Multi-metal zinc complex, preparation method and application in polymer depolymerization

By synthesizing a polymetallic zinc complex, the problems of low catalyst activity and low product selectivity in existing polymer chemical recycling technologies have been solved. This enables efficient and low-dosage catalysis of the depolymerization of various polymers, and is applicable to polymer substrates with different structures. It has broad applicability and excellent industrial application prospects.

CN121202897APending Publication Date: 2025-12-26DALIAN UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202511433652.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-09
Publication Date
2025-12-26

AI Technical Summary

Technical Problem

Existing polymer chemical recycling technologies suffer from low catalyst activity, low product selectivity, and the need for additional solvents, which severely restricts their large-scale application and commercial promotion.

Method used

We designed and synthesized multi-metal zinc complexes to achieve highly efficient catalysis of depolymerization reactions of various polymers by forming stable coordination bonds with the molecular backbone of organic ligands. The ligand framework is highly tunable and applicable to polymer substrates with different compositions and structures. The multi-metal synergistic catalysis mechanism significantly reduces the amount of catalyst required.

Benefits of technology

It can efficiently catalyze the depolymerization of various polymers in the range of 100~250 ℃, with a depolymerization reaction time of 0.5~24.0 h. It significantly suppresses side reactions, has wide applicability, and is suitable for bulk depolymerization and depolymerization under nucleophilic reagent conditions. It requires low catalyst dosage and is applicable to polymers with different molecular weight ranges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_5
    Figure SMS_5
  • Figure SMS_6
    Figure SMS_6
Patent Text Reader

Abstract

The invention relates to a multi-metal zinc complex, a preparation method and application in polymer depolymerization. The multi-metal zinc complex forms a stable coordinate bond with an organic ligand molecular skeleton, shows excellent chemical stability and substrate adaptability, and can efficiently catalyze the depolymerization reaction of various polymers in a temperature range of 100-250 DEG C. In addition, the ligand framework has adjustability, polymer substrates with different compositions and structures can be optimized, and high-yield recovery of various types of monomers is realized. The catalytic system has wide applicability, can catalyze the bulk depolymerization of the polymer, and also can catalyze the depolymerization in the presence of a nucleophilic reagent. Through a multi-metal concerted catalysis mechanism, the dosage of the catalyst is remarkably reduced, various polymers with the number-average molecular weight in the range of 3.8-807.5 kg / mol can be depolymerized, the depolymerization reaction time is 0.5-24.0 h, side reactions are remarkably inhibited, and excellent industrial application prospects are shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer materials, specifically relating to a class of multimetallic zinc complexes, their preparation methods, and their application in polymer depolymerization. Background Technology

[0002] Polymers play a crucial role in modern society. Their lightweight, low cost, and ease of large-scale production have led to their widespread application in daily life and industry, significantly benefiting socio-economic development. With the rapid development of the polymer market, a large amount of plastic waste has been generated, making polymer recycling and reuse technologies increasingly important. Among various recycling strategies, chemical recycling can convert waste polymers into virgin monomers, achieving a closed-loop cycle. This approach not only alleviates polymer pollution at its source but also reduces dependence on fossil fuels and lowers production costs. The organometallic sulfonic acid-based solid acid catalysts used in CN120268456A and CN118290750A can achieve targeted recycling of waste polymers. Although they can obtain the target monomers in high yields, the depolymerization process requires extremely high catalyst loading (20wt%~40wt%). CN120247864A and CN120247800A report a chiral aluminum catalyst that can achieve targeted depolymerization of L-polylactic acid and polycaprolactone. However, this type of polymer chemical recovery technology still faces many bottlenecks in practical applications, mainly including low catalyst activity (<1 h). -1 Problems such as low product selectivity (>51%) and the need for additional solvents severely restrict its large-scale application and commercialization. Therefore, developing efficient, highly tolerant, and universally applicable depolymerization catalysts is of great significance for promoting the transformation of polymers into a circular economy, addressing the numerous problems existing in polymer chemical recycling. Summary of the Invention

[0003] This invention addresses the shortcomings of current polymer chemical recovery technologies by designing and synthesizing a class of multi-metallic zinc complexes for polymer depolymerization. These complexes exhibit excellent chemical stability and substrate adaptability through stable coordination bonds with organic ligand molecular skeletons, enabling efficient catalysis of depolymerization reactions of various polymers within a temperature range of 100–250 °C. Furthermore, the ligand framework is tunable, allowing optimization for polymer substrates with different compositions and structures, achieving high-yield recovery of various monomer types. This catalytic system possesses broad applicability, capable of catalyzing both bulk and nucleophilic depolymerization. Through a multi-metal synergistic catalytic mechanism, the catalyst dosage is significantly reduced, and it can depolymerize various polymers with number-average molecular weights ranging from 3.8 to 807.5 kg / mol, with depolymerization reaction times ranging from 0.5 to 24.0 h. It also significantly suppresses side reactions, demonstrating excellent prospects for industrial applications.

[0004] The technical solution of the present invention:

[0005] A class of polymetallic zinc complexes, with the following structural formula:

[0006]

[0007] In the formula:

[0008] R 1 It can be H, OH, C1~C4 alkyl, cyano, nitro, C1~C4 alkoxy, F, Cl, Br, or I;

[0009] R 2 It can be H, OH, C1~C4 alkyl, cyano, nitro, C1~C4 alkoxy, F, Cl, Br, or I;

[0010] X is OH-, C1~C4 alkyl, C1~C4 alkoxy, F-, Cl-, Br-, I-, OTf-, OTs-, AcO-, NO3-, or CF3COO-;

[0011] a, b, and c are either 0 or 1;

[0012] n is a natural number.

