Photovoltaic cell, preparation method thereof and photovoltaic module

CN120769597AActive Publication Date: 2025-10-10ZHEJIANG JINKO SOLAR CO LTD

Patent Information

Application Number
CN202511274244.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-09-08
Publication Date
2025-10-10
Estimated Expiration
2045-09-08

AI Technical Summary

Technical Problem

然而,传统的硅基光伏电池中,钝化层对掺杂硅层的钝化性能有限

Benefits of technology

[0030] Furthermore, in conventional plasma nitridation treatment, a process gas comprising only ammonia is used for treatment, which only forms an aluminum oxynitride layer, and its surface is rough and has poor bonding with the anti-reflection layer. However, the present application uses a process gas comprising silane and ammonia to perform plasma nitridation treatment on the aluminum oxide layer, so that the aluminum oxide layer is converted into an aluminum oxynitride layer. At the same time, a silicon nitride layer is formed on the surface of the aluminum oxynitride layer away from the silicon substrate, which can enhance the interfacial bonding force, improve the bonding force between the aluminum oxynitride layer and the anti-reflection layer, and improve the open circuit voltage of the photovoltaic cell. At the same time, the silicon nitride layer can also protect the aluminum oxynitride layer during the preparation of the anti-reflection layer, thereby increasing the negative fixed charge in the aluminum oxynitride layer. This can thereby achieve a higher conversion efficiency of the photovoltaic cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120769597A_ABST
    Figure CN120769597A_ABST
Patent Text Reader

Abstract

The invention relates to a photovoltaic cell, a preparation method thereof and a photovoltaic module. The preparation method of the photovoltaic cell comprises the following steps that a photovoltaic cell intermediate is provided, and the photovoltaic cell intermediate comprises a silicon substrate and an aluminum oxide layer located on at least one surface of the silicon substrate; and carrying out plasma nitriding treatment on the aluminum oxide layer by using a process gas comprising silane and ammonia gas so as to convert the aluminum oxide layer into an aluminum oxynitride layer, and forming a silicon nitride layer on the surface of the aluminum oxynitride layer far away from the silicon substrate. According to the preparation method of the photovoltaic cell, damage to the film layer in the preparation process of the aluminum oxynitride layer can be reduced, the interface defect state density is reduced, the passivation effect is improved, and then the conversion efficiency of the photovoltaic cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photovoltaic technology, and in particular to photovoltaic cells and methods for preparing the same, and photovoltaic modules. Background Art

[0002] Silicon-based photovoltaic cells are a widely used type of photovoltaic cell. In silicon-based photovoltaic cells, P-type silicon and N-type silicon are formed through doping, creating a PN junction at their junction, generating a built-in electric field. The passivation layer is a key component in improving the photoelectric conversion efficiency of photovoltaic cells. This is achieved primarily by passivating the doped silicon layer to reduce surface recombination. However, in traditional silicon-based photovoltaic cells, the passivation layer has limited performance in passivating the doped silicon layer. Summary of the Invention

[0003] Based on this, it is necessary to provide a photovoltaic cell and its preparation method, and a photovoltaic module. The photovoltaic cell preparation method of the present application can reduce the damage to the film layer during the preparation of the aluminum oxynitride layer, reduce the interface defect state density, improve the passivation effect, and thus improve the conversion efficiency of the photovoltaic cell.

[0004] In a first aspect, the present application provides a method for preparing a photovoltaic cell, comprising the following steps:

[0005] Providing a photovoltaic cell intermediate, the photovoltaic cell intermediate comprising a silicon substrate and an aluminum oxide layer located on at least one surface of the silicon substrate;

[0006] The aluminum oxide layer is subjected to a plasma nitridation treatment using a process gas including silane and ammonia, so as to transform the aluminum oxide layer into an aluminum oxynitride layer, and form a silicon nitride layer on a surface of the aluminum oxynitride layer away from the silicon substrate.

[0007] In some embodiments, the flow ratio of ammonia to silane in the process gas is (100-1000):1.

[0008] In some embodiments, in the process gas, the flow rate of silane is 0.1 sccm~1 sccm, and the flow rate of ammonia is 100 sccm~300 sccm.

