Electromagnetic track surface coating detection system and wear failure test analysis method

By combining the mobile device, galvanometer, and temperature measurement module of the laser detection system, rapid and accurate detection of electromagnetic track coatings is achieved, solving the problem of insufficient resolution in existing technologies, improving detection efficiency and reliability, and ensuring the safe and stable operation of electromagnetic tracks.

CN121049340APending Publication Date: 2025-12-02ZHEJIANG PROVINCIAL SPECIAL EQUIP INSPECTION & RES INST

Patent Information

Application Number
CN202511165674.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-20
Publication Date
2025-12-02

AI Technical Summary

Technical Problem

Existing technologies struggle to efficiently and accurately detect microscopic defects in electromagnetic track coatings, especially under high-speed wear conditions. Traditional detection methods lack sufficient resolution and are not applicable to copper alloy materials.

Method used

A laser inspection system is used, in which a moving device drives the laser, galvanometer, and temperature measurement module to move along the length of the track. The system utilizes laser heating of the coating for non-contact temperature measurement, and combines a control module and an analysis module to achieve automated detection of coating defects.

Benefits of technology

It enables rapid and accurate detection of electromagnetic track coatings, identifies macroscopic and microscopic defects, reduces human error, avoids coating contamination, provides a scientific basis for repair, and improves track reliability and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121049340A_ABST
    Figure CN121049340A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of track defect detection, in particular to a detection system for an electromagnetic track surface coating and a wear failure test analysis method. The system comprises a mobile device, a laser, a galvanometer, a temperature measurement module, an analysis module, a control module and the like, and the method comprises the steps of macroscopic inspection, parameter setting of laser defect inspection, laser defect inspection, data processing, failure form analysis and the like. The temperature measuring module measures temperature and transmits data, and the surface of the whole track is detected through laser spots and movement of the moving device. The method can solve the problem that an existing detection technology cannot rapidly and accurately detect the coating abrasion defect of the electromagnetic track, can effectively standardize the defect, failure and even accident analysis process of the coating of the electromagnetic track, and has the advantages of avoiding track failure caused by coating abrasion failure of the electromagnetic track, improving the reliability of the track and improving the reliability of the track. It is of great significance to ensure safe and stable operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of track defect detection technology, and in particular to a detection system for electromagnetic track surface coatings and a method for wear failure testing and analysis. Background Technology

[0002] The core components of various electromagnetic launching devices are two parallel electromagnetic tracks, which are usually made of copper alloy. However, they are prone to wear and failure under harsh environments of high temperature, strong current and high-speed friction.

[0003] To improve the wear resistance of rails, existing technologies extend service life by constructing reinforcing coatings on the copper alloy surface (such as the Ti-Al-TiC / Cu composite coating proposed in patent CN202411091035.0 and the TiB2 / Cu-B composite material proposed in patent CN202410646750.X). However, during the operation of electromagnetic rails, the armature slides at extremely high speeds on the rail surface (up to 2-3 km / s), and the coating still inevitably experiences wear, including macroscopic defects such as surface shearing and grooves, as well as microscopic defects such as subsurface pitting and shallow peeling (the smallest size can be less than 1 micrometer).

[0004] Currently, the detection of defects in electromagnetic rail coatings faces significant challenges. Traditional detection techniques such as X-ray and ultrasonic testing suffer from low resolution and insufficient efficiency, making it difficult to accurately detect minute internal defects. Visual inspection can only identify surface defects; penetrant testing (PT) is only applicable to open defects and is cumbersome; while eddy current testing (ET) and magnetic particle testing (MT) are unsuitable due to the non-ferromagnetic nature of copper alloys. Furthermore, existing technologies lack systematic analytical methods for the wear failure of electromagnetic rail coatings, making it difficult to detect and repair defects in a timely manner, increasing the failure risk and maintenance costs of electromagnetic rails. Summary of the Invention

[0005] The main objective of this invention is to overcome the shortcomings of the prior art and provide a test and detection system for electromagnetic track surface coatings and a test and analysis method for wear failure.

[0006] The technical solution adopted by this invention to achieve its technical objective is: a detection system for electromagnetic track surface coatings, comprising:

[0007] The mobile device includes a sliding track parallel to the electromagnetic track and a sliding platform that can move along the sliding track. The movement of the sliding platform drives the laser, galvanometer, and temperature measurement module to move along the length direction (X direction) of the track, thereby achieving scanning coverage of the entire track surface.

[0008] A laser, mounted on a sliding platform, is used to output laser light; it outputs laser light of a specific wavelength (0.8–1000.0 μm) and power (0.2–200.0 W) to provide a heat source for defect detection. The characteristic of the coating absorbing laser energy and then heating up reflects the defect.

[0009] A galvanometer, mounted on a sliding platform, receives the laser output from the laser and focuses it onto the coating surface of the electromagnetic track. It receives the laser transmitted via optical fiber. The laser direction is adjusted by a reflector, and then focused by a field lens to form a nanometer- to millimeter-sized spot (40–1200 nm), precisely illuminating the coating surface. An automatic focus tracking function ensures the laser focus remains on the detection point surface.

[0010] The temperature measurement module, mounted on a sliding platform, is used to measure the temperature of the laser irradiation point; it moves synchronously with the galvanometer on the sliding platform. It performs non-contact temperature measurement of the laser irradiation point, detects heat transfer anomalies caused by defects such as temperature rise or uneven distribution, and transmits the data to the analysis module in real time.