[0013] A method for preparing a class of polymetallic zinc complexes, with the reaction equation as follows:

[0014] .

[0015] The specific preparation steps of the aforementioned multimetallic zinc complex are as follows:

[0016] Under the protection of an inert gas, sodium hydride and raw material 1 are thoroughly mixed at a molar ratio of 1:1000~2000 and added to a reaction vessel. Ethylene oxide at a molar ratio of 2~16:1 to raw material 1 is added at a uniform rate at 100~150 °C for 4~6 h. After the addition of ethylene oxide is complete, the mixture is aged for 5~30 min and cooled to room temperature to obtain intermediate 1. Under an inert gas atmosphere, intermediate 1 and pyridine were mixed in a molar ratio of 1:2.5–5. The mixture was dissolved in organic solvent 1 at a mass ratio of 5–10:1 to intermediate 1. At 25–50 °C, thionyl chloride at a molar ratio of 2.5–5:1 to intermediate 1 was added dropwise to the mixed solvent containing intermediate 1 over a period of 2–4 h. After the addition was complete, the reaction temperature was raised to 80–120 °C, and the reaction was allowed to proceed for another 8–12 h. After the reaction was complete, the mixture was cooled to room temperature, filtered, and the filtrate was collected. Organic solvent 1 and unreacted thionyl chloride and pyridine were removed by vacuum distillation to obtain intermediate 2. Intermediate 2 was then mixed with an ammonia solution at a molar ratio of 15–20:1. The reaction temperature was raised to 60–80 °C, and the reaction was allowed to proceed for another 12–24 h. After the reaction is complete, cool to room temperature, add sodium hydroxide to adjust the pH to 12-13, add organic solution 4 (mass ratio of 5-10:1 to intermediate 2) for extraction, dry the organic phase, and remove organic solution 4 by vacuum distillation to obtain a yellow oily liquid, which is intermediate 3. Under inert gas protection, mix raw material 2 and intermediate 3 in a molar ratio of 2.0-4.5:1, dissolve in organic solvent 2 (5-10 times the total mass of raw material 2 and intermediate 3), and react at 25-120 °C for 2-8 h. After the reaction is complete, cool to room temperature, remove excess organic solvent 2 by vacuum distillation to obtain a yellow oily liquid, and dry under vacuum to obtain a multi-metallic zinc ligand. Under inert gas protection, dissolve the multi-metallic zinc ligand in organic solvent 3 (mass ratio of 1:5-10), and add ZnX2 (molar ratio of 1:2-6 to the multi-metallic zinc ligand) at -20-25 °C, and react for 12-24 h. After the reaction was completed, the unreacted ZnX2 was removed by filtration. The mixture was kept at -20~0 ℃ for 12~24 h to precipitate a yellow precipitate. The precipitate was filtered, collected, and washed with organic solvent 5. After vacuum drying, the multi-metallic zinc complex was obtained.

[0017] The method of polymer depolymerization using polymetallic zinc complexes involves the following reaction process: adding polymetallic zinc complexes and polymers to a reactor, selectively adding nucleophiles, reacting for a certain time at depolymerization temperature and pressure, stopping the reaction, and obtaining depolymerized monomers by cooling crystallization or vacuum distillation.

[0018] Further, the polymer is polyethylene, polypropylene, polystyrene, nylon 6, L-type polylactic acid, polyglycolic acid, poly(lactic-glycolic acid), poly(ε-caprolactone), poly(ε-decanoic acid), poly(δ-valerolactone), poly(δ-hexanolactone), poly(butylene octyl lactone), poly(δ-nonanolactone), poly(ε-thiocaprolactone), poly(δ-thiovalerolactone), polytrimethylene carbonate, polycyclohexene carbonate, polytrimethylene trithiocarbonate, polyethylene terephthalate, polyethylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, or bisphenol A type polycarbonate, with the following specific structure:

[0019] .

[0020] Further, the depolymerization monomer is ethylene, propylene, styrene, ε-caprolactam, L-lactide, glycolide, methyl glycolide, ε-caprolactone, ε-decanolide, δ-valerolide, δ-hexanolactone, butyloctyl lactone, δ-nonanolide, ε-thiocaprolactone, δ-thiovalerolide, trimethylene carbonate, cyclohexene carbonate, trimethylene trithiocarbonate, terephthalic acid, dimethyl terephthalate, diethyl terephthalate, dipropyl terephthalate, dibutyl terephthalate, 2,6-naphthalenedicarboxylic acid, dimethyl 2,6-naphthalenedicarboxylic acid, diethyl 2,6-naphthalenedicarboxylic acid, or bisphenol A, with the specific structure as follows:

[0021] .

[0022] Furthermore, the molar ratio of zinc to polymer repeating units in the polymetallic zinc complex is 1:500~80000.

[0023] Furthermore, the depolymerization temperature is 100~250 ℃.

[0024] Furthermore, the depolymerization pressure is 0.05~101 kPa.

[0025] Furthermore, the depolymerization reaction lasts for 0.2 to 24 hours.

[0026] Furthermore, the number-average molecular weight of the polymer ranges from 3.8 to 807.5 kg / mol.

[0027] Furthermore, the nucleophile is one of water, methanol, ethanol, n-propanol, isopropanol, n-butanol, tert-butanol, ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, ammonia, methylamine, dimethylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, tert-butylamine, and ethylenediamine.

