Copper-based catalyst for catalyzing hydrochlorination reaction of acetylene as well as preparation method and application of copper-based catalyst

By introducing phosphine-containing ligands into copper-based catalysts to form a stable coordination structure and enhance the hydrophobicity and anti-reduction ability of the catalyst, the problem of insufficient activity and stability of copper-based catalysts in acetylene hydrochlorination reaction is solved, and efficient catalytic performance and long-life catalyst application are achieved.

CN120586937APending Publication Date: 2025-09-05SHIHEZI UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510708933.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-29
Publication Date
2025-09-05

AI Technical Summary

Technical Problem

Traditional copper-based catalysts are easily affected by water vapor and hydrogen in the acetylene hydrochlorination reaction, resulting in the loss of active sites and changes in the active center structure, reducing the activity and stability of the catalyst, making it difficult to replace mercury chloride catalysts in industrial applications.

Method used

Phosphine-containing ligands are used to form a stable coordination structure with copper ions to enhance the surface hydrophobicity and reduction resistance of the catalyst. By controlling the molar ratio of copper to ligand to 2:1-16:1, a copper-based catalyst is prepared to improve its activity and stability in the acetylene hydrochlorination reaction.

Benefits of technology

It significantly improves the hydrophobicity and anti-reduction properties of the catalyst, extends the service life of the catalyst, improves the efficiency and selectivity of the acetylene hydrochlorination reaction, reduces production costs, and complies with the concept of green chemistry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120586937A_ABST
    Figure CN120586937A_ABST
Patent Text Reader

Abstract

The invention relates to a copper-based catalyst for catalyzing acetylene hydrochlorination and a preparation method and application thereof, the copper-based catalyst comprises a carrier, a phosphine-containing ligand and a copper-containing stable metal precursor; the molar ratio of the stable-state metal precursor to the phosphine-containing ligand is (2: 1)-(16: 1), and the mass of copper in the copper-containing stable-state metal precursor is 5-10% of the mass of the copper-based catalyst. For a copper-based catalyst containing ligand dimethyl phosphine oxide, when reaction gas contains a certain amount of water vapor, the activity and selectivity of the catalyst are still maintained at a relatively high level; when the reaction gas contains a certain amount of hydrogen, the influence on the activity and selectivity of the catalyst is small, which indicates that the catalyst has excellent hydrophobicity and reduction resistance in the acetylene hydrochlorination reaction, thereby not only enhancing the generation efficiency of the vinyl chloride monomer, but also prolonging the service life of the catalyst and lowering the production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalyst preparation and application, and in particular to a copper-based catalyst containing a specific ligand, specifically a copper-based catalyst for catalyzing acetylene hydrochlorination reaction, and a preparation method and application thereof. Background Art

[0002] Acetylene hydrochlorination is a chemical process in which acetylene (C2H2) reacts with hydrogen chloride (HCl) in the presence of a catalyst to produce vinyl chloride (C2H3Cl). This reaction is a key link in the chlor-alkali chemical industry chain. Its product, vinyl chloride, is an important monomer in the production of polyvinyl chloride (PVC), a versatile polymer material with a wide range of applications. Due to its excellent physical and chemical properties and low cost, PVC is widely used in a variety of fields, including construction materials (such as pipes and profiles), packaging materials (such as films and containers), electronic appliances (such as wires and cables, insulation materials), and medical devices. Therefore, the efficiency and environmental friendliness of the acetylene hydrochlorination reaction directly impact the economic benefits and sustainable development of the entire PVC industry chain.

[0003] For a long time, the industry has primarily used catalysts containing the highly toxic substance mercuric chloride (HgCl2) as the active component to catalyze the hydrochlorination of acetylene. Although mercuric chloride catalysts have high catalytic activity and selectivity, their volatility and bioaccumulation make mercury vapor and mercury compounds highly susceptible to entering the environment, ultimately endangering human health through the food chain. Mercury pollution not only damages organs such as the nervous system and kidneys, but also affects the reproductive system and immune system. Furthermore, the disposal of discarded mercuric chloride catalysts faces significant environmental pressures and economic costs.

