemical cells are generally limited to industry-standard cell sizes (e.g., LR6, LR03, etc.), the amount of active material added to the cell must be reduced to accommodate any increase in separator volume. Therefore, adjusting alkaline electrochemical cell design to maximize high-rate performance (e.g., run time) can reduce low-rate performance (e.g., run time), at least in part due to the reduction in active material caused by increasing the interfacial area and, therefore, the volume of separator material in the cell. This effect on low-rate performance can be mitigated by using thinner separator materials (which occupy less volume), however, thinner separators can suffer from structural integrity issues, including perforation during electrochemical cell fabrication and the potential for internal short circuiting during discharge.

[0006] In reality, consumers use the same electrochemical cell for both high-rate and low-rate applications. Therefore, optimizing the interfacial area is necessary to achieve optimal performance for both high-rate and low-rate discharge in alkaline battery packs. Summary of the Invention

[0007] Generally, embodiments of the present disclosure provide electrochemical cells and / or the like.

[0008] According to various embodiments, an electrochemical cell is provided that includes a container; an electrolyte; an anode; a cathode; a current collector; and a separator disposed between the anode and the cathode, wherein the anode and the cathode define an interfacial area y, and the separator defines a thickness x, and wherein the relationship between the interfacial area y and the separator thickness x is defined by between.

[0009] In some embodiments, the relationship between the interfacial area y and the membrane thickness x is defined as between.

[0010] In some embodiments, the relationship between the interfacial area y and the membrane thickness x is defined as between.

[0011] According to various embodiments, an electrochemical cell is provided, comprising a container; an electrolyte; an anode; a cathode; a current collector; and a separator disposed between the anode and the cathode, wherein the anode and the cathode define an interfacial area and the separator defines a thickness, and wherein the separator thickness is selected from a first group of between 0.1 mil and 1 mil, a second group of between 1 mil and 5 mils, a third group of between 5 mils and 10 mils, and a fourth group of between 10 mils and 18 mils.

[0012] In some embodiments, the membrane thickness is selected from the first group between 0.1 mil and 1 mil, and the interfacial area is selected from the first group between 27 and 1346 cm 2 between groups.

[0013] In some embodiments, the membrane thickness is selected from the first group between 0.1 mil and 1 mil, and the interfacial area is selected from the first group between 32 and 959 cm 2 between groups.

[0014] In some embodiments, the membrane thickness is selected from the first group between 0.1 mil and 1 mil, and the interfacial area is selected from the first group between 39 and 716 cm 2 between groups.

[0015] In some embodiments, the membrane thickness is selected from the second group between 1 mil and 5 mils, and the interfacial area is selected from the second group between 21 and 285 cm 2 between groups.

[0016] In some embodiments, the membrane thickness is selected from the second group between 1 mil and 5 mils, and the interfacial area is selected from the second group between 24 and 225 cm 2 between groups.

[0017] In some embodiments, the membrane thickness is selected from the second group between 1 mil and 5 mils, and the interfacial area is selected from the second group between 27 and 183 cm 2 between groups.

[0018] In some embodiments, the membrane thickness is selected from the third group between 5 mils and 10 mils, and the interfacial area is selected from the third group between 19 and 96 cm 2 between groups.

[0019] In some embodiments, the membrane thickness is selected from the third group between 5 mils and 10 mils, and the interfacial area is selected from the third group between 21 and 82 cm 2 between groups.

[0020] In some embodiments, the membrane thickness is selected from the third group between 5 mils and 10 mils, and the interfacial area is selected from the third group between 23 and 71 cm 2 between groups.

[0021] In some embodiments, the membrane thickness is selected from the fourth group between 10 mils and 18 mils, and the interfacial area is selected from the fourth group between 17 and 60 cm 2 between groups.

[0022] In some embodiments, the membrane thickness is selected from the fourth group between 10 mils and 18 mils, and the interfacial area is selected from the fourth group between 19 and 53 cm 2 between groups.

[0023] In some embodiments, the membrane thickness is selected from the fourth group between 10 mils and 18 mils, and the interfacial area is selected from the fourth group between 20 and 47 cm 2 between groups.

[0024] According to various embodiments, an electrochemical cell is provided that includes a container; an electrolyte; an anode; a cathode; a current collector; and a separator disposed between the anode and the cathode, wherein the anode and the cathode define an interfacial area, wherein the interfacial area is selected so that the electrochemical cell has an average ANSI performance within 8% of the maximum theoretical performance of the electrochemical cell, wherein the separator is provided. The maximum theoretical performance is defined by Theoretical electrochemical cell realization with defined interfacial area.

[0025] In some embodiments, the electrochemical cell has an average ANSI performance that is within 5% of the maximum theoretical performance of the electrochemical cell.

[0026] In some embodiments, the electrochemical cell has an average ANSI performance that is within 3% of the maximum theoretical performance of the electrochemical cell.

[0027] The above summary is provided only to summarize some exemplary aspects to provide a basic understanding of some aspects of the present disclosure. Therefore, it is to be understood that the above aspects are merely examples. It is to be understood that in addition to those aspects summarized herein, the scope of the present disclosure also includes many potential aspects, some of which will be further described below. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Having generally described the present disclosure, reference will now be made to the accompanying drawings, which are not necessarily drawn to scale, and in which:

[0029] Figure 1 is a side cross-sectional elevation view of an exemplary electrochemical cell design according to some embodiments;

[0030] Figure 2A and 2B is a radial cross-sectional view of an exemplary jellyroll electrode assembly according to some embodiments, wherein Figure 2A Shows cathode outer wrap design, Figure 2B Shows anode outsourcing design;

[0031] Figure 3 shows a discharge curve of an exemplary electrochemical cell according to some embodiments;

[0032] Figure 4 、 5 , 6 and 7 graphically illustrate the relationship between run time, active material input and discharge efficiency and inter-electrode interface area in alkaline cells according to some embodiments;

[0033] Figure 8 shows electrochemical cell performance measured relative to interfacial area according to some embodiments;

[0034] Figure 9 shows electrochemical cell performance and optimized interfacial area according to some embodiments; and

[0035] Figure 10 、 11 12 show the maximum performance and optimized interfacial area of various electrochemical cells as measured by interfacial area and separator thickness according to some embodiments. DETAILED DESCRIPTION

[0036] Various embodiments will now be described more fully below with reference to the accompanying drawings, some but not all of which are shown. In fact, the various embodiments can be embodied in many different forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided so that this disclosure satisfies applicable legal requirements. Similar reference numerals always represent similar elements. In the following description, various components may be identified as having specific values or parameters, however, these items are provided as exemplary embodiments. In fact, the exemplary embodiments do not limit the various aspects and concepts of the embodiments, as many comparable parameters, sizes, ranges and / or values may be achieved. The terms "first", "second", etc., "primary", "exemplary", "minor", etc. do not indicate any order, quantity or importance, but are used to distinguish one element from another. In addition, the terms "a", "an", and "the" do not indicate a limit on the quantity, but rather indicate the presence of "at least one" of the items mentioned. For example, an "organic additive" without specifying a specific number may refer to two or more organic additives.

