Preparation method of binder for lithium battery
By preparing ternary composite adhesives of polybutadiene, polyvinyl alcohol and polymaleic anhydride, the problems of insufficient solubility and bonding strength of existing lithium-ion battery adhesives are solved, and high stability, low internal resistance and environmentally friendly battery performance improvements are achieved.
Patent Information
- Application Number
- CN202510718941.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-30
- Publication Date
- 2025-08-26
AI Technical Summary
The existing lithium-ion battery binders have problems such as poor solubility, limited bonding strength and poor environmental protection, which affect the battery's cycle life and charge and discharge performance.
Polybutadiene, polyvinyl alcohol and polymaleic anhydride are used as raw materials to prepare ternary composite binders through graft copolymerization to form graft copolymers with high peeling force and flexibility, enhancing the interaction with active substances and conductive agents, and forming a uniform conductive network.
It improves the structural stability and electrochemical stability of the electrode, reduces internal resistance, extends the cycle life of the battery, and improves the charge and discharge efficiency, while also having the characteristics of environmental protection and easy industrial production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a binder for lithium batteries. Background Art
[0002] In recent years, the promotion of new energy vehicles and the widespread use of various electronic products in people's daily lives have greatly promoted the rapid development of lithium-ion batteries. As a key component of lithium-ion battery electrode materials, the performance of binders has a crucial impact on the overall performance of the battery. Oily binders represented by polyvinylidene fluoride (PVDF) have excellent chemical stability and electrochemical window, but have significant defects: First, PVDF has poor solubility in organic solvents and requires the use of highly toxic and expensive solvents such as N-methylpyrrolidone (NMP) for dissolution, which not only increases production costs but also poses a threat to the environment and the health of operators; second, PVDF molecules have weak polarity and only form physical adsorption with active substances (such as ternary materials, lithium iron phosphate) and conductive agents (carbon black, carbon nanotubes), with limited bonding strength. During the battery charging and discharging process, the volume change of the active substance can easily lead to damage to the electrode structure, thereby affecting the battery's cycle life and rate performance. While water-based binders, such as polyacrylic acid (PAA) and styrene-butadiene rubber (SBR), offer advantages such as environmental friendliness and low cost, their relatively weak bonding and mechanical properties fail to meet the electrode structural stability requirements of high-energy-density lithium-ion batteries. Furthermore, these binders lack strong interactions with the active material and conductive agent, making it difficult to form a uniform and stable conductive network. This results in high internal resistance and low charge and discharge efficiency. The performance bottlenecks of existing binders (high toxicity of organic binders and weak strength of aqueous binders) and the limitations of their preparation processes (solvent dependence and demanding reaction conditions) have become key technical shortcomings hindering the development of high-energy-density, long-life lithium-ion batteries. Therefore, developing a method for preparing a binder for lithium batteries with excellent bonding properties, good electrochemical stability, low internal resistance, and environmental friendliness is of significant industrial and technological value. Summary of the Invention
[0003] The object of the present invention is to provide a method for preparing a binder for lithium batteries to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for preparing a binder for a lithium battery comprises the following steps: S1: dissolving polybutadiene in toluene solvent to form a polybutadiene solution; adding hydrogen peroxide and catalyst A, continuously stirring, and reacting to obtain carboxylated polybutadiene; S2: dissolving polyvinyl alcohol in dimethylformamide to form a polyvinyl alcohol solution; dissolving the carboxylated polybutadiene in dimethylformamide to form a carboxylated polybutadiene solution; Mixing the polyvinyl alcohol solution and the carboxylated polybutadiene solution; adding catalyst B, continuously stirring, and reacting to obtain a reaction solution; S3: dissolving polymaleic anhydride in dimethylformamide to form a polymaleic anhydride solution; Adding the polymaleic anhydride solution to the reaction solution obtained in S2, stirring continuously, and reacting to obtain a copolymer reaction solution; S4: After the reaction is completed, the copolymer reaction solution obtained in S3 is cooled to room temperature and poured into ethanol to precipitate the copolymer; the precipitate is collected by filtration and dried in a vacuum oven to obtain a binder.