[0004] In recent years, extensive research has been conducted on non-mercury catalysts, with copper-based catalysts attracting significant attention due to their excellent catalytic activity and low price. They are considered one of the most promising alternatives to mercuric chloride catalysts. However, copper-based catalysts still face numerous challenges in practical application. During the acetylene hydrochlorination reaction, the reaction gas often contains a certain amount of water vapor, which adsorbs on the catalyst surface, leading to the loss of active components and destruction of the catalyst structure, thereby reducing the catalyst's activity and stability. Furthermore, hydrogen, as a reaction raw material or byproduct, can easily reduce the copper-based catalyst during the reaction, causing changes in the valence state of the active components and affecting the catalyst's activity and selectivity. Consequently, the hydrophobicity and reduction resistance of copper-based catalysts become significant factors limiting their industrial application.

[0005] Traditional copper-based catalysts and other non-mercury catalysts are vulnerable to the negative effects of water vapor and hydrogen during the acetylene hydrochlorination reaction. Water vapor adsorbs on the catalyst surface, covering active sites and accelerating the loss of active components. Hydrogen, on the other hand, can easily over-reduce the catalyst, altering the structure of the active centers. Both significantly reduce the catalyst's activity and stability. Summary of the Invention

[0006] In order to overcome the problems of low activity and poor stability of catalysts for acetylene hydrochlorination in the prior art, the present invention aims to provide a copper-based catalyst for catalyzing acetylene hydrochlorination, a preparation method, and an application thereof. The catalyst can be used to catalyze acetylene hydrochlorination, has hydrophobicity and anti-reduction ability, and has high activity and high stability.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A copper-based catalyst for catalyzing acetylene hydrochlorination comprises: a carrier, a phosphine-containing ligand, and a copper-containing stable metal precursor; the molar ratio of the stable metal precursor to the phosphine-containing ligand is 2:1-16:1, and the mass of copper in the copper-containing stable metal precursor is 5-10% of the mass of the copper-based catalyst.

[0009] Furthermore, the copper-containing stable metal precursor is a copper-containing salt compound.

[0010] Furthermore, the copper-containing salt compound is CuCl2, CuSO4 or Cu(NO3)2.

[0011] Furthermore, the carrier is activated carbon.

[0012] Furthermore, the carrier is spherical activated carbon, and the particle size of the spherical activated carbon is 40 to 60 meshes.

[0013] Furthermore, the phosphine-containing ligand is a phosphine oxide-containing compound.

[0014] Furthermore, the phosphine-containing ligand is one of dimethylphosphine oxide, trimethylphosphine oxide, triethylphosphine oxide, tri-n-propylphosphine oxide, tri-n-butylphosphine oxide and tri-n-octylphosphine oxide.

[0015] A method for preparing a copper-based catalyst for catalyzing acetylene hydrochlorination comprises the following steps:

[0016] adding a phosphine-containing ligand to an ethanol solution of a copper-containing stable metal precursor, mixing the mixture uniformly, and then adding a carrier, mixing the mixture uniformly to obtain a mixture;

[0017] The mixture is heated at 70-90° C. for 6-8 hours and then dried to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination.

[0018] A method for preparing a copper-based catalyst for catalyzing acetylene hydrochlorination reaction and its application in acetylene hydrochlorination reaction.

