Hot stamping system and method
By preheating the steel billet in a batch heating furnace and further heating it in a roller hearth furnace, the problem of long cycle time in the hot stamping process is solved, achieving a more efficient production process while maintaining the mechanical properties of the product.
Patent Information
- Application Number
- CN202480023805.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-03
- Filing Date
- 2024-04-03
- Publication Date
- 2025-11-04
Smart Images

Figure CN120897806A_ABST
Abstract
Description
[0001] Cross-references to related applications
[0002] This PCT international patent application claims the benefit and priority of U.S. Provisional Patent Application Serial No. 63 / 456,581 entitled “Hot Stamping System and Method”, filed on April 3, 2023, the entire disclosure of which is incorporated herein by reference. Technical Field
[0003] This disclosure relates to a hot stamping system for forming components from steel billets. Background Technology
[0004] Hot stamping (also known as press forming or hot pressing) is a process of shaping steel billets into desired forms. Due to their lightweight and high rigidity, hot-stamped parts are used in various industries, such as the automotive industry. According to a typical hot stamping process, an unformed steel billet is first heated in a furnace, then shaped in a die while still hot, and finally quenched to provide high strength properties.
[0005] More specifically, the hot stamping process typically involves heating a steel billet to a temperature of approximately 850°C to 950°C in a roller hearth furnace until the billet acquires an austenitic microstructure. Next, the heated billet is transferred from the hearth furnace to a hot forming apparatus comprising a pair of dies. The heated billet is then stamped or pressed into a predetermined shape between the dies. The hot-formed part is then quenched by cooling to a sufficiently low temperature to transform the austenitic microstructure into a martensitic microstructure.
[0006] The problem with conventional hot stamping processes lies in their relatively long cycle times. This is due to the specific heating requirements of the steel billets, especially the time required to heat each billet in a roller hearth furnace to meet those requirements. More specifically, hot stamping processes are typically limited by the rate at which the billets can be heated before stamping. Techniques have been developed to attempt to improve the overall cycle time of hot stamping processes, but further improvements to hot stamping systems are still needed. Summary of the Invention
[0007] According to one aspect of this disclosure, a method for hot stamping multiple billets includes providing multiple billets. The method further includes simultaneously heating the multiple billets in a batch heating furnace at an intermediate temperature below the stamping temperature for a first predetermined time period. The method further includes, after heating at least one of the multiple billets in the batch heating furnace, heating the at least one of the multiple billets in a roller hearth furnace at the stamping temperature for a second predetermined time period. The method further includes, after heating the at least one of the multiple billets in the roller hearth furnace, stamping the at least one of the multiple billets in a die.
[0008] According to another aspect of the disclosure, a system for hot stamping a plurality of billets includes a batch furnace configured to simultaneously heat a plurality of billets at an intermediate temperature below a stamping temperature for a first predetermined period of time. A roller hearth furnace is configured to heat the plurality of billets at a stamping temperature for a second predetermined period of time. Further, a die is configured to stamp the plurality of billets after heating the at least one billet of the plurality of billets in the roller hearth furnace.
[0009] By preheating a large number of billets simultaneously in a batch furnace at an intermediate temperature below the stamping temperature, a significant portion of the time required for heating can be effectively saved, as the billets can spend minimal time in the roller hearth furnace to obtain an austenitic microstructure prior to stamping. This shortens the overall cycle time of the stamping process relative to existing processes. Since the residence time in the batch furnace is at a temperature below the stamping temperature, the final mechanical properties are not affected by the residence time in the batch furnace. For example, the interdiffusion layer of the AlSi coating can be kept below a predetermined critical thickness while in the batch furnace. BRIEF DESCRIPTION OF DRAWINGS
[0010] Other advantages of the present application will be readily appreciated as the same becomes better understood by reference to the following detailed description when considered in connection with the accompanying drawings wherein:
[0011] Figure 1 is a schematic illustration of a system for hot stamping;
[0012] Figure 2 is a graph illustrating the temperature of a billet as a function of time according to the subject system;
[0013] Figure 3 is a side sectional view of a component manufactured using the subject system, showing the total thickness of the resulting coating and the thickness of the interdiffusion layer;
[0014] Figure 4 is a graph illustrating the thickness of the interdiffusion layer of a billet as a function of time as the billet is heated in a furnace; and
[0015] Figure 5 is a schematic illustration of a hot stamping method using the subject system. DETAILED DESCRIPTION
[0016] With reference to the drawings, wherein like numerals refer to like sections throughout the several views, a system 10 for hot stamping steel components is provided. The system 10 can be used to form various types of components in various shapes, such as automotive components such as body pillars, roof rails, rocker panels, bumpers, and door intrusion beams. Generally, according to the subject system 10, an unformed billet 12 of steel is first heated in a batch furnace 14, then heated in a roller hearth furnace 16, then formed in a die 17 in a hot state, and then quenched in the die 17 to provide high strength properties.