[0037] Each embodiment disclosed herein is considered applicable to each of the other disclosed embodiments, to the extent they are not explicitly mutually inconsistent. All combinations and subcombinations of the various elements described herein are within the scope of the embodiments.

[0038] It is to be understood that where parameter ranges are provided, the embodiments also provide all integers and ranges within the range, as well as tenths, hundredths, thousandths, ten thousandths, and hundred thousandths thereof. For example, "5-10%" includes 5%, 6%, 7%, 8%, 9%, and 10%; 5.0%, 5.1%, 5.2% ... 9.8%, 9.9%, and 10.0%; and 5.00%, 5.01%, 5.02% ... 9.98%, 9.99%, and 10.00%, as well as, for example, 6-9%, 7-10%, 5.1%-9.9%, and 5.01%-9.99%. As another example, "0.00001-1 M" includes 0.00005-0.0001 M and 0.001-0.01 M.

[0039] As used herein, "about" in the context of a numerical value or range means within ±10% of the recited or claimed numerical value or range.

[0040] As used herein, "run time" refers to the length of time that an electrochemical cell is able to provide a certain level of charge.

[0041] As used herein, unless otherwise indicated, the terms listed below are defined and used throughout this disclosure as follows:

[0042] Ambient or Room Temperature – Between about 20° C. and about 25° C. Unless otherwise stated, all examples, data, and other performance and manufacturing information are performed at ambient temperature and normal atmospheric conditions.

[0043] Anode—the negative electrode, serving as the primary electrochemically active material, an exemplary primary active material being zinc.

[0044] Capacity—The capacity delivered by a single electrode or the entire cell during discharge under a specified set of conditions (e.g., drain rate, temperature, etc.); typically expressed in milliampere-hours (mAh) or milliwatt-hours (mWh), or in minutes or images captured in a digital still camera (DSC) test. As discussed herein, capacity can be expressed and / or measured at low-rate discharge or high-rate discharge.

[0045] Cathode—positive electrode; in some embodiments, the active material of the cathode can be manganese dioxide (MnO2), such as electrolytic manganese dioxide (EMD).

[0046] Battery housing—the structure that physically encloses the electrode assembly (e.g., anode, cathode, separator, and current collector). The battery housing contains all internally enclosed safety devices, inert components, and interconnecting materials that comprise a functionally complete battery; typically, these include a container (formed in a cup shape, also called a "can" or "receptacle") and a closure (fits over the opening of the container and typically includes venting and sealing mechanisms to prevent electrolyte egress and moisture / atmospheric ingress); sometimes used interchangeably with the terms can or container, depending on the context.

[0047] Cylindrical Battery Dimensions – Any battery housing having a cylindrical shape with a height greater than its diameter;

[0048] Electrochemically active material—one or more chemical compounds that are part of the battery discharge reaction and contribute to the battery discharge capacity, but include impurities and other small amounts of moieties inherent to the material;

[0049] LR6 or AA size batteries - Zinc-manganese dioxide (Zn-MnO2) batteries with cylindrical cell dimensions of approximately 50.5 mm and a maximum outer diameter of approximately 14.5 mm, as referenced by international standard IEC-60086-1 published by the International Electrotechnical Commission after November 2000;

[0050] LR03 or AAA size batteries - Zinc-manganese dioxide (Zn-MnO2) batteries with cylindrical cell dimensions of approximately 44.5 mm and a maximum outer diameter of approximately 10.5 mm, as referenced by international standard IEC-60086-1 published by the International Electrotechnical Commission after November 2000;

[0051] Interfacial area—the surface area between the anode and cathode;

[0052] "Jellyroll" (or "spirally wound") electrode assemblies—anode and cathode strips and appropriate separators are combined into an assembly by winding them along their length or width (e.g., around a mandrel or central core);

[0053] exist Figure 1 In FIG, cell 10 is shown as one embodiment of an LR6 (AA) cylindrical Zn—MnO2 battery cell, although the present disclosure is similarly applicable to LR03 (AAA) or other cylindrical cells. Cell 10, in one embodiment, has a housing comprising a container in the form of a can 12 having a closed bottom and an open top, which is closed by a cell cover 14 and a gasket 16. Can 12 has a bead or reduced diameter step near the top to support gasket 16 and cover 14. Gasket 16 is compressed between can 12 and cover 14 to seal anode or negative electrode 18, cathode or positive electrode 20, and electrolyte within cell 10.

[0054] The anode 18, cathode 20, and separator 26 are spirally wound together to form an electrode assembly. The cathode 20 has a metal current collector 22 that extends from the top of the electrode assembly and is connected to the inner surface of the lid 14 via a contact spring 24. The anode 18 is electrically connected to the inner surface of the can 12 via a metal lead (or tab) 36. The lead 36 is fastened to the anode 18, extends from the bottom of the electrode assembly, and spans the bottom and folds upward along the side of the electrode assembly. The lead 36 is in pressure contact with the inner surface of the side wall of the can 12. It should be understood that this configuration is merely exemplary, and in other embodiments, the cathode can be in electrical contact with the can and the anode can be in electrical contact with the lid. In such embodiments, the physical structure of the can and lid can vary (for example, the positive terminal bump (pip) shown as integrated with the lid can be integrated with the can, and the lid can have a generally flat configuration). After the electrode assembly is wound, it may be held together prior to insertion by using tooling during the manufacturing process, or the exterior of the material (eg, separator or polymer film overwrap 38) may be secured by, for example, heat sealing, gluing, or taping.

[0055] In the illustrated embodiment, an insulating cone 46 is located around the peripheral portion of the top of the electrode assembly to prevent the cathode current collector 22 from contacting the can 12, and contact between the bottom edge of the cathode 20 and the bottom of the can 12 is prevented by an inwardly folded extension of the separator 26 and an electrically insulating bottom disk 44 located at the bottom of the can 12.

[0056] In one embodiment, the battery 10 has a separate positive terminal cap 40 that is held in place by the inwardly curled top edge of the can 12 and the gasket 16 and has one or more vent holes (not shown). The can 12 serves as the negative contact terminal. An insulating jacket, such as an adhesive label 48, may be applied to the sidewall of the can 12.

[0057] In one embodiment, a positive temperature coefficient (PTC) device 42 is disposed between the peripheral flange of the terminal cover 40 and the cell cover 14 to substantially limit the flow of current under abusive electrical conditions. In another embodiment, the cell 10 may also include a pressure relief vent. The cell cover 14 has an aperture containing an inwardly projecting central vent shaft 28 with vent holes 30 at the bottom of the shaft 28. The aperture is sealed by a vent ball 32 and a thin-walled thermoplastic sleeve 34 compressed between the vertical walls of the vent shaft 28 and the periphery of the vent ball 32. When the internal pressure of the cell exceeds a predetermined level, the vent ball 32, or both the ball 32 and the sleeve 34, are forced out of the aperture to release pressurized gas from the cell 10. In other embodiments, the pressure relief vent can be a hole enclosed by a rupture membrane as disclosed in U.S. Patent Application Publication Nos. 20050244706 and 20080213651 (which are incorporated herein by reference in their entireties), or a relatively thin area, such as a coined groove, which can be torn or otherwise broken to form a vent in a portion of the battery, such as a sealing plate or container wall.

