Ferromagnetic core-shell nanorod wave-absorbing material with adjustable frequency band and preparation method thereof
By preparing nanorod-shaped iron(III) oxide and coating it with an ultrathin carbon layer, and combining it with magnetic field-controlled orientation, a band-tunable ferrimagnetic core-shell nanorod absorbing material is formed. This solves the problems of large weight, large thickness and poor high-frequency performance of existing Fe3O4 composite materials, achieving lightweight and dynamic band-tuning, and improving electromagnetic wave absorption performance.
Patent Information
- Application Number
- CN202511249149.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-03
- Publication Date
- 2025-12-05
AI Technical Summary
Existing Fe3O4 composite materials suffer from problems such as complex preparation, large weight, high thickness, poor high-frequency performance, and inability to dynamically and precisely control the absorption frequency band, which cannot meet the requirements of broadband absorption and lightweight design for modern miniaturized electronic devices in complex electromagnetic environments.
Nanorod-shaped iron(III) oxide was prepared by hydrothermal synthesis, coated with an ultrathin carbon layer, and oriented and aligned by magnetic field control to form a band-tunable ferrimagnetic core-shell nanorod absorbing material. The dielectric and magnetic permeability properties were improved by utilizing the synergistic effect of the nanorod structure and the ultrathin carbon layer, and the dynamic adjustment was achieved by adjusting the aspect ratio and orientation angle.
It achieves lightweight material, enhanced absorption performance across the entire frequency band, and dynamic adjustment of the absorption band. It solves the problems of high-frequency magnetic loss and impedance mismatch, broadens the electromagnetic wave absorption band, and enhances electromagnetic loss across multiple frequency bands.
Smart Images

Figure CN121064790A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of electromagnetic functional materials, and particularly relates to a frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material and a preparation method thereof. BACKGROUND
[0002] With the rapid development of electromagnetic technology and the continuous widening of communication frequency bands, electromagnetic wave absorbing materials are facing new challenges. Multi-band compatible devices and wideband radar detection applications require wave-absorbing materials to cover a wider frequency range, and the limited space of modern miniaturized electronic devices also puts strict requirements on the thickness, weight and adjustability of wave-absorbing materials. Traditional spinel structure ferrimagnetic material Fe3O4, as a low-cost and efficient wave-absorbing material, is widely used in the field of electromagnetic wave absorption. However, its low dielectric performance and high-frequency magnetic permeability reduction have made it unable to meet the current complex electromagnetic environment requirements of wideband absorption and lightweight.
[0003] In the prior art, the wave-absorbing performance of Fe3O4 material is improved by introducing a heterojunction. Chinese Patent Publication No. CN118421262A discloses a two-dimensional composite wave-absorbing material loaded with Fe3O4 / CoCO3 nanoparticles and a preparation method thereof. The method introduces a heterojunction to enhance polarization relaxation, which can improve dielectric loss to some extent. However, the weight and thickness of the material are increased, and the skin effect caused by this brings limitations to the high-frequency performance of the material. The problems of impedance mismatch and reduced magnetic loss caused by the reduction of high-frequency magnetic permeability cannot be solved.
[0004] In terms of expanding and regulating the effective absorption frequency band of the material, the traditional method is to use multi-element compounding. However, this method introduces non-magnetic or weakly magnetic components, which further reduces the magnetic permeability of the material due to magnetic dilution. Moreover, the preparation and regulation process is complicated, which is not conducive to the precise and dynamic adjustment of the wave-absorbing frequency band.
[0005] In summary, the existing Fe3O4 composite material has the problems of complex preparation, large weight and thickness, poor high-frequency performance, and inability to dynamically and accurately regulate the absorption frequency band. Therefore, how to design an Fe3O4 composite electromagnetic wave absorbing material with simple preparation, lightweight, enhanced wave-absorbing performance in the full frequency band, and dynamically adjustable wave-absorbing frequency band to meet the current complex electromagnetic environment requirements of electromagnetic wave absorption applications is a technical problem that needs to be solved and an important development direction in the field of electromagnetic wave absorbing materials that combines low cost, high stability, lightweight, wide frequency band, and strong absorption requirements. SUMMARY
[0006] Therefore, in order to overcome the shortcomings of the prior art, the present application aims to provide a frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material and a preparation method thereof.
[0007] According to a first aspect of the present application, a preparation method of a band-tunable ferrimagnetic core-shell nanorod wave-absorbing material is provided, the method comprising: Step one: preparing a ferric oxyhydroxide precursor by a hydrothermal synthesis method, and reducing the ferric oxyhydroxide precursor by a liquid phase pyrolysis method to obtain nanorod-shaped ferroferric oxide; Step two: growing a carbon layer on the surface of the nanorod-shaped ferroferric oxide by a high-temperature sintering method to obtain a nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer; Step three: performing orientation arrangement on the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer by magnetic field control.
