Method for reducing silver powder production wastewater treatment difficulty by adopting silver sulfate as precursor

By using silver sulfate as a precursor and calcium oxide precipitation-microporous aeration treatment, combined with the method of recycling ammonia resources, the problems of high nitrate, high ammonia nitrogen and high organic matter in silver powder production wastewater were solved, and efficient preparation of silver powder and low-cost treatment of wastewater were achieved.

CN120622719APending Publication Date: 2025-09-12FUZHOU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202510813283.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-18
Publication Date
2025-09-12

AI Technical Summary

Technical Problem

The existing silver powder production process causes serious pollution in the wastewater due to high nitrate, high ammonia nitrogen and high organic matter. The traditional biological treatment method has a long treatment cycle and wastes resources. It is difficult to effectively remove the organic matter residue on the surface of the silver powder, which increases the cleaning cost.

Method used

Silver sulfate is used as a precursor, and ultrafine silver powder is prepared and wastewater is treated through calcium oxide precipitation-microporous aeration treatment, combined with the method of ammonia resource recycling. Sulfate ions are used as a protective agent to reduce nitrate pollution, and ammonia resources are recovered through aeration ammonia extraction technology.

Benefits of technology

The method achieves effective removal of inorganic residues on the surface of silver powder, reduces wastewater treatment costs, improves the sphericity and dispersibility of silver powder, realizes the recycling of ammonia resources, and simplifies the wastewater treatment process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120622719A_ABST
    Figure CN120622719A_ABST
Patent Text Reader

Abstract

The invention discloses a method for reducing silver powder production wastewater treatment difficulty by using silver sulfate as a precursor. The method comprises the following steps: dissolving silver sulfate in ammonia water to form a silver-ammonia complex solution, adding a reducing agent, reacting, filtering to obtain a solid and a reaction tail liquid, washing the solid until the conductivity is less than 25 [mu] s / cm, drying, crushing and screening to obtain superfine silver powder; adding calcium oxide into the obtained reduction tail liquid, filtering after reaction to obtain calcium sulfate precipitate and ammonia-rich reduction tail liquid, adding an aerator into the ammonia-rich reduction tail liquid, introducing compressed air for aeration treatment, absorbing volatilized ammonia gas by using a serial absorption device, and recycling the obtained ammonia gas to dissolve silver sulfate. Silver sulfate is used as a silver precursor, and the growth of a silver crystal face is regulated and controlled through the directional adsorption effect of sulfate ions; and the reduction tail liquid is subjected to calcium oxide precipitation-aeration treatment-series adsorption, so that ammonia resources are recycled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of precious metal material preparation and chemical waste liquid treatment, and in particular to a method for reducing the difficulty of silver powder production wastewater treatment by using silver sulfate as a precursor. Background Art

[0002] Ultrafine spherical silver powders, due to their excellent electrical properties, optical response, catalytic activity, and thermal stability, have significant applications in consumer electronics, catalysts, chemical sensing, and surface-enhanced Raman scattering. With technological advancements, the global annual demand for silver powder continues to grow, and the development of green silver powder production processes has become a key research direction for efficient resource utilization. Current industrial silver powder production methods primarily include thermal plasma treatment, spray pyrolysis, electrochemical reduction, chemical reduction, and microemulsion technology. Among these, wet chemical reduction, based on a silver-ammine complex precursor and a reducing agent, has become the mainstream production process due to its mild reaction conditions, highly controllable morphology, low equipment investment, and simple production process. However, this technology still faces two major technical bottlenecks: First, the reduction process requires the addition of a high-molecular-weight organic compound as a silver powder shape protector. This organic compound chemically adsorbs onto the silver particle surface, forming a dense 1-3 nm coating that allows for targeted manipulation of the silver powder morphology. However, this type of protective agent is difficult to completely remove through conventional water-washing and alcohol-washing processes, resulting in excessively high levels of organic matter residue on the silver powder surface, significantly reducing sintering activity and increasing subsequent cleaning costs. Furthermore, the production wastewater generated by the reaction system is characterized by high levels of organic matter, nitrates, and ammonia nitrogen. High concentrations of nitrates easily cause scaling in evaporation and crystallization equipment, while the combined pollution of ammonia nitrogen and organic matter severely inhibits microbial activity, leading to long treatment cycles for traditional biological treatment methods (such as nitrification and denitrification) and sensitivity to microbial growth conditions and environmental factors. Furthermore, the ammonia resources contained in the wastewater are not effectively recycled, a situation that not only leads to significant waste of resources but also further increases the cost of wastewater treatment.