[0005] Furthermore, the adhesive includes the following components by mass: 100 parts of polybutadiene, 80-110 parts of polyvinyl alcohol, and 80-100 parts of polymaleic anhydride.
[0006] Furthermore, in S1, the reaction is followed by post-treatment, wherein the post-treatment process is as follows: after the reaction is completed, the carboxylated polybutadiene reaction solution is cooled to room temperature; poured into ethanol to precipitate the carboxylated polybutadiene, the precipitate is collected by filtration, and washed three times with ethanol to remove unreacted hydrogen peroxide and catalyst; and finally, the precipitate is dried in a vacuum oven at 80-100° C. for 4-6 hours.
[0007] Furthermore, in said S1, the mass concentration of the polybutadiene solution is 10%; Furthermore, the mass ratio of polybutadiene, hydrogen peroxide, and catalyst A is 100:(7.5-8.5):(0.3-0.7).
[0008] Furthermore, catalyst A is sodium tungstate.
[0009] Furthermore, in S2, the mass concentration of the polyvinyl alcohol solution is 10%.
[0010] Furthermore, the mass concentration of the carboxylated polybutadiene solution is 10%.
[0011] Furthermore, the mass ratio of the polyvinyl alcohol solution to the carboxylated polybutadiene solution is 1:1.
[0012] Furthermore, the catalyst B is p-toluenesulfonic acid, and the amount used is 0.2%wt-0.3%wt of the mass of the polyvinyl alcohol solution.
[0013] Furthermore, in S3, the mass concentration of the polymaleic anhydride solution is 10%.
[0014] Furthermore, the mass ratio of the reaction solution obtained in S2 to the polymaleic anhydride solution is 2:(0.8-1.0).
[0015] Furthermore, in S1, the reaction conditions are: reaction temperature is 60-80° C., and reaction time is 6-8 hours.
[0016] Furthermore, during the continuous stirring, the stirring speed is 100-200 rpm.
[0017] Furthermore, in S2 and S3, the reaction conditions are: reaction temperature is 80-120° C., and reaction time is 6-8 hours.
[0018] Furthermore, in S4, the drying conditions are: drying temperature is 130-150° C., and drying time is 4-6 hours.
[0019] In the above technical solution, the binder is a graft copolymer formed by carboxylated polybutadiene, polyvinyl alcohol, and polymaleic anhydride. The polybutadiene molecular chain is carboxylated, and hydrogen peroxide generates hydroxyl radicals (·OH) under the action of a catalyst, which attack the double bonds of the polybutadiene and are ultimately oxidized to carboxyl groups. The carboxylated polybutadiene is grafted onto the polyvinyl alcohol, undergoing an esterification reaction. The anhydride groups of the polymaleic anhydride react with the hydroxyl and carboxyl groups to ultimately generate the binder.
[0020] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the carbon-coated foil prepared with a ternary composite binder prepared from polybutadiene, polyvinyl alcohol, and polymaleic anhydride exhibits high peeling force with the positive electrode active material and demonstrates a high capacity retention rate during the cycle process; the elastic chain segments of polybutadiene give the electrode good flexibility, which can adapt to the volume change of the active material during the charge and discharge process and reduce the deformation of the electrode; the polar groups (such as carboxyl and hydroxyl) in the graft copolymer can form a stronger interaction with the conductive agent (such as carbon black), improve the uniformity of the conductive network, reduce the internal resistance of the electrode, and improve the rate performance of the battery.
[0021] The present invention copolymerizes a polymer monomer containing a double bond and a monomer with a polar group, and introduces a cross-linking agent to form a three-dimensional network structure, so that the binder has a stronger bonding force with the active material, the conductive agent and the current collector, effectively improving the structural stability of the electrode and reducing the shedding of the active material and the deformation of the electrode during the charge and discharge process.
[0022] The binder of the present invention has high electrochemical stability: the cross-linked network structure can inhibit the swelling and dissolution of the binder in the electrolyte, thereby improving the electrochemical stability of the binder, thereby extending the cycle life of the battery and reducing the performance degradation of the battery during use.