[0009] In some embodiments, the difference in thickness between the aluminum oxide layer and the aluminum oxynitride layer is less than or equal to 1 nm.

[0010] In some embodiments, the power of the plasma nitridation process is 200W~500W.

[0011] In some embodiments, the pressure of the plasma nitridation process is 500 mTorr to 1000 mTorr.

[0012] In some embodiments, the temperature of the plasma nitridation treatment is 350° C. to 450° C.

[0013] In some embodiments, the plasma nitridation treatment lasts for 1 min to 5 min.

[0014] In some embodiments, the plasma nitridation process satisfies at least one of the following characteristics:

[0015] (1) Control the nitrogen concentration in the aluminum nitride oxide layer to 5×10 20 cm -3 ~1×10 22 cm -3 ;

[0016] (2) The thickness of the silicon nitride layer is controlled to be 1 nm to 3 nm.

[0017] In some embodiments, the method for preparing the photovoltaic cell intermediate comprises the following steps:

[0018] providing a silicon substrate;

[0019] forming a first doped silicon layer and a second doped silicon layer on two oppositely disposed surfaces of the silicon substrate, wherein the first doped silicon layer is doped with P-type doping and the second doped silicon layer is doped with N-type doping;

[0020] The aluminum oxide layer is formed on a surface of the first doped silicon layer away from the silicon substrate.

[0021] In a second aspect, the present application provides a photovoltaic cell comprising: a silicon substrate, and an aluminum oxynitride layer and a silicon nitride layer stacked on the surface of the silicon substrate, the aluminum oxynitride layer being located between the silicon nitride layer and the silicon substrate, and the thickness of the silicon nitride layer being 1 nm to 3 nm.

[0022] In some embodiments, the silicon substrate has a first surface and a second surface disposed opposite to each other;

[0023] A first doped silicon layer, an aluminum oxynitride layer, a silicon nitride layer, and a first anti-reflection layer are sequentially stacked on the first surface; the first doped silicon layer is P-type doped; a first electrode is provided on the first anti-reflection layer, and the first electrode is electrically connected to the first doped silicon layer;

[0024] A tunneling oxide layer, a second doped silicon layer and a second anti-reflection layer are sequentially stacked on the second surface; the doping type of the second doped silicon layer is N-type doping; a second electrode is provided on the second anti-reflection layer, and the second electrode is electrically connected to the second doped silicon layer.

[0025] In a third aspect, the present application provides a photovoltaic module, comprising:

[0026] cover;

[0027] At least one cell string, the cell string comprising a photovoltaic cell prepared by any of the above-described methods for preparing a photovoltaic cell, or a photovoltaic cell described in any of the above-described methods;

[0028] and an encapsulation layer, wherein the encapsulation layer is located between the cover plate and the battery string, and the cover plate is connected to the battery string through the encapsulation layer.

[0029] In conventional plasma nitridation, a process gas consisting solely of ammonia is used. The bombardment of high-energy hydrogen ions (H+) can damage the surface of the aluminum oxide layer, resulting in an interface state defect density as high as 1×10 12 cm -2 eV -1 In the above-mentioned method for preparing photovoltaic cells, a process gas including silane and ammonia is used to perform plasma nitridation on the aluminum oxide layer to convert the aluminum oxide layer into an aluminum oxynitride layer. During the plasma nitridation process, silane can react with high-energy hydrogen ions as follows: SiH4+H + →SiH3+H2 reduces the energy of hydrogen ions by 30%~50%, reduces the damage of high-energy hydrogen ions to the aluminum oxide layer, and can also reduce the interface state defect density to 5×10 10 cm -2 eV -1 the following.