[0011] The control module coordinates the operation of the moving device, laser, galvanometer, and temperature measurement module; it is electrically connected to these components. It coordinates the operation of each component, including controlling the movement of the sliding platform, switching and adjusting the laser parameters, deflecting and focusing the galvanometer, rotating the temperature probe, and acquiring data, ensuring the scanning path covers the entire track surface in an "arch" shape.

[0012] The analysis module is used to receive temperature data from the temperature measurement module (4) and analyze coating defects. The analysis module receives temperature data from the temperature measurement module, processes the temperature data, draws a temperature distribution map of the coating surface, identifies abnormal areas (such as high temperature points or low temperature points), and analyzes the defect type (such as shallow peeling, grooves, etc.) in combination with the defect size and morphology.

[0013] Preferably, the laser is connected to the galvanometer via an optical fiber, and the laser output wavelength is 0.8–1000.0 μm and the power is 0.2–200.0 W.

[0014] The two ends of the optical fiber are connected to the output end of the laser and the input end of the galvanometer, respectively. The optical fiber is used to transmit the laser between the laser and the galvanometer, ensuring that the laser is transmitted to the galvanometer efficiently and with low loss. The wavelength and power range (0.8~1000.0 μm, 0.2~200.0W) are adapted to the absorption characteristics of different coating materials.

[0015] Preferably, the galvanometer is also used for focusing and deflecting the laser beam, and includes:

[0016] The reflective mirror is used to adjust the direction of the laser beam; by deflecting the two mirrors, the direction of the laser beam is adjusted, so as to achieve laser scanning in the Y direction (perpendicular to the length of the track).

[0017] A field lens is used to focus a laser beam to form a laser spot of 40–1200 nm; focusing the laser beam to form a nanoscale spot (40–1200 nm) improves detection resolution; and automatic focus tracking is achieved by moving along the Z direction to ensure that the laser energy is always focused on the coating surface.

[0018] Preferably, the field lens can move along a direction perpendicular to the sliding track surface to achieve automatic tracking of the laser focus. Dynamic adjustment of the focus height (Z direction) compensates for unevenness or curvature changes on the track surface, ensuring the accuracy of temperature data at the detection point.

[0019] Preferably, the temperature measurement module includes a temperature probe that can rotate to quickly detect the temperature at the laser focal point. The rotatable temperature probe allows for rapid alignment with the laser focal point, enabling non-contact real-time temperature measurement with sensitivity meeting the requirements for micron-level defect detection.

[0020] Preferably, the control module controls the laser spot to move at a constant speed along a direction parallel or perpendicular to the length of the electromagnetic track, forming a "bow" shape scanning path. By controlling the deflection of the galvanometer (Y direction) and the stepping movement of the sliding platform (X direction), a "bow" shaped scanning path covering the entire track surface is formed, avoiding missed detections.

[0021] This invention also provides a method for testing and analyzing the wear failure of an electromagnetic track surface coating, comprising the following steps:

[0022] S1. Macroscopic inspection: Inspect the electromagnetic track and its coating for macroscopic defects; conduct preliminary screening for obvious defects (such as coating peeling, grooves) by visual inspection or tools.

[0023] S2. Parameter settings for laser defect inspection: Input environment, track, coating, laser, and field lens parameters; input coating physical parameters (such as thermal conductivity and laser absorptivity) and environmental parameters; optimize laser power, wavelength, and other settings to improve detection accuracy.

[0024] S3. Laser defect inspection: The laser is started and outputs a stable laser after preheating for 10-30 minutes. The laser is focused by a galvanometer and irradiates the coating surface. The temperature measurement module measures the temperature and transmits it to the analysis system. The moving device and the galvanometer work together to complete the scanning of the entire track surface. Laser preheating ensures stability. The galvanometer and the temperature measurement module work together to complete the scanning and record temperature anomalies in real time.

[0025] S4. Data Processing and Failure Mode Analysis: The analysis system processes temperature data, plots temperature distribution maps, marks abnormal areas, and determines defect types and failure modes. Defect locations are marked using the temperature distribution map, and defect types (e.g., abrasive wear, spalling) are confirmed through non-destructive testing (e.g., microscopy) or destructive testing (e.g., cross-sectional analysis).

[0026] Preferably, the coating parameters include thickness, density, thermal conductivity, laser absorptivity, reflectivity, and refractive index. Thickness, density, etc., determine the laser energy absorption and heat transfer characteristics, affecting defect detection.

[0027] Preferably, in the laser defect inspection step, the laser spot moves at a constant speed along a direction parallel or perpendicular to the length direction of the electromagnetic track, and the constant speed scanning avoids temperature data fluctuations.

[0028] Preferably, the failure mode analysis includes non-destructive or destructive testing to confirm the defect type, and combining non-destructive and destructive testing improves the reliability of the conclusions.

[0029] Compared with the prior art, the beneficial effects of the present invention are:

[0030] The detection system and wear failure test analysis method for the electromagnetic track surface coating can quickly and accurately detect micro-defects on the coating surface and inside by using a focused laser beam (the spot size can be as small as 40-200 nm) and non-contact temperature measurement technology. This solves the problem of insufficient resolution in the existing technology and has high precision and high efficiency.

[0031] The detection system and wear failure test analysis method for the electromagnetic track surface coating are comprehensive. The system can simultaneously identify macroscopic and microscopic defects, including surface and subsurface wear and peeling, filling the gap in existing technology for internal defect detection.

[0032] The detection system and wear failure test analysis method for the electromagnetic track surface coating are automated and standardized. The control module automates the detection process, standardizes the defect analysis process, improves detection efficiency, and reduces human error.

