Method for preparing high-entropy gamma-ray shielding filler based on multilayer electrophoresis method

High-entropy gamma-ray shielding fillers were prepared by multilayer electrophoresis and sintering in a mixed H2/Ar atmosphere, which solved the problems of uneven composition and complex process of traditional materials and achieved efficient and uniform gamma-ray attenuation effect.

CN121096708APending Publication Date: 2025-12-09HARBIN INST OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511018333.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-23
Publication Date
2025-12-09

AI Technical Summary

Technical Problem

Traditional gamma-ray shielding materials suffer from problems such as uneven composition, weak interfacial bonding, and complex manufacturing processes, making it difficult to achieve efficient and uniform gamma-ray attenuation.

Method used

High-entropy gamma-ray shielding filler was prepared by multilayer electrophoresis. A multilayer structure was formed by electrophoretic deposition of various high atomic number metal salts on a conductive substrate. Combined with sintering in a mixed atmosphere of H2/Ar and ball milling, a dense high-entropy gamma-ray shielding filler was obtained.

Benefits of technology

It achieves multi-element synergistic shielding, gradient structure optimization performance, simplified process and significant cost-effectiveness, and improves gamma-ray shielding efficiency and material density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121096708A_ABST
    Figure CN121096708A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing high-entropy gamma-ray shielding filler based on a multilayer electrophoresis method, and belongs to the technical field of shielding materials. The invention aims to solve the problems of low shielding efficiency and complex process caused by non-uniform component distribution and weak interface bonding force of the traditional shielding filler. The method comprises the following steps: dispersing a plurality of high-atomic-number metal salts in deionized water, immersing a conductive base material into a polyelectrolyte solution for surface modification, performing electrophoretic deposition under the conditions of regulating and controlling voltage, pH and deposition time to realize gradient deposition of metal ions on the surface of the base material, drying, sintering, and grinding to obtain the compact high-entropy gamma-ray shielding filler. The method has the advantages that atomic-scale mixing can be achieved through the multi-layer electrophoresis method, and the segregation problem of traditional mechanical mixing is avoided; the multi-layer design enhances multiple scattering and absorption of gamma rays, so that the effect of improving the shielding efficiency is achieved; the process is simplified, high-temperature smelting or complex pressing equipment is not needed, and energy consumption and cost are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The application belongs to the technical field of shielding materials, and particularly relates to a method for preparing high-entropy gamma ray shielding filler based on a multilayer electrophoresis method. BACKGROUND

[0002] In the fields of nuclear industry, medical equipment and aerospace, effective shielding of gamma rays is a core requirement for personnel safety and stable operation of equipment. As high-energy electromagnetic waves, the shielding of gamma rays relies on the absorption and scattering effects of photons by materials. Traditional shielding materials such as lead, tungsten and their alloys mainly rely on high atomic number elements to achieve attenuation through photoelectric effect, Compton scattering and other mechanisms. However, single metal materials have significant defects: lead has high density (11.3 g / cm 3 ), is highly toxic, is difficult to process and shape, and is prone to secondary pollution; tungsten has excellent shielding efficiency, but its high hardness makes it difficult to process into complex structures, and the cost is high. In addition, the shielding mechanism of single elements has energy selectivity, making it difficult to deal with uniform attenuation of wide energy spectrum gamma rays. In recent years, multi-component composite materials (such as lead-polyethylene, tungsten-epoxy resin) have improved performance through physical blending, but problems such as poor interfacial compatibility and uneven element distribution still limit their practical application. As a new multi-principal element material, high-entropy alloys (HEA) can integrate the synergistic shielding ability of multiple high-atomic-number elements due to their unique "cocktail effect", which can theoretically break through the performance limits of single elements. However, existing high-entropy shielding materials are mainly prepared by mechanical alloying or melting method, which is complex and energy-consuming. At the same time, traditional methods are difficult to achieve gradient distribution of components, and the composition of the material is uneven, and the structure is not dense enough, which seriously weakens the multi-stage attenuation effect of gamma rays. SUMMARY

[0003] The purpose of the present application is to solve the problems of uneven composition of traditional materials, weak interfacial bonding, complex process and insufficient element synergistic effect, and to provide a method for preparing high-entropy gamma ray shielding filler based on a multilayer electrophoresis method.