[0058] In one embodiment, the terminal portion of the electrode lead 36 disposed between the side of the electrode assembly and the side wall of the tank can have a preferably non-planar shape before the electrode assembly is inserted into the tank, which enhances electrical contact with the side wall of the tank and provides a spring-like force to bias the lead toward the side wall of the tank. During battery manufacturing, the shaped terminal portion of the lead can be deformed, for example, toward the side of the electrode assembly to facilitate its insertion into the tank, after which the terminal portion of the lead can partially rebound toward its initial non-planar shape, but remain at least partially compressed to apply force to the inner surface of the side wall of the tank, thereby achieving good physical and electrical contact with the tank. Alternatively, this connection and / or other connections within the battery can be maintained by welding.

[0059] The battery container may in some embodiments be a metal can with a closed bottom, such as Figure 1 The canister material and container wall thickness depend in part on the active materials and electrolyte used in the battery. A common material type is steel. For example, the canister may be made of cold rolled steel (CRS) and may be nickel plated on at least the outside to protect the outside of the canister from corrosion. The type of plating can be varied to provide varying degrees of corrosion resistance, improve contact resistance, or provide a desired appearance. The type of steel depends in part on how the canister is formed. For die-drawn cans, the steel may be diffusion-annealed, low-carbon, aluminum-killed SAE 1006 or equivalent with an ASTM 9 to 11 grain size and an equiaxed, slightly elongated grain shape. Other steels, such as stainless steel, may be used to meet specific needs. For example, when the canister is in electrical contact with the cathode, stainless steel may be used to improve resistance to corrosion caused by the cathode and electrolyte.

[0060] The battery cover can be metal. Nickel-plated steel can be used, but stainless steel is generally ideal, especially when the closure and cover are in electrical contact with the cathode. The complexity of the cover shape is also a factor in material selection. The battery cover can have a simple shape, such as a thick flat disk, or it can have a more complex shape, such as Figure 1 When the cover has the Figure 4 When the complex shape shown in , can use 304 type soft annealed stainless steel with ASTM 8-9 grain size to provide required corrosion resistance and metal formability. The formed cover can also be nickel plated, or made of stainless steel or other known metals and their alloys.

[0061] Terminal covers should have good resistance to corrosion from water or other corrosive substances commonly found in the surrounding environment during battery manufacturing and use, good electrical conductivity, and, when visible on consumer batteries, an attractive appearance. Terminal covers are typically made of nickel-plated cold-rolled steel or steel that is nickel-plated after the cover is formed. In cases where the terminals are located above the pressure relief holes, the terminal covers typically have one or more holes to facilitate venting of the battery.

[0062] The gasket for improving the seal between the jar and the closure / terminal cover can be made of any suitable thermoplastic material that provides required sealing properties. The material selection part is based on the electrolyte composition. The example of suitable material comprises polypropylene, polyphenylene sulfide, tetrafluoride-perfluoroalkyl vinyl ether copolymer, polybutylene terephthalate and combination thereof. Preferred gasket materials comprise polypropylene (for example, from Basell Polyolefins in Wilmington, Del., USA's PRO-FAX® 6524) and polyphenylene sulfide (for example, from Chevron Phillips in The Woodlands, Tex., USA's XTEL™ XE3035 or XE5030). Also a small amount of other polymers, reinforcing inorganic fillers and / or organic compounds can be added to the base resin of the gasket. The example of suitable material is found in U.S. Patent Publication Nos. 20080226982 and 20050079404, which are incorporated herein by reference.

[0063] The gasket may be coated with a sealant to provide an optimum seal. Ethylene propylene diene terpolymer (EPDM) is a suitable sealant material, but other suitable materials may be used.

[0064] The anode comprises a mixture of one or more active materials, a conductive material, optionally solid zinc oxide, and a surfactant. The negative electrode may optionally include other additives, such as binders or gelling agents. Zinc is an exemplary primary active material for the negative electrode of embodiments. Preferably, the volume of active material used in the negative electrode is sufficient to maintain the desired interparticle contact and the desired anode:cathode (A:C) ratio. In some embodiments, the anode may comprise micron-sized zinc particles suspended in a concentrated potassium hydroxide (KOH) / water gel electrolyte.

[0065] Interparticle contact should be maintained throughout the useful life of the battery. If the active material volume in the negative electrode is too low, the battery's voltage may suddenly drop to unacceptably low values when the battery is powering a device. The voltage drop is believed to be caused by a loss of continuity in the conductive matrix of the negative electrode. The conductive matrix can be formed by undischarged active material particles, conductive electrochemically formed oxides, or a combination thereof. The voltage drop may occur after the oxide begins to form but before a sufficient network is established to bridge all active material particles present.

[0066] Zinc suitable for use in the embodiments can be purchased from many different commercial sources under various names, such as BIA 100, BIA 115. Umicore SA, Brussels, Belgium is an example of a zinc supplier. In a preferred embodiment, the zinc powder typically has 25 to 40% fines less than 75 μm, preferably 28 to 38% fines less than 75 μm. Generally, lower percentages of fines make it impossible to achieve the desired DSC service, while using higher percentages of fines can result in increased gassing. The correct zinc alloy is required to reduce negative electrode gassing in the battery and maintain test service results.

[0067] A surfactant is typically present in the anode and is either a nonionic or anionic surfactant or a combination thereof. It has been found that the addition of solid zinc oxide alone causes an increase in anode resistance during discharge, but this is mitigated by the addition of a surfactant. The addition of a surfactant increases the surface charge density of the solid zinc oxide and reduces anode resistance as described above.

[0068] As in Figure 1 In batteries in which the anode is coated, a separate current collector (i.e., a conductive member such as a metal foil onto which the anode is coated, or a conductive strip extending along a substantial portion of the length of the anode such that the current collector is spirally wound within a jellyroll) can be used. If used, the anode current collector comprises copper, aluminum, zinc, and / or other suitable high-conductivity metal that is stable when exposed to other internal components of the battery (e.g., the electrolyte).

[0069] An electrical connection is maintained between each electrode and an opposing external battery terminal located adjacent to or integral with the housing. Electrical leads 36 may consist of thin metal strips connecting the anode or cathode to one of the battery terminals (at Figure 1 In the embodiment of the LR6 battery shown in FIG, the negative electrode may be provided with a lead before being wound into a jellyroll configuration. The lead may also be connected by appropriate welding.

[0070] The metal strip comprising lead 36 is typically made of nickel or nickel-plated steel, having a sufficiently low electrical resistance (e.g., typically less than 15 mΩ / cm, preferably less than 4.5 mΩ / cm) to facilitate adequate current transfer through the lead. Examples of suitable negative electrode lead materials include, but are not limited to, copper, copper alloys such as copper alloy 7025 (a copper-nickel alloy comprising approximately 3% nickel, approximately 0.65% silicon, and approximately 0.15% magnesium, with the balance being copper and minor impurities); copper alloy 110; and stainless steel. The lead material should be selected so that the composition is stable within an electrochemical cell comprising a non-aqueous electrolyte.