[0019] Furthermore, hydrogen chloride and acetylene gas are introduced into a reactor containing the copper-based catalyst according to any one of claims 1 to 6, the volume ratio of hydrogen chloride to acetylene is controlled to be 1.15:1, and the gas hourly space velocity of acetylene is controlled to be 180 h-1, and the acetylene hydrochlorination reaction is carried out at 180°C.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention introduces a specific phosphine-containing ligand to form a stable coordination structure with copper ions, significantly changing the electron cloud distribution and physicochemical properties of the catalyst surface. On the one hand, the catalyst surface's repulsion of water molecules is enhanced, achieving efficient hydrophobicity, inhibiting water vapor erosion of active sites, and maintaining the stability of the active components. On the other hand, the electronic state of the copper ions is regulated, enhancing their resistance to reduction and preventing excessive hydrogen reduction of the catalyst. The oxygen lone pair electrons (P=O) in the ligand provide electron density to the empty copper d orbitals, forming a stable high-valence copper species, thereby achieving high catalyst activity and good stability. The catalyst's service life is significantly extended. The molar ratio of copper to ligand is controlled within a range of 2:1 to 16:1; excessive or insufficient ligand content is detrimental to the catalyst's performance. The present invention utilizes a simple method to prepare a copper-based catalyst, eliminating a complex preparation process. This method not only improves the efficiency of catalyst preparation but also enhances its reproducibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The conversion rate of acetylene under different water vapor contents of 5% Cu-L1 / AC copper-based catalyst;

[0023] Figure 2 The selectivity of chloroethylene for 5% Cu-L1 / AC copper-based catalyst at different water vapor contents is shown;

[0024] Figure 3 is the acetylene conversion rate diagram of the copper-based catalyst under the condition of water vapor content of 800 ppm;

[0025] Figure 4 is the selectivity graph of vinyl chloride for copper-based catalyst under the condition of water vapor content of 800 ppm;

[0026] Figure 5 The acetylene conversion rate of the copper-based catalyst was measured with the mass fraction of hydrogen maintained at 1 wt.%;

[0027] Figure 6 The vinyl chloride selectivity of the copper-based catalyst was determined by maintaining the mass fraction of hydrogen at 1 wt.%;

[0028] Figure 7 This is the acetylene conversion rate diagram of 5% Cu-L1 / AC copper-based catalyst at different hydrogen contents;

[0029] Figure 8 This is the selectivity graph of vinyl chloride for 5% Cu-L1 / AC copper-based catalyst at different hydrogen contents. DETAILED DESCRIPTION

[0030] To facilitate understanding of the features and effects of the present invention by those skilled in the art, the following provides a general description and definition of the terms and expressions used in the specification and claims. Unless otherwise indicated, all technical and scientific terms used herein have the ordinary meanings as understood by those skilled in the art regarding the present invention. In the event of conflict, the definitions in this specification shall prevail.

[0031] The theories or mechanisms described and disclosed herein should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0032] Herein, all features such as values, amounts, amounts, and concentrations defined in numerical ranges or percentage ranges are for brevity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to include and specifically disclose all possible subranges and individual values ​​within the range (including integers and fractions).

[0033] In this document, unless otherwise specified, “include,” “including,” “contains,” “has” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0034] In this document, for the sake of brevity, not all possible combinations of the various technical features in each embodiment or example are described. Therefore, as long as there are no contradictions in the combination of these technical features, the various technical features in each embodiment or example can be combined in any way, and all possible combinations should be considered to be within the scope of this specification.

[0035] Below in conjunction with specific embodiment, further set forth the present invention.Should be understood that these embodiments are only used to illustrate the present invention and are not used in limiting the scope of the present invention.In addition, should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall equally within the scope limited by the appended claims of the application.

[0036] The examples of the present invention use conventional instruments and equipment in the art. Experimental methods in the following examples, where specific conditions are not specified, are generally performed under conventional conditions or according to the conditions recommended by the manufacturer. The various raw materials used in the following examples, unless otherwise specified, are conventional commercially available products, and their specifications are conventional in the art. In the present specification and the following examples, unless otherwise specified, "%" indicates weight percentage, "part" indicates weight part, and "ratio" indicates weight ratio.

[0037] The present invention will be further described in detail below with reference to specific embodiments, which are intended to explain the present invention rather than to limit it.

[0038] The present invention provides a copper-based catalyst for catalyzing acetylene hydrochlorination reaction, comprising: a carrier, a ligand and a stable metal precursor; the stable metal precursor is a copper-containing salt compound (i.e., an active component); the carrier is activated carbon, more preferably spherical activated carbon, and the particle size of the spherical activated carbon is 40-60 mesh; the ligand is a phosphine oxide compound containing carbon chains of different lengths; the molar ratio of the stable metal precursor to the ligand is 2:1-16:1, and the mass of copper in the catalyst is 5-10% of the total mass of the catalyst.