[0003] Therefore, it is necessary to find a method to solve the problem of high nitrate, high ammonia nitrogen and high organic matter in wastewater during the traditional wet reduction silver powder production process. Summary of the Invention

[0004] In order to solve the above technical problems, the present invention proposes a method for preparing ultrafine silver powder at low cost by using silver sulfate as a precursor and aerating to extract ammonia. In this method, silver sulfate (Ag2SO4) replaces traditional silver nitrate (AgNO3) to form a silver-ammine complex solution with ammonia water. Under the action of a protective agent of sulfate ion, spherical silver powder is obtained by reduction with a reducing solution. The obtained silver powder has the characteristics of good sphericity, good dispersibility and narrow particle size distribution; the reduction wastewater is treated by calcium oxide precipitation-microporous aeration to achieve the recycling of ammonia resources.

[0005] To achieve the above object, the present invention provides the following solutions: A method for reducing the difficulty of treating silver powder production wastewater using silver sulfate as a precursor comprises the following steps: (1) dissolving silver sulfate in ammonia water to form a silver ammonia complex solution, wherein the silver ion concentration in the ammonia complex solution is 20-100 g / L; (2) Add a reducing agent solution with a concentration of 10-50 g / L to the silver ammonia complex solution under stirring, maintain the temperature at 20-80 °C, react for 10-15 minutes, filter to obtain a solid and a reaction tail liquid, wash the solid until the conductivity is less than 25 μs / cm, dry it, and grind and screen it to obtain ultrafine silver powder; (3) adding calcium oxide to the reduced tail liquid obtained in step (2), filtering after the reaction to obtain calcium sulfate precipitate and ammonia-rich reduced tail liquid; (4) Add an aerator to the ammonia-rich reduction tail liquid, introduce compressed air and aerate it at a certain flow rate, and use a series absorption device to absorb the volatilized ammonia. The obtained ammonia can be recycled to dissolve silver sulfate.

[0006] Furthermore, the concentration of the ammonia water in step (1) is 1-5 mol / L.

[0007] Furthermore, in step (2), the reducing agent is one or more combinations of ethanol, ascorbic acid, hydrazine hydrate, sodium borohydride, sodium bisulfite, and glucose, and the reducing agent solution is prepared by dissolving the reducing agent in 5% ammonia water.

[0008] Furthermore, the stirring speed in step (2) is 500-1000 r / min, and the reducing agent solution is added to the silver ammonia complex solution at a speed of 5-10 L / min.

[0009] Furthermore, the particle size distribution D of the ultrafine silver powder obtained in step (2) is 10 At 0.1-0.2 μm, D 50 At 0.6 μm, D 90 <0.90 μm, tap density 5 ~6 g / cm 3 , with a specific surface area of ​​1.2~1.5m 2 / g Furthermore, the molar ratio of calcium oxide to silver sulfate in the reduction tail liquid in step (3) is 1 to 1.5.

[0010] Furthermore, the compressed air flow rate in step (4) is 10~50 m 3 / h, the exposure treatment time is 20~40min, and the temperature is maintained at 50℃ during the exposure treatment process.

[0011] Furthermore, the absorption rate of the volatilized ammonia gas absorbed by the series device in step (4) is ≥98%. Compared with the existing silver powder preparation method, the advantages and beneficial effects of the present invention are: This invention innovatively proposes a low-cost method for preparing ultrafine silver powder using silver sulfate as a precursor and aeration to extract ammonia. Silver sulfate replaces silver nitrate, completely eliminating nitrate pollution and reducing the burden of wastewater treatment. Sulfate ions simultaneously serve as a protective agent to prepare spherical silver powder. Leveraging the volatility of ammonia molecules (NH3) in wastewater, microporous aeration technology is combined to efficiently extract ammonia gas, which is then absorbed by deionized water to produce a reusable ammonia solution, achieving a closed-loop ammonia resource cycle. Silver sulfate is dissolved in an ammonia solution to form a silver-ammine complex solution. A reducing solution is prepared and added to the silver-ammine complex solution. Reaction conditions are controlled, and solid-liquid separation is performed to produce ultrafine spherical silver powder and reduced wastewater. The reduced wastewater is then treated through a calcium oxide precipitation-aeration-multi-stage evaporative liquid absorption process to precipitate the main salt ions in the wastewater. Ammonia in the solution is then aerated and absorbed by deionized water. The resulting dilute ammonia solution is then reused to dissolve the silver sulfate. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 Schematic diagram of the process of the present invention.

[0013] Figure 2 This is a scanning electron microscope image of the silver powder obtained in Example 1 of the present invention at a magnification of 30,000 times.