[0071] The cathode is in the form of a strip that may include a current collector and a mixture of one or more electrochemically active materials, typically in particulate form. The active material at the cathode of an alkaline battery may be EMD. EMD is present in an amount of typically about 80 to about 92 weight percent, preferably about 81 to 85 weight percent, based on the total weight of the positive electrode, i.e., manganese dioxide, conductive material, positive electrolyte, and additives (including organic additives, if present). The cathode may also contain a small amount of one or more additional active materials, depending on the desired electrical and discharge characteristics of the battery. The additional active cathode material may be any suitable active cathode material. Examples include metal oxides, Bi2O3, C2F, CF x 、(CF) n , CoS2, CuO, CuS, FeS, FeCuS2, MnO2, Pb2Bi2O5 and S.

[0072] The cathode may include other components such as a conductive material, for example graphite, which, when mixed with the EMD, provides a conductive matrix substantially throughout the positive electrode. The conductive material may be natural, i.e., mined, or synthetic, i.e., manufactured. In one embodiment, the battery includes a positive electrode having an active material or oxide to carbon ratio (O:C ratio) of about 12 to about 24. In one embodiment, the O:C ratio is about 12-14. Too high an oxide:carbon ratio increases the resistance of the container to the cathode, which affects the overall cell resistance and can have an adverse effect on high rate discharge performance, as evident from DSC testing, and / or may have an adverse effect on battery uses that rely on higher cutoff voltages (e.g., cutoff voltages greater than 1.05V). In addition, the graphite may be expandable or non-expandable. Suppliers of graphite for alkaline batteries include Superior Graphite Company of Chicago, 111.; and Lonza, Ltd. of Basel, Switzerland. The conductive material is typically present in an amount of about 5 to about 10 wt % based on the total weight of the positive electrode. Too much graphite reduces the EMD input and therefore reduces the battery capacity; too little graphite increases the contact resistance between the current collector and the cathode and / or the cathode body resistance. Based on the specific electrochemical cell chemistry used, other additives such as barium sulfate (BaSO4), barium acetate, titanium dioxide, binders such as coathylene and calcium stearate, nickelate materials (as described in U.S. Patent Application No. 17 / 032,496, the subject matter of which is incorporated herein by reference in its entirety) and / or other additives may be used. In addition, certain additives may be provided to facilitate the manufacture of a cathode suitable for inclusion in a wound electrode. For example, in certain embodiments, additives that enable the cathode material to be extruded, spread, coated, or otherwise provided onto the cathode current collector and then rolled into a roll shape without breaking may be mixed with the cathode material.

[0073] In one embodiment, the cathode components (EMD), conductive materials, and optional additives are mixed together to form a homogeneous mixture. During the mixing process, an alkaline electrolyte solution, such as KOH solution, which may include organic additives, is uniformly dispersed into the mixture, thereby ensuring uniform distribution of the solution throughout the cathode material.

[0074] The cathode mixture can be applied to one or both sides of a thin metal strip or mesh or expanded or perforated metal (typically nickel having a thickness of between about 16 and about 20 μm) that acts as the cathode current collector. Nickel is a commonly used material, although steel and other metal foils and alloys thereof are also possible. The current collector can extend beyond the cathode portion containing the cathode mixture. This extended portion of the current collector can provide a convenient area for contacting an electrical lead connected to the positive terminal, preferably via a spring or pressure contact, which eliminates the need for a lead and / or welded contact. It is desirable to keep the volume of the extended portion of the current collector to a minimum so that as much of the internal volume of the battery as possible is used for active materials and electrolyte.

[0075] Connect the cathode electrically to the positive terminal of the battery. Figure 1 As shown in , this can be realized with the electric lead that is generally thin metal strip or spring form, although welding connection is also possible.If used, this lead can be made of nickel-plated stainless steel or other suitable materials.In this case, use optional current limiting device, such as standard PTC as safety mechanism.Suitable PTC is sold by Tyco Electronics in Menlo Park, Calif., USA.Typical standard PTC device usually comprises the resistance of about 36 mΩ / cm.Other alternatives, including lower resistance device, are available and may be preferred.Alternative current limiting device is found in U.S. Publication Nos. 20070275298 and 20080254343, which are incorporated herein by reference in their entirety.

[0076] A separator is provided to separate the cathode and anode. The separator maintains a physical dielectric separation between the electrochemically active materials of the positive electrode and the negative electrode and allows ions to be transported between the electrode materials. Furthermore, the separator acts as a wicking medium for the electrolyte and as a collar to prevent broken portions of the negative electrode from contacting the top of the positive electrode. The separator can be a layered, ion-permeable, nonwoven fiber fabric. A typical separator typically comprises two or more layers of paper.

[0077] The battery cells of the present invention use electrolytes such as potassium hydroxide (KOH) that contain only minimal amounts of water as a contaminant (e.g., no more than about 500 ppm by weight, depending on the electrolyte salt used). The electrolyte may additionally contain an alkali metal hydroxide, such as potassium hydroxide (KOH), sodium hydroxide (NaOH), or mixtures thereof. Potassium hydroxide is preferred. The alkaline electrolyte used to form the gel electrolyte of the negative electrode contains alkali metal hydroxide in an amount of about 26 wt % to about 36 wt %, for example, about 26 wt % to about 32 wt %, and especially about 26 wt % to about 30 wt %, based on the total weight of the alkaline electrolyte. Less alkaline electrolytes are preferred but can lead to rapid electrolyte separation at the anode. Increasing the alkali metal hydroxide concentration produces a more stable anode but can reduce high-rate performance. In some embodiments with solid ZnO designs, the dissolved ZnO concentration may increase significantly. The metal ions in the electrolyte may have a concentration of 0.1-60,000 ppm. In alternative embodiments, the electrolyte may be neutral or salt-based, as in zinc-carbon batteries.

[0078] The anode, cathode and separator strips are combined together in an electrode assembly. The electrode assembly can be a spiral wound design, such as Figure 1 , which is made by winding alternating strips of cathode, separator, anode and diaphragm around a mandrel, and when the winding is completed, the mandrel is withdrawn from the electrode assembly. Usually at least one separator layer and / or at least one electrically insulating film layer is wrapped around the outside of the electrode assembly. This has many uses: it helps to hold the assembly together and can be used to adjust the width or diameter of the assembly to the desired size. The outermost end of the separator or other outer film layer can be fixed with a piece of tape or by heat sealing. The anode can be as shown. Figure 1 and 2B The outermost electrode, or cathode, shown in FIG. Figure 2A The outermost electrode is shown in . Either electrode can make electrical contact with the battery container, but internal shorting between the outermost electrode and the container sidewall can be avoided by matching the polarity of the outermost wrap of the electrode assembly with the polarity of the can.