[0023] The binder of the present invention can reduce internal resistance: the monomer with polar groups has a strong interaction with the conductive agent, which can promote the uniform dispersion of the conductive agent in the electrode, form a more complete conductive network, effectively reduce the internal resistance of the electrode, and improve the charge and discharge efficiency and rate performance of the battery.
[0024] The adhesive of the present invention is environmentally friendly: in the preparation process, water can be selected as a solvent, avoiding the use of toxic and harmful organic solvents, reducing pollution to the environment and harm to the health of operators, and conforming to the development concept of green chemistry.
[0025] The preparation process of the binder of the present invention is simple: the reaction conditions are mild, no complicated equipment and harsh reaction conditions are required, and the binder is easy to industrialize and is conducive to reducing production costs and improving production efficiency.
[0026] In summary, the present invention has developed a method for preparing a binder for lithium batteries with excellent bonding performance, good electrochemical stability, low internal resistance and environmental protection. DETAILED DESCRIPTION
[0027] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0028] In the following specific embodiments: Polybutadiene (PB), LI2774, Hubei Xinhongli Chemical Co., Ltd.; Toluene, Tianjin Fuyu Chemical Co., Ltd.; Hydrogen peroxide, Hangzhou Jingxin Chemical Co., Ltd.; Sodium tungstate, Shanghai Pudong Xingbang Chemical Development Co., Ltd.; Ethanol, Tianjin Yongda Chemical Reagent Co., Ltd.; Polyvinyl alcohol, (PVA-205) 0588 low viscosity type, alcoholysis degree: 87~89mol%, Shanghai MacLean Biochemical Technology Co., Ltd. Dimethylformamide (DMF), Shandong Aowei Chemical Co., Ltd.; p-Toluenesulfonic acid (p-TSA), Henan Annuo Chemical Technology Co., Ltd.; Polymaleic anhydride (PMA), Shandong Taihe Science and Technology Co., Ltd.
[0029] Example 1: A method for preparing a binder for a lithium battery, comprising the following steps: S1: Dissolve 100 g of polybutadiene in 1 kg of toluene solvent to prepare a 10% polybutadiene solution; add 8 g of hydrogen peroxide and 0.5 g of catalyst, and stir at 200 rpm at 60°C for 6 hours to obtain carboxylated polybutadiene; Post-treatment: After the reaction is completed, the reaction solution is cooled to room temperature and poured into 10 kg of ethanol to precipitate the carboxylated polybutadiene. The precipitate is collected by filtration and washed three times with 2 kg of ethanol to remove unreacted hydrogen peroxide and catalyst; the product is dried in a vacuum oven at 100°C for 8 hours; S2: 80 g of polyvinyl alcohol was dissolved in 800 g of dimethylformamide to prepare a 10% polyvinyl alcohol solution; 100 g of carboxylated polybutadiene was dissolved in 1 kg of dimethylformamide to prepare a 10% homocarboxylated polybutadiene solution; the polyvinyl alcohol solution and the carboxylated polybutadiene solution were mixed in a mass ratio of 1:1; 2.7 g of p-toluenesulfonic acid was added, and the mixture was stirred at 80° C. and 250 rpm for 8 hours to obtain a reaction solution; S3: 80 g of polymaleic anhydride was dissolved in 800 g of dimethylformamide to prepare a polymaleic anhydride solution with a mass fraction of 10%. The polymaleic anhydride solution was added to the S2 reaction solution, and the mixture was stirred at 80°C and 200 rpm for 6 hours to obtain a copolymer reaction solution. S4: After the reaction is completed, the copolymer reaction solution obtained in S3 is cooled to room temperature and poured into 10 kg of ethanol to precipitate the copolymer; the precipitate is collected by filtration and dried in a vacuum oven at 150° C. for 5 hours to obtain a binder.