[0004] To achieve the above-mentioned purpose, the technical solutions adopted by the present application are as follows: A method for preparing high-entropy gamma ray shielding filler based on a multilayer electrophoresis method, the method comprising the following steps: Step one: dissolve a plurality of metal salts of target high-atomic-number elements in deionized water in equal molar ratios, and stir to form a uniform solution; Step two: immerse the conductive substrate in a polyelectrolyte solution, adsorb the surface to make it negatively charged, take it out and dry, and then place it in the solution obtained in step one, adjust the voltage, deposition time and pH to make the metal ions electrophoretically deposit on the conductive substrate; take it out after a certain time, repeat the process, and thus form a multilayer structure; Step three: after drying the deposited substrate, sintering in a tube furnace under a hydrogen-argon mixed atmosphere to obtain dense high-entropy gamma-ray shielding particles; Step four: ball milling the high-entropy gamma-ray shielding particles under an inert atmosphere to obtain high-entropy gamma-ray shielding fillers.

[0005] Further, in step one, the metal elements of the high-atomic-number metal salt are at least two of Ta, W, Nb, Mo, V, Sn, Bi, Hf, Zr, Pb, and Gd, which synergistically enhance the absorption and scattering of gamma rays through multiple mechanisms such as photoelectric effect and Compton scattering, and the metal ion concentration in the uniform solution is 0.05-0.3 mol / L.

[0006] Further, in step two, the conductive substrate is one of graphite sheet, copper mesh, stainless steel sheet, titanium sheet, metal foil, or conductive ceramic, and the polyelectrolyte is sodium polystyrene sulfonate, and the polyelectrolyte solution concentration is 0.5-2 wt%.

[0007] Further, in step two, the soaking time of the conductive substrate is 10-60 minutes.

[0008] Further, in step two, the voltage is 1-20 V, the pH is 3-6, the single deposition time is 30-120 seconds, the substrate needs to be washed with deionized water and dried after each electrophoretic deposition, and the number of repeated depositions is ≥3 times.

[0009] Further, in step three, the volume fraction of hydrogen in the hydrogen-argon mixed gas is 5%-15%. H2 reduces metal oxides, and Ar inhibits grain coarsening.

[0010] Further, in step three, the sintering process adopts a stepwise heating program: heating at 5-10 ℃ / min to 300-400 ℃ for 1 hour of pretreatment, and then heating at 3-10 ℃ / min to 800-1200 ℃ for 1-5 hours of holding.

[0011] Further, in step four, the inert atmosphere is nitrogen or argon.

[0012] Further, in step four, the ball milling speed is 200-500 rpm, the ball-to-material mass ratio is 10:1-20:1, and the ball milling time is 2-8 h.

[0013] Compared with the prior art, the present application has the following beneficial effects: 1. Multi-element synergistic shielding: multiple high-atomic-number elements in high-entropy alloys synergistically act through multiple mechanisms such as photoelectric effect and Compton scattering, significantly improving the gamma-ray shielding efficiency.

[0014] 2. Gradient structure optimizes performance: the multi-layer structure formed by multiple electrophoretic depositions can grade attenuate different energy gamma rays, reducing the risk of radiation leakage.

[0015] 3. The densification process advantage: H2 / Ar mixed atmosphere sintering inhibits element segregation, improves material density and structural stability.

[0016] 4. Strong process compatibility: reusable conductive substrate, controllable electrophoretic deposition parameters, suitable for large-scale production, significant cost-effectiveness. BRIEF DESCRIPTION OF DRAWINGS

[0017] Figure 1 Scanning electron microscope image of W-Mo-Nb-V-Ta five-element high-entropy gamma-ray shielding filler; Figure 2 W-Mo-Nb-V-Ta five-element high-entropy gamma-ray shielding filler linear attenuation coefficient changes with thickness at 1.17 MeV; Figure 3 W-Mo-Nb-V-Ta five-element high-entropy gamma-ray shielding filler linear attenuation coefficient changes with thickness at 1.33 MeV; Figure 4 Scanning electron microscope image of W-Sn-Bi-Hf-Pb five-element high-entropy gamma-ray shielding filler; Figure 5 W-Sn-Bi-Hf-Pb five-element high-entropy gamma-ray shielding filler shielding efficiency changes with mass at 1.17 MeV; Figure 6 Bi-Pb-Sn-Hf-Zr five-element high-entropy gamma-ray shielding filler scanning electron microscope image; Figure 7 Bi-Pb-Sn-Hf-Zr five-element high-entropy gamma-ray shielding filler shielding efficiency changes with mass at 1.33 MeV; Figure 8 W-Mo-Nb-V-Ta five-element high-entropy gamma-ray shielding filler X-ray diffraction spectrum. DETAILED DESCRIPTION

[0018] The technical solutions of the present application will be further described below in conjunction with the drawings and examples, but are not limited thereto. Any modification or equivalent replacement of the technical solutions of the present application without departing from the spirit and scope of the present application shall be covered within the protection scope of the present application.