[0079] Any suitable method may be used to close and seal the battery. Such methods may include, but are not limited to, crimping, redrawing, collecting, and combinations thereof. For example, for Figure 1The battery in the embodiment of the present invention, after inserting the electrode and the insulating cone, forms a crimp in the can, and the gasket and the cover assembly (comprising the battery cover, the contact spring and the vent bushing) are placed on the open end of the can. When the gasket and the cover assembly are pushed down against the crimp, the battery is supported on the crimp. The diameter of the can top above the crimp is reduced with a segmented chuck to fix the gasket and the cover assembly in place in the battery. After the electrolyte is distributed in the battery via the hole in the vent bushing and the cover, the vent ball is inserted into the liner to seal the hole in the battery cover. The PTC device and the terminal cover are placed on the battery above the battery cover, and with a crimping die, the top edge of the can is bent inwardly to keep and position the gasket, the cover assembly, the PTC device and the terminal cover, and complete the sealing of the open end of the can by the gasket.

[0080] It is also desirable to use cathode materials with small particle size to minimize the risk of puncturing the separator and / or to improve rate performance under certain conditions.

[0081] The cathode mixture is applied to the foil current collector using a number of suitable methods, such as three roll reverse, comma coating, or slot die coating. A mass-free zone on one or more preferably both sides of the cathode current collector can be incorporated into the coating process to facilitate electrical connection (welding or pressure contact) along the top edge of the cathode, which effectively corresponds to the longitudinal uncoated portion along the top edge of each cathode. After or simultaneously with drying to remove any unwanted solvent, the resulting cathode strip is densified by calendaring or the like to further compact the entire positive electrode. This densification maximizes the loading of electrochemical materials in the jelly-wound electrode assembly, given that the strip is then spirally wound with a separator and an anode strip of similar (but not necessarily identical) size to form a jelly-wound electrode assembly.

[0082] In a fixed space, such as an LR6 can, the thickness of the electrodes at least partially determines the amount of interfacial area between the electrodes. Thicker electrodes occupy more space within the fixed interior space of the battery, and therefore fewer turns of a jellyroll can fit within the battery can. However, the thickness of the separator also affects the number of turns of a jellyroll electrode that can fit within the fixed interior space of the battery can. Thicker separators occupy more space, and as the interfacial area of the electrodes increases (e.g., by reducing the thickness of the electrodes), the volume of separator material required to fully cover the interfacial surface area increases proportionally, thus limiting the number of turns of a jellyroll that can be inserted into a battery can of fixed dimensions.

[0083] An example of a cathode outer wrap cell design is shown in cross-sectional view (ie, taken along a radius of the jellyroll 19). Figure 2A In, Figure 2BThe anode-encased design is shown. In both figures, the cathode 20 is shown in black, the anode 18 is shown in white, and the separator 26 is shown in dashed lines. The remaining elements of the battery (described below) are omitted to better illustrate the design differences. As used herein, cathode-encased designs and batteries include any wound electrode assembly in which a portion of the surface area of the active material on the outermost circumference of the jellyroll is attributable to the cathode (or less than 50% of its outermost circumference is attributable to the anode). An anode-encased battery refers to an electrode assembly in which more than 50% of the outermost circumference of its active material is attributable to the anode, although in preferred embodiments, the outermost active material is essentially all anode. When determining whether a battery is anode-encased or cathode-encased, any separators, leads, insulating tape, and other inactive components are not considered, and the interfacial orientation of the electrodes is not considered. Instead, the outermost circumference of the jellyroll is evaluated based solely on the outermost portions of the anode and cathode that are exposed or will be exposed. Furthermore, as used herein, leads are considered to be separate components compared to current collectors because the leads establish electrical contact between the electrode assembly and the terminals of the battery, whereas the current collectors are only used within the electrode assembly itself (e.g., the current collectors conduct electrons to the leads).

[0084] In either case (i.e., anode or cathode overpack design), the electrodes, particularly the anode, have a substantially uniform thickness because of ease of fabrication and the fact that this arrangement maintains the lowest possible internal resistance throughout the battery's discharge. The cathode coating, applied to a single side of the current collector, also has a uniform thickness, although intermittent coating techniques can be employed to optimize active material volume and improve cathode utilization.

[0085] The above discussion of wound electrochemical cell designs is provided as an example only. The interfacial area between the anode and cathode can be easily adjusted in a wound configuration by varying the thickness of the anode and cathode electrodes. However, for other electrochemical cell structures, the interface area between the anode and cathode can also be adjusted, for example by adjusting the electrode shape of a bobbin electrochemical cell structure (e.g., as discussed in U.S. Patent No. 6,074,781 or U.S. Patent Publication No. 2020 / 0203713, the contents of both of which are incorporated herein by reference in their entirety), a dual anode electrochemical cell structure (e.g., as discussed in U.S. Patent Publication No. 2022 / 0077473; U.S. Patent No. 5,962,163; or U.S. Patent No. 5,869,205, the contents of which are incorporated herein by reference in their entirety), a central cathode electrochemical cell structure (e.g., as discussed in U.S. Patent Publication No. 2020 / 0411878, the contents of which are incorporated herein by reference in their entirety), by alternating disks of anode and cathode material (with a central separator disk) stacked within a cylindrical battery cell, and / or similar methods.

[0086] Experimental results and optimized interface area design

[0087] Figure 3 Shown are discharge curves of electrochemical cells according to some embodiments. Figure 3 The results of a discharge performance test using LR6 (AA) Zn-MnO2 alkaline bobbin batteries according to the standard ANSI digital still camera (DSC) test method are shown. Discharge time is shown in minutes on the x-axis and voltage is shown in volts on the y-axis. During the test, voltage was measured versus discharge time for cells with high interfacial area and cells with low interfacial area. The low interfacial area cell had a standard bobbin cell configuration with a 13 mil separator thickness and approximately 12 cm 2 interfacial area. The high interfacial area cell has three cylindrical anodes with a 13 mil separator and a total of 19 cm 2 The two batteries are discharged with the same current / voltage consumption. Figure 3 As shown in , the high interfacial area cell has a discharge time of approximately 148 minutes (measured until the cell voltage exceeds the lower threshold voltage of 1.05 V), while the cell with low interfacial area has a discharge time of approximately 65 minutes. Figure 3 As reflected in the increase in interfacial area from a low-interfacial-area cell to a high-interfacial-area cell, the cathode (MnO2) discharge efficiency, based on 1 electron discharge from the cathode, increased from 24% to 44% during DSC discharge conditions. Therefore, it is believed that increasing the interfacial area between the anode and cathode is generally desirable for increasing the run time of a cell in high-rate discharge applications (e.g., as tested in DSC). However, as discussed above, high-interfacial-area designs require a higher separator volume, which reduces the amount of volume within a fixed-sized battery cell that can be occupied by the active materials in the electrochemical cell. This reduction in the amount of active material (cathode and anode) that can be input into the cell can reduce the battery run time performance for low-rate discharge applications, which are typically characterized by higher discharge efficiencies of the active materials.

[0088] Figure 4-12The effects of varying the interfacial area within an alkaline cell at different separator thicknesses are shown. These figures illustrate theoretical experiments demonstrating how varying the interfacial area affects the amount of active material added to the cell, the discharge efficiency of the active material, and the battery's run time under various discharge conditions. For both run time and active material input, the figures indicate the percentage change relative to a control cell (a standard bobbin-type electrochemical cell). For example, a run time of 110% means the cell's run time is 110% of that of the control cell. Similarly, a cell with 85% active material input means it contains 85% as much active material as the control cell. Discharge efficiency is expressed as a percentage and refers to the percentage of cathode active material discharged, based on 1-electron EMD capacity, once the cell reaches a specified cutoff voltage (e.g., 1.05V for DSC and 1.0V for a 50mA discharge rate). For example, a discharge efficiency of 95% means that 95% of the active material in the cell has been discharged once the cell reaches a specified output voltage. It is noted that the active material chemistry (ie, the mixture of anode materials within the anode gel and the mixture of cathode materials within the cathode mix) remains the same for all cell designs.