[0030] Furthermore, in conventional plasma nitridation treatment, a process gas comprising only ammonia is used for treatment, which only forms an aluminum oxynitride layer, and its surface is rough and has poor bonding with the anti-reflection layer. However, the present application uses a process gas comprising silane and ammonia to perform plasma nitridation treatment on the aluminum oxide layer, so that the aluminum oxide layer is converted into an aluminum oxynitride layer. At the same time, a silicon nitride layer is formed on the surface of the aluminum oxynitride layer away from the silicon substrate, which can enhance the interfacial bonding force, improve the bonding force between the aluminum oxynitride layer and the anti-reflection layer, and improve the open circuit voltage of the photovoltaic cell. At the same time, the silicon nitride layer can also protect the aluminum oxynitride layer during the preparation of the anti-reflection layer, thereby increasing the negative fixed charge in the aluminum oxynitride layer. This can thereby achieve a higher conversion efficiency of the photovoltaic cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A schematic diagram of a structure for preparing a first doped silicon layer on a first surface of a silicon substrate;

[0032] Figure 2 For Figure 1 A schematic diagram of a structure for preparing a tunnel oxide layer and a second doped silicon layer based on the structure shown;

[0033] Figure 3 For Figure 2 Schematic diagram of the structure of preparing an aluminum oxide layer based on the structure shown;

[0034] Figure 4 For Figure 3 A schematic diagram of a structure in which an aluminum oxynitride layer and a silicon nitride layer are formed on the basis of the structure shown;

[0035] Figure 5 For Figure 4 A schematic diagram of a structure in which a first anti-reflection layer and a second anti-reflection layer are formed on the basis of the structure shown;

[0036] Figure 6 For Figure 5 A schematic diagram of the structure of forming the first electrode and the second electrode on the basis of the structure shown.

[0037] Description of reference numerals:

[0038] 10 - silicon substrate; 20 - first doped silicon layer; 30 - tunneling oxide layer; 40 - second doped silicon layer; 50 - aluminum oxide layer; 60 - aluminum oxynitride layer; 70 - silicon nitride layer; 80 - first anti-reflection layer; 90 - second anti-reflection layer; 100 - first electrode; 110 - second electrode. DETAILED DESCRIPTION

[0039] To make the above-mentioned objects, features, and advantages of the present application more clearly understood, the specific embodiments of the present application are described in detail below. The following description sets forth many specific details to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the scope of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0041] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0042] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be understood to indicate or imply relative importance or implicitly specify the number of the technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of such features. In the description of this application, "plurality" means at least two, for example, two, three, etc., unless otherwise specifically defined.

[0043] In this application, unless otherwise specified or limited, the terms "installed," "connected," "connect," "fixed," etc. should be understood in a broad sense. For example, they can refer to fixed connection, detachable connection, or integration; mechanical connection or electrical connection; direct connection or indirect connection through an intermediate medium; internal communication between two elements or interaction between two elements, unless otherwise specified. Those skilled in the art will understand the specific meanings of the above terms in this application based on specific circumstances.

[0044] Reference Figures 1 to 6 As shown, an embodiment of the present application provides a method for preparing a photovoltaic cell, comprising the following steps:

[0045] A photovoltaic cell intermediate is provided, the photovoltaic cell intermediate including a silicon substrate 10 and an aluminum oxide layer 50 located on at least one surface of the silicon substrate 10;

[0046] The aluminum oxide layer 50 is subjected to a plasma nitridation treatment using a process gas including silane and ammonia, so as to transform the aluminum oxide layer 50 into an aluminum oxynitride layer 60 , and form a silicon nitride layer 70 on a surface of the aluminum oxynitride layer 60 away from the silicon substrate 10 .

[0047] In conventional plasma nitridation, a process gas consisting solely of ammonia is used for treatment. The bombardment of high-energy hydrogen ions (H+) can damage the surface of the aluminum oxide layer 50, resulting in an interface state defect density as high as 1×10 12 cm -2 eV -1In the above-mentioned method for preparing a photovoltaic cell, a process gas including silane and ammonia is used to perform plasma nitridation on the aluminum oxide layer 50, so as to convert the aluminum oxide layer 50 into an aluminum nitride layer 60. During the plasma nitridation process, silane can react with high-energy hydrogen ions as follows: SiH4+H + →SiH3+H2 reduces the energy of hydrogen ions by 30%~50%, reduces the damage of high-energy hydrogen ions to the aluminum oxide layer 50, and can also reduce the interface state defect density to 5×10 10 cm -2 eV -1 the following.