[0028] Furthermore, the molar ratio of the nucleophile to the polymer repeating unit is 5~50:1.

[0029] Further, the organic solvent 1 is one of toluene, N,N-dimethylformamide, dioxane, chloroform, and dichloromethane; the organic solvent 2 is one of methanol, ethanol, isopropanol, and tert-butanol; the organic solvent 3 is one of benzene, toluene, dichloromethane, tetrahydrofuran, n-hexane, and dioxane; the organic solvent 4 is one of dichloromethane, chloroform, tetrachloromethane, and 1,2-dichloroethane; and the organic solvent 5 is one of n-hexane, n-pentane, diethyl ether, methyl tert-butyl ether, and petroleum ether.

[0030] The beneficial effects of this invention:

[0031] (1) The multi-metallic zinc complex for polymer depolymerization described in this invention exhibits excellent chemical stability and substrate adaptability by forming stable coordination bonds with the organic ligand molecular backbone. It can efficiently catalyze the depolymerization reactions of various polymers in a temperature range of 100~250 °C. The ligand framework is tunable and can be optimized for polymer substrates with different compositions and structures to achieve high-yield recovery of various types of monomers.

[0032] (2) The multi-metallic zinc complex for polymer depolymerization described in this invention has wide applicability, capable of catalyzing both bulk and nucleophilic depolymerization. Through a multi-metal synergistic catalytic mechanism, it significantly reduces catalyst dosage and can depolymerize various polymers with number-average molecular weights ranging from 3.8 to 807.5 kg / mol. The depolymerization reaction time is only 0.5 to 24.0 h, and it significantly suppresses side reactions, demonstrating excellent prospects for industrial application. Detailed Implementation

[0033] The technical solution of the present invention is further illustrated below through specific embodiments. Unless otherwise explicitly stated, the terms used herein have the meanings commonly understood by those skilled in the art. In the following embodiments, all processes and operations not described in detail are conventional methods known in the art. Given the diversity of catalyst types and polymer structures, the present invention does not list all possible preparation methods, but rather selects representative embodiments to illustrate the specific implementation steps of the present invention.

[0034] Examples 1-3 are examples of methods for preparing polymetallic zinc complexes, Comparative Examples 1-1 are examples of methods for preparing bimetallic zinc complexes, and Comparative Examples 1-2 are examples of methods for preparing monometallic zinc complexes.

[0035] Examples 4-17 are examples of polymer depolymerization using the polymetallic zinc complexes of the present invention. The polymetallic zinc complex numbers, the depolymerized polymers, and the names of the recovered monomers are shown in the following formulas:

[0036]

[0037]

[0038] .

[0039] Example 1

[0040] The synthesis reaction equation for polymetallic zinc complex 1 is as follows:

[0041] .

[0042] The specific preparation steps of the multimetallic zinc complex 1 are as follows:

[0043] Using a 250 mL high-pressure reactor as the reaction vessel, sodium hydride (2.40 mg, 0.10 mmol) and raw material 1-1 (9.21 g, 100.00 mmol) at a molar ratio of 1:1000 were thoroughly mixed in a steel reactor within a glove box. The reactor was sealed, and ethylene oxide (25.20 g, 600.00 mmol) was added at a uniform rate at 130 °C over a period of 4 h. After the ethylene oxide was completely added, the mixture was aged for 10 min, cooled to room temperature, and the reactor was opened to obtain intermediate 1-1 with a yield of 100%. Under inert gas protection, intermediate 1-1 (35.64 g, 100.00 mmol) and pyridine (27.68 g, 350.00 mmol) at a molar ratio of 1:3.5 were mixed, and 1,4-dioxane (178.20 g) was added at a mass ratio of 5:1 to intermediate 1-1. g) Dissolve the mixture. At 50°C, add thionyl chloride (41.63 g, 350.00 mmol) in a molar ratio of 3.5:1 to intermediate 1-1 dropwise to the mixed solvent containing intermediate 1-1 over 2 h. After the addition is complete, raise the reaction temperature to 80°C and react for another 12 h. After the reaction is complete, cool to room temperature, filter, collect the filtrate, and remove 1,4-dioxane, unreacted thionyl chloride, and pyridine by vacuum distillation to obtain intermediate 1-2 (37.06 g, 90.00 mmol), with a yield of 90%. Mix intermediate 1-2 (37.06 g, 90.00 mmol) with an ammonia solution (25% by mass, 252.00 g, 1.80 mol) in a molar ratio of 20:1 to intermediate 1-2 and add to the reaction flask. Raise the reaction temperature to 70°C and react for 12 h. After the reaction was complete, the mixture was cooled to room temperature. Sodium hydroxide was added to the solution to adjust the pH to 12-13. Dichloromethane (370.00 g) at a mass ratio of 10:1 to intermediate 1-2 was added for extraction. The organic phase was dried, and the dichloromethane was removed by vacuum distillation to obtain a yellow oily liquid, which was intermediate 1-3 (23.22 g, 65.70 mmol), with a yield of 73%. Under inert gas protection, raw material 1-2 (37.65 g, 197.10 mmol) and intermediate 1-3 (23.22 g, 65.70 mmol) at a molar ratio of 3:1 were mixed and dissolved in anhydrous ethanol (304.00 g) at a mass ratio of 5 times the total mass of raw material 1-2 and intermediate 1-3. The reaction was carried out at 60 °C for 6 hours. After the reaction was completed, the mixture was cooled to room temperature, and excess ethanol was removed by vacuum distillation to obtain a yellow oily liquid. After vacuum drying, the polymetallic zinc 1 ligand (56.17 g, 64.39 mmol) was obtained, with a yield of 98%. Under the protection of an inert gas, the polymetallic zinc 1 ligand (34.90 g, 40.00 mmol) was reacted with tetrahydrofuran (174 mmol) at a mass ratio of 5:1.Dissolve 50 g of Zn(NO3)2·6H2O (47.60 g, 160.00 mmol) in water. At 25 °C, add Zn(NO3)2·6H2O (47.60 g, 160.00 mmol) in a 1:4 molar ratio with the polymetallic zinc ligand 1. React for 24 h. After the reaction is complete, filter to remove unreacted Zn(NO3)2·6H2O. Incubate at -20 °C for 24 h, and a yellow precipitate will form. Filter, collect the filter cake, and wash the cake with n-hexane (50 mL × 3). Dry under vacuum to obtain polymetallic zinc complex 1 (46.06 g, 36.80 mmol), with a yield of 92%. 1 H NMR (400MHz, CDCl3) δ8.13(s,3H),7.53(s,3H),7.48(s,3H),3.82(t,6H),3.70-3.48(m,23H).