[0030] Example 2: A method for preparing a binder for a lithium battery, comprising the following steps: S1: Dissolve 100 g of polybutadiene in 1 kg of toluene solvent to prepare a 10% polybutadiene solution; add 7.5 g of hydrogen peroxide and 0.3 g of sodium tungstate, and stir at 80°C and 100 rpm for 8 hours to obtain carboxylated polybutadiene; Post-treatment: After the reaction is completed, the reaction solution is cooled to room temperature and poured into 10 kg of ethanol to precipitate the carboxylated polybutadiene. The precipitate is collected by filtration and washed three times with 2 kg of ethanol to remove unreacted hydrogen peroxide and catalyst; the product is dried in a vacuum oven at 120°C for 6 hours; S2: dissolving 100 g of polyvinyl alcohol in 1 kg of dimethylformamide to prepare a 10% by mass polyvinyl alcohol solution; dissolving 100 g of carboxylated polybutadiene in 1 kg of dimethylformamide to prepare a 10% by mass homocarboxylated polybutadiene solution; mixing the polyvinyl alcohol solution and the carboxylated polybutadiene solution in a mass ratio of 1:1; adding 2.2 g of p-toluenesulfonic acid, and stirring continuously at 100 rpm at 120° C. for 8 hours to obtain a reaction solution; S3: 80 g of polymaleic anhydride was dissolved in 800 g of dimethylformamide to prepare a polymaleic anhydride solution with a mass fraction of 10%; the polymaleic anhydride solution was added to the S2 reaction solution, and the mixture was stirred at 120°C and 100 rpm for 8 hours to obtain a copolymer reaction solution; S4: After the reaction is completed, the copolymer reaction solution obtained in S3 is cooled to room temperature and poured into 10 kg of ethanol to precipitate the copolymer; the precipitate is collected by filtration and dried in a vacuum oven at 140° C. for 4 hours to obtain a binder.
[0031] Example 3: A method for preparing a binder for a lithium battery, comprising the following steps: S1: Dissolve 100 g of polybutadiene in 1 kg of toluene solvent to prepare a 10% polybutadiene solution; add 8.5 g of hydrogen peroxide and 0.7 g of sodium tungstate, and stir at 70°C and 150 rpm for 7 hours to obtain carboxylated polybutadiene; Post-treatment: After the reaction is completed, the reaction solution is cooled to room temperature and poured into 10 kg of ethanol to precipitate the carboxylated polybutadiene. The precipitate is collected by filtration and washed three times with 2 kg of ethanol to remove unreacted hydrogen peroxide and catalyst. The product is dried in a vacuum oven at 90°C for 5 hours. S2: dissolving 110 g of polyvinyl alcohol in 1.1 kg of dimethylformamide to prepare a 10% polyvinyl alcohol solution; dissolving 100 g of carboxylated polybutadiene in 1 kg of dimethylformamide to prepare a 10% homocarboxylated polybutadiene solution; mixing the polyvinyl alcohol solution and the carboxylated polybutadiene solution in a mass ratio of 1:1; adding 3.3 g of p-toluenesulfonic acid, and stirring at 100° C. and 150 rpm for 7 hours to obtain a reaction solution; S3: Dissolve 100 g of polymaleic anhydride in 1 kg of dimethylformamide to prepare a 10% polymaleic anhydride solution; add the polymaleic anhydride solution to the S2 reaction solution, and continue stirring at 100°C and 150 rpm for 7 hours to obtain a copolymer reaction solution; S4: After the reaction is completed, the copolymer reaction solution obtained in S3 is cooled to room temperature and poured into 10 kg of ethanol to precipitate the copolymer; the precipitate is collected by filtration and dried in a vacuum oven at 130° C. for 6 hours to obtain a binder.
[0032] Comparative Example 1: T108 copper foil primer adhesive was used as the adhesive.
[0033] Comparative Example 2: XHL-D7001 carbon-coated aluminum foil adhesive was used as the adhesive.
[0034] Comparative Example 3: K-702 was used as the binder.
[0035] Experiment: Take the adhesives obtained in Examples 1-3 and Comparative Examples 1-3, prepare samples, test their properties respectively and record the test results: Peel strength test: A positive electrode slurry was prepared in a mass ratio of lithium iron phosphate: conductive carbon black: polyvinylidene fluoride = 96:2:2, and polyvinylidene fluoride: N-methylpyrrolidone = 8:92. The positive electrode slurry was evenly coated onto carbon-coated aluminum foil to obtain an unrolled positive electrode sheet. The sheet was then rolled at a compaction density of 2.55 g / cc to obtain a rolled positive electrode sheet. The peel strength was then tested using an electronic peel tester.