[0019] The core advantages of the present application are as follows: first, the composition uniformity is high, atomic-level mixing is achieved through electrophoretic deposition technology, segregation problems of traditional mechanical mixing are avoided (compared with the high-temperature sintering process of patent CN117758096A), and the composition of the gradient layer can be precisely controlled, significantly improving the multiple scattering effect of gamma rays; second, the process is relatively low-temperature and efficient, sintering at 300-600°C (patent CN119020656A requires high-temperature treatment at 900-1700°C), which greatly reduces energy consumption and avoids element volatilization, ensuring the stability of the material composition; at the same time, it can ensure the compactness and toughness of the structure, the interlayer chemical bonding formed by electrophoretic deposition makes the interface bonding strength reach more than 15 MPa (the lead fiber of patent CN117637223A only relies on physical bundling), combined with the lattice distortion effect of high-entropy alloy, the strength and plasticity and wear resistance of the material are further improved. Through multi-dimensional innovation, the present application provides a breakthrough solution for efficient and low-cost radiation protection.

[0020] Example 1: Target product: Ta-W-Bi-Hf-Pb five-element high-entropy shielding filler 1. Solution configuration: Take TaCl5, WCl6, Bi(NO3)3, HfCl4, Pb(NO3)2 each 0.004 mol, dissolve in 200 mL deionized water, total metal ion concentration 0.1 mol / L.

[0021] 2. Substrate modification: titanium sheet (10x10x0.5mm) is immersed in 1.0 wt% sodium polystyrene sulfonate solution for 20 minutes, and then dried at 60°C to obtain a negatively charged substrate.

[0022] 3. Layered deposition: electrophoretic parameters: direct current voltage 5 V, pH=4.0, single deposition time 60 seconds; repeat deposition 5 times (after each deposition, vacuum drying at 60°C for 10 minutes).

[0023] 4. Sintering: H2 / Ar mixed gas (H2 volume ratio 10%) is introduced into the tube furnace, preheated to 400°C at 5°C / min for 1 hour, then heated to 1000°C at 5°C / min, and kept for 2 hours.

[0024] 5. Ball milling: under argon protection, zirconia grinding balls (ball-to-material ratio 15:1), planetary ball mill speed 400 rpm, ball milling time 4 hours. Example 2: Target product: W-Sn-Bi-Hf-Pb five-element high-entropy shielding filler 1. Solution configuration: Take WCl6, SnCl2, Bi(NO3)3, HfCl4, Pb(NO3)2 each 0.0032 mol, dissolve in 200 mL deionized water, total metal ion concentration 0.08 mol / L.

[0025] 2. Substrate modification: graphite sheet immersed in 0.8 wt% sodium polystyrene sulfonate solution for 25 minutes, dried at 50°C to obtain a negatively charged substrate.

[0026] 3. Layer-by-layer deposition: electrophoresis parameters: direct current voltage 3 V, pH = 4.5, single deposition time 90 seconds; repeated deposition 8 times (vacuum dried at 50°C for 15 minutes after each deposition).

[0027] 4. Sintering: H2 / Ar mixed gas (H2 volume ratio 8%) was introduced into the tube furnace, heated to 300°C at 5°C / min for 1 hour pretreatment, and then heated to 800°C at 3°C / min, and kept for 3 hours.

[0028] 5. Ball milling: under nitrogen protection, tungsten carbide balls were used (ball-to-material ratio 12:1), the planetary ball mill was rotated at 350 rpm, and the ball milling time was 6 hours.

[0029] Example 3: Target product: Bi-Pb-Sn-Hf-Zr five-element high-entropy shielding filler 1. Solution preparation: 0.008 mol of Bi(NO3)3, Pb(NO3)2, SnCl2, HfCl4, and ZrOCl2 were dissolved in 200 mL of deionized water, and the total metal ion concentration was 0.2 mol / L.

[0030] 2. Substrate modification: stainless steel sheet immersed in 2.0 wt% sodium polystyrene sulfonate solution for 15 minutes, dried at 55°C to obtain a negatively charged substrate.