[0033] The detection system and wear failure test analysis method for the electromagnetic track surface coating are non-contact and pollution-free. They use laser heating and infrared thermometry, avoiding the pollution or damage to the coating surface caused by traditional detection methods (such as penetrant testing).

[0034] The detection system and wear failure test analysis method for the electromagnetic track surface coating are highly practical. Combining temperature distribution analysis and failure mode judgment, it provides a scientific basis for coating repair, effectively prevents track failures caused by coating failure, and improves the reliability and service life of the equipment.

[0035] In summary, this electromagnetic track surface coating detection system and wear failure test analysis method address the challenge of rapid and accurate detection of coatings, especially microscopic wear within the coating itself, which is difficult to achieve with existing technologies. Furthermore, this method effectively standardizes the analysis process for electromagnetic track coating defects, failures, and even accidents. It is of great significance for preventing electromagnetic launch device failure due to electromagnetic track coating wear failure, improving the device's reliability, and ensuring its safe and stable operation. Attached Figure Description

[0036] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0037] Figure 1 This is a flowchart of the failure analysis based on a laser defect detection system.

[0038] Figure 2 This is a schematic diagram of the spatial orientation of an electromagnetic track.

[0039] Figure 3 This is a structural diagram of a laser defect inspection system.

[0040] Figure 4 This is a schematic diagram of the laser spot's movement path.

[0041] Figure 5 This is a temperature distribution map of a portion of the track coating surface obtained by the laser defect detection system in Example 1.

[0042] Figure 6 This is a segment of orbital X-ray image obtained using DR technology in Comparative Example 1.

[0043] Figure 7 This is a temperature distribution map of a portion of the track coating surface obtained by the laser defect detection system in Example 2.

[0044] Wherein: 1-Electromagnetic track; 2-Laser; 3-Galvanometer; 4-Temperature measuring module; 5-Sliding track; 6-Sliding platform; 7-Fiber optic cable; 8-Laser beam. Detailed Implementation

[0045] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. However, it should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of the invention. Furthermore, descriptions of well-known structures and technologies are omitted in the following description to avoid unnecessarily obscuring the concept of the invention.

[0046] In the description of this invention, it should be noted that when an element is referred to as being "fixed to" or "set on" another element, it can be directly on or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to or indirectly connected to the other element.

[0047] In the description of this invention, it should be noted that the terms "center," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship commonly used when the product of this invention is in use. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third," etc., are used only to distinguish descriptions and should not be construed as indicating or implying relative importance. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified. "Several" means one or more, unless otherwise explicitly specified.

[0048] In the description of this invention, it should also be noted that, unless otherwise explicitly specified and limited, the terms "set," "install," "connect," and "link" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0049] Example 1:

[0050] Please see Figures 1-4 A detection system for electromagnetic track surface coating includes a moving device, a laser 2, a galvanometer 3, a high-resolution temperature measurement module 4, an analysis module, and a control module.

[0051] The moving device consists of a sliding rail 5 and a sliding platform 6. The sliding rail 5 is parallel to the electromagnetic rail 1 and is located directly above the electromagnetic rail 1. The sliding platform 6 is installed on the sliding rail 5 and can move along the sliding rail 5.

[0052] Laser 2, mounted on sliding platform 6 within the mobile device, is the device that generates laser light and can continuously output laser light of a specific wavelength and power. The laser wavelength range output by laser 2 can be selected from 0.8 to 1000.0 μm, and the power can be selected from 0.2 to 200.0 W. The selection of wavelength and power should be determined by the relevant physical parameters of the coating on electromagnetic track 1.

[0053] The galvanometer 3, mounted on the sliding platform 6 and between the sliding track 5 and the electromagnetic track 1 in the moving device, is the device for focusing and guiding the laser beam 8. The laser beam 8 is generated by the laser 2 and introduced into the galvanometer 3 through the optical fiber 7. Under the control of the control module, the galvanometer 3 changes the direction of the laser beam 8 through a reflective mirror, so that the laser beam 8 is first focused by the field lens in the galvanometer 3, and then illuminates the desired location. After being focused by the field lens, the focal spot size of the laser beam 8 should be as small as possible, with a diameter ranging from 40 to 200 nm.

[0054] The field mirror in galvanometer 3 can move along a direction perpendicular to the surface of sliding track 5 to adjust the laser focus height. Before the system begins testing, the field mirror with a specific operating wavelength should be replaced according to the wavelength of the laser used.

[0055] The high-resolution temperature measurement module 4 is installed on the sliding platform 6, between the sliding track 5 and the electromagnetic track 1. The system mainly includes a temperature measuring probe, which can quickly and non-contactly detect the temperature in the laser focal area by rotating its direction, and transmit the temperature data and detection position information to the analysis module.

[0056] The control module is used to operate the moving device, laser 2, galvanometer 3, and temperature measuring module 4 during the detection process, including: controlling the movement of the sliding device; controlling the output, shutdown, and laser parameter adjustment of laser 2; controlling the operation of galvanometer 3; and controlling temperature measuring module 4 for positioning and temperature measurement.

[0057] The analysis module is used for controlling the wear defect detection and location process and analyzing defect data, including analyzing and processing the data returned by the temperature measurement module 4 and performing defect location and defect type analysis.