[0044] Example 2

[0045] The synthesis reaction equation for polymetallic zinc complex 2 is as follows:

[0046] .

[0047] The specific preparation steps of the multimetallic zinc complex 2 are as follows:

[0048] Using a 250 mL high-pressure reactor as the reaction vessel, sodium hydride (1.20 mg, 0.05 mmol) and raw material 2-1 (10.61 g, 100.00 mmol) at a molar ratio of 1:2000 were thoroughly mixed in a steel reactor within a glove box. The reactor was sealed, and ethylene oxide (12.60 g, 300.00 mmol) was added at a uniform rate over a period of 4 h at 130 °C. After the ethylene oxide was completely added, the mixture was aged for 10 min, cooled to room temperature, and the reactor was opened to obtain intermediate 2-1 with a yield of 100%. Under inert gas protection, intermediate 2-1 (25.23 g, 100.00 mmol) and pyridine (27.68 g, 350.00 mmol) at a molar ratio of 1:3.5 were mixed, and 1,4-dioxane (126.15 g) was added at a mass ratio of 5:1 to intermediate 2-1. g) Dissolve the mixture. At 50°C, add thionyl chloride (41.63 g, 350.00 mmol) in a molar ratio of 3.5:1 to intermediate 2-1 dropwise to the mixed solvent containing intermediate 2-1 over 2 h. After the addition is complete, raise the reaction temperature to 80°C and react for another 12 h. After the reaction is complete, cool to room temperature, filter, collect the filtrate, and remove 1,4-dioxane, unreacted thionyl chloride, and pyridine by vacuum distillation to obtain intermediate 2-2 (28.61 g, 93.00 mmol), with a yield of 93%. Mix intermediate 2-2 (27.69 g, 90.00 mmol) with an ammonia solution (25% by mass, 252.00 g, 1.80 mol) in a molar ratio of 20:1 to intermediate 2-2 and add to the reaction flask. Raise the reaction temperature to 70°C and react for 12 h. After the reaction was complete, the mixture was cooled to room temperature. Sodium hydroxide was added to the solution to adjust the pH to 12-13. Dichloromethane (280.00 g) at a mass ratio of 10:1 to intermediate 2-2 was added for extraction. The organic phase was dried, and the dichloromethane was removed by vacuum distillation to obtain a yellow oily liquid, which was intermediate 2-3 (18.63 g, 74, 70 mmol), with a yield of 83%. Under inert gas protection, raw material 2-2 (38.23 g, 224.10 mmol) and intermediate 2-3 (18.63 g, 74, 70 mmol) at a molar ratio of 3:1 were mixed and dissolved in anhydrous ethanol (284.30 g) at 5 times the total mass of raw material 2-2 and intermediate 2-3. The reaction was carried out at 60 °C for 6 hours. After the reaction was completed, the mixture was cooled to room temperature, and excess ethanol was removed by vacuum distillation to obtain a yellow oily liquid. After vacuum drying, the polymetallic zinc 2-ligand (50.71 g, 71.71 mmol) was obtained, with a yield of 96%. Under the protection of an inert gas, the polymetallic zinc 2-ligand (28.28 g, 40.00 mmol) was reacted with tetrahydrofuran (141 mmol) at a mass ratio of 5:1.Dissolve 0.00 g of ZnCl2 and add it at 25 °C with a molar ratio of 1:4 to the polymetallic zinc 2 ligand (21.81 g, 160.00 mmol). React for 24 h. After the reaction is complete, filter to remove unreacted ZnCl2. Incubate at -20 °C for 24 h to precipitate a yellow precipitate. Filter, collect the filter cake, and wash the cake with n-hexane (50 mL × 3). Dry under vacuum to obtain polymetallic zinc complex 2 (38.65 g, 38.40 mmol), with a yield of 96%. 1 H NMR (400MHz, CDCl3) δ8.15(s,3H),7.50(s,3H),7.19(s,3H),3.87(t,6H),3.72(t,6H),3.64(s,6H),2.15(s,9H),1.03(s,3H).

[0049] Example 3

[0050] The synthesis reaction equation for polymetallic zinc complex 3 is as follows:

[0051] .