[0031] 3. Layer-by-layer deposition: electrophoresis parameters: direct current voltage 10 V, pH = 3.0, single deposition time 30 seconds; repeated deposition 3 times (vacuum dried at 55°C for 5 minutes after each deposition).

[0032] 4. Sintering: H2 / Ar mixed gas (H2 volume ratio 5%) was introduced into the tube furnace, heated to 350°C at 5°C / min for 1 hour pretreatment, and then heated to 1200°C at 10°C / min, and kept for 1 hour.

[0033] 5. Ball milling: under argon protection, stainless steel balls were used (ball-to-material ratio 18:1), the planetary ball mill was rotated at 450 rpm, and the ball milling time was 3 hours.

[0034] Example 4: Target product: Ta-W-Nb-Mo-V five-element high-entropy shielding filler 1. Solution preparation: 0.006 mol of TaCl5, WCl6, MoCl5, VCl3, and NbCl5 were dissolved in 200 mL of deionized water, and the total metal ion concentration was 0.15 mol / L. 2. Substrate modification: Nickel foil immersed in 0.5 wt% sodium polystyrene sulfonate solution for 30 minutes, dried at 45°C to obtain a negatively charged substrate.

[0035] 3. Layer-by-layer deposition: Electrophoresis parameters: DC voltage 7 V, pH = 4.2, single deposition time 90 seconds; repeated deposition 6 times (vacuum dried at 45°C for 12 minutes after each deposition).

[0036] 4. Sintering: H2 / Ar mixed gas (H2 volume ratio 12%) was introduced into the tube furnace, heated to 350°C at a rate of 6°C / min for 1 hour of pretreatment, and then heated to 950°C at a rate of 8°C / min, and held for 2.5 hours.

[0037] 5. Ball milling: Under argon protection, tungsten carbide balls were used (ball-to-material ratio 20:1), the planetary ball mill was rotated at 500 rpm, and the ball milling time was 5 hours.

[0038] Example 5: Target product: W-Bi-Hf-Pb quaternary high-entropy shielding filler 1. Solution preparation: 0.0025 mol of WCl6, Bi(NO3)3, HfCl4, and Pb(NO3)2 were dissolved in 200 mL of deionized water, and the total metal ion concentration was 0.05 mol / L.

[0039] 2. Substrate modification: Copper mesh immersed in 0.6 wt% sodium polystyrene sulfonate solution for 28 minutes, dried at 40°C to obtain a negatively charged substrate.

[0040] 3. Layer-by-layer deposition: Electrophoresis parameters: DC voltage 1 V, pH = 5.0, single deposition time 120 seconds; repeated deposition 7 times (vacuum dried at 40°C for 20 minutes after each deposition) 4. Sintering: H2 / Ar mixed gas (H2 volume ratio 15%) was introduced into the tube furnace, heated to 1100°C at a rate of 4°C / min, and held for 3 hours.

[0041] 5. Ball milling: Under nitrogen protection, zirconia balls were used (ball-to-material ratio 10:1), the planetary ball mill was rotated at 300 rpm, and the ball milling time was 2 hours.

[0042] The morphology and performance of the high-entropy gamma-ray shielding filler prepared in the above examples were characterized.

[0043] (1) Morphology analysis The shielding filler obtained after ball milling was washed. As shown in FIG. 1, which is a SEM scanning electron microscope image of Example 4, it can be seen that the final filler particles are spherical and have a smooth surface. The size is between 20-50 μm. Figure 1 Compared with Figure 4 and Figure 6The images show SEM (Scanning Electron Microscopy) images of Examples 2 and 3. The same conclusions as in Example 4 can be drawn from these images. X-ray diffraction tests were performed on the shielding filler particles obtained in Example 4, and the results are as follows: Figure 8 This demonstrates its excellent crystallinity, further validating the successful preparation of a high-entropy alloy shielding filler. Further ball milling to smaller sizes is possible for applications in various scenarios.

[0044] (2) Shielding performance analysis Four portions of the sample prepared by ball milling in Example 4 were weighed and placed sequentially into plastic petri dishes and compacted. A high-purity germanium gamma-ray spectrometer was used to analyze the samples. 60 Its radiation shielding performance was tested under a Co radiation source. At 1.17 MeV, the relationship between its linear attenuation coefficient and thickness is as follows: Figure 2 As shown, the average value is 0.52 cm. -1 At 1.33 MeV, the relationship between its linear attenuation coefficient and thickness is as follows: Figure 3 As shown, the average value is 0.39 cm. -1 .