[0058] Specifically, during use, when performing testing, the control module issues a command to turn on laser 2 and continuously output laser light with specific parameters. The laser light enters galvanometer 3 via fiber optic cable 7. Under the control of the control module, galvanometer 3 focuses the laser beam 8 onto the coating surface of the electromagnetic track 1 below. The field mirror in galvanometer 3 can automatically track the focal point, ensuring that the focal point is always at the surface position of the detection point. The energy of the laser beam 8 is concentrated at the laser focal point, and the energy of the laser focal point is quickly absorbed by the track coating surface at the detection point and diffuses downwards, causing the coating at the detection point to heat up rapidly. At the same time, high-resolution temperature measurement module 4 accurately measures the temperature of the detection point. When there are defects on the surface or inside the coating of electromagnetic track 1, the heat transfer at the detection point will be affected, so temperature measurement module 4 will detect the abnormal surface temperature at that point. Galvanometer 3 guides the laser spot to move slowly and uniformly along a direction perpendicular to the direction of electromagnetic track 1, continuously irradiating different points to raise their temperature. Simultaneously, temperature measurement module 4 follows the laser spot to detect the temperature and transmits the temperature data to the analysis module in real time. After the laser spot moves from one end to the other along a direction perpendicular to the electromagnetic track 1, the sliding platform 6, under the control of the control module, moves a certain distance along the track. The galvanometer 3 then guides the laser spot to continuously irradiate the coating surface along the direction perpendicular to the track. The temperature measurement module 4 tracks and measures the temperature and transmits the data. The above steps are repeated to detect the entire track coating. By plotting the distribution of temperature anomalies, the location of defects is determined.

[0059] Because of the high energy at the laser focal point, the temperature rise at the detection point is almost instantaneous. The temperature measurement module 4 reads the temperature change at the detection point in real time. Therefore, the irradiation, heating, and measurement processes are very fast, enabling the detection system to achieve rapid detection. After the laser spot is focused by the galvanometer 3, the spot size at the focal point is extremely small, accurate to the sub-micron to tens of nanometer level. This is the basis for the detection system to achieve accurate detection.

[0060] Example 2:

[0061] Please see Figures 1-7 Based on the above embodiments, the present invention also provides a method for wear failure test analysis of electromagnetic track surface coatings, comprising the following steps:

[0062] S1. Macroscopic inspection:

[0063] Macroscopic inspection, conducted visually or with the aid of tools and equipment, mainly consists of macroscopic inspection of the track itself and macroscopic inspection of the track coating.

[0064] ① Macroscopic inspection of the track: Determine whether there are obvious macroscopic surface defects such as thinning, bending, warping and cracking in electromagnetic track 1.

[0065] ② Macroscopic inspection of the coating: Check whether there are obvious macroscopic surface defects in the track coating, such as obvious detachment from the substrate, deep and wide grooves, and deep and large pits.

[0066] If macroscopic surface defects are found during macroscopic inspection, their locations are marked, and the defects are photographed and measured. The failure mode is determined based on their morphological characteristics and dimensions. Depending on the identified failure mode, the track or coating is replaced or repaired.

[0067] S2. Parameter settings for laser defect inspection:

[0068] Since no obvious macroscopic defects were found on the surface of electromagnetic track 1 in step 1, laser temperature measurement module 4 was used to further detect microscopic defects on the coating surface and inside.

[0069] Input relevant parameters such as the inspection environment, track, track coating, and laser into the control module. These parameters include, but are not limited to:

[0070] ①Environmental information: Temperature and humidity information of the space where the track is located;

[0071] ② Track information: Geometric shape and size information of the track, such as length, width, and surface curvature;

[0072] ③ Coating information: Light absorption and heat transfer parameters such as the thickness, density, thermal conductivity, absorptivity and reflectivity of specific wavelength lasers, refractive index, electrical conductivity and magnetic permeability of the track coating;

[0073] ④ Laser parameters: laser wavelength, power, laser spot diameter at the focal point after focusing, light intensity at the focal point, etc.

[0074] ⑤ Field lens parameters: parameters such as the focal length, numerical aperture, and distance between the plane of galvanometer 3 and the surface of the electromagnetic track 1 coating.

[0075] The environmental information, such as temperature and humidity, must be measured before parameter input. The relevant parameters of the track coating are determined by the coating material and should be determined during the coating design and manufacturing process. The wavelength and power of the laser are determined by the coating material and related physical properties to be tested. The focal length and numerical aperture of the three field mirrors are determined by the field mirror's own size, shape, material, and coating. The laser spot diameter and intensity at the laser's focal point are determined by the laser's own parameters, such as power and wavelength, as well as the relevant parameters of the three field mirrors.

[0076] S3, Laser Defect Inspection:

[0077] The control module issues a command to power on laser 2. To ensure the stability of the output laser, laser 2 needs to be preheated for 10-30 minutes. Once the output laser parameters of laser 2 have reached a stable state, the aperture between fiber optic 7 and the output end of laser 2 is opened, and the laser beam enters galvanometer 3 from laser 2 through fiber optic 7. Galvanometer 3 operates under the control of the control module. The two reflective mirrors inside galvanometer 3 change the laser direction, causing the laser beam 8 to pass through the field mirror in galvanometer 3 and converge at the detection point. Galvanometer 3 can automatically track the focal height. When the laser focal point is higher or lower than the plane where the detection point is located, the field mirror in galvanometer 3 moves slightly in the vertical direction under the control of the control module, always keeping the laser focal point at the plane of the detection point.

[0078] The laser, focused by the field lens, has its focal point located on the surface of the detection point through focus tracking. The energy of the focal point is rapidly absorbed by the orbital coating and conducted downwards to the detection point.