[0039] A method for preparing a copper-based catalyst for catalyzing acetylene hydrochlorination of the present invention comprises the following steps:

[0040] 1) adding a copper-containing salt compound to an ethanol solution and stirring to fully dissolve it; then adding a phosphine oxide compound and stirring to fully dissolve it and mix it evenly; then adding spherical activated carbon (as a carrier) and stirring to mix it evenly to obtain a mixture;

[0041] Wherein, the copper-containing salt compound is CuCl2, CuSO4 or Cu(NO3)2, preferably CuCl2.

[0042] The phosphine oxide compound is one of dimethyl phosphine oxide, trimethyl phosphine oxide, triethyl phosphine oxide, tri-n-propyl phosphine oxide, tri-n-butyl phosphine oxide and tri-n-octyl phosphine oxide.

[0043] 2) placing the mixture in a water bath at 70-90° C. for 6-8 hours; and then drying it in a forced air oven at 70-90° C. for 12-24 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination.

[0044] The molar ratio of copper to phosphine-containing ligand in the copper-based catalyst is 2:1-16:1.

[0045] A copper-based catalyst for catalyzing acetylene hydrochlorination reaction, wherein the loading amount of Cu atoms in the copper-based catalyst is 5-10 wt.%.

[0046] The application of the copper-based catalyst in the acetylene hydrochlorination reaction comprises the following steps:

[0047] Water vapor and hydrogen were introduced during the reaction to change the contents of water vapor and hydrogen in the reaction gas, and the acetylene conversion rate and vinyl chloride selectivity during the reaction were measured.

[0048] The water vapor content in the reaction gas was controlled between 800-1000 ppm, and the conversion rate and selectivity of the catalyst were tested at different water vapor contents; the hydrogen content in the reaction gas was controlled between 1-2%, and the conversion rate and selectivity of the catalyst were tested at different hydrogen contents.

[0049] The catalyst for catalyzing acetylene hydrochlorination in the present invention has hydrophobic and anti-reduction properties in the acetylene hydrochlorination reaction.

[0050] Example 1

[0051] In a 50mL beaker, add 0.74048g of copper chloride to 15mL of anhydrous ethanol and stir for 30 minutes. Then, add 0.107465g of dimethylphosphine oxide (dimethylphosphine oxide with a purity greater than 98%) and stir for 30 minutes. Then, add 6.1521g of 40-60 mesh spherical activated carbon and stir for 2 hours. Then, place the mixture in a 70°C constant temperature water bath for 6 hours. Finally, dry the mixture in a 70°C forced air drying oven for 12 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination, designated as 5% Cu-L1 / AC.

[0052] Example 2

[0053] In a 50mL beaker, add 0.74048g of copper chloride to 15mL of anhydrous ethanol and stir for 30 minutes. Then, add 0.1268g of 98% pure trimethylphosphine oxide and stir for 30 minutes. Then, add 6.1327g of 40-60 mesh spherical activated carbon and stir for 2 hours. Then, place the mixture in a 70°C waterbath for 6 hours. Finally, dry it in a 70°C forced air drying oven for 12 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination, designated 5% Cu-L2 / AC.

[0054] Example 3

[0055] In a 50mL beaker, add 0.74048g of copper chloride to 15mL of anhydrous ethanol and stir for 30 minutes. Then, add 0.1847g of 97% pure triethylphosphine oxide and stir for 30 minutes. Then, add 6.0748g of spherical 40-60 mesh activated carbon and stir for 2 hours. Then, place the mixture in a 70°C constant temperature water bath for 6 hours. Finally, dry the mixture in a 70°C forced air drying oven for 12 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination, designated 5% Cu-L3 / AC.