[0089] Figure 4 and Figure 5 Demonstrating the effect of varying the interfacial area within a cell subjected to low rate discharge (50 mA discharge). Figure 4 shows the effect of varying the interfacial area in a cell with an 18 mil separator thickness. Figure 5 The effect of varying the interfacial area in a cell with a 0.1 mil separator (nearly zero thickness separator) is shown. Figure 4 As shown in , for a 18 mil thick membrane, as the interfacial area increases from 11 cm 2 Increased to 100 cm 2 , the low rate discharge ANSI 50 mA discharge operating time is reduced from 100% to about 31%, and the cathode discharge efficiency is reduced from 11 cm 2 The interfacial area increased to 88% at 100 cm 2 95% of the following. Figure 4 The reduction in input for the high interfacial area design shown in is attributed to the relatively thicker ( Figure 4 The volume of the separator increases with the thickness of the separator (18 mil in Fig. 1). Thinner separators are believed to have less (possibly negligible) effect on the input of active materials, and electrochemical cell performance improves with increasing interfacial area. This is shown in Figure 5 , which shows the effect of interfacial area on active material input, operating time and discharge efficiency (e.g. Figure 4 ), using a theoretical diaphragm thickness of 0.1 mil. Figure 5As shown in , as the interfacial area increases, the active material input remains at 100% (even though the interfacial area increases because the separator has negligible thickness / volume), the run time and discharge efficiency each increase with the interfacial area, with the run time approaching approximately 117% and the discharge efficiency approaching approximately 96%.

[0090] Figure 6 and Figure 7 The effect of varying the interfacial area within a cell subjected to high rate discharge (eg, discharge according to the ANSI standardized DSC test) is shown. Figure 6 Specifically shown is the effect of varying the interfacial area in a cell with a negligible separator thickness (0.1 mil thickness). Figure 7 The effect of varying the interfacial area in a cell with an 18 mil separator thickness is shown. In general, electrochemical cells with high interfacial area are believed to perform better at high-rate discharge conditions than at low-rate discharge conditions (i.e., have longer run times and higher discharge efficiencies, even with lower active material input). Reference is now made to Figure 6 , which shows the performance of a battery pack with a 0.1 mil separator when subjected to DSC discharge parameters, the run time was from 2 The interfacial area increased by 113% to 100 cm 2 The interface area is 313%, and the corresponding discharge efficiency increases from 25% to 69%. The active material input is kept at 100%. Therefore, it is believed that for high rate performance devices such as DSC ( Figure 7 ) and low rate capability devices such as 50 mA ( Figure 5 ), reducing the separator thickness (e.g., down to 0.1 mil) and increasing the interfacial area can lead to a substantial increase in operating time and discharge efficiency.

[0091] Now refer to Figure 7 Even when using an 18 mil diaphragm thickness, the DSC run time can be reduced from 11 cm 2 The interfacial area increases to 100% at 30 cm 2 194% of the total cost of ownership, despite the reduction in active material input. Figure 7 DSC service in 30 cm 2 The performance reaches a maximum of 194% at the interface area, and then decreases with the increase of interface area. Figure 6 and Figure 5 The comparison between the same, Figure 7 and Figure 4 Parameter comparisons between the two seem to indicate a greater relative benefit of high-rate performance compared to low-rate performance. However, Figure 7It was also shown that as the separator thickness increases (eg, 18 mils), after the interfacial area reaches a certain value, the performance decreases accordingly (as indicated by, for example, run time and active material input).

[0092] like Figure 8 As reflected in Figure 1, for an electrochemical cell with an 18 mil separator, the average ANSI performance is plotted against the interfacial area. The straight-line average ANSI was calculated based on seven ANSI 2021 standard tests for an LR6 size Zn / MnO2 alkaline battery pack; that is, seven ANSI 2021 standard tests were performed, summed, and divided by 7 to obtain the calculated result. Figure 8 As shown in , the performance increases with the interfacial area until around 25 cm 2 An optimum point (or “peak performance”) is reached at 100 nm, after which performance decreases as the interfacial area increases.

[0093] and Figure 8 The diagram illustrates how variations in interfacial area of an alkaline electrochemical cell affect performance, and as mentioned above, performance reaches its maximum possible performance at an optimized interfacial area. The inventors of the present invention have discovered that the optimized interfacial area depends on the thickness of the separator used in the cell. Figure 9 The graph depicts the maximum performance of an alkaline battery (depicted as a percentage of the performance of a control battery) versus separator thickness. The maximum performance is plotted on the z-axis on the right side of the graph. Figure 9 A graphical representation of the optimal interfacial area versus separator thickness is also shown. The interfacial area is plotted on the y-axis on the left side of the graph. As mentioned above, the maximum possible performance of an alkaline battery is the performance of an alkaline battery with the optimized interfacial area for a given separator thickness. In other words, to achieve the maximum possible performance for a battery with a given separator thickness, the battery should be designed to have the optimal interfacial area.

[0094] like Figure 9 As reflected in , the maximum performance of the battery can be calculated according to the following equation (1):

[0095] .

[0096] In equation (1), z is the maximum performance (as a percentage of the control cell performance) and x is the separator thickness in mils. Figure 9 It is also shown that the optimized interfacial area decreases as the membrane thickness increases. The optimized interfacial area can be calculated according to equation (2) as follows:

[0097] .

[0098] In equation (2), y is expressed in cm 2 , and x is the thickness of the membrane in mils.

[0099] The inventors of the present invention have found that cells exhibiting performance within 8% of maximum performance provide acceptable performance while providing sufficient manufacturing tolerances to provide cells with optimized interfacial areas. More preferably, electrochemical cells exhibiting performance within 5% of maximum performance, and even more preferably, electrochemical cells exhibiting performance within 3% of maximum performance provide acceptable performance within sufficient manufacturing tolerances. Figure 10 Shown is a range of interfacial area vs. separator thickness that can be selected to achieve an alkaline electrochemical cell having performance within 8% of maximum performance. Figure 11 Shown is a range of interfacial area vs. separator thickness that can be selected to achieve an alkaline electrochemical cell having performance within 5% of maximum performance. Figure 12 Figure 2 shows the range of interfacial area vs. separator thickness that can be selected to achieve an alkaline electrochemical cell having a performance within 3% of the maximum performance. Figure 10-12 As reflected in each of the ranges, the interfacial area of the alkaline electrochemical cell can be higher or lower than the optimal interfacial area while still achieving performance within the respective ranges. Note that the values corresponding to these ranges are reflected in Table 1 below. Figure 10 Corresponding to interface area range 1 (8% below peak performance), Figure 11 corresponds to interface area range 2 (5% below peak performance), and Figure 12 Corresponds to interface area range 3 (3% below peak performance).