[0036] Electrode resistance test: Use Chuanyuan electrode resistance meter to test the electrode resistance.
[0037] The test results are shown in Table 1: Table 1 Adhesive performance test results
[0038] Conclusion: Comparing the data in the table, it can be seen that the carbon-coated foil prepared with a ternary composite binder made of polybutadiene, polyvinyl alcohol, and polymaleic anhydride exhibits high peel force with the positive electrode active material and high capacity retention during cycling. The elastic segments of polybutadiene impart good flexibility to the electrode, adapting to the volume changes of the active material during charge and discharge, reducing electrode deformation. The polar groups (such as carboxyl and hydroxyl) in the graft copolymer can form stronger interactions with conductive agents (such as carbon black), improving the uniformity of the conductive network, reducing the internal resistance of the electrode, and improving the rate performance of the battery. Compared with the binders of Examples 1-3, the three binders used in Comparative Examples 1-3 have significantly lower electrode peel force, higher electrode resistance, and lower capacity retention during cycling.
[0039] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the invention can be embodied in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as illustrative and non-restrictive, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations that come within the meaning and range of equivalents of the claims be embraced therein.
Claims
1. A method for preparing a binder for lithium batteries, characterized in that: The following steps are involved: S1: dissolving polybutadiene in toluene solvent to form a polybutadiene solution; adding hydrogen peroxide and catalyst A, continuously stirring, and reacting to obtain carboxylated polybutadiene; S2: dissolving polyvinyl alcohol in dimethylformamide to form a polyvinyl alcohol solution; dissolving the carboxylated polybutadiene in dimethylformamide to form a carboxylated polybutadiene solution; mixing the polyvinyl alcohol solution and the carboxylated polybutadiene solution; Add catalyst B, continue stirring, and react to obtain a reaction solution; S3: dissolving polymaleic anhydride in dimethylformamide to form a polymaleic anhydride solution; Adding the polymaleic anhydride solution to the reaction solution obtained in S2, stirring continuously, and reacting to obtain a copolymer reaction solution; S4: After the reaction is completed, the copolymer reaction solution obtained in S3 is cooled to room temperature and poured into ethanol to precipitate the copolymer; the precipitate is collected by filtration and dried in a vacuum oven to obtain a binder.
2. The method for preparing a binder for lithium batteries according to claim 1, wherein: In S1, the reaction is followed by post-treatment, wherein the post-treatment process is as follows: after the reaction is completed, the carboxylated polybutadiene reaction solution is cooled to room temperature; poured into ethanol to precipitate the carboxylated polybutadiene, the precipitate is collected by filtration, and washed with ethanol to remove unreacted hydrogen peroxide and catalyst; and finally, the precipitate is dried in a vacuum oven at 80-100° C. for 4-6 hours.
3. The method for preparing a binder for lithium batteries according to claim 1, wherein: The polyvinyl alcohol is of 0588 low viscosity type and has an alcoholysis degree of 87-89 mol%.
4. The method for preparing a binder for lithium batteries according to claim 1, wherein: In the S1, the mass ratio of polybutadiene, hydrogen peroxide and catalyst A is 100:(7.5-8.5):(0.3-0.7).
5. The method for preparing a binder for lithium batteries according to claim 4, wherein: In the above-mentioned S1, the catalyst A is sodium tungstate.
6. The method for preparing a binder for lithium batteries according to claim 1, wherein: In the S2, the catalyst B is p-toluenesulfonic acid.
7. The method for preparing a binder for lithium batteries according to claim 4, wherein: In the above-mentioned S1, the reaction conditions are: reaction temperature is 60-80° C., and reaction time is 6-8 hours.
8. The method for preparing a binder for lithium batteries according to claim 1, wherein: During the continuous stirring, the stirring speed is 100-200 rpm.
9. The method for preparing a binder for lithium batteries according to claim 1, wherein: In the above-mentioned S2 and S3, the reaction conditions are: reaction temperature is 80-120° C., and reaction time is 6-8 hours.
10. The method for preparing a binder for lithium batteries according to claim 1, wherein: In the step S4, the drying conditions are as follows: drying temperature is 130-150° C., and drying time is 4-6 hours.