[0056] Example 4

[0057] In a 50mL beaker, add 0.74048g of copper chloride to 15mL of anhydrous ethanol and stir for 30 minutes. Then, add 0.2427g of 97% pure tri-n-propylphosphine oxide and stir for 30 minutes. Then, add 6.0169g of 40-60 mesh spherical activated carbon and stir for 2 hours. Then, place the mixture in a 70°C constant temperature water bath for 6 hours. Finally, dry the mixture in a 70°C forced air drying oven for 12 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination, designated as 5% Cu-L4 / AC.

[0058] Example 5

[0059] In a 50mL beaker, add 0.74048g of copper chloride to 15mL of anhydrous ethanol and stir for 30 minutes. Then, add 0.3006g of 97% pure tri-n-butylphosphine oxide and stir for 30 minutes. Then, add 5.9589g of 40-60 mesh spherical activated carbon and stir for 2 hours. Then, place the mixture in a 70°C constant temperature water bath for 6 hours. Finally, dry the mixture in a 70°C forced air drying oven for 12 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination, designated 5% Cu-L5 / AC.

[0060] Example 6

[0061] In a 50mL beaker, add 0.74048g of copper chloride to 15mL of anhydrous ethanol and stir for 30 minutes. Then, add 0.5323g of 97% pure tri-n-butylphosphine oxide and stir for 30 minutes. Then, add 5.7272g of 40-60 mesh spherical activated carbon and stir for 2 hours. Then, place the mixture in a 70°C waterbath for 6 hours. Finally, dry the mixture in a 70°C forced air drying oven for 12 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination, designated 5% Cu-L6 / AC.

[0062] Example 7

[0063] In a 50mL beaker, add 0.74048g of CuSO4 to 15mL of anhydrous ethanol and stir for 30 minutes. Then, add dimethylphosphine oxide (97% purity) and stir for 30 minutes. The molar ratio of copper to dimethylphosphine oxide is 2:1. Then, add 40-60 mesh spherical activated carbon and stir for 2 hours. Then, place the mixture in a 70℃ constant temperature water bath for 6 hours. Finally, dry it in a 70℃ forced air drying oven for 12 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination. The copper atomic loading in the copper-based catalyst is 5 wt.%.

[0064] Example 8

[0065] In a 50mL beaker, 0.74048g of Cu(NO₃)₂ was added to 15mL of anhydrous ethanol and stirred for 30 minutes. Triethylphosphine oxide (97% purity) was then added and stirred for 30 minutes. The molar ratio of copper to triethylphosphine oxide was 10:1. 40-60 mesh spherical activated carbon was then added and stirred for 2 hours. The mixture was then placed in a 70°C constant temperature water bath for 6 hours. Finally, the mixture was dried in a 70°C forced air drying oven for 12 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination. The copper-based catalyst had a Cu atomic loading of 10 wt.%.

[0066] Example 9

[0067] In a 50mL beaker, add 0.74048g of CuSO4 to 15mL of anhydrous ethanol and stir for 30 minutes. Then, add tri-n-propyl phosphine oxide (97% purity) and stir for 30 minutes. The molar ratio of copper to tri-n-propyl phosphine oxide is 5:1. Then, add 40-60 mesh spherical activated carbon and stir for 2 hours. Then, place the mixture in a 70℃ constant temperature water bath for 6 hours. Finally, dry it in a 70℃ forced air drying oven for 12 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination. The copper-based catalyst has a Cu atomic loading of 7 wt.%.

[0068] Example 10

[0069] In a 50mL beaker, add 0.74048g of CuSO4 to 15mL of anhydrous ethanol and stir for 30 minutes. Then, add tri-n-octylphosphine oxide (97% purity) and stir for 30 minutes. A molar ratio of copper to tri-n-octylphosphine oxide of 16:1 is used. Then, add 40-60 mesh spherical activated carbon and stir for 2 hours. Then, place the mixture in a 70℃ constant temperature water bath for 6 hours. Finally, dry it in a 70℃ forced air drying oven for 12 hours to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination. The copper-based catalyst has a Cu atomic loading of 8 wt.%.