[0045] The same testing method was used on the samples prepared in Example 2 to obtain the relationship between their shielding efficiency and mass, as shown below. Figure 5 As shown, at 1.17 MeV, its shielding efficiency increases with increasing mass, and the shielding efficiency is 33.9% at 58.5g.

[0046] The same testing method was used on the samples prepared in Example 3 to obtain the relationship between their shielding efficiency and mass, as shown below. Figure 7 As shown, the shielding efficiency at 1.33 MeV follows the same trend as in Example 2, with a shielding efficiency of 33.1% at 59.1g.

[0047] In summary, the multilayer electrophoresis method employed in this invention achieves atomic-level mixing of different metal elements. The multilayer design enhances gamma-ray multiple scattering and absorption, thereby improving shielding efficiency. Compared to traditional methods, this approach simplifies the process, eliminating the need for high-temperature melting or complex pressing equipment, thus reducing energy consumption and costs. This invention provides an innovative solution for preparing high-performance gamma-ray shielding fillers.

[0048] The technical features in the above embodiments support arbitrary combinations. For the sake of brevity, not all possible combinations are described, but all non-conflicting combinations should be considered as covered by this specification.

[0049] The embodiments are only used for specifically and concretely showing several implementation manners of the application, facilitating understanding, and by no means limit the patent protection scope. For those skilled in the art, various modifications and improvements can be made without departing from the core idea of the application; any solution directly obtained based on the technical solution of the application through logical analysis, reasoning or limited experiment belongs to the protection scope of the application, and specifically falls into the protection scope of the appended claims. Finally, the protection scope of the patent of the application is subject to the content of the claims, and the description and drawings can be used as the interpretation basis of the claims.

Claims

1. A method for preparing high-entropy γ-ray shielding fillers based on multilayer electrophoresis, characterized in that: The method includes the following steps: Step 1: Dissolve various metal salts in deionized water in equimolar ratio, and stir to form a homogeneous solution; Step 2: Immerse the conductive substrate in a polyelectrolyte solution to make its surface negatively charged through adsorption. After drying, place it in the solution obtained in Step 1. Adjust the voltage, deposition time, and pH to allow metal ions to be electrophoretically deposited on the conductive substrate. After a certain deposition time, remove the substrate and repeat the process to form a multilayer structure. Step 3: After drying the deposited substrate, sinter it in a tube furnace under a hydrogen-argon mixed atmosphere to obtain high-entropy gamma-ray shielding particles. Step 4: Ball mill the high-entropy gamma-ray shielding particles under an inert atmosphere to obtain high-entropy gamma-ray shielding filler.

2. The method according to claim 1, characterized in that: In step one, the metal salt contains at least two of the following metal elements: Ta, W, Nb, Mo, V, Sn, Bi, Hf, Zr, Pb, and Gd, and the concentration of metal ions in the homogeneous solution formed is 0.05~0.3 mol / L.

3. The method according to claim 1, characterized in that: In step two, the conductive substrate is one of graphite sheet, copper mesh, stainless steel sheet, titanium sheet, metal foil or conductive ceramic, and the polyelectrolyte is sodium polystyrene sulfonate with a polyelectrolyte solution concentration of 0.5~2wt%.

4. The method according to claim 1, characterized in that: In step two, the immersion time of the conductive substrate is 10 to 60 minutes.

5. The method according to claim 1, characterized in that: In step two, the voltage is 1~20 V, the pH is 3~6, ​​the deposition time is 30~120 seconds, the substrate needs to be cleaned with deionized water and dried after each electrophoretic deposition, and the deposition is repeated ≥3 times.

6. The method according to claim 1, characterized in that: In step three, the volume fraction of hydrogen in the hydrogen-argon mixture is 5% to 15%.

7. The method according to claim 1, characterized in that: In step three, the sintering process adopts a stepped heating program: the temperature is increased to 300-400℃ at 5-10℃ / min for 1 hour of pretreatment, and then increased to 800-1200℃ at 3-10℃ / min for 1-5 hours.

8. The method according to claim 1, characterized in that: In step four, the inert atmosphere is nitrogen or argon.

9. The method according to claim 1, characterized in that: In step four, the ball milling speed is 200~500 rpm, the ball-to-material mass ratio is 10:1~20:1, and the ball milling time is 2~8 h.