[0079] The amount of laser irradiation on the coating at the detection point This can be described by the following equation:

[0080] ;

[0081] in, The radiation intensity at the detection point is related to the laser wavelength, power, and relevant parameters of the three field mirrors. A represents the irradiated area, determined by the diameter of the laser spot at the detection point. Let be the solid angle of the light source, whose value is related to the focal length of the three field mirrors of the galvanometer. The transmission of laser energy in the coating can be described by the following equation:

[0082] ;

[0083] in, The electric field intensity is the intensity of the laser beam propagating within the coating. For transmission time, At the speed of light, The attenuation coefficient is the laser energy transmitted in the coating. Since the temperature at the laser focal point is extremely high and the coating thickness is low, the transmission of laser energy into the coating is almost instantaneous. It can be approximated that the energy entering the coating below the detection point is equal to the absorbed laser focal energy.

[0084] When the detection point absorbs laser energy, the energy enters the gaps between the detection point and the atoms below it. Electrons within these gaps are excited and undergo transitions due to the absorbed energy, releasing energy between atoms. All these processes cause the surface temperature of the detection point to rise. (Detection point temperature) The relationship between laser energy and the physical properties of the detection point can be described by the following equation:

[0085] ;

[0086] As can be seen from the equation, the temperature at the detection point is related to the electromagnetic field strength and irradiance of the laser, and is also affected by the laser wavelength and attenuation coefficient. The effect of attenuation coefficient. It is a function of the physical properties of the energy transfer medium, determined by factors such as the medium's density, homogeneity, and geometric dimensions. When defects such as voids, holes, or inhomogeneities exist at or below the detection point, the detection point... The value will differ from that of a coating location without defects, therefore the temperature at the test point will also be different.

[0087] Because the energy at the laser focal point is extremely high and the coating thickness is small, heat transfer and temperature rise are completed almost instantaneously. Temperature measurement module 4 can detect and read the temperature of the detection point at the same time as the laser irradiates it, and then transmit the temperature data to the analysis module.

[0088] The galvanometer 3 guides the laser spot to move slowly and uniformly along a direction perpendicular to the length of the electromagnetic track 1, continuously irradiating different points to raise their temperature. Simultaneously, the temperature measuring module 4 follows the laser spot to detect the temperature and transmits the temperature data to the analysis module in real time. After the laser spot moves from one end to the other along a direction perpendicular to the electromagnetic track 1, the sliding platform 6, under the control of the control module, moves a certain distance along the track. The galvanometer 3 then guides the laser spot again to continuously irradiate the coating surface along the direction perpendicular to the track, and the temperature measuring module 4 tracks, measures, and transmits the temperature data. These steps are repeated to complete the detection of the entire track coating surface.

[0089] S4. Data Processing and Failure Mode Analysis:

[0090] After the laser inspection system completes the inspection of the entire track surface coating, the analysis module processes all temperature data, draws a temperature distribution map of the track coating, identifies and marks the locations of temperature anomalies, and makes a preliminary judgment on defects and failure modes based on the size and shape of the temperature anomaly areas.

[0091] With the aid of tools or equipment, inspectors conduct non-destructive or destructive testing to determine the type of defect and failure, and propose a repair plan accordingly.

[0092] The solution in this embodiment can be selectively combined with solutions in other embodiments.

[0093] Example 3:

[0094] Please see Figures 1-7Based on Example 2 above, this example uses the wear failure test analysis method for the surface coating of an electromagnetic track to conduct defect testing and wear failure analysis on the coating defects of an electromagnetic track 1 sample of an electromagnetic launching device using a laser defect detection system. The following is an example:

[0095] The electromagnetic track 1 is made of a Cu alloy containing 0.1% Cr. A CuAl alloy reinforced coating was prepared on its surface using an electroplating method. Based on the coating preparation process, the thickness of the reinforced coating is approximately 120.0 μm. After conducting multiple electromagnetic launch experiments, defect inspection and analysis of the track surface coating are required. The following method was used... Figure 1 The defect inspection and failure analysis steps shown analyzed coating defects and failure modes.

[0096] Step 1: Macroscopic inspection:

[0097] First, a macroscopic inspection was conducted on the track coating surface, which consisted of two parts: a macroscopic inspection of the track itself and a macroscopic inspection of the track surface coating. The macroscopic inspection revealed no obvious deformation, cracks, or damage to the track, nor any obvious coating peeling or grooves on the track coating surface.

[0098] Step 2: Setting parameters for laser defect inspection:

[0099] The track coating was inspected using a laser defect inspection system. Before starting the inspection, relevant parameters were first input into the control module. A total of five parts of information and parameters were input:

[0100] ①Environmental information: The temperature of the space where the orbit is located is 25.2℃; the humidity is 35.6%.

[0101] ② Track information: The track length is 3.0 m; the track is a planar track, so the radius of curvature is infinite; the track width is 50.0 mm.

[0102] ③ Coating information: Coating thickness is 120.0±10.0 μm; Coating density is 5.0 g / cm³. 3 The coating has a thermal conductivity of 15.0 W / (m·K); an absorption rate of 85.0% for laser light (wavelength 1064.0 nm); a reflectivity of 10% for laser light (wavelength 1064.0 nm); a refractive index of 1.8 for laser light (wavelength 1064.0 nm); and an electrical conductivity of 5.0 × 10⁻⁶. 6 S / m; the magnetic permeability of the coating material is 1.05 μ0.

[0103] ④ Laser parameters: The laser wavelength used is 1064.0 nm; the maximum average power is 100.0 W, and the average power was set to 60.0 W for this test; the output spot diameter of laser 2 is approximately 6.0 mm, and the spot diameter at the focal point after focusing by the field lens is approximately 2.0 μm; the light intensity at the focal point is approximately 3.27 × 10⁻⁶. 6 W / cm 2 .