[0008] Optionally, in the preparation method of the band-tunable ferrimagnetic core-shell nanorod wave-absorbing material, in step one, the ferric oxyhydroxide precursor is prepared in the following manner: dissolving ferric chloride and branched polyethyleneimine in deionized water to form a clear solution under stirring, performing a hydrothermal reaction on the clear solution, and vacuum drying the hydrothermal reaction product to obtain the ferric oxyhydroxide precursor.
[0009] Optionally, in the preparation method of the band-tunable ferrimagnetic core-shell nanorod wave-absorbing material, in step one, the clear solution is prepared by dissolving 10 mmol of ferric chloride and 0.05-0.2 mmol of branched polyethyleneimine in 30 mL of deionized water, the hydrothermal reaction is performed at a temperature of 120℃ for 4 h, and the vacuum drying is performed at a temperature of 60℃ for 10 h.
[0010] Optionally, in the preparation method of the band-tunable ferrimagnetic core-shell nanorod wave-absorbing material, in step one, the ferric oxyhydroxide precursor is reduced by a liquid phase pyrolysis method, which comprises: dispersing the ferric oxyhydroxide precursor in sufficient oleylamine, obtaining a mixed dispersion liquid by ultrasonic treatment, performing a liquid phase pyrolysis reaction on the mixed dispersion liquid under a nitrogen atmosphere, and centrifuging, washing, and vacuum drying the liquid phase pyrolysis reaction product.
[0011] Optionally, in the preparation method of the band-tunable ferrimagnetic core-shell nanorod wave-absorbing material, in step one, the ferric oxyhydroxide precursor is reduced by a liquid phase pyrolysis method, which comprises: placing the mixed dispersion liquid in a nitrogen atmosphere, heating it to 220℃ at a heating rate of 5℃ / min, continuously reacting for 4 h under stirring to obtain a precipitate, centrifuging the precipitate at a speed of 5000 r / min using cyclohexane, vacuum drying the washed product at a temperature of 60℃ for 10 h, and obtaining the nanorod-shaped ferroferric oxide material.
[0012] Optionally, the preparation method of the frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material of the present application, step two, comprises: placing the nanorod-shaped ferroferric oxide in a nitrogen atmosphere, heating to 500 DEG C at a heating rate of 5 DEG C / min, and then maintaining for 3h to obtain an ultrathin carbon layer coated nanorod-shaped ferroferric oxide composite material.
[0013] Optionally, the preparation method of the frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material of the present application, step three, comprises: distributing the ultrathin carbon layer coated nanorod-shaped ferroferric oxide composite material in the mold through the flowable matrix, and applying a magnetic field of a preset angle to the material in the mold to obtain the frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material.
[0014] Optionally, the preparation method of the frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material of the present application, the weight ratio of the flowable matrix to the ultrathin carbon layer coated nanorod-shaped ferroferric oxide composite material is 6:4.
[0015] Optionally, the preparation method of the frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material of the present application, the flowable matrix is one of paraffin, hydrogel or resin.
[0016] According to the second aspect of the present application, a frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material is provided, which is prepared according to the above method.
[0017] The frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material and the preparation method thereof of the present application have the following beneficial technical effects.
[0018] I. Structural design and lightweight synergistic advantage Unique rod structure: nanorod-shaped ferroferric oxide has significant shape anisotropy, which can significantly improve the magnetic crystal anisotropy field, resulting in the natural resonance frequency moving to high frequency, which helps to solve the problem of reduced high-frequency magnetic loss of ferroferric oxide material; nanorod-shaped ferroferric oxide has a larger specific surface area, which can provide more interfaces in the core-shell structure, induce strong interface polarization, and significantly improve dielectric loss.
[0019] Ultrathin carbon layer uniform coating: the uncracked oil amine molecules and organic functional groups remaining on the surface of the ferroferric oxide product after oil phase pyrolysis are used to obtain a uniform ultrathin carbon layer after high-temperature sintering. The ultrathin carbon layer provides electrical conductivity, improves interface polarization, regulates electromagnetic properties and impedance matching, while almost not increasing additional weight, realizing the overall lightweight of the material.
[0020] II. Electromagnetic property improvement and regulation Significant improvement of electromagnetic properties: the ultra-thin carbon layer improves the electrical conductivity and interface dipole of the ferroferric oxide, brings strong interface polarization relaxation and dipole polarization relaxation, and obtains higher dielectric performance; the shape anisotropic rod structure helps to break through the Snoek limit, realizes the improvement of high-frequency magnetic permeability, makes the material more sensitive to the magnetic field, and enhances the magnetic hysteresis loss.
[0021] Dynamic adjustment of electromagnetic properties: by adjusting the content of branched polyethyleneimine, the aspect ratio of the nanorod-shaped ferroferric oxide material can be adjusted, the interface dipole distribution of the material is changed, and then the dielectric performance of the composite material is adjusted; by controlling the orientation arrangement of the composite material through a magnetic field, the angle between the magnetic moment and the electromagnetic wave vector can be adjusted, and the magnetic performance of the material can be optimized.