[0014] Figure 3 This is a scanning electron microscope image of the silver powder obtained in Example 2 of the present invention at a magnification of 30,000 times. DETAILED DESCRIPTION

[0015] In order to make the contents of the present invention easier to understand, the technical solutions of the present invention are further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0016] Example 1 In the embodiment of the present invention, the steps for preparing ultrafine silver powder at low cost by using sulfate as a precursor and a synergistic process of aeration and ammonia extraction are as follows: (1) Weigh 31.18 g of silver sulfate and dissolve it in 1000 mL of 20% ammonia solution to form a silver-ammine complex solution with a silver concentration of 0.2 mol / L.

[0017] (2) Weigh 17.61 g of ascorbic acid and dissolve it in 1000 mL of 5% ammonia solution to obtain an ascorbic acid solution with a concentration of 0.1 mol / L.

[0018] (3) The ascorbic acid solution was pumped into the silver ammonia complex solution at a stirring speed of 1000 r / min using a peristaltic pump at a flow rate of 5 L / min. The reaction was continued for 10 min. After filtration, the solid-liquid separation was performed to obtain a reducing tail liquid and a solid. The solid was filtered and washed until the conductivity was less than 25 μs / cm, dried at 60 °C for 10 h, and crushed and sieved to obtain ultrafine silver powder.

[0019] (4) Add calcium oxide to the reduction tail liquid at a molar ratio of sulfate to calcium oxide of 1:1.5, stir and settle for 30 minutes, and filter to obtain calcium sulfate precipitate and ammonia-rich reduction waste liquid.

[0020] (5) Add an aerator to the ammonia-rich reduction wastewater and introduce compressed air at a speed of 15 m 3 Aeration was performed for 30 minutes at a flow rate of 100 / h. The solution temperature was maintained at 50°C during the aeration process to accelerate the volatilization of ammonia. A two-stage series absorption device was used to absorb the volatilized ammonia (first, the aerator was added to the solution to initiate aeration, while the device was used to absorb the volatilized ammonia). The resulting ammonia was dissolved in water and prepared into a 20% concentration of ammonia water.

[0021] Example 2 (1) Weigh 31.18 g of silver sulfate and dissolve it in 1000 mL of 20% ammonia solution to form a silver-ammine complex solution with a silver concentration of 0.2 mol / L.

[0022] (2) Weigh 3.783 g of sodium borohydride and dissolve it in 1000 mL of 5% ammonia solution to obtain a sodium borohydride solution with a concentration of 0.1 mol / L.

[0023] (3) The sodium borohydride solution was pumped into the silver ammonia complex solution at a stirring speed of 1000 r / min using a peristaltic pump at a flow rate of 5 L / min. The reaction was carried out for 10 minutes. After filtration, the solid-liquid separation was performed to obtain a reduction tail liquid and a solid. The solid was filtered and washed until the conductivity was less than 25 μs / cm, dried at 60 °C for 10 hours, and crushed and sieved to obtain ultrafine silver powder.

[0024] (4) Add calcium oxide to the reduction tail liquid at a molar ratio of sulfate to calcium oxide of 1:1.5, stir and settle for 30 minutes, and filter to obtain calcium sulfate precipitate and ammonia-rich reduction waste liquid.

[0025] (5) Add an aerator to the ammonia-rich reduction wastewater and introduce compressed air at a speed of 15 m 3 Aeration was performed for 30 minutes at a flow rate of 100 / h. The solution temperature was maintained at 50°C during the aeration process to accelerate the volatilization of ammonia. A two-stage series absorption device was used to absorb the volatilized ammonia. The resulting ammonia was dissolved in water and prepared into a 20% ammonia solution.

[0026] Comparative Example 1 (1) Weigh 33.97 g of silver nitrate and dissolve it in 1000 mL of 20% ammonia solution to form a silver-ammine complex solution with a silver concentration of 0.2 mol / L.

[0027] (2) Weigh 17.61 g of ascorbic acid and dissolve it in 1000 mL of 5% ammonia solution to obtain a reducing solution with an ascorbic acid concentration of 0.1 mol / L.

[0028] (3) The ascorbic acid solution was pumped into the silver ammonia complex solution at a stirring speed of 1000 r / min using a peristaltic pump at a flow rate of 5 L / min. The reaction was continued for 10 min. After filtration, the solid-liquid separation was performed to obtain a reducing tail liquid and a solid. The solid was filtered and washed until the conductivity was less than 25 μs / cm, dried at 60 °C for 10 h, and crushed and sieved to obtain ultrafine silver powder.