[0104] ⑤ Field lens parameters: The focal length of the field lens used is approximately 900.0 mm; the numerical aperture of the field lens is 0.25; the distance between the field lens plane and the coating surface is approximately 900.0 mm.

[0105] Among them, the temperature and humidity of the space where the track is located are measured and input during parameter input; track parameters such as length, width, and surface curvature radius are obtained during track manufacturing and installation; coating thickness, density, and thermal conductivity are obtained through testing during coating design and preparation; the design parameters of laser 2, such as the wavelength and maximum average power of the laser output by laser 2, are obtained during laser 2 installation; parameters and information such as laser spot diameter are obtained through experiments before testing; the laser power selected during testing is determined based on the physical properties of the coating; parameters such as the focal length, numerical aperture, and distance between the field lens and electromagnetic track 1 are determined during galvanometer 3 installation.

[0106] The solution in this embodiment can be selectively combined with solutions in other embodiments.

[0107] Step 3: Laser Defect Inspection

[0108] like Figure 2 As shown, the length direction of electromagnetic track 1 is defined as the X direction, the direction perpendicular to the length direction of electromagnetic track 1 in the track plane is defined as the Y direction, and the direction perpendicular to the length direction in space is defined as the Z direction.

[0109] Inspection is performed using a laser defect inspection system. Part of the structure of the laser defect inspection system is shown below. Figure 3 As shown. The electromagnetic track 1 to be tested is located below the detection system, which consists of a moving device, a laser 2, a galvanometer 3, a temperature measurement module 4, an analysis module, and a control module. The moving device consists of a sliding track 5 and a sliding platform 6. The sliding track 5 is located approximately 1.0 m above and parallel to the electromagnetic track 1. The laser 2, galvanometer 3, and temperature measurement module 4 are mounted on the sliding platform 6. The laser is transmitted between the laser 2 and the galvanometer 3 via an optical fiber 7.

[0110] During testing, the laser 2 is powered on via the control module. After a 15-minute warm-up, the aperture between the output end of laser 2 and optical fiber 7 is opened, allowing the laser beam to enter the galvanometer 3 through optical fiber 7. The galvanometer 3 operates under the control of the control module. Two reflective mirrors within the galvanometer 3 are used to change the direction, ensuring the laser beam 8 from the field lens illuminates the detection point. Through automatic focus tracking, the field lens in the galvanometer 3 can be slightly moved along the Z-direction under the control of the control module, ensuring the focal point of the laser beam 8 is always located on the surface of the detection point.

[0111] The energy of the laser beam 8 focal point is rapidly absorbed by the coating material at the detection point, causing the detection point and the area below it to heat up rapidly. The temperature measurement module 4 measures the temperature at the detection point and transmits it to the analysis module.

[0112] like Figure 4 As shown, under the control of the control module, the galvanometer 3 continuously changes the focal position of the laser beam 8 at a speed of 10.0 mm / s, making it move at a constant speed along the Y direction to completely cover the plane of track 1 on the Y-direction path. After the scan is completed, the sliding platform 6 moves about 1.5 μm along the X direction, and the galvanometer 3 guides the laser beam 8 to scan the entire straight path at a constant speed along the Y direction. The above steps are repeated, and the spot path of the laser beam 8 forms an overall "bow" shape, scanning the entire surface of track 1. During the scanning process, the temperature measurement module 4 continuously detects the temperature at different detection points and transmits the temperature data to the analysis module.

[0113] Step 4: Data Processing and Failure Mode Analysis:

[0114] After the laser inspection system completes the inspection of the entire track surface coating, the analysis module processes all temperature data, draws a temperature distribution map of the track coating, identifies and marks locations of temperature anomalies. Figure 5 The image shows a portion of the coating distribution map generated after the analysis module processes the track surface temperature data. It can be seen that the temperature of one area is significantly higher than that of the surrounding area. This area is approximately circular in shape, with a diameter ranging from 23.5 to 27.0 μm. Based on its shape and size, it can be preliminarily inferred that the defect is a shallow peeling.

[0115] Inspectors, using the markings on the detection system and with the aid of tools such as leak detectors and portable microscopes, further examined the defect. The initial inspection revealed no surface defects in the coating at that location. Further grinding of the coating surface revealed the defect to be located approximately 22.0 μm below the coating surface. Based on its size, shape, and distribution characteristics, the defect was determined to be shallow peeling. This occurred during electromagnetic launch, when the high-speed armature rubbed against the coating surface of track 1. The subsurface layer of the coating experienced high shear stress, resulting in severe plastic deformation. With each launch, repeated shear stress and plastic deformation weakened the coating material at this location, ultimately leading to an internal defect.

[0116] Based on the inspection results, the inspectors developed a repair plan and repaired the defect, effectively preventing shallow peeling from developing into serious failures such as contact fatigue and coating cracking.

[0117] Furthermore, this embodiment compares the effectiveness of different inspection methods in inspecting the shallow peeling defects found in Example 3.

[0118] The laser defect inspection system and the inspection and analysis method based on the system proposed in this invention were used for inspection. The inspection system and method are exactly the same as those described in Example 3. The inspection results are the same as those described in Example 3.

[0119] The defect at this location was detected using penetrant testing (PT). Penetrant testing is a non-destructive testing technique based on capillary effect, which can be used to detect open defects on the surface of metallic materials. A penetrant solution containing dye is applied to the test location, allowing the solution to penetrate into the defect through capillary effect. After washing away any remaining penetrant and allowing the surface to dry, a developer is applied. Through a chemical reaction, the penetrant within the defect is adsorbed onto the material surface, achieving high-precision defect detection. In this comparative example, the defect in Example 1 was detected using penetrant testing. Since the defect found in Example 1 was located inside the coating, penetrant testing could not detect it.