[0100] Now refer to Figure 10 , it is possible to provide alkaline cell performance within 8% of maximum performance for an LR6 size cell by utilizing an interfacial area within the range of the following equation (3):

[0101] .

[0102] In equation (3), y is expressed in cm 2 The interfacial area is the interfacial area in cm and x is the thickness of the separator in mils. As reflected in Table 1 below, for cells using separators with a thickness between 0.1 and 1 mil, the cells can utilize separators with a thickness between 27 and 1346 cm 2 The interfacial area between the cells achieves performance within 8% of the maximum performance of the cell. For cells using separators with thicknesses between 1 and 5 mils, the cell can utilize separators with thicknesses between 21 and 285 cm 2 The interfacial area between the cells achieves performance within 8% of the maximum performance of the cell. For cells using separators with a thickness between 5 and 10 mils, the cell can utilize separators with a thickness between 19 and 96 cm. 2The interfacial area between the cells achieves performance within 8% of the maximum performance of the cell. For cells using separators with a thickness between 10-18 mils, the cell can utilize separators with a thickness between 17-60 cm 2 The interface area between the cells achieves performance within 8% of the maximum performance of the cell.

[0103] Now refer to Figure 11 , alkaline cell performance within 5% of maximum performance can be provided for LR6 size cells by utilizing an interfacial area within the range of the following equation (4):

[0104] .

[0105] In equation (4), y is expressed in cm 2 The interfacial area is the interfacial area in mils, and x is the thickness of the separator in mils. As reflected in Table 1 below, for cells using separators with a thickness between 0.1 and 1 mil, the cells can utilize separators with a thickness between 32 and 959 cm 2 The interfacial area between the cells achieves performance within 5% of the maximum performance of the cell. For cells using separators with a thickness between 1 and 5 mils, the cell can utilize separators with a thickness between 24 and 225 cm 2 The interfacial area between the cells achieves performance within 5% of the maximum performance of the cell. For cells using separators with a thickness between 5 and 10 mils, the cell can utilize separators with a thickness between 21 and 82 cm. 2 The interfacial area between the cells achieves performance within 5% of the maximum performance of the cell. For cells using separators with a thickness between 10-18 mils, the cell can utilize separators with a thickness between 19-53 cm 2 The interface area between the cells achieves performance within 5% of the maximum performance of the cell.

[0106] Now refer to Figure 12 , alkaline cell performance within 3% of maximum performance can be provided for an LR6 size cell by utilizing an interfacial area within the range of the following equation (5):

[0107] .

[0108] In equation (5), y is expressed in cm 2 The interfacial area is the interfacial area in mils, and x is the thickness of the separator in mils. As reflected in Table 1 below, for cells using separators with a thickness between 0.1 and 1 mil, the cells can utilize separators with a thickness between 39 and 716 cm 2 The interfacial area between the cells achieves performance within 3% of the maximum performance of the cell. For cells using separators with thicknesses between 1 and 5 mils, the cell can utilize separators with thicknesses between 27 and 183 cm 2The interfacial area between the cells achieves performance within 3% of the maximum performance of the cell. For cells using separators with a thickness between 5 and 10 mils, the cell can utilize separators with a thickness between 23 and 71 cm 2 The interfacial area between the cells achieves performance within 3% of the maximum performance of the cell. For cells using separators with a thickness between 10-18 mils, the cell can utilize separators with a thickness between 20-47 cm 2 The interface area between the electrodes achieves performance within 3% of the battery's maximum performance.

[0109] Can be used Figure 9 The optimum interfacial area formula disclosed in and previously discussed as equation (2) determines the peak or optimal performance of an alkaline battery. However, manufacturing a battery that fully complies with this equation may be difficult and economically unfeasible. Figure 10-12 As described by equations (3), (4) and (5), it has been found that performance that is 8%, 5% (preferably) and 3% (more preferably) lower, respectively, provides improved performance while remaining within reasonable manufacturing tolerances. As shown below and discussed, Table 1 details how to manufacture alkaline batteries with separator thicknesses and interfacial areas that will achieve performance within 8%, 5% or 3% of the peak / optimum performance of alkaline batteries.

[0110] The following table (Table 1) provides a straight average of the ANSI 2021 test results for the aforementioned LR6 / AA Zn-MnO2 alkaline battery pack based on seven ANSI 2021 standard tests:

[0111] Table 1

[0112]

[0113] Table 1 shows the membrane thickness in mils in the leftmost column and the interfacial area in cm in the remaining columns. 2 The separator values in one row correspond to the lower and upper limits of the interfacial area in the same row. Table 1 is divided into three parts. The left part shows the separator values and interfacial area within 8% of the peak performance, the middle part shows the separator values and interfacial area within 5% of the peak performance, and the right part shows the separator values and interfacial area within 3% of the peak performance. For example, for an alkaline cell with a thickness of 1 mil, in order to achieve performance within 8% of the peak performance, the interfacial area can be 27 cm 2 Up to 285 cm 2 As another example, for the same cell with a thickness of 1 mil, to achieve performance within 5% of peak performance, the interfacial area may be 32 cm 2 Up to 225 cm 2 .

[0114] According to various embodiments, one or more LR6 alkaline electrochemical cells may be designed based on the above ratio between the interfacial area of the anode and cathode and the thickness of the separator. These various electrochemical cells may be based on the previously discussed and Figure 1 、 2A , a "wound-type" cell as shown in FIG2B. However, it should be understood that other cell configurations may be utilized while adhering to the interfacial area / separator thickness mentioned above.

[0115] In some embodiments, an LR6 alkaline electrochemical cell may include a container; an electrolyte; an anode; a cathode; a current collector; and a separator disposed between the anode and the cathode, wherein the separator may have a thickness x, and wherein the interfacial area of the cathode and the anode may be y, and wherein the relationship between the thickness of the separator and the interfacial area of the anode and the cathode may be as described in reference to Figure 10 、 Figure 11 or Figure 12 The scope of the interface area under discussion is limited.

[0116] In some embodiments, the LR6 alkaline electrochemical cell may include a container; an electrolyte; an anode; a cathode; a current collector; and a separator disposed between the anode and the cathode, wherein the separator may have a thickness between 0.1 and 1 mils of the first set of separator thicknesses and have a thickness between 27 and 1346 cm 2 The interfacial area between 32 and 959 cm 2 The interfacial area between the electrodes is such that the battery has a performance within 5% of the maximum performance, or within the range of 39-716 cm 2 The interface area between the two groups is such that the battery has a performance within 3% of the maximum performance. In other embodiments, the separator may have a thickness between 1 and 5 mils in the second group of separator thicknesses and have a thickness between 21 and 285 cm 2 The interface area between the electrodes is such that the battery has a performance within 8% of the maximum performance; in the range of 24-225 cm 2 The interfacial area between the electrodes should be such that the battery has a performance within 5% of the maximum performance; or between 27 and 183 cm 2 In a further embodiment, the separator may have a thickness between 5 and 10 mils of the third set of separator thicknesses and have an interface area between 19 and 96 cm 2 The interface area between the electrodes is such that the battery has a performance within 8% of the maximum performance; in the range of 21-82 cm 2 The interface area between the cells should be within 5% of the maximum performance; or between 23 and 71 cm2 In yet further embodiments, the separator may have a thickness between 10-18 mils of the fourth set of separator thicknesses and have an interface area between 17-60 cm 2 The interface area between the electrodes is such that the battery has a performance within 8% of the maximum performance; in the range of 19-53 cm 2 The interface area between the electrodes is such that the battery has a performance within 5% of the maximum performance; in the range of 20-47 cm 2 The interface area between the electrodes is increased to provide a battery with a performance within 3% of the maximum performance.