[0052] The specific preparation steps of the multimetallic zinc complex 3 are as follows:

[0053] Using a 250 mL high-pressure reactor as the reaction vessel, sodium hydride (2.40 mg, 0.05 mmol) and raw material 3-1 (13.62 g, 100.00 mmol) at a molar ratio of 1:1000 were thoroughly mixed in a steel reactor within a glove box. The reactor was sealed, and ethylene oxide (33.60 g, 800.00 mmol) was added at a uniform rate at 130 °C over a period of 4 h. After the ethylene oxide was completely added, the mixture was aged for 20 min, cooled to room temperature, and the reactor was opened to obtain intermediate 3-1 with a yield of 100%. Under inert gas protection, intermediate 3-1 (48.86 g, 100.00 mmol) and pyridine (35.49 g, 450.00 mmol) at a molar ratio of 1:4.5 were mixed with 1,4-dioxane (244.30 mg) at a mass ratio of 5:1 to intermediate 3-1. g) Dissolve the mixture. At 50 °C, add thionyl chloride (53.52 g, 450.00 mmol) in a molar ratio of 4.5:1 to intermediate 3-1 dropwise to the mixed solvent containing intermediate 3-1 over 2 h. After the addition is complete, raise the reaction temperature to 80 °C and react for another 12 h. After the reaction is complete, cool to room temperature, filter, collect the filtrate, and remove 1,4-dioxane, unreacted thionyl chloride, and pyridine by vacuum distillation to obtain intermediate 3-2 (50.61 g, 90.00 mmol), with a yield of 90%. Mix intermediate 3-2 (50.61 g, 90.00 mmol) with an ammonia solution (25% by mass, 1.80 mol) in a molar ratio of 20:1 to intermediate 3-2 and add to the reaction flask. Raise the reaction temperature to 70 °C and react for 12 h. After the reaction was complete, the mixture was cooled to room temperature. Sodium hydroxide was added to the solution to adjust the pH to 12-13. Dichloromethane (506.10 g) at a mass ratio of 10:1 to intermediate 3-2 was added for extraction. The organic phase was dried, and dichloromethane was removed by vacuum distillation to obtain a yellow oily liquid, which was intermediate 3-3 (31.84 g, 65.70 mmol), with a yield of 73%. Under inert gas protection, the starting material 3-2 (50.20 g, 262.80 mmol) and intermediate 3-3 (31.84 g, 65.70 mmol) at a molar ratio of 4:1 were mixed and dissolved in anhydrous ethanol (410.20 g), which was 5 times the total mass of the starting material 3-2 and intermediate 3-3. The mixture was reacted at 60 °C for 6 h. After the reaction was complete, the mixture was cooled to room temperature, and excess ethanol was removed by vacuum distillation to obtain a yellow oily liquid. After vacuum drying, the polymetallic zinc 3-ligand (75.76 g) was obtained. The yield was 98%; under the protection of an inert gas, the polymetallic zinc 3-ligand (47.06 g, 40 mmol) was prepared.0.00 mmol) was dissolved in tetrahydrofuran (235.30 g) at a mass ratio of 5:1. At 25 °C, Zn(NO3)2·6H2O (59.50 g, 200.00 mmol) with a molar ratio of 1:5 to the polymetallic zinc 3 ligand was added. The reaction was allowed to proceed for 24 h. After the reaction was complete, unreacted Zn(NO3)2·6H2O was removed by filtration. The mixture was then kept at -20 °C for 24 h, resulting in a yellow precipitate. This precipitate was filtered, and the filter cake was collected and washed with n-hexane (50 mL × 3). After vacuum drying, polymetallic zinc complex 3 (61.90 g, 36.80 mmol) was obtained, with a yield of 92%. 1 H NMR (400MHz, CDCl3) δ8.13 (s, 4H), 7.53 (s, 4H), 7.48 (s, 4H), 3.82 (t, 8H), 3.70-3.48 (m, 32H).

[0054] Comparative Example 1-1

[0055] The synthesis reaction equation for bimetallic zinc complex 4 is as follows:

[0056] .

[0057] The specific preparation steps for bimetallic zinc complex 4 are as follows:

[0058] Under an inert gas atmosphere, starting material 4-1 (19.01 g, 100.00 mmol) and starting material 4-2 (7.41 g, 50.00 mmol) in a molar ratio of 2:1 were mixed and dissolved in ethanol (132.00 g) at approximately 5 times the total mass of starting materials 4-1 and 4-2. The mixture was reacted at 60 °C for 5 h. After the reaction was completed, the mixture was cooled to room temperature, and excess ethanol was removed by vacuum distillation to obtain a yellow solid. After vacuum drying, the bimetallic zinc 4-ligand (24.21 g, 49.00 mmol) was obtained, with a yield of 98%. Under an inert gas atmosphere, the bimetallic zinc 4-ligand (19.77 g, 40.00 mmol) was dissolved in tetrahydrofuran (100.00 g) at a mass ratio of 1:5 and reacted at 25 °C. Under conditions of ℃, Zn(NO3)2·6H2O (28.56 g, 96.00 mmol) with a molar ratio of 1:2.4 to the bimetallic zinc 4 ligand was added, and the reaction was carried out for 18 h. After the reaction was completed, the unreacted Zn(NO3)2·6H2O was removed by filtration, and the mixture was kept at -20 ℃ for 24 h, resulting in the precipitation of a yellow precipitate. The precipitate was filtered, collected, and washed with n-hexane (30 mL × 3). After vacuum drying, the bimetallic zinc complex 4 (27.49 g, 36.80 mmol) was obtained, with a yield of 92%. 1H NMR (400MHz, CDCl3) δ8.10(s,2H),7.43(s,2H),7.04(s,2H),3.95(t,4H),3.72(t,4H),3.57(t,4H).