[0048] Furthermore, in conventional plasma nitridation treatment, a process gas comprising only ammonia is used for treatment, which only forms an aluminum oxynitride layer 60, and its surface is rough and has poor bonding strength with the anti-reflection layer. However, the present application uses a process gas comprising silane and ammonia to perform plasma nitridation treatment on the aluminum oxide layer 50, so that the aluminum oxide layer 50 is converted into an aluminum oxynitride layer 60. At the same time, a silicon nitride layer 70 is formed on the surface of the aluminum oxynitride layer 60 away from the silicon substrate 10, which can enhance the interfacial bonding strength, improve the bonding strength between the aluminum oxynitride layer 60 and the anti-reflection layer, and improve the open circuit voltage of the photovoltaic cell. At the same time, the silicon nitride layer 70 can also protect the aluminum oxynitride layer 60 during the preparation of the anti-reflection layer, thereby increasing the negative fixed charge in the aluminum oxynitride layer 60. This can thereby achieve a higher conversion efficiency of the photovoltaic cell.

[0049] In some embodiments, the flow ratio of ammonia to silane in the process gas is (100-1000):1.

[0050] When the flow ratio of ammonia to silane in the process gas is too low, that is, when the amount of ammonia is too small, it is easy to cause poor nitridation effect on the aluminum oxide layer 50, low nitrogen concentration in the nitrided aluminum oxide layer 60, and limited passivation effect. When the flow ratio of ammonia to silane in the process gas is too high, that is, when the amount of silane is too small, it is easy to cause poor effect in reducing the bombardment damage of high-energy hydrogen ions on the aluminum oxide layer 50, and limited effect in reducing the interface state defect density. Optionally, the flow ratio of ammonia to silane in the process gas is 100:1, 200:1, 300:1, 400:1, 500:1, 600:1, 700:1, 800:1, 900:1 or 1000:1, or the flow ratio of ammonia to silane in the process gas can also be within the range between any two of the above flow ratios.

[0051] In some embodiments, in the process gas, the flow rate of silane is 0.1 sccm-1 sccm, and the flow rate of ammonia is 100 sccm-300 sccm.

[0052] Within the flow range of the silane and the flow range of the ammonia, the effect of the conversion of the aluminum oxide layer 50 into the aluminum oxynitride layer 60 is better, and the aluminum oxynitride layer 60 can have a proper nitrogen concentration, and the effect of reducing the bombardment damage of the high-energy hydrogen ions to the aluminum oxide layer 50 and reducing the interface state defect density is better. Optionally, the flow of the silane in the process gas is 0.1 sccm, 0.2 sccm, 0.3 sccm, 0.4 sccm, 0.5 sccm, 0.6 sccm, 0.7 sccm, 0.8 sccm, 0.9 sccm, or 1 sccm, or the flow of the silane in the process gas can also be within the range between any two of the above flows. Optionally, the flow of the ammonia in the process gas is 100 sccm, 120 sccm, 140 sccm, 160 sccm, 180 sccm, 200 sccm, 220 sccm, 240 sccm, 260 sccm, 280 sccm, or 300 sccm, or the flow of the ammonia can also be within the range between any two of the above flows.

[0053] In some embodiments, the difference between the thickness of the aluminum oxide layer 50 and the thickness of the aluminum oxynitride layer 60 is less than or equal to 1 nm.