[0070] Comparative Example 1

[0071] In a 50 mL beaker, add 0.74048 g of copper chloride to 15 mL of anhydrous ethanol and stir for 30 minutes. Then, add 6.2595 g of spherical activated carbon and stir for 2 hours. Then, place the mixture in a 70°C waterbath for 6 hours. Finally, dry it in a 70°C forced air drying oven for 12 hours to obtain a copper-based catalyst, designated as 5% Cu / AC.

[0072] In order to test the catalytic reaction performance of Examples 1-6 and Comparative Example 1, the performance of the catalyst was evaluated in a fixed-bed glass microreactor under normal pressure and 180°C. First, nitrogen was introduced into the pipeline 30 minutes before the start of the reaction to remove residual moisture and impurity gases. Subsequently, the nitrogen was switched to hydrogen chloride gas, which was used to activate the catalyst (3 mL) in the reactor for 30 minutes. When the temperature in the reactor rose to 180°C, acetylene gas was introduced into the reaction system, and the acetylene hydrochlorination reaction began immediately. The volume ratio of hydrogen chloride to acetylene (V HCl / V C2H2 ) is 1.15:1, and the acetylene gas hourly space velocity (GHSV) is controlled at 180h -1 After impurities are removed and dried, the gaseous products are quantitatively analyzed by gas chromatography. Finally, the performance of the catalyst is evaluated based on the calculated acetylene conversion and vinyl chloride selectivity. The total weight of the catalyst is calculated as follows: m 总 =m 载体 +m 稳定态金属前驱体 +m 配体 The calculation method for the loading of 5wt.% catalyst is: m Cu :m 总 =5wt.%.

[0073] In the present invention, two indicators including conversion rate and selectivity are used to evaluate the catalytic performance. The specific calculation is as follows:

[0074]

[0075] Among them, C inlet and C outlet Represents the concentration of acetylene (C2H2) at the reactor inlet and outlet respectively. C2H3Cl is the concentration of vinyl chloride (C2H3Cl) at the reactor outlet, Conversion is the conversion rate, and Selectivity is the selectivity.

[0076] Taking 5% Cu-L1 / AC catalyst as an example, water vapor is introduced during the reaction process, and the water vapor content is controlled at 800ppm, and the reaction temperature is maintained at 180°C. The water vapor content is then changed so that the water vapor content increases to 800ppm, 850ppm, 900ppm, 950ppm, and 1000ppm. Acetylene can react chemically with water vapor to produce ethanol, acetaldehyde, and other chlorinated derivatives. Changing the water vapor content in the reaction gas will affect the acetylene conversion rate and vinyl chloride selectivity. Copper-based catalysts containing different ligands also exhibit different performances in a water vapor atmosphere. The acetylene conversion rate and vinyl chloride selectivity during the reaction are measured separately, as shown in the following example. Figure 1 and Figure 2 As shown in the figure, with the increase of water vapor content, the conversion rate of acetylene and the selectivity of vinyl chloride tend to decrease slowly.

[0077] In the present invention, a mixture of hydrogen and acetylene is introduced during the reaction, and the mass fraction of hydrogen is controlled to be maintained at 1 wt.%, and the acetylene conversion rate and vinyl chloride selectivity of the catalyst are measured. Thereafter, the hydrogen content is changed so that the hydrogen content increases in steps of 1%, 1.2%, 1.4%, 1.6%, 1.8%, and 2%. Figure 7 and Figure 8 As shown in the figure, the acetylene conversion rate and vinyl chloride selectivity during the reaction were measured to explore the effect of different hydrogen contents on the catalyst activity. As the hydrogen content increased, the acetylene conversion rate and selectivity decreased.

[0078] The present invention compares the acetylene conversion and vinyl chloride selectivity of copper-based catalysts containing different ligands under the conditions of a water vapor content of 800 ppm and a hydrogen mass fraction maintained at 1 wt.%. Figure 3 and Figure 4 As shown in FIG, the copper-based catalyst containing the ligand dimethylphosphine oxide exhibits the best acetylene conversion and vinyl chloride selectivity at a water vapor content of 800 ppm, with the acetylene conversion reaching 64.6% and the vinyl chloride selectivity reaching 93.96%. Figure 5 and Figure 6 As shown, the copper-based catalyst containing the ligand dimethylphosphine oxide exhibited the best acetylene conversion and vinyl chloride selectivity under the condition of a hydrogen content of 1 wt.%, with the acetylene conversion reaching 61.39% and the vinyl chloride selectivity reaching 90.39%.