[0022] III. Improvement of electromagnetic wave absorption efficiency Impedance matching optimization and dielectric loss improvement: the ultra-thin carbon layer can accurately control the dielectric constant and optimize the impedance matching of the material; the heterojunction interface formed by the carbon layer and the ferroferric oxide core will produce additional interface polarization loss, and the dielectric loss performance of the material is enhanced.
[0023] Broadening and adjusting of electromagnetic absorption frequency band: the nanorod-shaped ferroferric oxide composite material coated with an ultra-thin carbon layer optimizes the impedance and widens the overall effective absorption frequency band; by changing the orientation arrangement angle of the composite material, the electromagnetic properties of the material can be adjusted in real time, and the impedance matching and loss of the material in each frequency band can be flexibly adjusted according to specific needs. This real-time adjustable feature enables the material to enhance electromagnetic loss in multiple frequency bands, providing an effective solution to the problem of limited absorption capacity of current electromagnetic wave absorption materials in a multi-frequency band environment. BRIEF DESCRIPTION OF DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings needed in the embodiments will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present application, and other drawings can be obtained by those skilled in the art without creative labor.
[0025] Figure 1 A scanning electron microscope image of the nanorod-shaped ferroferric oxide composite material coated with an ultra-thin carbon layer prepared in Example 1 of the present application; Figure 2 A scanning electron microscope image of the nanorod-shaped ferroferric oxide composite material coated with an ultra-thin carbon layer prepared in Example 2 of the present application; Figure 3 A scanning electron microscope image of the nanorod-shaped ferroferric oxide composite material coated with an ultra-thin carbon layer prepared in Example 3 of the present application; Figure 4Complex permittivity plot for the band tunable ferrimagnetic core-shell nanorod wave absorbing material prepared in Example 1 of the present application oriented at 30°, wherein, Figure 4 (a) is a plot of the real part of the complex permittivity (ε'), and Figure 4 (b) is a plot of the imaginary part of the complex permittivity (ε"); Figure 5 Complex permittivity plot for the band tunable ferrimagnetic core-shell nanorod wave absorbing material prepared in Example 4 of the present application oriented at 90°, wherein, Figure 5 (a) is a plot of the real part of the complex permittivity (ε'), and Figure 5 (b) is a plot of the imaginary part of the complex permittivity (ε"); Figure 6 Complex permittivity plot for the band tunable ferrimagnetic core-shell nanorod wave absorbing material prepared in Example 5 of the present application oriented at 180°, wherein, Figure 6 (a) is a plot of the real part of the complex permittivity (ε'), and Figure 6 (b) is a plot of the imaginary part of the complex permittivity (ε"); Figure 7 Complex permeability plot for the band tunable ferrimagnetic core-shell nanorod wave absorbing material prepared in Example 1 of the present application oriented at 30°, wherein, Figure 7 (a) is a plot of the real part of the complex permeability (μ'), and Figure 7 (b) is a plot of the imaginary part of the complex permeability (μ"); Figure 8 Complex permeability plot for the band tunable ferrimagnetic core-shell nanorod wave absorbing material prepared in Example 4 of the present application oriented at 90°, wherein, Figure 8 (a) is a plot of the real part of the complex permeability (μ'), and Figure 8 (b) is a plot of the imaginary part of the complex permeability (μ"); Figure 9 Complex permeability plot for the band tunable ferrimagnetic core-shell nanorod wave absorbing material prepared in Example 5 of the present application oriented at 180°, wherein, Figure 9 (a) is a plot of the real part of the complex permeability (μ'), and Figure 9 (b) is a plot of the imaginary part of the complex permeability (μ"); Figure 10 Reflection loss plot for the band tunable ferrimagnetic core-shell nanorod wave absorbing material prepared in Example 1 of the present application oriented at 30°, at a frequency range of 2-18 GHz and a thickness range of 0-10 mm; Figure 11 Reflection loss plot for the band tunable ferrimagnetic core-shell nanorod wave absorbing material prepared in Example 4 of the present application oriented at 90°, at a frequency range of 2-18 GHz and a thickness range of 0-10 mm; Figure 12The 180° oriented band-tunable ferrimagnetic core-shell nanorod wave-absorbing material prepared for the embodiment 5 of the present application has a reflection loss graph in the 2-18 GHz frequency band and with a thickness of 0-10 mm. DETAILED DESCRIPTION
[0026] The embodiments of the present application are described in detail below with reference to the accompanying drawings.
[0027] It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict; and all other embodiments obtained by those skilled in the art on the basis of the embodiments in the present disclosure without creative labor belong to the protection scope of the present disclosure.
[0028] It should be noted that various aspects of the embodiments described below are within the scope of the appended claims. It should be apparent that the aspects described herein can be embodied in a wide variety of forms and that any specific structure and / or function described herein is merely illustrative. Based on the teachings herein one skilled in the art should appreciate that an aspect described herein can be implemented independently of any other aspects and that two or more aspects can be combined in various ways. For example, an apparatus can be implemented and / or a method practiced using any number of the aspects described herein. In addition, an apparatus can be implemented and / or a method practiced using other structure and / or functionality in addition to or other than one or more of the aspects described herein.