[0054] In a conventional plasma nitridation process, a process gas including only ammonia is used for processing, and the aluminum oxide layer 50 receives greater damage from the bombardment of high-energy hydrogen ions, and the damage to the thickness of the aluminum oxide layer 50 is usually greater than or equal to 1.67 nm, that is, the difference between the thickness of the aluminum oxide layer 50 and the thickness of the aluminum oxynitride layer 60 is greater than or equal to 1.67 nm. The method for preparing a photovoltaic cell provided in the present application has less damage to the aluminum oxide layer 50, and the difference between the thickness of the aluminum oxide layer 50 and the thickness of the aluminum oxynitride layer 60 can be controlled to be less than or equal to 1 nm. Optionally, the difference between the thickness of the aluminum oxide layer 50 and the thickness of the aluminum oxynitride layer 60 is less than or equal to 0.9 nm, or the difference between the thickness of the aluminum oxide layer 50 and the thickness of the aluminum oxynitride layer 60 is less than or equal to 0.8 nm, or the difference between the thickness of the aluminum oxide layer 50 and the thickness of the aluminum oxynitride layer 60 is less than or equal to 0.7 nm, or the difference between the thickness of the aluminum oxide layer 50 and the thickness of the aluminum oxynitride layer 60 is less than or equal to 0.6 nm, or the difference between the thickness of the aluminum oxide layer 50 and the thickness of the aluminum oxynitride layer 60 is less than or equal to 0.5 nm.

[0055] In some embodiments, the power of the plasma nitridation process is 200 W to 500 W.

[0056] Optionally, the power of the plasma nitridation process is 200 W, 250 W, 300 W, 350 W, 400 W, 450 W, or 500 W, or the power of the plasma nitridation process can also be within the range between any two of the above powers.

[0057] In some embodiments, the pressure of the plasma nitridation process is 500 mTorr to 1000 mTorr.

[0058] Optionally, the pressure of the plasma nitridation treatment is 500 mTorr, 600 mTorr, 700 mTorr, 800 mTorr, 900 mTorr or 1000 mTorr, or the pressure of the plasma nitridation treatment may also be within a range between any two of the above pressures.

[0059] In some embodiments, the temperature of the plasma nitridation process is 350° C. to 450° C.

[0060] Optionally, the temperature of the plasma nitridation treatment is 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C or 450°C, or, the temperature of the plasma nitridation treatment may be within the range between any two of the above temperatures.

[0061] In some embodiments, the plasma nitridation treatment lasts for 1 min to 5 min.

[0062] Optionally, the time of the plasma nitridation treatment is 1 min, 1.5 min, 2 min, 2.5 min, 3 min, 3.5 min, 4 min, 4.5 min or 5 min, or the time of the plasma nitridation treatment may also be within the range between any two of the above times.

[0063] Within the above-mentioned range of parameters for each plasma nitridation treatment, it is convenient to simultaneously achieve a better nitridation effect on the aluminum oxide layer 50, reduce the bombardment damage of high-energy hydrogen ions on the aluminum oxide layer 50, and reduce the interface state defect density.

[0064] In some embodiments, during the plasma nitridation process, the nitrogen concentration in the aluminum oxynitride layer 60 is controlled to be 5×10 20 cm -3 ~1×10 22 cm -3 .

[0065] Optionally, during the plasma nitridation process, the nitrogen concentration in the aluminum oxynitride layer 60 is controlled to be 5×10 20 cm -3 , 8×10 20 cm -3 , 1×10 21 cm -3 , 2×10 21 cm -3 , 5×10 21 cm -3, 8×10 21 cm -3 or 1×10 22 cm -3 Alternatively, during the plasma nitridation process, the nitrogen concentration in the aluminum oxynitride layer 60 may be controlled to be within a range between any two of the above concentrations.

[0066] In some embodiments, during the plasma nitridation process, the thickness of the silicon nitride layer 70 is controlled to be 1 nm to 3 nm.

[0067] When the thickness of the silicon nitride layer 70 is too low, the silicon nitride layer 70 improves the bonding strength between the aluminum oxynitride layer 60 and the anti-reflection layer, and the effect of improving the open circuit voltage of the photovoltaic cell is limited. When the thickness of the silicon nitride layer 70 is too high, it may affect the contact effect between the electrode and the doped silicon, affecting carrier transport. Optionally, during the plasma nitridation treatment, the thickness of the silicon nitride layer 70 is controlled to be 1 nm, 1.2 nm, 1.4 nm, 1.6 nm, 1.8 nm, 2 nm, 2.2 nm, 2.4 nm, 2.6 nm, 2.8 nm or 3 nm, or the thickness of the silicon nitride layer 70 may also be within a range between any two of the above thicknesses.