[0017] System 10 includes a plurality of blanks 12 that ultimately form a final component. As used herein, the term "blank" 12 can include a single component or a plurality of blank segments that are connected to one another, such as by welding. Blanks 12 can be made of various materials, including but not limited to ultra-high strength steel, such as 22MnB5 boron steel. In one embodiment, the steel material used to form blanks 12 includes 0.18% to 0.28% carbon, 0.7% to 1.0% silicon, 1.0% to 2.0% manganese, 0.12% to 0.7% chromium, 0.1% to 0.45% molybdenum, a maximum of 0.025% phosphorus, 0.008% to 0.01% sulfur, 0.02% to 0.05% titanium, 0.01% to 0.06% aluminum, and 0.002% to 0.004% boron, based on the total weight of the steel material. In another embodiment, the steel material includes a mixture of manganese and boron, such as 22MnB5. According to one embodiment, blanks 12 are initially provided with a coating formed of aluminum and silicon (AlSi). As Figure 3 As best shown, the coating generally ultimately forms an interdiffusion layer 22 along the surface of the resulting hot formed component. Interdiffusion layer 22 is a byproduct of heating the steel with the AlSi coating. Generally, design specifications for the resulting product require that the interdiffusion layer 22 thickness (a measured value of a particular intermetallic compound at the boundary of the steel base material and the AlSi coating) be less than 16 μιη, and the total coating thickness (from the surface of the component to the base steel substrate) be less than 50 μιη. It should be understood that if either of these thicknesses is too great, the weldability of the steel is affected.
[0018] Prior to hot forming, blanks 12 can undergo various cold forming processes, such as trimming and stamping, and can also be welded. These cold forming processes can be used to form blanks 12 into various desired initial positions.
[0019] Batch furnace 14 simultaneously heats any number of blanks 12 at an intermediate temperature that is below the stamping temperature and below a critical temperature at which interdiffusion layer 22 begins to overdevelop. According to one embodiment, the critical temperature is above 800°C, so the intermediate temperature is about 800°C. Blanks 12 are heated in batch furnace 14 at the intermediate temperature for a first predetermined period of time to sufficiently preheat blanks 12. According to one embodiment, the first predetermined period of time is between about five minutes and four hours, but can vary depending on factors such as the thickness of blanks 12 and the temperature selected for the intermediate temperature. Other intermediate temperatures can be used, but studies have shown that above 800°C is an upper limit at which interdiffusion layer 22 begins to overdevelop, and 700°C is a temperature at which interdiffusion layer 22 does not develop at all. The first predetermined period of time is generally limited only by the overdevelopment of interdiffusion layer 22, so any period of time that does not result in such overdevelopment can be used. According to another embodiment, the first predetermined period of time is between about five minutes and one hour.
[0020] The use of a batch heating furnace 14 in the above-discussed manner allows for the simultaneous heating of a large number of billets 12 before they enter the roller hearth furnace 16 and for an extended period of time at an intermediate temperature without excessive formation of the interdiffusion layer 22. This reduces the overall cycle time of the hot stamping process compared to existing systems because the billets 12 can spend significantly less time in the roller hearth furnace 16. The use of a batch heating furnace 14 also prevents contamination of the rollers 19 in the roller hearth furnace 16 and provides uniform patch heating of the billets 12. It should be understood that a large number of billets 12 may include, for example, batches of ten or more billets 12 at a time.
[0021] like Figure 1 As shown, the roller hearth furnace 16 is configured to heat individual billets 12 after preheating in the batch heating furnace 14. The roller hearth furnace includes a plurality of rollers 19 along the length of the roller hearth furnace 16 between an inlet 18 and an outlet 20, such that the billets 12 move along the rollers 19 in a conveyor belt manner between the inlet 18 and the outlet 20. According to an embodiment, the roller hearth furnace 16 heats the billets 12 at a stamping temperature for a second time period sufficient to impart an austenitic microstructure to the billets 12. According to an exemplary embodiment, the stamping temperature is approximately 930°C, and the second predetermined time period is in the range of approximately zero to 300 seconds. Because the billets 12 are preheated in the batch heating furnace 14, the effective heating time is much shorter than in conventional heating processes. The second predetermined time can vary depending on factors such as the thickness or material of the billets 12. For example, thicker billets typically require a longer second predetermined time than thinner billets. According to another embodiment, the second time period can be in the range of approximately zero to 60 seconds.