[0029] Embodiment 1 10 mmol of iron chloride and 0.05 mmol of branched polyethyleneimine were dissolved in 30 ml of deionized water to form a clear solution under stirring; the clear solution was transferred to a hydrothermal reactor for hydrothermal reaction, the temperature of the hydrothermal reaction was 120 DEG C, the time of the hydrothermal reaction was 4 h, after the reaction was completed, the product was cooled to room temperature, and then repeatedly washed with deionized water and ethanol, and then transferred to a vacuum drying oven for drying, the drying temperature was 60 DEG C, and the drying time was 10 h, thereby obtaining the iron oxyhydroxide precursor.
[0030] 2 mmol of the iron oxyhydroxide was dispersed into 50 ml of oleylamine, and then ultrasonically mixed and uniformly mixed to obtain a mixed dispersion liquid, the mixed dispersion liquid was transferred to a flask, nitrogen was introduced, and the temperature was increased to 220 DEG C at a rate of 5 DEG C / min, and then the reaction was continuously carried out for 4 h under stirring to obtain a precipitated product, the precipitated product was washed by centrifugation at a rotation speed of 5000 r / min using cyclohexane, and then the washed product was placed in a vacuum drying oven, and the product after washing was vacuum dried at a temperature of 60 DEG C for 10 h, thereby obtaining the nanorod-shaped ferroferric oxide material.
[0031] The nanorod-shaped ferroferric oxide material is transferred to a tube furnace, heated to 500 DEG C at a rate of 5 DEG C / min under nitrogen atmosphere, and kept for 3h to obtain the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer.
[0032] The nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer is distributed in a mold through a flowable matrix, the weight ratio of the flowable matrix to the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer is 6:4, a magnetic field of 30 DEG is applied to the material in the mold to obtain the 30 DEG oriented frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material.
[0033] It should be noted that in the present application, the flowable matrix can also be a gel, a polymer resin, etc. At the corresponding liquefaction temperature of the flowable matrix, the composite material is dispersed in a base with certain flowability such as paraffin, gel, polymer resin, etc., and injected into the mold cavity, and an external magnetic field of different angles is applied to the mold to obtain the frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material.
[0034] Example 2 10mmol of iron chloride and 0.1mmol of branched polyethyleneimine are dissolved in 30ml of deionized water to form a clear solution under stirring; the clear solution is transferred to a hydrothermal reaction kettle for hydrothermal reaction, the temperature of the hydrothermal reaction is 120 DEG C, the time of the hydrothermal reaction is 4h, after the reaction is completed, the product is cooled to room temperature, and then washed repeatedly with deionized water and ethanol, and then transferred to a vacuum drying oven for drying, dried at a temperature of 60 DEG C for 10h to obtain the iron oxyhydroxide precursor.
[0035] 2mmol of iron oxyhydroxide is dispersed into 50mL of oleylamine, ultrasonically mixed and uniformly obtained as a mixed dispersion liquid, the mixed dispersion liquid is transferred to a flask, nitrogen is introduced and heated to 220 DEG C at a rate of 5 DEG C / min, and the precipitation product is obtained under stirring for 4h, the precipitation product is centrifuged with cyclohexane at a speed of 5000r / min, and the washed product is placed in a vacuum drying oven and vacuum dried at a temperature of 60 DEG C for 10h to obtain the nanorod-shaped ferroferric oxide material.
[0036] The nanorod-shaped ferroferric oxide material is transferred to a tube furnace, heated to 500 DEG C at a rate of 5 DEG C / min under nitrogen atmosphere, and kept for 3h to obtain the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer.
[0037] The nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer is distributed in a mold through a flowable matrix, the weight ratio of the flowable matrix to the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer is 6:4, a magnetic field of 30 DEG is applied to the material in the mold to obtain the 30 DEG oriented frequency band adjustable ferrimagnetic core-shell nanorod wave-absorbing material.
[0038] Example 3 10 mmol of ferric chloride and 0.2 mmol of branched polyethyleneimine were dissolved in 30 ml of deionized water to form a clear solution under stirring; the clear solution was transferred to a hydrothermal reactor for hydrothermal reaction, the temperature of the hydrothermal reaction was 120℃, the time of the hydrothermal reaction was 4 h, after the reaction was completed, the product was cooled to room temperature, and then repeatedly washed with deionized water and ethanol, and then transferred to a vacuum drying oven for drying, dried at a temperature of 60℃ for 10 h to obtain the iron oxyhydroxide precursor.
[0039] 2 mmol of the iron oxyhydroxide was dispersed in 50 ml of oleylamine, ultrasonically mixed and uniformly mixed to obtain a mixed dispersion liquid, the mixed dispersion liquid was transferred to a flask, nitrogen was introduced and the temperature was raised to 220℃ at a rate of 5℃ / min, and the reaction was continued for 4 h under stirring to obtain a precipitated product, the precipitated product was washed by centrifugation at a speed of 5000 r / min using cyclohexane, and the washed product was placed in a vacuum drying oven and vacuum dried at a temperature of 60℃ for 10 h to obtain a nanorod-shaped ferroferric oxide material.