[0068] In some embodiments, the method for preparing a photovoltaic cell intermediate comprises the following steps:

[0069] Providing a silicon substrate 10;

[0070] A first doped silicon layer 20 and a second doped silicon layer 40 are formed on two opposite surfaces of the silicon substrate 10, wherein the first doped silicon layer 20 is doped with P-type doping and the second doped silicon layer 40 is doped with N-type doping.

[0071] An aluminum oxide layer 50 is formed on a surface of the first doped silicon layer 20 away from the silicon substrate 10 .

[0072] In some embodiments, the surface of the first doped silicon layer 20 away from the silicon substrate 10 is a textured surface.

[0073] In some embodiments, the method for preparing a photovoltaic cell comprises the following steps:

[0074] S10: Providing a silicon substrate 10, the silicon substrate 10 having a first surface and a second surface opposite to each other, cleaning and texturing the first surface of the silicon substrate 10, and forming a P-type doped first doped silicon layer 20 on the first surface;

[0075] Reference Figure 1 As shown, Figure 1 FIG. 1 is a schematic structural diagram of preparing a first doped silicon layer 20 on a first surface of a silicon substrate 10 .

[0076] S20: forming a tunnel oxide layer 30 on the second surface; forming an N-type doped second doped silicon layer 40 on the surface of the tunnel oxide layer 30;

[0077] Reference Figure 2 As shown, Figure 2 For Figure 1 A schematic diagram of a structure in which a tunneling oxide layer 30 and a second doped silicon layer 40 are prepared based on the structure shown.

[0078] S30: forming an aluminum oxide layer 50 on the surface of the first doped silicon layer 20 away from the silicon substrate 10;

[0079] Reference Figure 3 As shown, Figure 3 For Figure 2 A schematic diagram of the structure of preparing an aluminum oxide layer 50 based on the structure shown.

[0080] S40 : performing a plasma nitridation treatment on the aluminum oxide layer 50 using a process gas including silane and ammonia, so as to convert the aluminum oxide layer 50 into an aluminum oxynitride layer 60 , and forming a silicon nitride layer 70 on a surface of the aluminum oxynitride layer 60 away from the silicon substrate 10 ;

[0081] Reference Figure 4 As shown, Figure 4 For Figure 3 FIG. 1 is a schematic structural diagram of forming an aluminum oxynitride layer 60 and a silicon nitride layer 70 on the basis of the structure shown.

[0082] S50: forming a first anti-reflection layer 80 on the surface of the silicon nitride layer 70 away from the silicon substrate 10, and forming a second anti-reflection layer 90 on the surface of the second doped silicon layer 40 away from the silicon substrate 10;

[0083] Reference Figure 5 As shown, Figure 5 For Figure 4 Schematic diagram of the structure in which the first anti-reflection layer 80 and the second anti-reflection layer 90 are formed on the basis of the structure shown.

[0084] S60: A first electrode 100 is formed on a surface of the first anti-reflection layer 80 away from the silicon nitride layer 70 , and the first electrode 100 is electrically connected to the first doped silicon layer 20 ; a second electrode 110 is formed on a surface of the second anti-reflection layer away from the second doped silicon layer 40 , and the second electrode 110 is electrically connected to the second doped silicon layer 40 .

[0085] Reference Figure 6 As shown, Figure 6 For Figure 5 A schematic structural diagram of a first electrode 100 and a second electrode 110 is formed on the basis of the structure shown.

[0086] A further embodiment of the present application provides a photovoltaic cell, comprising: a silicon substrate 10, and an aluminum oxynitride layer 60 and a silicon nitride layer 70 which are stacked on a surface of the silicon substrate 10, the aluminum oxynitride layer 60 being between the silicon nitride layer 70 and the silicon substrate 10, and the silicon nitride layer 70 having a thickness of 1 nm to 3 nm.

[0087] Referring again to Figure 6 In some embodiments, the silicon substrate 10 has a first surface and a second surface which are oppositely arranged;

[0088] The first surface has a first doped silicon layer 20, the aluminum oxynitride layer 60, the silicon nitride layer 70 and a first anti-reflection layer 80 which are sequentially stacked thereon; the first doped silicon layer 20 is P-type doped; the first anti-reflection layer 80 has a first electrode 100 arranged thereon, and the first electrode 100 is electrically connected to the first doped silicon layer 20.