[0022] According to an embodiment, heating the billet 12 in a roller hearth furnace 16 in this manner results in the formation of an austenitic microstructure throughout the steel. More specifically, during these heating steps, all carbides in the steel billet are likely to dissolve, leaving no residual carbides. After the heating steps, the microstructure of the steel is substantially austenitic, for example, at least 75% austenitic, or entirely austenitic (100% austenitic).
[0023] After heating in the roller hearth furnace 16 for a second predetermined period of time, the heated billet 12, while still above the austenitic temperature and thus still containing a substantially austenitic microstructure, is rapidly transferred from the roller hearth furnace 16 to a die 17, where it is shaped into the desired form. The die 17 may include an upper assembly 24 and a lower assembly 26, wherein one or more of the upper and lower assemblies 24, 26 are configured to move relative to each other. During operation, the billet 12 is positioned between the upper and lower assemblies 24, 26 such that the billet can be shaped as they move abut against each other. After shaping in the die 17, the billet 12 is quenched to provide high strength properties.
[0024] In accordance with the foregoing and with reference to FIG. 23, a method for hot stamping includes a step 100 of providing a plurality of billets 12. The method further includes a step 102 of simultaneously heating the plurality of billets 12 in a batch furnace 14 at an intermediate temperature for a first predetermined time period. According to an embodiment, the intermediate temperature is approximately 800 °C and the first predetermined time period is between approximately 5 minutes and 4 hours, as previously described. According to another embodiment, the first predetermined time period is between approximately 5 minutes and 1 hour.
[0025] The method further includes a step 104 of heating at least one of the plurality of billets 12 in the batch furnace 14 for a second predetermined time period at a stamping temperature in a roller hearth furnace 16 after the at least one of the plurality of billets 12 is heated in the batch furnace 14. According to an embodiment, the stamping temperature is approximately 930 °C and the second predetermined time period is approximately zero to 300 seconds. The method further includes a step 106 of stamping the at least one of the plurality of billets 12 in a die 17 after the at least one of the plurality of billets 12 is heated in the roller hearth furnace 16. According to another embodiment, the second time period can range from approximately zero to 60 seconds. The method can further include a step 108 of quenching the at least one of the plurality of billets 12.
[0026] By preheating a large number of billets in the batch furnace 16 at an intermediate temperature simultaneously, a significant portion of the time required for heating can be effectively saved because the parts can spend less time in the roller hearth furnace 16 compared to existing methods, which shortens the overall cycle time of the hot stamping process. Since the billets 12 are treated in the batch furnace 14 at an intermediate temperature below the critical temperature, the final mechanical properties of the billets 12 are not affected by the residence time in the batch furnace 16. As shown in FIG. 24, the interdiffusion layer 22 does not become too thick (at approximately 16 pm) until the billets reach the critical temperature. Figure 4 Figure 2 It is shown that the billets 12 can reach the intermediate temperature in the batch furnace 14 for a first predetermined time period and then enter the roller hearth furnace 16, where they are heated at a stamping temperature for a second predetermined time period to provide an austenitic microstructure. Tests have shown that the material properties of the billets 12 are not affected by the length of time spent at the intermediate temperature in the batch furnace 16 according to embodiments of the present disclosure.
[0027] The terminology used herein is for the purpose of describing particular example embodiments only and is not intended to be limiting. As used herein, the singular forms "a," "an," and "the" can be intended to include the plural forms as well, unless the context clearly indicates otherwise. The terms "comprises," "comprising," "including," and "having," are inclusive and therefore specify the presence of stated features, integers, steps, operations, elements, and / or components, but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof. The method steps, processes, and operations described herein are not to be construed as necessarily requiring their performance in the particular order
[0028] When an element or layer is referred to as being "on," "engaged to," "connected to," or "coupled to" another element or layer, it can be directly on the other element or layer or intervening elements or layers can be present. In contrast, when an element is referred to as being "directly on," "directly engaged to," "directly connected to," or "directly coupled to" another element or layer, there are no intervening elements or layers present. Other words used to describe the relationship between elements should be interpreted in a like fashion (e.g., "between" versus "directly between," "adjacent" versus "directly adjacent," etc.). As used herein, the term "and / or" includes all combinations of one or more of the associated listed items.