[0040] The nanorod-shaped ferroferric oxide material was transferred to a tube furnace, heated to 500℃ at a rate of 5℃ / min under a nitrogen atmosphere, and then held for 3 h to obtain an ultrathin carbon layer coated nanorod-shaped ferroferric oxide composite material.
[0041] The ultrathin carbon layer coated nanorod-shaped ferroferric oxide composite material was distributed in a mold by a flowable matrix, the weight ratio of the flowable matrix to the ultrathin carbon layer coated nanorod-shaped ferroferric oxide composite material was 6:4, a magnetic field of 30° was applied to the material in the mold to obtain a 30° oriented band-tunable ferrimagnetic core-shell nanorod wave-absorbing material.
[0042] Example 4 10 mmol of ferric chloride and 0.2 mmol of branched polyethyleneimine were dissolved in 30 ml of deionized water to form a clear solution under stirring; the clear solution was transferred to a hydrothermal reactor for hydrothermal reaction, the temperature of the hydrothermal reaction was 120℃, the time of the hydrothermal reaction was 4 h, after the reaction was completed, the product was cooled to room temperature, and then repeatedly washed with deionized water and ethanol, and then transferred to a vacuum drying oven for drying, dried at a temperature of 60℃ for 10 h to obtain the iron oxyhydroxide precursor.
[0043] 2mmol of iron hydroxyl oxide was dispersed into 50mL of oleylamine, ultrasonic and mixed uniformly to obtain a mixed dispersion, the mixed dispersion was transferred into a flask, nitrogen was introduced and heated to 220℃ at a rate of 5℃ / min, the precipitated product was obtained under stirring for 4h, the precipitated product was washed by centrifugation at a speed of 5000r / min using cyclohexane, the washed product was placed in a vacuum drying oven, the washed product was vacuum dried at a temperature of 60℃ for 10h, and a nanorod-shaped ferroferric oxide material was obtained.
[0044] The nanorod-shaped ferroferric oxide material was transferred into a tube furnace, heated to 500℃ at a rate of 5℃ / min under a nitrogen atmosphere, and then kept for 3h, to obtain a nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer.
[0045] The nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer was distributed in a mold by a flowable matrix, the weight ratio of the flowable matrix to the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer was 6:4, a magnetic field of 90° was applied to the material in the mold, and a 90° oriented band-tunable ferrimagnetic core-shell nanorod wave-absorbing material was obtained.
[0046] Example 5 10mmol of iron chloride and 0.05mmol of branched polyethyleneimine were dissolved in 30ml of deionized water to form a clear solution under stirring; the clear solution was transferred into a hydrothermal reactor for hydrothermal reaction, the temperature of the hydrothermal reaction was 120℃, the time of the hydrothermal reaction was 4h, after the reaction was completed, the product was cooled to room temperature, washed repeatedly with deionized water and ethanol, and then transferred into a vacuum drying oven for drying, dried at a temperature of 60℃ for 10h, to obtain an iron hydroxyl oxide precursor.
[0047] 2mmol of iron hydroxyl oxide was dispersed into 50mL of oleylamine, ultrasonic and mixed uniformly to obtain a mixed dispersion, the mixed dispersion was transferred into a flask, nitrogen was introduced and heated to 220℃ at a rate of 5℃ / min, the precipitated product was obtained under stirring for 4h, the precipitated product was washed by centrifugation at a speed of 5000r / min using cyclohexane, the washed product was placed in a vacuum drying oven, the washed product was vacuum dried at a temperature of 60℃ for 10h, and a nanorod-shaped ferroferric oxide material was obtained.
[0048] The nanorod-shaped ferroferric oxide material was transferred into a tube furnace, heated to 500℃ at a rate of 5℃ / min under a nitrogen atmosphere, and then kept for 3h, to obtain a nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer.
[0049] The nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer is distributed in a mold through a flowable matrix, the weight ratio of the flowable matrix to the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer is 6:4, a 180° magnetic field is applied to the material in the mold, and a 180° oriented band-tunable ferrimagnetic core-shell nanorod wave-absorbing material is obtained.
[0050] Example 6 The surface morphology of the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer prepared in Example 1, Example 2 and Example 3 is observed by using a cold field emission scanning electron microscope with a model of Hitachi Regulus 8100, and the acceleration voltage used is 5kV. Figure 1 The scanning electron microscope image of the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer prepared in Example 1 of the present application is shown in Figure 1, Figure 2 The scanning electron microscope image of the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer prepared in Example 2 of the present application is shown in Figure 2, Figure 3 The scanning electron microscope image of the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer prepared in Example 3 of the present application is shown in Figure 3.
[0051] From the above, Figure 1 , Figure 2 , Figure 3 It can be seen that the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer prepared in Example 1, Example 2 and Example 3 of the present application has a complete shape, a uniform distribution, and a size controlled between 50nm-200nm, and as the amount of branched polyethyleneimine added increases, the length of the nanorod gradually shortens, and the ultrathin carbon layer is uniformly coated on the nanorod.