[0089] The second surface has a tunneling oxide layer 30, a second doped silicon layer 40 and a second anti-reflection layer 90 which are sequentially stacked thereon; the second doped silicon layer 40 is N-type doped; the second anti-reflection layer 90 has a second electrode 110 arranged thereon, and the second electrode 110 is electrically connected to the second doped silicon layer 40.

[0090] In some embodiments, the P-type doped doping element includes at least one of boron, aluminum, gallium and indium.

[0091] In some embodiments, the N-type doped doping element includes at least one of phosphorus, arsenic, antimony and nitrogen.

[0092] In some embodiments, the material of the tunneling oxide layer 30 includes at least one of silicon dioxide and silicon oxynitride.

[0093] In some embodiments, the material of the first anti-reflection layer 80 and the material of the second anti-reflection layer 90 each independently includes at least one of silicon nitride and aluminum nitride.

[0094] A further embodiment of the present application provides a photovoltaic module, comprising:

[0095] A cover plate;

[0096] At least one cell string, the cell string comprising a photovoltaic cell prepared by the preparation method of the photovoltaic cell of any one of the above, or the photovoltaic cell of any one of the above;

[0097] And a packaging layer, the packaging layer being between the cover plate and the cell string, and the cover plate being connected to the cell string through the packaging layer.

[0098] The following are specific embodiments:

[0099] Embodiment 1

[0100] Preparation method of photovoltaic cells:

[0101] (1) Providing an N-type silicon substrate 10, performing standard RCA cleaning and texturing on the front side of the silicon substrate 10, and performing boron diffusion on the front side to prepare a P-type doped first doped silicon layer 20;

[0102] (2) removing the borosilicate glass layer on the back side of the silicon substrate 10, depositing a 1.5 nm thick silicon dioxide tunneling oxide layer 30 on the back side of the silicon substrate 10, depositing a 150 nm thick amorphous silicon layer on the surface of the tunneling oxide layer 30 away from the silicon substrate 10, performing phosphorus diffusion on the amorphous silicon layer and annealing at 900°C for 30 min, thereby converting the amorphous silicon layer into an N-type doped second doped silicon layer 40;

[0103] (3) depositing an aluminum oxide layer 50 with a thickness of 5 nm on the surface of the first doped silicon layer 20 away from the silicon substrate 10, and performing a plasma nitridation treatment on the aluminum oxide layer 50 using silane and ammonia to convert the aluminum oxide layer 50 into an aluminum oxynitride layer 60, and forming a silicon nitride layer 70 on the surface of the aluminum oxynitride layer 60 away from the silicon substrate 10; the flow ratio of ammonia to silane is 800:1, the power is 400 W, the temperature is 400 ° C, and the time is 2 min;

[0104] (4) forming a silicon nitride anti-reflection layer with a thickness of 80 nm on the surface of the silicon nitride layer 70 away from the silicon substrate 10 and on the surface of the second doped silicon layer 40 away from the silicon substrate 10;

[0105] (5) Prepare the first electrode 100 and the second electrode 110.

[0106] Comparative Example 1

[0107] The preparation method of the photovoltaic cell in Comparative Example 1 is basically the same as that in Example 1, with the only difference being that in step (3), silane is replaced by ammonia at the same flow rate.

[0108] The photovoltaic cells prepared in Example 1 and Comparative Example 1 were tested, and the test results were the average values ​​of the test results of multiple samples. The test results are shown in Table 1 below:

[0109]

[0110] It can be seen from the test results that the photovoltaic cell prepared in Example 1 has improved open circuit voltage and conversion efficiency compared with the photovoltaic cell prepared in Comparative Example 1.

[0111] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0112] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art could make several modifications and improvements without departing from the spirit of the present application, all of which fall within the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the appended claims, and the specification and drawings may be used to interpret the claims.