[0059] Comparative Examples 1-2

[0060] The synthesis reaction equation for monometallic zinc complex 5 is as follows:

[0061]

[0062] The specific preparation steps for monometallic zinc complex 5 are as follows:

[0063] Under an inert gas atmosphere, starting material 5-1 (9.55 g, 50.00 mmol) and starting material 5-2 (3.76 g, 50.00 mmol) in a molar ratio of 1:1 were mixed and dissolved in ethanol (66.00 g), which was approximately 5 times the total mass of starting materials 5-1 and 5-2. The mixture was reacted at 60 °C for 5 h. After the reaction was completed, the mixture was cooled to room temperature, and excess ethanol was removed by vacuum distillation to obtain a yellow solid. After vacuum drying, a monometallic zinc 5-ligand (12.16 g, 49.00 mmol) was obtained, with a yield of 98%. Under an inert gas atmosphere, the monometallic zinc 5-ligand (9.92 g, 40.00 mmol) was dissolved in tetrahydrofuran (50.00 g) in a mass ratio of 1:5. The mixture was then dissolved at 25 °C in Zn(NO3)2·6H2O (14.28 g) in a molar ratio of 1:1.2 to the monometallic zinc 5-ligand. The reaction was carried out for 18 h. After the reaction was completed, the unreacted Zn(NO3)2·6H2O was removed by filtration. The mixture was kept at -20 ℃ for 24 h, and a yellow precipitate was formed. The precipitate was filtered, the filter cake was collected, and the filter cake was washed with n-hexane (30 mL × 3). After vacuum drying, the monometallic zinc complex 5 (13.48 g, 36.00 mmol) was obtained, with a yield of 90%. 1 H NMR (400MHz, CDCl3) δ8.10(s,1H),7.93(s,1H),7.47(s,1H),3.53(t,2H),3.35(t,2H),3.23(s,3H).

[0064] Example 4

[0065] A 100 mL reaction flask equipped with a magnetic stirrup was dried overnight at 130 °C, evacuated, and purged with nitrogen three times. Under nitrogen protection, a certain amount of polyzinc complex 1 (166.87 mg, 0.13 mmol) was weighed at 25 °C and added to L-type polylactic acid (MnO2) with a polymer repeating unit to polyzinc complex 1 molar ratio of 1500:1.n =177.4 kg / mol, 14.40 g, 200.00 mmol), the reaction flask was placed in an oil bath at 180 °C. After the polymer was completely melted, the vacuum degree of the system was set to 80 Pa. After reacting for 13 h, the reaction was stopped and cooled to room temperature. The L-lactide product obtained from the depolymerization of the polymer was collected, weighed, and the yield was calculated. The calculated yield of L-lactide was 99%. A very small portion of the depolymerization product was used for... 1 The results of ¹H NMR and gas chromatography showed that the selectivity of L-lactide in the depolymerization products was >99%. 1 H NMR (400MHz, CDCl3) δ5.03 (q, 2H), 1.68 (d, 6H).

[0066] Comparative Example 4-1

[0067] A 100 mL reaction flask equipped with a magnetic stirrup was dried overnight at 130 °C, evacuated, and purged with nitrogen three times. Under nitrogen protection, a certain amount of bimetallic zinc complex 4 (149.39 mg, 0.20 mmol) was weighed at 25 °C and added to L-type polylactic acid (MnO4) with a polymer repeating unit to bimetallic zinc complex 4 molar ratio of 1000:1. n =177.4 kg / mol, 14.40 g, 200.00 mmol), the reaction flask was placed in an oil bath at 180 °C. After the polymer was completely melted, the vacuum degree of the system was set to 80 Pa. After reacting for 13 h, the reaction was stopped and cooled to room temperature. The L-lactide product obtained from the depolymerization of the polymer was collected, weighed, and the yield was calculated. The calculated yield of L-lactide was 53%. A very small portion of the depolymerization product was used for... 1 The results of ¹H NMR and gas chromatography showed that the selectivity for L-lactide in the depolymerization products was 95%. 1 H NMR (400MHz, CDCl3) δ5.03 (q, 2H), 1.68 (d, 6H).

[0068] The experimental procedures for Examples 5 to 10 in Table 1 are the same as those for Example 4, except that the experimental conditions are: polymer structure, number-average molecular weight, structure and amount of the multimetallic zinc complex, temperature, time, depolymerization monomer structure, or depolymerization monomer yield and selectivity. The experimental procedures for the comparative examples are the same as those for Comparative Example 4-1, except that the experimental conditions are: polymer structure, number-average molecular weight, structure and amount of the zinc complex, temperature, time, depolymerization monomer structure, or depolymerization monomer yield and selectivity. Details are as follows:

[0069] Table 1. Test results of zinc complex catalyzing the depolymerization of different polymers.

[0070]

[0071] The catalyst numbers in the table are the numbers of the final products in the examples and comparative examples, respectively. Referring to Table 1, the multi-metallic zinc complex catalyst of this invention exhibits excellent catalytic activity and reaction selectivity at low concentrations, and is applicable to polymer raw materials with different molecular weight ranges and chemical structures; while using bimetallic zinc complexes or monometallic zinc complexes requires higher catalyst loadings to achieve similar depolymerization performance. The multi-metallic zinc complex developed in this invention can significantly reduce catalyst loading through a multi-metallic synergistic catalytic mechanism while maintaining excellent catalytic performance.