[0052] The electromagnetic parameter test of the band-tunable ferrimagnetic core-shell nanorod wave-absorbing material prepared in Example 1, Example 4 and Example 5 is performed by using a vector network analyzer with a model of Keysight PNA-X N5244A, the test method is a coaxial cable method, the test frequency is a frequency range of 2-18GHz, the complex permittivity and the complex permeability of each material are obtained, and the reflection loss is calculated by using a transmission line method.
[0053] Figure 4 The complex permittivity curve of the 30° oriented band-tunable ferrimagnetic core-shell nanorod wave-absorbing material prepared in Example 1 of the present application is shown in Figure 4, wherein, Figure 4 (a) is the complex permittivity real part (ε′) curve, Figure 4 (b) is the complex permittivity imaginary part (ε″) curve, and the complex permittivity can be obtained from the formula ε r =ε′-jε″; Figure 5The graph shows the complex permittivity of the 90° oriented, band-tunable ferrimagnetic core-shell nanorod absorbing material prepared in Example 4 of this invention. Figure 5 (a) is a graph showing the real part (ε′) of the complex permittivity. Figure 5 (b) is a graph of the imaginary part (ε″) of the complex permittivity. The complex permittivity can be derived from ε. r The formula =ε′-jε″ is derived from this. Figure 6 The graph shows the complex permittivity of the 180° oriented, band-tunable ferrimagnetic core-shell nanorod absorbing material prepared in Example 5. Figure 6 (a) is a graph showing the real part (ε′) of the complex permittivity. Figure 6 (b) is a graph of the imaginary part (ε″) of the complex permittivity. The complex permittivity can be derived from ε. r The formula =ε′-jε″ is derived from this.
[0054] pass Figure 4 , Figure 5 and Figure 6 It can be seen that when the magnetic field is oriented at 30°, the maximum real part of the complex permittivity of the band-tunable subferromagnetic core-shell nanorod absorbing material prepared in Example 1 of the present invention is 7.1. As the frequency increases, the average value of the real part of the complex permittivity remains around 6.8, and the imaginary part of the complex permittivity remains in the range of 0.4-1.0. When the frequency is 16.2 GHz, the maximum value reaches 0.97. When the magnetic field is oriented at 90°, the real part of the complex permittivity of the band-tunable subferromagnetic core-shell nanorod absorbing material prepared in Example 4 of this invention increases across the entire frequency band from 2 to 18 GHz compared to the 30° orientation, with an average value remaining at 7.2. Resonance occurs in the 12.8-14.3 GHz range, with a maximum value reaching 8.8, an increase of 23% compared to the 30° orientation. The imaginary part of the complex permittivity also shows a significant increase across the entire frequency band from 2 to 18 GHz, especially in the 13.8-16.8 GHz range, with an average value reaching 0.95. At a frequency of 15.2 GHz, the maximum value reaches 1.39, an increase of approximately 43% compared to the 30° orientation. When the magnetic field is oriented at 180°, the real part of the complex permittivity of the band-tunable subferromagnetic core-shell nanorod absorbing material prepared in Example 5 of this invention increases across the entire frequency band from 2 to 18 GHz. The value further increases across the entire 18GHz band, reaching an average of 7.6. At a frequency of 12.1GHz, the maximum value reaches 7.95. The imaginary part of the complex permittivity is concentrated between 0.5 and 1.1, and at a frequency of 16GHz, the maximum value reaches 1.1.
[0055] Figure 7 This is a graph showing the complex permeability of the 30° oriented, band-tunable subferromagnetic core-shell nanorod absorbing material prepared in Example 1 of this invention. Figure 7 (a) is a graph of the real part (μ′) of the complex permeability. Figure 7(b) is a complex magnetic permeability imaginary part (μ") graph, the complex magnetic permeability can be obtained from μr=μ'-jμ"; Figure 8 The complex magnetic permeability graph of the frequency band adjustable ferrimagnetic core-shell nanorod wave absorbing material prepared in the embodiment 4 of the present application is shown in the figure, wherein, Figure 8 (a) is a complex magnetic permeability real part (μ') graph, Figure 8 (b) is a complex magnetic permeability imaginary part (μ") graph, the complex magnetic permeability can be obtained from μr=μ'-jμ"; Figure 9 The complex magnetic permeability graph of the frequency band adjustable ferrimagnetic core-shell nanorod wave absorbing material prepared in the embodiment 5 of the present application is shown in the figure, wherein, Figure 9 (a) is a complex magnetic permeability real part (μ') graph, Figure 9 (b) is a complex magnetic permeability imaginary part (μ") graph, the complex magnetic permeability can be obtained from μr=μ'-jμ".