Claims

1. A method for preparing a photovoltaic cell, characterized in that: The steps include: Providing a photovoltaic cell intermediate, the photovoltaic cell intermediate comprising a silicon substrate and an aluminum oxide layer located on at least one surface of the silicon substrate; The aluminum oxide layer is subjected to plasma nitridation treatment using a process gas including silane and ammonia, wherein the flow ratio of ammonia to silane in the process gas is (100~1000):1, so that the aluminum oxide layer is converted into an aluminum oxynitride layer, and a silicon nitride layer is formed on the surface of the aluminum oxynitride layer away from the silicon substrate.

2. The method for preparing a photovoltaic cell according to claim 1, wherein: In the process gas, the flow rate of silane is 0.1 sccm~1 sccm, and the flow rate of ammonia is 100 sccm~300 sccm.

3. The method for preparing a photovoltaic cell according to claim 1, wherein: A difference in thickness between the aluminum oxide layer and the aluminum oxynitride layer is less than or equal to 1 nm.

4. The method for preparing a photovoltaic cell according to claim 1, wherein: The plasma nitridation process satisfies at least one of the following characteristics: (1) Power is 200W~500W; (2) The pressure is 500mTorr~1000mTorr.

5. The method for preparing a photovoltaic cell according to claim 1, wherein: The plasma nitridation process satisfies at least one of the following characteristics: (1) Temperature is 350℃~450℃; (2) The time is 1 minute to 5 minutes.

6. The method for preparing a photovoltaic cell according to claim 1, wherein: The plasma nitridation process satisfies at least one of the following characteristics: (1) Control the nitrogen concentration in the aluminum nitride oxide layer to 5×10 20 cm -3 ~1×10 22 cm -3 ; (2) The thickness of the silicon nitride layer is controlled to be 1 nm to 3 nm.

7. The preparation method according to any one of claims 1 to 6, characterized in that The preparation method of the photovoltaic cell intermediate comprises the following steps: providing a silicon substrate; forming a first doped silicon layer and a second doped silicon layer on two oppositely disposed surfaces of the silicon substrate, wherein the first doped silicon layer is doped with P-type doping and the second doped silicon layer is doped with N-type doping; The aluminum oxide layer is formed on a surface of the first doped silicon layer away from the silicon substrate.

8. A photovoltaic cell, characterized in that: The photovoltaic cell is prepared by the preparation method of any one of claims 1 to 7, comprising: a silicon substrate, and an aluminum oxynitride layer and a silicon nitride layer stacked on the surface of the silicon substrate, the aluminum oxynitride layer being located between the silicon nitride layer and the silicon substrate, and the thickness of the silicon nitride layer being 1 nm to 3 nm.

9. The photovoltaic cell according to claim 8, characterized in that The silicon substrate has a first surface and a second surface arranged opposite to each other; A first doped silicon layer, an aluminum oxynitride layer, a silicon nitride layer, and a first anti-reflection layer are sequentially stacked on the first surface; the first doped silicon layer is P-type doped; a first electrode is provided on the first anti-reflection layer, and the first electrode is electrically connected to the first doped silicon layer; A tunneling oxide layer, a second doped silicon layer, and a second anti-reflection layer are sequentially stacked on the second surface; the doping type of the second doped silicon layer is N-type doping; A second electrode is disposed on the second anti-reflection layer, and the second electrode is electrically connected to the second doped silicon layer.

10. A photovoltaic module, characterized in that: include: cover; At least one cell string, the cell string comprising a photovoltaic cell prepared by the method for preparing a photovoltaic cell according to any one of claims 1 to 7, or a photovoltaic cell according to any one of claims 8 to 9; as well as An encapsulation layer is located between the cover plate and the battery string, and the cover plate is connected to the battery string through the encapsulation layer.

Citation Information

Patent Citations

  • Method for easy-to-clean substrates and articles therefrom

    CN101528975A

  • Solar cell, production method and photovoltaic module

    CN110289333A

  • Manufacturing method of TOPCon photovoltaic cell

    CN116169186A

  • Preparation method of photovoltaic cell and photovoltaic cell

    CN119584675A

  • Manufacturing method for solar cell element

    JP2006332510A

Cited By

  • Preparation method of photovoltaic cell

    CN122161205A