[0072] Example 11

[0073] A 100 mL reaction flask equipped with a magnetic stir bar was dried overnight at 130 °C, evacuated, and purged with nitrogen three times. Under nitrogen protection, a certain amount of polymetallic zinc complex 2 (26.47 mg, 0.03 mmol) was weighed at 25 °C and added to polyethylene terephthalate (M) with a polymer repeating unit to polymetallic zinc complex 2 molar ratio of 15000:1. n = 23.4 kg / mol, 76.80 g, 400.00 mmol), methanol was used as the nucleophile, and the molar ratio of methanol to polyethylene terephthalate repeating units was 20:1. The reaction flask was placed in an oil bath at 150 °C and reacted at atmospheric pressure for 6 h. The reaction was then stopped, and the mixture was filtered while hot. The filtrate was cooled to room temperature, filtered again, and the filter cake was collected. The filter cake was washed with cold methanol (50 mL × 3), and then dried under vacuum to obtain dimethyl terephthalate with a yield of 99% and a selectivity >99%. 1 H NMR (400MHz, TFA) δ 8.09 (s, 4H), 3.99 (s, 6H).

[0074] Comparative Example 11-1

[0075] A 100 mL reaction flask equipped with a magnetic stir bar was dried overnight at 130 °C, evacuated, and purged with nitrogen three times. Under nitrogen protection, a certain amount of monometallic zinc complex 5 (29.96 mg, 0.08 mmol) was weighed at 25 °C and added to polyethylene terephthalate (M...) at a molar ratio of polymer repeating unit to monometallic zinc complex 5 of 5000:1. n= 23.4 kg / mol, 76.80 g, 400.00 mmol), methanol was used as the nucleophile, and the molar ratio of methanol to polyethylene terephthalate repeating units was 20:1. The reaction flask was placed in an oil bath at 150 °C and reacted at atmospheric pressure for 6 h. The reaction was then stopped, and the mixture was filtered while hot. The filtrate was cooled to room temperature, filtered again, and the filter cake was collected. The filter cake was washed with cold methanol (50 mL × 3), and then dried under vacuum to obtain dimethyl terephthalate with a yield of 55% and a selectivity of 88%. 1 H NMR (400MHz, TFA) δ 8.09 (s, 4H), 3.99 (s, 6H).

[0076] The experimental procedures for Examples 12 to 17 in Table 2 are the same as those for Example 11, except that the experimental conditions are: polymer structure, number-average molecular weight, structure and amount of the multimetallic zinc complex, molar ratio of the nucleophile to the repeating unit of the polymer, temperature, time, depolymerization monomer structure, or depolymerization monomer yield and selectivity. The experimental procedures for the comparative examples are the same as those for Comparative Example 11-1, except that the experimental conditions are: polymer structure, number-average molecular weight, structure and amount of the zinc complex, molar ratio of the nucleophile to the repeating unit of the polymer, temperature, time, depolymerization monomer structure, or depolymerization monomer yield and selectivity. Specifically:

[0077] Table 2. Test results of zinc complex catalyzing the depolymerization of different polymers.

[0078]

[0079] The catalyst numbers in the table are the numbers of the final products in the examples and comparative examples, respectively. Referring to Table 2, the multi-metallic zinc complex catalyst of this invention exhibits excellent catalytic activity and reaction selectivity at low concentrations, and is applicable to polymer raw materials with different molecular weight ranges and chemical structures; while using bimetallic zinc complexes or monometallic zinc complexes requires higher catalyst loadings to achieve the same depolymerization performance. The multi-metallic zinc complex developed in this invention can significantly reduce catalyst loading through a multi-metallic synergistic catalytic mechanism while maintaining excellent catalytic performance.

Claims

1. A class of polymetallic zinc complexes, characterized in that, Its structural formula is as follows: ; In the formula: R 1 It can be H, OH, C1~C4 alkyl, cyano, nitro, C1~C4 alkoxy, F, Cl, Br, or I; R 2 It can be H, OH, C1~C4 alkyl, cyano, nitro, C1~C4 alkoxy, F, Cl, Br, or I; X is OH-, C1~C4 alkyl, C1~C4 alkoxy, F-, Cl-, Br-, I-, OTf-, OTs-, AcO-, NO3-, or CF3COO-; a, b, and c are either 0 or 1; n is a natural number.