[0056] In the embodiment of the present application, the magnetic permeability of the frequency band adjustable ferrimagnetic core-shell nanorod wave absorbing material is different in each frequency band, which brings different absorption frequency bands, so the absorption frequency band can be changed by adjusting the orientation angle. Figure 7 、 Figure 8 and Figure 9 It can be seen that the real part and the imaginary part of the complex magnetic permeability of the frequency band adjustable ferrimagnetic core-shell nanorod wave absorbing material show a gradually decreasing trend with the frequency, in the frequency range of 7-12 GHz, the real part of the complex magnetic permeability of the 90° orientation and the 180° orientation material is higher than that of the 30° orientation, while in the range of 13.4-18 GHz, the real part of the complex magnetic permeability of the 90° orientation and the 180° orientation material is lower than that of the 30° orientation, wherein, the 90° orientation sample decreases by about 6%, and the 180° orientation sample decreases by about 4%, the imaginary part of the complex magnetic permeability has a small increase in 2-4.8 GHz, and has a decrease in 7.5-11.8 GHz, at the frequency of 12.4 GHz, the imaginary part of the complex magnetic permeability of the 90° orientation sample reaches the maximum value 0.1.
[0057] Figure 10 The reflection loss graph of the frequency band adjustable ferrimagnetic core-shell nanorod wave absorbing material prepared in the embodiment 1 of the present application in the frequency range of 2-18 GHz, with the thickness of 0-10 mm; Figure 11 The reflection loss graph of the frequency band adjustable ferrimagnetic core-shell nanorod wave absorbing material prepared in the embodiment 4 of the present application in the frequency range of 2-18 GHz, with the thickness of 0-10 mm; Figure 12The reflection loss diagram of the 180° oriented band-tunable ferrimagnetic core-shell nanorod wave-absorbing material prepared for the embodiment 5 of the present application in the 2-18 GHz frequency band and with a thickness of 0-10 mm. As shown in the diagram, the three kinds of oriented materials exhibit different absorption performance in different frequency bands. In the 8-18 GHz frequency band, the 90° oriented sample exhibits a stronger absorption peak compared with the 30° and 180° oriented samples. When the sample thickness is 9 mm and the frequency is 10.14 GHz, the reflection loss value of the 90° oriented sample reaches a maximum of -48.84 dB. In the 4-8 GHz frequency band, the 180° oriented sample has a wider effective absorption frequency band. When the thickness is 4.5 mm, the effective absorption frequency band of the sample reaches 2.25 GHz. In the low thickness region, the 180° oriented sample exhibits a stronger absorption peak. When the thickness is 4.2 mm and the frequency is 6.4 GHz, the reflection loss value of the sample reaches -15 GHz. The 30° oriented sample exhibits a stronger absorption peak in the high thickness and high frequency region. When the frequency is 16.9 GHz and the thickness is 8.7 mm, the reflection loss value of the sample reaches -44.87 dB.
[0058] The band-tunable ferrimagnetic core-shell nanorod wave-absorbing material and the preparation method thereof have the following beneficial technical effects: I. Structural design and lightweight synergistic advantage Unique rod structure: the nanorod-shaped ferroferric oxide has significant shape anisotropy, which can significantly improve the magnetic crystal anisotropy field, causing the natural resonance frequency to move to a high frequency, which helps to solve the problem of reduced high-frequency magnetic loss of ferroferric oxide material; the nanorod-shaped ferroferric oxide has a larger specific surface area, which can provide more interfaces in the core-shell structure, induce strong interface polarization, and significantly improve dielectric loss.
[0059] Uniformly coated with an ultrathin carbon layer: the uncracked oil amine molecules and organic functional groups remaining on the surface of the ferroferric oxide product after oil phase pyrolysis are sintered at high temperature to obtain a uniform ultrathin carbon layer. The ultrathin carbon layer provides electrical conductivity, improves interface polarization, regulates electromagnetic properties and impedance matching, while almost not increasing additional weight, realizing the overall lightweight of the material.
[0060] II. Electromagnetic property improvement and regulation Significant improvement of electromagnetic properties: the ultrathin carbon layer improves the electrical conductivity and interface dipole of the ferroferric oxide, brings strong interface polarization relaxation and dipole polarization relaxation, and obtains higher dielectric properties; the shape anisotropic rod structure helps to break through the Snoek limit, realizes high-frequency magnetic permeability improvement, makes the material more sensitive to the magnetic field, and enhances the magnetic hysteresis loss.
[0061] Dynamic adjustment of electromagnetic properties: By adjusting the content of branched polyethyleneimine, the aspect ratio of nanorod-shaped ferroferric oxide material can be adjusted, the interface dipole distribution of the material can be changed, and the dielectric properties of the composite material can be adjusted; by controlling the orientation arrangement of the composite material through a magnetic field, the angle between the magnetic moment and the electromagnetic wave vector can be adjusted, and the magnetic properties of the material can be optimized.
[0062] III. Electromagnetic wave absorption efficiency improvement Impedance matching optimization and dielectric loss improvement: The ultra-thin carbon layer can accurately regulate the dielectric constant and optimize the impedance matching of the material; the heterojunction interface formed by the carbon layer and the ferroferric oxide core will produce additional interface polarization loss, enhancing the dielectric loss performance of the material.