[0029] Although the terms first, second, third, etc. can be used herein to describe various elements, components, regions, layers and / or sections, these elements, components, regions, layers and / or sections should not be limited by these terms. These terms can be only used to distinguish one element, component, region, layer or section from another region, layer or section. Terms such as "first," "second," and other numerical terms when used herein do not necessarily have to follow a sequential or chronological order, unless otherwise indicated by the context. Thus, a first element, component, region, layer or section discussed below could be termed a second element, component, region, layer or section without departing from the teachings of example embodiments.
[0030] Spatially relative terms, such as "inner," "outer," "beneath," "below," "lower," "above," "upper," and the like, can be used herein for ease of description to describe one element or feature's relationship to another element(s) or feature(s) as illustrated in the figures. Spatially relative terms can be intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. For example, if the device in the figures is turned over, elements described as "below" or "beneath" other elements or features would then be oriented "above" the other elements or features. Thus, the exemplary term "below" can encompass both an orientation of above and below. The device can be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein interpreted accordingly.
[0031] The foregoing description of the embodiments is presented for the purpose of illustration and description. It is not intended to be exhaustive or to limit the disclosure to the precise form disclosed. Many modifications and variations are possible in light of the above teaching. The embodiments were chosen and described in order to best explain the principles of the disclosure and its practical application to thereby enable others skilled in the art to best utilize the disclosure for its intended purposes. All such modifications and variations are intended to be included within the scope of the disclosure.
Claims
1. A method for hot stamping multiple blanks, comprising: Multiple blanks are available; The multiple billets are simultaneously heated in a batch heating furnace at an intermediate temperature lower than the stamping temperature for a first predetermined time period. After heating at least one of the plurality of billets in a batch heating furnace, heating at least one of the plurality of billets at a stamping temperature in a roller hearth furnace for a second predetermined time period; and After heating at least one of the plurality of billets in a roller hearth furnace, at least one of the plurality of billets is stamped in a die.
2. The method according to claim 1, wherein the intermediate temperature is approximately 800°C.
3. The method of claim 2, wherein the first predetermined time period is between about 5 minutes and 4 hours.
4. The method according to claim 1, wherein the stamping temperature is about 930°C.
5. The method of claim 4, wherein the second predetermined time period is approximately zero to 300 seconds.
6. The method of claim 1, wherein each of the plurality of billets is individually heated in a roller hearth furnace.
7. The method of claim 1, wherein the roller hearth furnace has an inlet and an outlet, and a plurality of rollers are positioned along the length of the roller hearth furnace between the inlet and the outlet, and wherein heating at least one of the plurality of billets in the roller hearth furnace comprises moving each of the plurality of billets along the rollers through the roller hearth furnace at a stamping temperature between the inlet and the outlet of the roller hearth furnace.
8. The method of claim 1, wherein heating at least one of the plurality of billets in a roller hearth furnace produces an interdiffusion layer thickness of less than 16 μm on the aluminum-silicon coating on the billet.
9. A system for hot stamping multiple blanks, comprising: A batch heating furnace configured to simultaneously heat the plurality of billets at an intermediate temperature for a first time period, the intermediate temperature being lower than the stamping temperature; A roller hearth furnace configured to heat the plurality of billets at a stamping temperature for a second predetermined time period; and A die configured to stamp the plurality of billets after heating at least one of the billets in a roller hearth furnace.
10. The system of claim 9, wherein the intermediate temperature is approximately 800°C.
11. The system of claim 10, wherein the first time period is between about 5 minutes and 4 hours.
12. The system according to claim 9, wherein the stamping temperature is about 930°C.
13. The system of claim 12, wherein the second predetermined time period is approximately zero to 300 seconds.
14. The system of claim 9, wherein the roller hearth furnace is configured to heat each of the plurality of billets individually.
15. The system of claim 9, wherein the roller hearth furnace has an inlet and an outlet, and a plurality of rollers are positioned along the length of the roller hearth furnace between the inlet and the outlet, and wherein the roller hearth furnace is configured to, after the plurality of billets have been heated at a stamping temperature in a batch heating furnace, move each of the plurality of billets along the rollers between the inlet and the outlet of the roller hearth furnace at a stamping temperature.
Citation Information
Patent Citations
System and method for hot stamping of components
CN105682817A
System and method for hot stamping of components
CN105682818A
Steel-aluminum mixed hot stamping automatic production line
CN108772712A
Methods to avoid over-developed aluminized coatings during hot stamping line stoppages
CN111408645A
Hot stamping molding production line with precooling apparatus
CN206838950U