[0079] For a copper-based catalyst containing the ligand dimethylphosphine oxide, the activity and selectivity of the catalyst remain high when a certain amount of water vapor is present in the reaction gas. A certain amount of hydrogen has minimal impact on the activity and selectivity of the catalyst, demonstrating that the catalyst exhibits excellent hydrophobicity and reduction resistance in the acetylene hydrochlorination reaction. This invention not only improves the efficiency of vinyl chloride monomer production, but also extends the catalyst's service life and reduces production costs. Furthermore, the catalyst contains no harmful substances such as mercury, aligning with the concept of green chemistry and providing strong support for the sustainable development of the polyvinyl chloride industry.

[0080] The above description is merely a preferred embodiment of the present invention and is not intended to impose any limitation on the technical solution of the present invention. Those skilled in the art should understand that, without departing from the spirit and principles of the present invention, the technical solution can also be subjected to several simple modifications and replacements, and these modifications and replacements are also within the scope of protection covered by the claims.

Claims

1. A copper-based catalyst for catalyzing acetylene hydrochlorination, characterized in that: include: A carrier, a phosphine-containing ligand and a copper-containing stable metal precursor; the molar ratio of the stable metal precursor to the phosphine-containing ligand is 2:1-16:1, and the mass of copper in the copper-containing stable metal precursor is 5-10% of the mass of the copper-based catalyst.

2. The copper-based catalyst for catalyzing acetylene hydrochlorination according to claim 1, characterized in that The copper-containing stable metal precursor is a copper-containing salt compound.

3. The copper-based catalyst for catalyzing acetylene hydrochlorination according to claim 2, characterized in that The copper-containing salt compound is CuCl2, CuSO4 or Cu(NO3)2.

4. The copper-based catalyst for catalyzing acetylene hydrochlorination according to claim 2, characterized in that The carrier is activated carbon.

5. The copper-based catalyst for catalyzing acetylene hydrochlorination according to claim 1 or 4, characterized in that The carrier is spherical activated carbon, and the particle size of the spherical activated carbon is 40 to 60 meshes.

6. The copper-based catalyst for catalyzing acetylene hydrochlorination according to claim 1, characterized in that The phosphine-containing ligand is a phosphine-oxygen-containing compound.

7. The copper-based catalyst for catalyzing acetylene hydrochlorination according to claim 1 or 6, characterized in that The phosphine-containing ligand is one of dimethylphosphine oxide, trimethylphosphine oxide, triethylphosphine oxide, tri-n-propylphosphine oxide, tri-n-butylphosphine oxide and tri-n-octylphosphine oxide.

8. A method for preparing a copper-based catalyst for catalyzing acetylene hydrochlorination according to any one of claims 1 to 7, characterized in that: The following steps are involved: adding a phosphine-containing ligand to an ethanol solution of a copper-containing stable metal precursor, mixing the mixture uniformly, and then adding a carrier, mixing the mixture uniformly to obtain a mixture; The mixture is heated at 70-90° C. for 6-8 hours and then dried to obtain a copper-based catalyst for catalyzing acetylene hydrochlorination.

9. Use of the preparation method of the copper-based catalyst for catalyzing acetylene hydrochlorination according to any one of claims 1 to 6 in acetylene hydrochlorination.

10. The use according to claim 9, characterized in that Hydrogen chloride and acetylene gas are introduced into a reactor containing the copper-based catalyst according to any one of claims 1 to 6, the volume ratio of hydrogen chloride to acetylene is controlled to be 1.15:1, and the gas hourly space velocity of acetylene is controlled to be 180 h-1, and the acetylene hydrochlorination reaction is carried out at 180°C.

Citation Information

Cited By

  • A copper-based catalyst for acetylene hydrochlorination reaction, its preparation method and application

    CN122644128A