[0063] Broadening and adjusting of electromagnetic absorption frequency band: The nanorod-shaped ferroferric oxide composite material coated with an ultra-thin carbon layer optimizes the impedance and widens the overall effective absorption frequency band; by changing the orientation arrangement angle of the composite material, the electromagnetic properties of the material can be adjusted in real time, and the impedance matching and loss of the material in each frequency band can be flexibly adjusted according to specific needs. This real-time adjustable feature enables the material to enhance electromagnetic loss in multiple frequency bands, providing an effective solution to the problem of limited absorption capacity of current electromagnetic wave absorption materials in multi-frequency band environments.
[0064] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions within the technical scope disclosed by the present application can be easily thought of by those skilled in the art, and should be covered within the protection scope of the present application. Therefore, the protection scope of the present application should be subject to the protection scope of the claims.
Claims
1. A method for preparing a frequency band-adjustable ferrimagnetic core-shell nanorod wave-absorbing material, characterized in that, The method comprises: Step one: preparing a ferric oxyhydroxide precursor by a hydrothermal synthesis method, and reducing the ferric oxyhydroxide precursor by a liquid phase pyrolysis method to obtain nanorod-shaped ferroferric oxide; Step two: growing a carbon layer on the surface of the nanorod-shaped ferroferric oxide by a high-temperature sintering method to obtain a nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer; Step three: arranging the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer by a magnetic field control.
2. The method for preparing the band-tunable subferromagnetic core-shell nanorod absorbing material according to claim 1, characterized in that, In step one, the ferric oxyhydroxide precursor is prepared as follows: dissolving ferric chloride and branched polyethyleneimine in deionized water to form a clear solution under stirring, subjecting the clear solution to a hydrothermal reaction, and vacuum drying the hydrothermal reaction product to obtain the ferric oxyhydroxide precursor.
3. The method for preparing the band-tunable subferromagnetic core-shell nanorod absorbing material according to claim 2, characterized in that, In step one, the clear solution is prepared by dissolving 10 mmol of ferric chloride and 0.05-0.2 mmol of branched polyethyleneimine in 30 mL of deionized water, the hydrothermal reaction is performed at a temperature of 120°C for 4 h, and the vacuum drying is performed at a temperature of 60°C for 10 h.
4. The method for preparing the band-tunable subferromagnetic core-shell nanorod absorbing material according to claim 1, characterized in that, In step one, the ferric oxyhydroxide precursor is reduced by the liquid phase pyrolysis method, which comprises: dispersing the ferric oxyhydroxide precursor in sufficient oleylamine, obtaining a mixed dispersion liquid by ultrasonic treatment, performing a liquid phase pyrolysis reaction on the mixed dispersion liquid under a nitrogen atmosphere, and centrifuging and washing the liquid phase pyrolysis reaction product and vacuum drying.
5. The method for preparing the band-tunable subferromagnetic core-shell nanorod absorbing material according to claim 4, characterized in that, In step one, the ferric oxyhydroxide precursor is reduced by the liquid phase pyrolysis method, which comprises: placing the mixed dispersion liquid in a nitrogen atmosphere, heating it to 220°C at a heating rate of 5°C / min, continuously reacting for 4 h under stirring to obtain a precipitate, centrifuging the precipitate at a speed of 5000 r / min using cyclohexane, vacuum drying the washed product at a temperature of 60°C for 10 h, and obtaining a nanorod-shaped ferroferric oxide material.
6. The method of claim 1, wherein the band-tunable ferrimagnetic core-shell nanorod wave-absorbing material is prepared by the following steps of: In step two, the nanorod-shaped ferroferric oxide is placed in a nitrogen atmosphere, heated to 500°C at a heating rate of 5°C / min, and held for 3 h to obtain a nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer.
7. The method for preparing the band-tunable subferromagnetic core-shell nanorod absorbing material according to claim 1, characterized in that, In step three, the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer is distributed in a mold by a flowable matrix, a magnetic field with a preset angle is applied to the material in the mold, and a band-adjustable ferrimagnetic core-shell nanorod wave-absorbing material is obtained.
8. The method of claim 8, wherein the band-tunable ferrimagnetic core-shell nanorod wave-absorbing material is prepared by the following steps of: The weight ratio of the flowable matrix to the nanorod-shaped ferroferric oxide composite material coated with an ultrathin carbon layer is 6:
4.
9. The method of claim 8, wherein the band-tunable ferrimagnetic core-shell nanorod wave-absorbing material is prepared by the following steps of: The flowable matrix is one of paraffin, hydrogel, or resin.
10. A band-tunable ferrimagnetic core-shell nanorod wave-absorbing material, characterized in that, The band-adjustable ferrimagnetic core-shell nanorod wave-absorbing material is prepared according to the method of any one of claims 1 to 9.
Citation Information
Patent Citations
Two-dimensional composite wave-absorbing material loaded with Fe3O4 / CoCO3 nanoparticles on surface and preparation method and application thereof
CN118421262A