2. The method for preparing a type of polymetallic zinc complex according to claim 1, characterized in that, The reaction equation is: ; The specific preparation steps of the aforementioned multimetallic zinc complex are as follows: Under an inert gas atmosphere, sodium hydride at a molar ratio of 1:1000-2000 and raw material 1 are thoroughly mixed and added to a reaction vessel. Ethylene oxide at a molar ratio of 2-16:1 to raw material 1 is added uniformly at 100-150 °C over a period of 4-6 h. After the ethylene oxide is added, the mixture is aged for 5-30 min and cooled to room temperature to obtain intermediate 1. Under an inert gas atmosphere, intermediate 1 at a molar ratio of 1:2.5-5 and pyridine are mixed and dissolved in organic solvent 1 at a mass ratio of 5-10:1 to intermediate 1. At 25-50 °C, thionyl chloride at a molar ratio of 2.5-5:1 to intermediate 1 is added dropwise to the mixed solvent containing intermediate 1 over a period of 2-4 h. After the addition is complete, the reaction temperature is raised to 80-120 °C, and the reaction is allowed to proceed for 8-12 hours. After the reaction is complete, cool to room temperature, filter, collect the filtrate, and remove organic solvent 1 and unreacted thionyl chloride and pyridine by vacuum distillation to obtain intermediate 2. Mix intermediate 2 with an ammonia solution at a molar ratio of 15-20:1, raise the reaction temperature to 60-80 °C, and react for 12-24 h. After the reaction is complete, cool to room temperature, add sodium hydroxide to adjust the pH to 12-13, add organic solution 4 at a mass ratio of 5-10:1 to intermediate 2 for extraction, dry the organic phase, and remove organic solution 4 by vacuum distillation to obtain a yellow oily liquid, which is intermediate 3. Mix raw material 2 and intermediate 3 at a molar ratio of 2.0-4.5:1 under an inert gas atmosphere, dissolve in organic solvent 2 at a mass ratio of 5-10 times the total mass of raw material 2 and intermediate 3, and react for 2-8 h at 25-120 °C. After the reaction was completed, the mixture was cooled to room temperature and the excess organic solvent 2 was removed by vacuum distillation to obtain a yellow oily liquid. After vacuum drying, the polymetallic zinc ligand was obtained. Under the protection of an inert gas, the polymetallic zinc ligand was dissolved in an organic solvent 3 with a mass ratio of 1:5 to 10. ZnX2 with a molar ratio of 1:2 to 6 to the polymetallic zinc ligand was added at -20 to 25 °C, and the reaction was carried out for 12 to 24 h. After the reaction was completed, the unreacted ZnX2 was removed by filtration, and the mixture was kept at -20 to 0 °C for 12 to 24 h to precipitate a yellow precipitate. The precipitate was filtered, collected, and washed with organic solvent 5. After vacuum drying, the polymetallic zinc complex was obtained.

3. The method for preparing a type of polymetallic zinc complex according to claim 2, characterized in that, The organic solvent 1 is one of toluene, N,N-dimethylformamide, dioxane, chloroform, and dichloromethane; the organic solvent 2 is one of methanol, ethanol, isopropanol, and tert-butanol; the organic solvent 3 is one of benzene, toluene, dichloromethane, tetrahydrofuran, n-hexane, and dioxane; the organic solvent 4 is one of dichloromethane, trichloromethane, tetrachloromethane, and 1,2-dichloroethane; and the organic solvent 5 is one of n-hexane, n-pentane, diethyl ether, methyl tert-butyl ether, and petroleum ether.

4. The application of the polymetallic zinc complex according to claim 1, or the polymetallic zinc complex prepared by any of the preparation methods according to claims 1-2, in polymer depolymerization, characterized in that, The process is as follows: a polymetallic zinc complex and a polymer are added to a reactor, a nucleophile is selectively added, the reaction is carried out at the depolymerization temperature and pressure for a certain time, the reaction is stopped, and the depolymerized monomer is obtained by cooling crystallization or vacuum distillation.

5. The application according to claim 4, characterized in that, The polymers mentioned are polyethylene, polypropylene, polystyrene, nylon 6, L-type polylactic acid, polyglycolic acid, poly(lactic-glycolic acid), poly(ε-caprolactone), poly(ε-decanoic acid), poly(δ-valerolactone), poly(δ-hexanolactone), poly(butylene octyl lactone), poly(δ-nonanolactone), poly(ε-thiocaprolactone), poly(δ-thiovalerolactone), polytrimethylene carbonate, polycyclohexene carbonate, polytrimethylene trithiocarbonate, polyethylene terephthalate, polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, propylene naphthalate, or bisphenol A polycarbonate, with the specific structures as follows: 。 6. The application according to claim 4, characterized in that, The depolymerization monomers are ethylene, propylene, styrene, ε-caprolactam, L-lactide, glycolide, methyl glycolide, ε-caprolactone, ε-decanolide, δ-valerolide, δ-hexanolactone, butyloctyl lactone, δ-nonanolide, ε-thiocaprolactone, δ-thiovalerolide, trimethylene carbonate, cyclohexene carbonate, trimethylene trithiocarbonate, terephthalic acid, dimethyl terephthalate, diethyl terephthalate, dipropyl terephthalate, dibutyl terephthalate, 2,6-naphthalenedicarboxylic acid, dimethyl 2,6-naphthalenedicarboxylic acid, diethyl 2,6-naphthalenedicarboxylic acid, or bisphenol A, with the specific structures as follows: 。 7. The application according to claim 4, characterized in that, The molar ratio of zinc to polymer repeating units in the polymetallic zinc complex is 1:500~80000; the molar ratio of nucleophile to polymer repeating units is 5~50:

1.

8. The application according to claim 4, characterized in that, The depolymerization temperature is 100~250 ℃; the depolymerization pressure is 0.05~101 kPa; and the depolymerization reaction time is 0.2~24 h.

9. The application according to claim 4, characterized in that, The number-average molecular weight of the polymer ranges from 3.8 to 807.5 kg / mol.

10. The application according to claim 4, characterized in that, The nucleophile is one of water, methanol, ethanol, n-propanol, isopropanol, n-butanol, tert-butanol, ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, ammonia, methylamine, dimethylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, tert-butylamine, and ethylenediamine.

Citation Information

Patent Citations

  • Sulfonic acid-based solid acid for catalyzing nylon 6 depolymerization recovery and preparation method of sulfonic acid-based solid acid

    CN118290750A

  • Method for directionally depolymerizing polycaprolactone into caprolactone monomer

    CN120247800A

  • Method for selectively depolymerizing polylactic acid to chiral lactide

    CN120247864A

  • Metal organic sulfonic acid-based solid acid catalyst applied to nylon 6 recovery and depolymerization and preparation method of metal organic sulfonic acid-based solid acid catalyst