[0029] (4) Add calcium oxide to the reduction tail liquid at a molar ratio of sulfate to calcium oxide of 1:1.5, stir and settle for 30 minutes, and filter to obtain calcium sulfate precipitate and ammonia-rich reduction waste liquid.

[0030] (5) Add an aerator to the reduced tail liquid, introduce compressed air and 3 Aeration was performed for 30 minutes at a flow rate of 100 / h. The solution temperature was maintained at 50°C during the aeration process to accelerate the volatilization of ammonia. A two-stage series absorption device was used to absorb the volatilized ammonia. The resulting ammonia was dissolved in water and prepared into a 20% ammonia solution.

[0031] Comparative Example 2 The same as Comparative Example 1, except that the reducing agent was changed to 3.783 g of sodium borohydride.

[0032] Calculation of ammonia absorption rate: Where, C 0 、C 1 are the ammonia concentrations in the solution before and after absorption by the series absorption device, mol / L; v 0 、v 1 are the volume of solution before and after absorption by the series absorption device, L; The performance comparison of Examples 1 and 2 and Comparative Examples 1 and 2 is shown in Table 1 below: Table 1 Performance test data of Examples 1-2 and Comparative Examples 1-2 It can be seen from Table 1 that the silver powder in Examples 1 and 2 of the present invention is spherical in shape, with a narrow particle size distribution range and a particle size distribution D 10 At 0.1-0.2 μm, D 50 At 0.6 μm, D 90 <0.90 μm and the tap density of the prepared samples is >5 g / cm 3 ; Combined with Figure 2 、 3 The corresponding silver powder has good sphericity and dispersibility.

[0033] The embodiments described above are merely descriptions of preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Without departing from the spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by persons skilled in the art should fall within the scope of protection defined by the claims of the present invention.

Claims

1. A method for reducing the difficulty of treating silver powder production wastewater using silver sulfate as a precursor, characterized in that: The following steps are involved: (1) dissolving silver sulfate in ammonia water to form a silver ammonia complex solution, wherein the silver ion concentration in the ammonia complex solution is 20-100 g / L; (2) Add a reducing agent solution with a concentration of 10-50 g / L to the silver ammonia complex solution under stirring, maintain the temperature at 20-80 °C, react for 10-15 minutes, filter to obtain a solid and a reaction tail liquid, wash the solid until the conductivity is less than 25 μs / cm, dry, crush and sieve to obtain ultrafine silver powder; (3) adding calcium oxide to the reduced tail liquid obtained in step (2), filtering after the reaction to obtain calcium sulfate precipitate and ammonia-rich reduced tail liquid; (4) Add an aerator to the ammonia-rich reduction tail liquid, introduce compressed air and aerate it at a certain flow rate, and use a series absorption device to absorb the volatilized ammonia. The obtained ammonia can be recycled to dissolve silver sulfate.

2. The method according to claim 1, wherein: The concentration of the ammonia water in step (1) is 1-5 mol / L.

3. The method according to claim 1, wherein: In step (2), the reducing agent is one or more combinations of ethanol, ascorbic acid, hydrazine hydrate, sodium borohydride, sodium bisulfite, and glucose, and the reducing agent solution is prepared by dissolving the reducing agent in 5% ammonia water.

4. The method according to claim 1, wherein: The stirring speed in step (2) is 500-1000 r / min, and the reducing agent solution is added to the silver ammonia complex solution at a speed of 5-10 L / min.

5. The method according to claim 1, wherein: The particle size distribution D of the ultrafine silver powder obtained in step (2) 10 At 0.1-0.2 μm, D 50 At 0.6 μm, D 90 <0.90 μm, tap density 5 ~6 g / cm 3 , with a specific surface area of ​​1.2~1.5m 2 / g.

6. The method according to claim 1, wherein: The molar ratio of calcium oxide to silver sulfate in the reduction tail liquid in step (3) is 1 to 1.

5.

7. The method according to claim 1, wherein: The compressed air flow rate in step (4) is 10~50 m 3 / h, the exposure treatment time is 20~40min, and the temperature is maintained at 50℃ during the exposure treatment process.

8. The method according to claim 1, wherein: The absorption rate of the volatilized ammonia gas absorbed by the series device in step (4) is ≥98%.

Citation Information

Patent Citations

  • Production method for separating silver from silver waste liquid

    CN107058757A

  • Grain-size-controllable high dispersion type spherical ultrathin silver powder preparing method

    CN111331150A

  • Method for green treatment and cyclic utilization of vanadium precipitation wastewater

    CN117466475A

  • Method of managing silver solution and method of producing silver powder

    JP2015071813A