[0120] The defect was detected using X-ray digital imaging (DR). DR utilizes the varying penetrability of X-rays to different materials and defects to pinpoint their location. Figure 6 This is a DR image of the location of the defect, taken from the side of the track. Due to the limitations of DR detection resolution, the defect was not observed in the image.

[0121] The defect was detected using ultrasonic testing (UT). UT utilizes the different effects of ultrasonic wave absorption and reflection on the energy of different materials and defects to locate the defect. In this comparative example, the UT method was applied to detect the defect found in Example 1. Due to the insufficient sensitivity of UT testing (approximately 100 μm), the small defect found in Example 1 was difficult to detect using the UT method.

[0122] Since neither the Cu alloy tracks nor the coatings are ferromagnetic, eddy current testing (ET) and magnetic particle testing (MT) methods cannot be used for defect detection.

[0123] This result demonstrates that conventional non-destructive testing methods are not suitable for inspecting all defects and failures in track coatings. Since electromagnetic track 1 and its coating use Cu and Cu alloys, they are non-ferromagnetic, rendering the ET and MT methods unsuitable for defect detection and analysis. The PT method offers high resolution but is only applicable to surface defects. The PT method involves applying and cleaning penetrants and developers, resulting in low efficiency, and the penetrants and developers can contaminate the track surface and surrounding space. The DR method can detect both surface and internal defects, but its low resolution makes it difficult to accurately detect small defects. Furthermore, DR requires sophisticated equipment, offering limited flexibility and convenience, and may pose health risks to personnel. The UT method is suitable for detecting internal defects, but its sensitivity is insufficient, making it difficult to detect even small defects. Additionally, the UT method struggles to detect and observe the size and morphology of defects.

[0124] The laser defect detection system and analysis method proposed in this invention have unique advantages in the inspection of defects in track coatings. The laser defect inspection system and method utilize laser heating to locate and identify defects, making it suitable for inspecting defects on the surface and inside of track coatings. By heating the detection point with a focused laser and selecting a suitable field lens, the spot size at the laser focal point can be reduced to the nanometer scale, achieving extremely high-resolution detection. The use of laser heating and non-contact temperature measurement methods constitutes a non-contact inspection method, avoiding damage and contamination to the coating surface during the inspection process. The detection is performed automatically under the control of the control module, which greatly improves inspection efficiency and reduces inspection difficulty.

[0125] Example 4: Please refer to Figures 1-7 Based on embodiments 2 and / or 3 above, and employing the wear failure analysis method for the surface coating of the electromagnetic track 1, this embodiment further conducts coating defect inspection and failure analysis on the track 1 of a certain electromagnetic launching device. Specifically, the following example illustrates this:

[0126] The electromagnetic track 1 is made of pure Cu. A reinforcing coating containing Al2O3 was constructed on its surface using a laser cladding method. The thickness of the reinforcing coating is approximately 300 μm. After the electromagnetic track had been running for a period of time, the staff found that the friction between the track coating surface and the armature was significantly increased. The detection system and method proposed in this invention were used to inspect the track coating for defects and perform failure analysis.

[0127] The defect inspection and failure analysis steps used in this embodiment are the same as those in the previous embodiment. Figure 1 The same as shown.

[0128] First, the macroscopic inspection of the track coating surface was divided into macroscopic inspection of the track itself and macroscopic inspection of the track surface coating. The macroscopic inspection of the track itself did not reveal any obvious deformation, cracks, or damage. The macroscopic inspection of the coating revealed multiple grooves on the coating surface. These grooves all extended along the length of the track. Measurements showed that the groove lengths ranged from 18.0 to 67.5 mm, the widths ranged from 2.4 to 16.2 mm, and the maximum depth was approximately 6.5 mm. Based on the morphology and size of the defects, it was inferred that the defects were caused by abrasive wear between the armature and the track coating surface during electromagnetic launch.

[0129] Macroscopic inspection can detect large defects on the coating surface, requiring further inspection of the track coating using a laser defect inspection system. Before starting the inspection, relevant parameters are first input into the control module, involving a total of five parts of information and parameters:

[0130] ①Environmental information: The temperature of the space where the orbit is located is 28.5℃; the ambient humidity is 10.0%.

[0131] ② Track information: The track length is 5.5 m; the track surface is curved, and the radius of curvature of the track section is 2.0 m; the track width is 80.0 mm.

[0132] ③ Coating information: Coating thickness is 300.0±5.0 μm; Coating density is 6.2 g / cm³. 3 The coating has a thermal conductivity of 120.0 W / (m·K); an absorption rate of 92.0% for laser light (wavelength 10.6 μm); a reflectivity of 5% for laser light (wavelength 1064 nm); a refractive index of 2.3 for laser light (wavelength 10.6 μm); and an electrical conductivity of 1.0 × 10⁻⁶. 4 S / m; the magnetic permeability of the coating material is 1.02 μ0.

[0133] ④ Laser parameters: A CO2 fiber 7 laser 2 with a wavelength of 10.6 μm was used; the maximum average power was 500.0 W, and the average power was set to 80.0 W for this test; the output spot diameter of laser 2 was approximately 10.0 mm, and the spot diameter at the focal point after focusing by the field lens was approximately 40.0 μm; the light intensity at the focal point was approximately 3.6 × 10⁻⁶. 7 W / cm 2 .

[0134] ⑤ Field lens parameters: The focal length of the field lens used is approximately 1500.0 mm; the numerical aperture of the field lens is 0.15; the distance between the field lens plane and the coating surface is approximately 1550.0 mm.