[0117] In some embodiments, an LR6 alkaline electrochemical cell may include a container; an electrolyte; an anode; a cathode; a current collector; and a separator disposed between the anode and the cathode, wherein the anode and the cathode define an interfacial area, wherein the interfacial area is selected so that the electrochemical cell has an average ANSI performance within 8% of the maximum theoretical performance of the electrochemical cell, wherein the maximum theoretical performance is determined by having a maximum theoretical performance according to a reference Figure 9 In some embodiments, the electrochemical cell may have an average ANSI performance that is within 5% of the maximum theoretical performance of the electrochemical cell. In some embodiments, the electrochemical cell may have an average ANSI performance that is within 3% of the maximum theoretical performance of the electrochemical cell.

[0118] All references cited above and all references cited herein are hereby incorporated by reference in their entirety.

[0119] Although the embodiments have been illustrated and described in detail above, such illustration and description are to be considered illustrative or exemplary rather than restrictive. It is to be understood that changes and modifications may be made by one of ordinary skill in the art within the scope and spirit of the following claims. The embodiments include any combination of features from the different embodiments described above and below.

[0120] Embodiment is described in addition to provide a better understanding of embodiment and its many advantages by the following exemplary non-limiting examples. The following examples are included to prove the preferred embodiment. Those skilled in the art will recognize that the technology representative disclosed in the following examples is for the technology used in the embodiment to operate well in the practice of the embodiment, and therefore can be considered to constitute the preferred mode of its practice. However, those skilled in the art should recognize that many changes can be made to the disclosed specific embodiment and still obtain the same or similar result, without departing from the spirit and scope of the embodiment.

[0121] Many modifications and other aspects of the disclosure described herein will occur to those skilled in the art having the benefit of the teachings presented in the foregoing description and the associated drawings. Therefore, it is to be understood that the disclosure is not limited to the specific aspects disclosed and that modifications and other aspects are intended to be included within the scope of the appended claims. Although specific terms are employed herein, they are used in a generic and descriptive sense only and not for purposes of limitation.

Claims

1. An electrochemical cell comprising: container; electrolytes; anode; cathode; a current collector; and A separator is provided between the anode and cathode, wherein the anode and the cathode define an interfacial area y, and the separator defines a thickness x, and The relationship between the interfacial area y and the membrane thickness x is defined as between.

2. The electrochemical cell of claim 1 , wherein the relationship between the interfacial area y and the separator thickness x is defined as between.

3. The electrochemical cell of claim 1 , wherein the relationship between the interfacial area y and the separator thickness x is defined as between.

4. An electrochemical cell comprising: container; electrolytes; anode; cathode; a current collector; and A separator is provided between the anode and cathode, wherein the anode and the cathode define an interfacial area, and the separator defines a thickness, and The membrane thickness is selected from a first group of 0.1 mil to 1 mil, a second group of 1 mil to 5 mils, a third group of 5 mils to 10 mils, and a fourth group of 10 mils to 18 mils.

5. The electrochemical cell of claim 4, wherein the separator thickness is selected from the first group consisting of 0.1 mil to 1 mil, and the interfacial area is selected from the first group consisting of 27 to 1346 cm 2 between groups.

6. The electrochemical cell of claim 5, wherein the separator thickness is selected from the first group consisting of 0.1 mil to 1 mil, and the interfacial area is selected from the first group consisting of 32 to 959 cm 2 between groups.

7. The electrochemical cell of claim 6, wherein the separator thickness is selected from the first group consisting of 0.1 mil to 1 mil, and the interfacial area is selected from the first group consisting of 39 to 716 cm 2 between groups.

8. The electrochemical cell of claim 4, wherein the separator thickness is selected from the second group consisting of 1 mil to 5 mils and the interfacial area is selected from the second group consisting of 21 to 285 cm 2 between groups.

9. The electrochemical cell of claim 8, wherein the separator thickness is selected from the second group consisting of 1 mil to 5 mils and the interfacial area is selected from the second group consisting of 24 to 225 cm 2 between groups.

10. The electrochemical cell of claim 9, wherein the separator thickness is selected from the second group consisting of 1 mil to 5 mils and the interfacial area is selected from the second group consisting of 27 to 183 cm 2 between groups.

11. The electrochemical cell of claim 4, wherein the separator thickness is selected from the third group consisting of 5 mils to 10 mils, and the interfacial area is selected from the third group consisting of 19 to 96 cm 2 between groups.

12. The electrochemical cell of claim 11, wherein the separator thickness is selected from the third group consisting of 5 mils to 10 mils, and the interfacial area is selected from the third group consisting of 21 to 82 cm 2 between groups.

13. The electrochemical cell of claim 12, wherein the separator thickness is selected from the third group consisting of 5 mils to 10 mils, and the interfacial area is selected from the third group consisting of 23 to 71 cm 2 between groups.

14. The electrochemical cell of claim 4, wherein the separator thickness is selected from the fourth group of between 10 mils and 18 mils, and the interfacial area is selected from the fourth group of between 17 and 60 cm 2 between groups.

15. The electrochemical cell of claim 14, wherein the separator thickness is selected from the fourth group of between 10 mils and 18 mils, and the interfacial area is selected from the fourth group of between 19 and 53 cm 2 between groups.

16. The electrochemical cell of claim 15, wherein the separator thickness is selected from the fourth group of between 10 mils and 18 mils, and the interfacial area is selected from the fourth group of between 20 and 47 cm 2 between groups.

17. An electrochemical cell comprising: container; electrolytes; anode; cathode; a current collector; and A separator is provided between the anode and cathode, wherein said anode and said cathode define an interfacial area, wherein the interfacial area is selected so that the electrochemical cell has an average ANSI performance within 8% of the maximum theoretical performance of the electrochemical cell, wherein The maximum theoretical performance is defined by Theoretical electrochemical cell realization with defined interfacial area.

18. The electrochemical cell of claim 17, wherein the electrochemical cell has an average ANSI performance that is within 5% of the maximum theoretical performance of the electrochemical cell.

19. The electrochemical cell of claim 18, wherein the electrochemical cell has an average ANSI performance that is within 3% of the maximum theoretical performance of the electrochemical cell.

Citation Information

Patent Citations

  • Nonaqueous cell with improved thermoplastic sealing member

    US20050079404A1

  • Housing for a sealed electrochemical battery cell

    US20050244706A1

  • Current interrupt device for batteries

    US20070275298A1

  • Housing for a Sealed Electrochemical Battery Cell

    US20080213651A1

  • Electrolyte-absorbing, non-permeable sealing materials

    US20080226982A1