[0135] Because the laser 2 used in this embodiment has a stronger thermal effect, a higher scanning speed of 1.0 m / s is used during detection.

[0136] Everything else is the same as in Example 1.

[0137] Figure 7 The image shows a portion of the coating distribution map generated after the analysis module processed the track surface temperature data. A strip-shaped area is visible in the map, with a significantly higher temperature than the surrounding area. This area is approximately 2.04 mm long, with a maximum width of about 200 μm and a minimum width of about 40 μm. Based on its shape and size, it can be preliminarily inferred that this defect is a small, chiseled groove.

[0138] Based on the markings on the detection system, inspectors, aided by tools such as leak detectors and portable microscopes, conducted further examination of the defect, confirming its existence. This was caused by abrasive wear between the track coating surface and the armature during electromagnetic launch.

[0139] Based on the inspection results, the inspectors developed a repair plan and repaired the defect, effectively preventing the small groove defect from developing into serious failures such as coating cracking.

[0140] The solution in this embodiment can be selectively combined with solutions in other embodiments.

[0141] It should be noted that although the above embodiments have been described herein, this does not limit the scope of patent protection of this invention. Therefore, any changes and modifications made to the embodiments described herein based on the innovative concept of this invention, or equivalent structural, procedural, or functional transformations made using the description and drawings of this invention, directly or indirectly applying the above technical solutions to other related technical fields, are all included within the scope of protection of this invention.

Claims

1. A detection system for electromagnetic track surface coatings, characterized in that, include: The moving device includes a sliding track (5) arranged parallel to the electromagnetic track (1) and a sliding platform (6) that can move along the sliding track (5). A laser (2) is mounted on a sliding platform (6) for outputting laser light; A galvanometer (3) is mounted on a sliding platform (6) to receive the laser output from the laser (2) and focus it onto the coating surface of the electromagnetic track (1); Temperature measurement module (4) is installed on sliding platform (6) and is used to measure the temperature of laser irradiation point; The control module is used to coordinate the operation of the mobile device, the laser (2), the galvanometer (3) and the temperature measurement module (4); The analysis module is used to receive temperature data from the temperature measurement module (4) and analyze coating defects.

2. The detection system for electromagnetic track surface coating according to claim 1, characterized in that: The laser (2) is connected to the galvanometer (3) via an optical fiber (7), and the laser output by the laser (2) has a wavelength of 0.8 to 1000.0 μm and a power of 0.2 to 200.0 W.

3. The detection system for electromagnetic track surface coating according to claim 1, characterized in that: The galvanometer (3) is also used to focus and deflect the laser beam (8), and includes: A reflective mirror is used to adjust the direction of the laser beam (8); A field lens is used to focus the laser beam (8) to form a laser spot of 40–1200 nm.

4. The detection system for electromagnetic track surface coating according to claim 3, characterized in that: The field lens can move along a direction perpendicular to the surface of the sliding track (5) to achieve automatic tracking of the laser focus.

5. The detection system for electromagnetic track surface coating according to claim 1, characterized in that: The temperature measurement module (4) includes a temperature measurement probe, which can rotate to quickly detect the temperature at the laser focal point.

6. The detection system for electromagnetic track surface coating according to claim 1, characterized in that: The control module controls the laser spot to move at a constant speed along a direction parallel or perpendicular to the length direction of the electromagnetic track (1), and the scanning path is in the shape of a bow.

7. A method for testing and analyzing the wear failure of an electromagnetic track surface coating, comprising using the testing and detection system for the electromagnetic track surface coating as described in any one of claims 1-6, characterized in that, Includes the following steps: S1. Macroscopic inspection: Inspect the electromagnetic track (1) and its coating for macroscopic defects; S2. Parameter settings for laser defect inspection: input environment, track, coating, laser, and field lens parameters; S3. Laser defect inspection: Start the laser (2), and the laser is focused by the galvanometer (3) and then irradiates the coating surface. The temperature measurement module (4) measures the temperature and transmits it to the analysis system. The moving device and the galvanometer (3) work together to complete the scanning of the entire track surface. S4. Data processing and failure mode analysis: Analyze the system's temperature data, draw temperature distribution maps and mark abnormal areas, and determine the defect type and failure mode.

8. The method for wear failure test analysis of electromagnetic track surface coating according to claim 7, characterized in that: The coating parameters include thickness, density, thermal conductivity, laser absorptivity, reflectivity, and refractive index.

9. The method for wear failure test analysis of electromagnetic track surface coating according to claim 7, characterized in that: In the laser defect inspection step, the laser spot moves at a constant speed along a direction parallel or perpendicular to the length direction of the railgun track (1).

10. The method for wear failure test analysis of electromagnetic track surface coating according to claim 7, characterized in that: The failure mode analysis includes non-destructive or destructive testing to identify the defect type.

Citation Information

Patent Citations

  • TiB2 / Cu-B composite material for current-carrying frictional wear and preparation method of TiB2 / Cu-B composite material

    CN118516586A

  • Ti-Al-TiC / Cu composite coating for improving current-carrying friction and wear performance of copper alloy and preparation method of Ti-Al-TiC / Cu composite coating

    CN119287306A

  • Device and method for detecting thermal barrier coating (TBC) surfaces based on area array pulse laser excitation

    CN109613063A

  • Bus bar laser welding quality detection method and device and computer storage medium

    CN119643637A

  • Non-contact automatic weld defect detection device

    CN210604481U

Cited By

  • New steel rail surface quality detection system

    CN122130765A